Electrode active material for electrochemical element and method for producing the same, electrode material for electrochemical element, electrode for electrochemical element, electrochemical element and mobile body

By using the oxide of specific structure AyM1αAlx-αNb12-x-zM2zO29-δ as electrode active substances in a nonaqueous electrolyte secondary battery, the problem of load characteristics and charge and discharge cycle characteristics is solved, and high energy density and long life are achieved. Electrochemical components.

CN115428191BActive Publication Date: 2024-11-01MAXELL LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202180029604.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-10-16
Filing Date
2021-09-17
Publication Date
2024-11-01
Estimated Expiration
2041-09-17

AI Technical Summary

Technical Problem

There are difficulties in existing non-aqueous electrolyte secondary batteries when taking into account both the load characteristics and the charge and discharge cycle characteristics, especially the theoretical capacity of the negative electrode active substance is small, which makes it difficult to meet the needs of high energy density and long life.

Method used

The oxide of specific structure AyM1αAlx-αNb12-x-zM2zO29-δ is used as the electrode active substance, and its characteristics are improved by the sintering process in a carbon container. A is Li and Na, M1 is certain metal elements, and M2 is others. The metal element is replaced by the element M1 to increase the lattice constant, and improve the load characteristics and charge and discharge cycle characteristics.

Benefits of technology

It achieves the balance between load characteristics and charge and discharge cycle characteristics, improves the energy density of electrochemical components and the stability of electrodes, and extends the service life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115428191B_ABST
    Figure CN115428191B_ABST
Patent Text Reader

Abstract

The present invention provides an electrochemical element having excellent load characteristics and charge-discharge cycle characteristics, an electrode active material that can constitute the above electrochemical element, a method for producing the same, an electrode material and an electrode, and a mobile body having the above electrochemical element. The electrode active material for the electrochemical element of the present invention is characterized in that it has a monoclinic crystal structure and contains an oxide that satisfies the following general formula (1). A y M 1 α Al x‑α Nb 12‑x‑z M 2 z O 29‑δ (1) In the above general formula (1), A is at least one element selected from Li and Na, and M 1 is at least one element selected from the group consisting of Fe, Mn, Zn, Cu, Ag, Mg, Ca, Sr, Ba, Co, Eu, Y, Bi, La, Ce, Nd, Sm and Gd, M 2 For a specific element, 0
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an electrochemical element having excellent load characteristics and charge-discharge cycle characteristics, an electrode active material that can constitute the electrochemical element, a method for producing the same, an electrode material and an electrode, and a mobile body having the electrochemical element. Background Art

[0002] As a type of electrochemical element, non-aqueous electrolyte secondary batteries are used as power sources for portable electronic devices such as mobile phones and notebook personal computers, electric vehicles, etc. However, as they become smaller and more functional, non-aqueous electrolyte secondary batteries are also required to be smaller, lighter, and have higher capacity and energy density.

[0003] In current non-aqueous electrolyte secondary batteries, generally, a lithium-containing composite oxide is used as a positive electrode active material, and graphite or the like is used as a negative electrode active material.

[0004] In addition, in order to construct a battery that can be charged and discharged at a large current without causing an internal short circuit caused by lithium precipitation in the negative electrode, attempts have been made to use spinel lithium titanate (Li4Ti5O 12 However, the theoretical capacity of lithium titanate (175 mAh / g (600 mAh / cm 3 )) than the theoretical capacity of graphite (372mAh / g (830mAh / cm 3 ))Small, there is a problem at this point.

[0005] Therefore, in recent years, TiNb2O7 and Ti2Nb have been studied as negative electrode active materials with larger capacity than lithium titanate. 10 O 29 、AlNb 11 O 29 、Zn2Nb 34 O 87 , Cu 0.02 Ti 0.94 Nb 2.04 Application of oxides of niobium and other metals such as O7 (Patent Documents 1 to 5, Non-Patent Documents 1 to 4, etc.).

[0006] Prior art literature

[0007] Patent Literature

[0008] Patent Document 1: Japanese Patent Application Publication No. 2018-160365

[0009] Patent Document 2: Japanese Patent Application Publication No. 2019-53945

[0010] Patent Document 3: Japanese Patent Application Publication No. 2019-160729

[0011] Patent Document 4: Japanese Patent Application Publication No. 2021-82420

[0012] Patent Document 5: International Publication No. 2021 / 074592

[0013] Non-patent literature

[0014] Non-patent document 1: Electrochemistry Communications, 2012, Vol. 25, pp. 39-42

[0015] Non-patent document 2: ACS Applied Material Interfaces, 2019, Vol. 11, pp. 6086-6096

[0016] Non-patent document 3: Journal of Materials Chemistry A, 2019, Vol. 7, pp. 25537-25547

[0017] Non-patent document 4: Journal of Power Sources, 2016, Vol. 328, pp. 336-344 Summary of the invention

[0018] Problems to be solved by the invention

[0019] However, non-aqueous electrolyte secondary batteries are also required to have improved load characteristics and charge-discharge cycle characteristics. However, when materials such as those disclosed in Patent Documents 1 to 5 and Non-Patent Documents 1 to 4 are used as active materials, it is difficult to achieve both load characteristics and charge-discharge cycle characteristics.

