A special release agent for polyester injection-molded transparent parts and preparation method thereof

By using a combination of specific proportions of solvent oil, methylene chloride, long carbon chain alkyl modified silicone oil and dimethyl silicone oil, a special release agent is prepared, which solves the problem of product whitening, fogging, and fogging during the polyester injection molding process. Strain and other problems improve the flatness and efficiency of the product.

CN115416191BActive Publication Date: 2024-10-11LUZHOU QIANQIU DAILY CHEM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210901224.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-07-28
Publication Date
2024-10-11
Estimated Expiration
2042-07-28

AI Technical Summary

Technical Problem

Existing general-purpose release agents cause problems such as product whitening, fogging, and strain during the polyester injection molding process, reducing product quality.

Method used

Use a combination of 75-80 parts No. 6 solvent oil, 5-10 parts No. 120 solvent oil, 3-5 parts methylene chloride, 3-5 parts long carbon chain alkyl modified silicone oil and 2-3 parts dimethyl silicone oil. As a special release agent, it is prepared through thorough mixing and stirring followed by filtration and defoaming to prepare a release agent with fine texture and moderate evaporation speed.

Benefits of technology

It improves the surface flatness and smoothness of injection molded products, reduces burns and oil marks on products, reduces the frequency of mold wiping, and improves injection molding efficiency and product quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003770952180000061
    Figure BDA0003770952180000061
  • Figure BDA0003770952180000071
    Figure BDA0003770952180000071
Patent Text Reader

Abstract

The invention discloses a special demoulding agent for polyester injection-molded transparent parts and a preparation method thereof, and relates to the technical field of polyester injection molding process; the demoulding agent comprises the following components in parts by weight: 70-82 parts of No. 6 solvent oil, 3-15 parts of No. 120 solvent oil, 2-8 parts of dichloromethane, 2-8 parts of long carbon chain alkyl modified silicone oil and 1-5 parts of dimethyl silicone oil; during preparation, the No. 6 solvent oil, No. 120 solvent oil and dichloromethane are fully mixed, and then the long carbon chain alkyl modified silicone oil and dimethyl silicone oil are added, and after fully stirring, the special demoulding agent for polyester injection-molded transparent parts is filtered and defoamed to obtain the special demoulding agent; the demoulding agent is specially used in polyester injection molding process, can effectively prevent polyester injection molding products from whitening, material, pulling, pitting and the like, and greatly improves the quality of injection molding products; and at the same time, the demoulding agent can greatly reduce the frequency of mold wiping, and effectively improves the preparation efficiency of injection molding products.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polyester injection molding technology, in particular to a special mold release agent for polyester injection-molded transparent parts and a preparation method thereof. Background Art

[0002] Polyester is a general term for thermoplastic linear saturated polyester represented by polyethylene terephthalate (PET). One of its important uses is in the packaging field. When polyester is used in the packaging field, it can not only be made into biaxially stretched packaging molds and stretch blow-molded bottles, but also can be made into highly transparent and high-strength packaging containers through injection molding processes; such as transparent wine packaging boxes, transparent cosmetic packaging boxes, etc. These transparent packaging containers have attracted the public's attention due to their transparent materials and simple appearance, especially their hard texture, which can protect the products inside to the greatest extent, and are well received by the public.

[0003] In order to meet the increasing demand of the market, the number of highly transparent and high-strength products made of polyester through injection molding has increased significantly; the preparation process of these highly transparent and high-strength products is generally as follows: first melt the polyester, then inject the molten polyester into the product mold using pressure, and cool and mold to obtain the desired various injection molded parts; during the injection molding process, in order to facilitate product demolding, a release agent is often required, and the release agent in the prior art is often a universal release agent, which can be applied to injection molding and demolding of various materials. However, for each individual material, the demolding effect is not optimal. During the production process, it is often found that the obtained products appear whitish, foggy, and have scratches, which greatly reduces the product quality. Summary of the invention

[0004] In view of the deficiencies in the prior art, the purpose of the present invention is to provide a special release agent for polyester injection molded transparent parts and a preparation method thereof. The release agent is specially used in polyester injection molding process, can prevent polyester injection molded transparent parts from turning white, causing material damage, and tearing, thereby further improving the quality of polyester injection molded products.