[0020] The present invention is completed in view of the above situation, and its purpose is to provide an electrochemical element with excellent load characteristics and charge-discharge cycle characteristics, an electrode active material that can constitute the above electrochemical element, a manufacturing method thereof, an electrode material and an electrode, and a mobile body having the above electrochemical element.

[0021] Methods for solving problems

[0022] The electrode active material for an electrochemical device of the present invention is characterized by having a monoclinic crystal structure and being an oxide satisfying the following general formula (1).

[0023] A y M 1 α Al x-α Nb 12-x-z M 2z O 29-δ (1)

[0024] In the above general formula (1), A is at least one element selected from Li and Na, and M 1 is at least one element selected from the group consisting of Fe, Mn, Zn, Cu, Ag, Mg, Ca, Sr, Ba, Co, Eu, Y, Bi, La, Ce, Nd, Sm and Gd, M 2 is at least one element selected from the group consisting of K, Ti, Ni, Zr, V, Mo, Ta and W, <x≤1.1,0≤y≤24,0≤z≤2,-1≤δ≤2,0<α≤0.4x。

[0025] Furthermore, the electrode material for an electrochemical device of the present invention is characterized by containing the electrode active substance for an electrochemical device of the present invention.

[0026] Furthermore, the electrode for an electrochemical device of the present invention is characterized by containing the electrode active material for an electrochemical device of the present invention, or containing the electrode material for an electrochemical device of the present invention.

[0027] Furthermore, the electrochemical device of the present invention is characterized by comprising a positive electrode and a negative electrode, and either the positive electrode or the negative electrode is the electrode for the electrochemical device of the present invention.

[0028] Furthermore, a mobile object of the present invention is characterized by comprising the electrochemical element of the present invention.

[0029] The electrode active material for an electrochemical device of the present invention can be produced through a step of calcining the oxide represented by the general formula (1) or a precursor thereof in a carbon container under a vacuum atmosphere, thereby further improving its characteristics.

[0030] Effects of the Invention

[0031] According to the present invention, it is possible to provide an electrochemical element having excellent load characteristics and charge-discharge cycle characteristics, an electrode active material that can constitute the electrochemical element, a method for producing the same, an electrode material and an electrode, and a mobile object having the electrochemical element. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 This is a cross-sectional view schematically showing an example of an electrochemical device according to an embodiment of the present invention.

[0033] Figure 2 This is a plan view schematically showing another example of the electrochemical device according to one embodiment of the present invention.

[0034] Figure 3 yes Figure 2 II line cross-sectional view. DETAILED DESCRIPTION

[0035] Hereinafter, the present invention will be described based on embodiments.

[0036] <Electrode active material for electrochemical device>

[0037] The electrode active material for an electrochemical device (hereinafter, sometimes simply referred to as “active material”) of the present embodiment has a monoclinic crystal structure and is an oxide satisfying the following general formula (1).

[0038] A y M 1 α Al x-α Nb 12-x-z M 2 z O 29-δ (1)

[0039] In the above general formula (1), A is at least one element selected from Li and Na, and M 1 is at least one element selected from the group consisting of Fe, Mn, Zn, Cu, Ag, Mg, Ca, Sr, Ba, Co, Eu, Y, Bi, La, Ce, Nd, Sm and Gd, M 2 is at least one element selected from the group consisting of K, Ti, Ni, Zr, V, Mo, Ta and W, <x≤1.1,0≤y≤24,0≤z≤2,-1≤δ≤2,0<α≤0.4x。

[0040] As element M 1 Fe(Fe 2+ )、Mn(Mn 2+ )、Zn(Zn 2+ )、Cu(Cu + , Cu 2+ )、Ag(Ag + ), Mg(Mg 2+ ), Ca(Ca 2+ )、Sr(Sr 2+ )、Ba(Ba 2+ )、Co(Co 2+ )、Eu(Eu 2+ 、Eu 3+ )、Y(Y 3+ )、Bi(Bi 3+ )、La(La 3+ )、Ce(Ce 3+ 、Ce 4 + )、Nd(Nd 3+ )、Sm(Sm 3+ ) and Gd(Gd3+ ) has an effective ionic radius larger than that of Nb(Nb 5+ )、Al(Al 3+ ) is large. Therefore, the oxide represented by the general formula (1) is AlNb 11 O 29 Based on, part of Al is replaced by element M 1 Replacement, thereby with AlNb 11 O 29 In contrast, the lattice constant of the crystal becomes larger, and the diffusivity of the element A ions inside increases. Therefore, in the electrochemical device formed using the active material of this embodiment, its load characteristics are improved.

[0041] It should be noted that in AlNb 11 O 29 In the present invention, Al has the function of stabilizing the crystal structure, and it is also believed that by replacing part of it with element M 1 The substitution impairs the stability of the crystal structure of the oxide, and thus, in an electrochemical device composed of the oxide as an active material, it is expected that the capacity will be more likely to decrease (the charge-discharge cycle characteristics will be reduced) during repeated charge and discharge.

[0042] However, contrary to such prediction, as shown in the above general formula (1), if the element M 1 When the amount of substituted Al is within a certain range, the electrochemical element using the oxide as the active material is more effective than that using AlNb 11 O 29 Compared with the case of Nb, the capacity reduction during repeated charge and discharge can be well suppressed. It is speculated that the reason is that by containing an ion radius larger than Nb (Nb 5+ )、Al(Al 3+ ) Large element M 1 Therefore, in the stage before the insertion of the element A ions that serve as the carrier, the lattice constant of the above-mentioned oxide becomes larger, and the space for absorbing the element A ions is expanded, thereby suppressing the volume change of the oxide (active material) during the insertion and release of the element A ions accompanying charging and discharging. Therefore, even if the electrochemical element is repeatedly charged and discharged, the degradation of the electrode can be suppressed.

[0043] As described above, according to the active material of this embodiment, it is possible to achieve both improvement in the load characteristics of the electrochemical device and maintenance of high charge and discharge cycle characteristics.

[0044] In the oxide represented by the above general formula (1), the element M 1 , may contain only one element selected from Fe, Mn, Zn, Cu, Ag, Mg, Ca, Sr, Ba, Co, Eu, Y, Bi, La, Ce, Nd, Sm and Gd, or may contain two or more elements.1 Among them, Al is particularly easily substituted from the perspective of electron configuration. Furthermore, Fe, Mn, Zn, and Cu are preferred, and Zn and Cu are more preferred because they have a high effect of improving the electron conductivity of the above oxides.

[0045] It should be noted that the oxide represented by the above general formula (1) contains, for example, Fe 3+ / Fe 2+ , Cu 2+ / Cu + Elements with mixed valences are used as element M 1 In the case of , a large amount of oxygen deficiency is sometimes generated (i.e., in the above general formula (1), δ is greater than 0), thereby further improving the electronic conductivity and ion conductivity of the oxide represented by the above general formula (1). Therefore, when the oxide represented by the above general formula (1) contains Fe and Cu as the element M, it can be expected that the load characteristics of the electrochemical device will be further improved.

[0046] In addition, in the oxide represented by the above general formula (1), except for the element M which replaces a part of Al 1 In addition, at least one element M selected from the group consisting of K, Ti, Ni, Zr, V, Mo, Ta and W may be contained. 2 These elements M 2 In the oxide represented by the general formula (1) having a monoclinic crystal structure, Nb is substituted without replacing a part of Al constituting the crystal, or a component is contained as a solid solution or impurity in the crystal. The oxide represented by the general formula (1) may not contain the element M 2 , the amount z can be 0, but in the presence of element M 2 In the case of , if the amount z is 2 or less, it does not affect the performance of the active material of this embodiment and is therefore permissible. In addition, the oxide represented by the above general formula (1) may contain water.

[0047] In the oxide represented by the general formula (1), Al is a component for improving the structural stability of the oxide. The action of Al improves the reversibility of the active material during charge and discharge of the electrochemical device.

[0048] In the oxide represented by the general formula (1), as described above, part of Al is replaced by the element M. 1 Replacement, but the amount of Al is related to the element M 1 The total amount x is greater than 0, so that Al and element M can be better utilized. 1 From the viewpoint of the above-mentioned effects, it is preferably 0.8 or more. 1If the amount of Al is too much, the amount of Nb in the above oxide becomes too small and may not play its role well. Therefore, the amount of Al is related to the element M. 1 The total amount x of is 1.1 or less, preferably 1.05 or less.

[0049] In the oxide represented by the above general formula (1), the element M 1 The amount α is greater than 0, and is preferably greater than 0.05 from the viewpoint of better ensuring the effect of improving the load characteristics of the electrochemical device. 1 If the amount of M is too large, the stability of the crystal structure decreases, and the charge-discharge cycle characteristics of the electrochemical device may not be maintained at a high level. Therefore, from the perspective of improving the charge-discharge cycle characteristics of the electrochemical device, in the oxide represented by the general formula (1), the element M 1 The amount α is 0.4x or less, more specifically, preferably 0.44 or less, and more preferably 0.4 or less.