[0005] The present invention is achieved through the following technical solutions:

[0006] A special demoulding agent for polyester injection-molded transparent parts comprises the following components in parts by weight: 75-80 parts of No. 6 solvent oil, 5-10 parts of No. 120 solvent oil, 3-5 parts of dichloromethane, 3-5 parts of long carbon chain alkyl modified silicone oil and 2-3 parts of dimethyl silicone oil.

[0007] As some possible implementation methods of the present application, the special release agent includes the following components in parts by weight: 76-78 parts of No. 6 solvent oil, 7-9 parts of No. 120 solvent oil, 3.8-4.5 parts of dichloromethane, 3.5-4.5 parts of long chain alkyl modified silicone oil and 2.2-2.8 parts of dimethyl silicone oil.

[0008] As some possible implementation modes of the present application, the model of the dimethyl silicone oil is 350CS.

[0009] As some possible implementation modes of the present application, the number of carbon atoms in the long-chain alkyl-modified silicone oil is 14.

[0010] As some possible implementation methods of the present application, the special release agent also includes 0.01-0.02 parts of fragrance.

[0011] As some possible implementation modes of the present application, the special release agent also includes 0.01-0.02 parts of a defoaming agent.

[0012] In addition, to achieve the above-mentioned purpose, the present application also provides a method for preparing a special mold release agent for the polyester injection molded transparent parts as described above, firstly, the No. 6 solvent oil, No. 120 solvent oil and dichloromethane are fully mixed, and then long-chain alkyl modified silicone oil and dimethyl silicone oil are added, and after sufficient stirring, the mixture is filtered and defoamed to obtain the special mold release agent for the polyester injection molded transparent parts.

[0013] As some possible implementation methods of the present application, the pore size of the filter during filtration is greater than 400 mesh.

[0014] As some possible implementation methods of the present application, during stirring, first stir at a stirring speed of 150-800 rpm for 2-3 min, and then stir at a stirring speed of 1-150 rpm for 2-3 min.

[0015] The beneficial effects of the present invention are:

[0016] Compared with the general release agent in the prior art, the release agent in the present invention is specifically used for polyester injection molding process, and has at least the following advantages in polyester injection molding process:

[0017] ① The release agent has a fine texture, can evenly cover the mold, will not drip, and can improve the surface flatness of the injection molded product; ② The obtained injection molded product has high smoothness, is easy to take out from the mold, and does not stick to the mold; ③ The obtained injection molded product will not turn white, fog, have surface scratches, burns, or pitting; ④ The release agent evaporates quickly, which can reduce the contact time with the injection molded product and avoid leaving oil marks and oil scars on the surface of the injection molded product; compared with the release agent in the prior art, the release agent evaporates more slowly and stays on the mold for a relatively long time, which can effectively reduce the mold temperature, thereby effectively avoiding product burns and improving product quality; ⑤ When the release agent is used, the mold wiping frequency of the mold is greatly reduced, and the mold wiping cycle is greatly extended, that is, in the injection molding process, the number and time of mold wiping are reduced, which can reduce injection molding scrap and manpower, and greatly improve the injection molding efficiency and the number of injection molded products. DETAILED DESCRIPTION

[0018] The technical solutions in the embodiments of the present application are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present application.

[0019] At present, in the process of preparing high-transparency and high-strength transparent parts by polyester injection molding, the release agent used is a universal release agent, which has a wide range of applications and can be widely used in the fields of automotive parts, glass products, rubber shoes production, etc. However, in the process of any of the above-mentioned fields, the demoulding effect is not optimal, especially in the polyester injection molding process. After using the universal release agent, the prepared products often appear whitish, foggy, scratched, and pitted on the surface, which greatly reduces the product quality.

[0020] Based on this, the present invention provides a special mold release agent for polyester injection-molded transparent parts, comprising the following components in parts by weight: 75-80 parts of No. 6 solvent oil, 5-10 parts of No. 120 solvent oil, 3-5 parts of dichloromethane, 3-5 parts of long carbon chain alkyl modified silicone oil and 2-3 parts of dimethyl silicone oil.

[0021] The present invention prepares a release agent by mixing No. 6 solvent oil, No. 120 solvent oil, dichloromethane, dimethyl silicone oil and modified long-chain alkyl silicone oil in a certain proportion, and the release agent is specially used in a polyester injection molding process; the release agent is a low-viscosity, highly transparent liquid with a fine texture, can evenly cover the mold, and does not cause dripping, thereby effectively improving the surface flatness of the injection-molded product; after the injection molding process is completed, the product is extremely easy to be taken out of the mold without sticking to the mold, and the product has high smoothness, does not cause whitening, material fogging, surface scratches, and pitting, and the solvent oil in the release agent can evaporate quickly, and can avoid leaving oil marks and oil scars on the surface of the product, and has no effect on secondary processing processes such as hot stamping, silk screen printing, and thermal transfer printing of the product; in addition, compared with the prior art, the release agent has a relatively long residence time on the mold, can effectively reduce the mold temperature, thereby preventing product scalding, effectively avoiding product scalding, and improving product quality.

[0022] The modified long-chain alkyl silicone oil in the present invention has good foaming performance, which can improve the mixing efficiency and lubricating properties between the raw materials, make the demoulding agent more stable, improve the demoulding effect and the ease of mold opening, effectively avoid product damage, and ensure that the product can be smoothly processed by hot stamping, silk screen printing, thermal transfer and other secondary processing; dimethyl silicone oil can reduce the viscosity of the demoulding agent, make it more dispersed when sprayed, improve the demoulding uniformity, avoid product sticking to the mold, make the product easy to open the mold, and have a large lubricating effect, avoid product damage, whitening, fogging and shrinkage; and it has defoaming properties, and can effectively reduce the defoaming time after the raw materials are fully mixed, and improve the clarity and transparency of the product. The present invention does not need to add an additional defoaming agent; dichloromethane can greatly improve the smoothness and transparency of the product; the evaporation speed of No. 6 solvent oil is too fast. If only it and dichloromethane are selected as solvents, the residence time of it and dichloromethane on the mold is short, and it evaporates almost quickly, resulting in The distance between the product and the mold is short, which leads to product burns, such as whitening, material fogging, etc.; the evaporation rate of No. 120 solvent oil is slow. If only it and dichloromethane are selected as solvent oil, the residence time of it and dichloromethane on the mold is too long, which can easily lead to oil scars on the product and affect the product quality; by configuring No. 6 solvent oil and No. 120 solvent oil together in a certain proportion, an ideal evaporation rate can be obtained, which effectively overcomes the above-mentioned defects of the product and greatly improves the quality of the product; in addition, after configuring the above 6 raw materials together, in addition to greatly improving the product quality, it is found that it can greatly reduce the frequency of mold wiping. According to actual production data, when using the release agent of the present invention, the injection 427-611 mold is only wiped once, while the commercially available release agent needs to wipe the mold once for injection 236 molds, which effectively reduces the frequency of mold wiping and greatly improves the product preparation efficiency.

[0023] In order to improve the demolding effect of the special demolding agent for the polyester injection molded transparent parts, as some feasible embodiments of the present application, the amount of each component of the special demolding agent for the polyester injection molded transparent parts is further limited, that is, the special demolding agent for the polyester injection molded transparent parts includes the following components in parts by weight: 76-78 parts of No. 6 solvent oil, 7-9 parts of No. 120 solvent oil, 3.8-4.5 parts of dichloromethane, 3.5-4.5 parts of long carbon chain alkyl modified silicone oil and 2.2-2.8 parts of dimethyl silicone oil.

[0024] In order to improve the demoulding effect of the special demoulding agent for the polyester injection-molded transparent parts, as some feasible embodiments of the present application, the model of the dimethyl silicone oil in the special demoulding agent for the polyester injection-molded transparent parts is further limited, that is, the model of the dimethyl silicone oil is 350CS.

[0025] The types of dimethyl silicone oil are divided into very fine categories, including ultra-low viscosity dimethyl silicone oil, low viscosity, medium viscosity, high viscosity, etc., and low viscosity dimethyl silicone oil includes multiple models, such as 350 viscosity, 500 viscosity and 1000 viscosity, etc., and the viscosity of each model is different. At present, the viscosity of 1000 is preferred in this field, and the viscosity initially selected by the present invention is also 1000 viscosity. However, during actual injection molding, it is found that the product will have a mold sticking phenomenon, which leads to surface unevenness, scratches, etc. After several experiments, it is found that the selection of 350CS dimethyl silicone oil can effectively overcome the above defects, while the effects of other models of dimethyl silicone oil are poor after testing.

[0026] In order to reduce the frequency of wiping the mold when using the special mold release agent for polyester injection-molded transparent parts, as some feasible implementation methods of the present application, the number of carbon atoms in the long-chain alkyl-modified silicone oil in the special mold release agent for polyester injection-molded transparent parts is further limited, that is, the number of carbon atoms in the long-chain alkyl-modified silicone oil is 14.

[0027] In order to suppress the severe odor of the special mold release agent for polyester injection molded transparent parts during use and improve the aroma of the product, as some feasible implementation methods of the present application, the special mold release agent for polyester injection molded transparent parts also includes 0.01-0.02 parts of flavor. Fragrances are well known to people in the field of flavors, and lemon flavor etc. can be selected. Flavors can be freely selected during actual production.

[0028] The demoulding effect of the release agent is not only related to the raw materials, but also to its preparation method. The preparation method can determine the quality of the release agent and the demoulding effect.

[0029] Based on this, in order to achieve the above-mentioned purpose, the present invention also provides a method for preparing the special mold release agent for the polyester injection molded transparent parts as described above, that is, firstly fully mixing the No. 6 solvent oil, No. 120 solvent oil and dichloromethane, then adding long carbon chain alkyl modified silicone oil and dimethyl silicone oil, stirring thoroughly and filtering and defoaming to obtain the special mold release agent for the polyester injection molded transparent parts.

[0030] The preparation method of the invention is simple, does not require large-scale equipment for operation, and takes a short time, thereby improving the production efficiency of the special release agent for polyester injection-molded transparent parts; it has low cost and high output, and is conducive to commercial promotion.

[0031] In order to improve the product quality and demolding effect of the special demolding agent for polyester injection-molded transparent parts, as some feasible embodiments of the present application, the mesh size of the filter screen in the preparation process of the special demolding agent for polyester injection-molded transparent parts is further limited, that is, the pore size of the filter screen during filtration is greater than 400 mesh.

[0032] In order to improve the product quality and demolding effect of the special mold release agent for polyester injection molded transparent parts, as some feasible embodiments of the present application, the stirring speed in the preparation process of the special mold release agent for polyester injection molded transparent parts is further limited, that is, when stirring, first stir at a stirring speed of 150-800 rpm for 2-3 minutes, and then stir at a stirring speed of 1-150 rpm for 2-3 minutes.

[0033] In actual implementation, the use of segmented stirring can improve the mixing efficiency of the release agent and reduce the volatilization of the solvent. If the speed is higher than 800 rpm, the volatilization rate of the solvent will be accelerated, resulting in the loss of the release agent. At the same time, when a large amount of solvent is lost, the injection molded product is very likely to be scalded during the injection molding process. If the stirring speed is too slow, the stirring cloth is uneven and the stirring time needs to be extended. When the time is too long, the solvent oil will gradually evaporate, resulting in the loss of the release agent and reducing the quality of the injection molded product.

[0034] The preparation of the pharmaceutical composition described in the present application is further described in detail below in conjunction with specific implementation methods; it is worth noting that: the various raw materials in the examples are commercially available products.

[0035] Example 1

[0036] Take 70 parts of No. 6 solvent oil, 4 parts of No. 120 solvent oil and 7 parts of dichloromethane and add the three parts into a reactor. After the three parts are fully mixed, add 3 parts of 14-carbon long-chain alkyl modified silicone oil and 5 parts of 350CS dimethyl silicone oil into the mixed reactor and stir them fully. When stirring, stir at a stirring speed of 300 rpm for 3 minutes, and then stir at a stirring speed of 150 rpm for 2 minutes. After the stirring is completed, the mixed solution is filtered through a 550-mesh filter and then allowed to stand for 1 minute to defoam, thereby obtaining the special release agent for the polyester injection-molded transparent parts.

[0037] Example 2

[0038] Take 80 parts of No. 6 solvent oil, 15 parts of No. 120 solvent oil and 2 parts of dichloromethane and add the three into a reactor. After the three are fully mixed, add 8 parts of 14-carbon long-chain alkyl modified silicone oil and 2 parts of 350CS dimethyl silicone oil into the mixed reactor and stir them fully. When stirring, stir at a stirring speed of 800 rpm for 2 minutes, and then stir at a stirring speed of 100 rpm for 2.5 minutes. After the stirring is completed, the mixed solution is filtered through a 400-mesh filter and then allowed to stand for 1 minute to defoam, thereby obtaining the special release agent for the polyester injection-molded transparent parts.

[0039] Example 3

[0040] Take 75 parts of No. 6 solvent oil, 8 parts of No. 120 solvent oil and 3 parts of dichloromethane and add the three into a reactor. After the three are fully mixed, add 5 parts of 14-carbon long-chain alkyl modified silicone oil and 2.5 parts of 350CS dimethyl silicone oil into the mixed reactor and stir them fully. Stir at a stirring speed of 150 rpm for 3 minutes and then stir at a stirring speed of 50 rpm for 3 minutes. After the stirring is completed, the mixed solution is filtered through a 600-mesh filter and then allowed to stand for 1 minute to defoam, thereby obtaining the special release agent for the polyester injection-molded transparent parts.

[0041] Example 4

[0042] Take 78 parts of No. 6 solvent oil, 9 parts of No. 120 solvent oil and 3.8 parts of dichloromethane and add the three into a reactor. After the three are fully mixed, add 4.5 parts of 14-carbon long-chain alkyl modified silicone oil and 2.8 parts of 350CS dimethyl silicone oil into the mixed reactor and stir them fully. Stir at a stirring speed of 500 rpm for 2.5 minutes and then stir at a stirring speed of 100 rpm for 2.5 minutes. After the stirring is completed, the mixed solution is filtered through a 500-mesh filter and then allowed to stand for 1 minute to defoam, thereby obtaining the special release agent for the polyester injection-molded transparent part.

[0043] Example 5

[0044] Take 78 parts of No. 6 solvent oil, 9 parts of No. 120 solvent oil and 3.8 parts of dichloromethane and add the three into a reactor. After the three are fully mixed, add 4.5 parts of 14-carbon long-chain alkyl modified silicone oil, 2.8 parts of 350CS dimethyl silicone oil and 0.01 parts of lemon essence into the mixed reactor, and stir them fully. When stirring, stir at a stirring speed of 500 rpm for 2.5 minutes, and then stir at a stirring speed of 100 rpm for 2.5 minutes. After the stirring is completed, the mixed solution is filtered through a 500-mesh filter and then allowed to stand for 1 minute to defoam, thereby obtaining the special release agent for the polyester injection-molded transparent parts.

[0045] Comparative Example 1

[0046] Compared with Example 4, 350CS of dimethyl silicone oil was replaced with 1000CS of dimethyl silicone oil, and the remaining parameters and steps were the same as those in Example 4.

[0047] Comparative Example 2

[0048] Compared with Example 4, 8 parts of No. 6 solvent oil and 9 parts of No. 120 solvent oil are replaced by 17 parts of No. 6 solvent oil, and the remaining parameters and steps are the same as those in Implementation 4.

[0049] Comparative Example 3

[0050] Compared with Example 4, 8 parts of No. 6 solvent oil and 9 parts of No. 120 solvent oil are replaced by 17 parts of No. 120 solvent oil, and the remaining parameters and steps are the same as those in Implementation 4.

[0051] Comparative Example 4

[0052] Compared with Example 4, the 300-mesh filter was replaced with a 600-mesh filter, and the other parameters and steps remained unchanged, all the same as in Example 4.

[0053] Comparative Example 5

[0054] Compared with Example 4, the stirring speed was changed to: stirring at a stirring speed of 1000 rpm for 2.5 min, and then stirring at a stirring speed of 500 rpm for 2.5 min. The remaining parameters and steps were the same as those in Example 4.

[0055] Comparative Example 6

[0056] Compared with Example 4, the amount of each raw material has changed. The changed raw material amount is: 80 parts of No. 6 solvent oil, 15 parts of No. 120 solvent oil, 1 part of dichloromethane, 1 part of 14-carbon long-chain alkyl modified silicone oil and 8 parts of dimethyl silicone oil; the remaining parameters and steps are the same as Implementation 4.

[0057] Comparative Example 7

[0058] Compared with Example 4, the 14-carbon long-chain alkyl-modified silicone oil is replaced with a 16-carbon long-chain alkyl-modified silicone oil; the remaining parameters and steps are the same as Example 4.

[0059] Comparative Example 8

[0060] Commercial release agent

[0061] Experimental example

[0062] The appearance of the release agents in the above-mentioned Examples 1-5 and Comparative Examples 1-8 was first observed, and then they were used in the injection molding process of the transparent wine packaging box.

[0063] How to use the release agent: Pour the release agent into a pressure tank, connect it to an air compressor, connect it to a manipulator or robot through a pipe, and then connect it to a nozzle with a nozzle diameter of 0.5-1.0. Adjust the time and position of the manipulator to spray the release agent from 0.5 seconds to 1.5 seconds, in the middle of the mold, with an interval of 10-25 cm. Adjust it according to each mold and spray once for each mold.

[0064] The appearance of the transparent wine packaging box after demolding and the frequency of mold wiping are shown in Table 1:

[0065] Table 1

[0066]

[0067]

[0068] According to Table 1, we can see that:

[0069] The surface of the product prepared by using the release agent in Examples 1-5 in the injection molding process of transparent wine packaging boxes is flat and smooth, without whitish, material fog, pitting, tearing, oil scar and scalding, which overcomes the defects of the general release agent in Comparative Example 8. At the same time, the mold wiping frequency in Examples 1-5 is low, and the 417-611 mold is only wiped once, and the mold wiping frequency is much lower than that in Comparative Example 8. In actual production, it can significantly improve the injection molding process and the preparation efficiency of transparent wine packaging boxes; specifically, the mold wiping frequency in Example 4 is the lowest, and a small amount of flavor is added in Example 5, which has almost no effect on the demoulding effect of the product. Therefore, the mold release agents in Examples 4 and 5 have the best effect; while the mold release agents in Comparative Examples 1-6 have poor demoulding effect in the injection molding process, and different problems will appear on the surface of the product after demoulding. Considering the industrial cost, the mold wiping frequency was not tested; specifically, the mold wiping frequency in Comparative Example 1 is The viscosity of the release agent is relatively large, and the product will be pulled during the demolding process, resulting in scratches on the product surface, affecting the product quality; the solvent in Comparative Example 2 evaporates quickly, resulting in close contact between the product and the mold, causing product scalding, whitening, and material fogging; the volumetric evaporation rate in Comparative Example 3 is slow, and the solvent is in contact with the product for a long time, resulting in oil scars on the product surface; the release agent in Comparative Example 4 is not fully filtered, resulting in impurities in the release agent, which in turn leads to pitting on the product surface; the stirring speed in Example 5 is too fast, resulting in product volatilization, which in turn leads to product scalding; the release agent in Comparative Example 6 does not adopt the dosage configuration of the present invention, and its demolding effect is extremely poor, even worse than that of commercially available release agents; Comparative Example 7 uses a long-chain alkyl modified silicone oil with a carbon content of 16, and the surface of the product molded therewith has no obvious defects, but the mold wiping frequency is high, which leads to reduced product production efficiency and more waste of finished products in the actual production process.

[0070] In summary, the demoulding agent in the present invention has a significant demoulding effect and can be widely used in various polyester injection molding processes.

[0071] Experimental Example 2

[0072] The release agent in Example 4 was used in the injection molding processes of automobile parts, glass products and rubber shoes, and it was found that its effects were worse than those of commercially available release agents, reflecting the specificity of the release agent in the present invention in polyester injection molding products.

[0073] The above are only preferred embodiments of the present invention. It should be understood that the present invention is not limited to the form disclosed herein, and should not be regarded as excluding other embodiments, but can be used in various other combinations, modifications and environments, and can be modified within the scope of the present invention through the above teachings or the technology or knowledge of the relevant field. The changes and modifications made by those skilled in the art do not depart from the spirit and scope of the present invention, and should be within the scope of protection of the claims attached to the present invention.

Claims

1. A special release agent for polyester injection molded transparent parts, It is characterized in that Comprising the following components in parts by weight, 70-82 parts No. 6 solvent oil, 3-15 parts No. 120 solvent oil, 2-8 parts of dichloromethane, 2-8 parts of long carbon chain alkyl modified silicone oil and 1-5 parts of dimethyl silicone oil; The model of the dimethyl silicone oil is 350CS; the number of carbon atoms in the long carbon chain alkyl modified silicone oil is 14.

2. A special release agent for polyester injection-molded transparent parts according to claim 1, It is characterized in that The invention comprises the following components in parts by weight: 75-80 parts of No. 6 solvent oil, 5-10 parts of No. 120 solvent oil, 3-5 parts of dichloromethane, 3-5 parts of long carbon chain alkyl modified silicone oil and 2-3 parts of dimethyl silicone oil.

3. A special release agent for polyester injection-molded transparent parts according to claim 1, It is characterized in that The invention comprises the following components in parts by weight: 78 parts of No. 6 solvent oil, 9 parts of No. 120 solvent oil, 3.8 parts of dichloromethane, 4.5 parts of long carbon chain alkyl modified silicone oil and 2.8 parts of dimethyl silicone oil.

4. A special release agent for polyester injection-molded transparent parts according to claim 1, It is characterized in that Also includes 0.01-0.02 parts of flavor.

5. A method for preparing a special release agent for polyester injection-molded transparent parts according to any one of claims 1 to 3, Features: First, the No. 6 solvent oil, No. 120 solvent oil and dichloromethane are fully mixed, and then long-chain alkyl modified silicone oil and dimethyl silicone oil are added, and after fully stirring, the mixture is filtered and defoamed to obtain the special release agent.

6. The method for preparing a special release agent for polyester injection-molded transparent parts according to claim 5, Features: The filter hole diameter during filtration is greater than 400 mesh.

7. The method for preparing a special release agent for polyester injection-molded transparent parts according to claim 5, Features: When stirring, first stir at a stirring speed of 150-800 rpm for 2-3 min, and then stir at a stirring speed of 1-150 rpm for 2-3 min.