[0050] In the oxide represented by the general formula (1), element A is at least one of Li and Na, and is absorbed by the oxide or released from the oxide (i.e., functions as a carrier) by the charge and discharge of the electrochemical element. The oxide may or may not contain element A. In the case of the oxide not containing element A, for example, by charging the electrochemical element used as a negative electrode active material or pre-doping of ions of element A before use in the electrochemical element, ions of element A are inserted and element A is contained.

[0051] The amount y of the element A in the oxide represented by the above general formula (1) is 0 or more and 24 or less.

[0052] In the oxide represented by the general formula (1), the amount of oxygen is originally equal to that of AlNb 11 O 29 The same is 29, but sometimes due to the element M 1 Specifically, in the general formula (1), δ is greater than -1 and less than 2, preferably less than 1.95. When δ in the general formula (1) is greater than 0, oxygen deficiency occurs in the oxide, but in this case, the electronic conductivity of the active material containing the oxide and the conductivity of the element A ion are improved, so by using such an active material, the energy density of the electrochemical element can be further improved.

[0053] In the oxide represented by the above general formula (1), the amount of oxygen δ is determined by the element M forming the cation. 1 Element M 2 , Nb and Al and the amount of oxygen that forms anions.

[0054] Among the active materials of the present embodiment, one of more preferred aspects is an active material containing a substance satisfying the following general formula (2) as the oxide represented by the above general formula (1).

[0055] M 1 α Al 1-1.5α Nb 11+0.5α O 29-δ (2)

[0056] The element M in the above general formula (2) 1 is at least one of Zn and Cu, 0<α≤0.4, 0≤δ≤0.5α. Moreover, the element M in the above general formula (2) 1 The amount α is preferably greater than or equal to 0.05, preferably less than or equal to 0.4, and more preferably less than or equal to 0.35. In the above general formula (2), δ about the amount of oxygen is greater than or equal to 0 and less than or equal to 0.5α, but as described above, since 0<α≤0.4, the value of δ is greater than or equal to 0 and less than or equal to 0.2.

[0057] The oxide represented by the above general formula (1) and satisfying the above general formula (2) satisfies, for example, the following general formula (3) by insertion of Li ions.

[0058] Li y M 1 α Al 1-1.5α Nb 11+0.5α O 29-δ (3)

[0059] In the above general formula (3), the element M 1 , the amount α and the amount δ of oxygen are the same as those in the above general formula (2), 0 <y≤22。

[0060] The active material of this embodiment is preferably a material obtained by reducing the oxide represented by the general formula (1). In general, in the above oxide, Nb is usually pentavalent (Nb 5+ ), but by reducing the tetravalent Nb (Nb 4+ ) are mixed. 4+ The ionic radius is larger than that of Nb 5+ Therefore, the presence of tetravalent Nb in the oxide increases the lattice size of the oxide having a monoclinic crystal structure. In addition, the oxide represented by the general formula (1) contains not only the element M 1, and oxygen deficiency is also generated by the reduction treatment (as a result, the value of δ in the above general formula (1) becomes larger). In the active material containing the oxide subjected to the reduction treatment, the action brought about by the increase in the above lattice size and the action brought about by the oxygen deficiency function synergistically, and the electronic conductivity and the diffusibility of element A ions are further improved. Accordingly, by using the active material containing the oxide subjected to the reduction treatment, for example, the energy density of the electrochemical element can be further increased.

[0061] When the active material satisfies the following (a) or (b), it can be said that the oxide in the active material is reduced to such an extent that the electronic conductivity and the diffusibility of element A ions in the active material are further improved.

[0062] (a) The ratio Z (atomic %) of Nb in all Nb in the oxide represented by the above general formula (1) contained in the active material 4+ is 3.5 ≤ Z ≤ 30.

[0063] (b) In the active material containing the above oxide, when the absorbance at a wavelength of 500 nm is set as A1, the absorbance at a wavelength of 600 nm is set as A2, and the absorbance at a wavelength of 700 nm is set as A3, the relationship A1 < A2 is satisfied, and the relationship A3 < A2 is satisfied.

[0064] The active material containing the above oxide changes color from white to yellow and then to blue by performing the reduction treatment. Therefore, when the above (b) is satisfied, that is, when the relationship A1 < A2 and the relationship A3 < A2 are satisfied, it can be judged that for the above oxide in the active material, the oxide is reduced to such an extent that the electronic conductivity and the diffusibility of the active material are improved.

[0065] As a more specific embodiment of the above oxide subjected to the reduction treatment, for example, in the oxide represented by the above general formula (1), element M 1 is at least one element selected from the group consisting of Fe, Cu, and Zn and 0 < δ ≤ 2.

[0066] It should be noted that in the active material containing the above oxide subjected to the reduction treatment, on its surface and inside, the proportion of element M 1 is different, and there is a tendency for element M 1 to be concentrated on the surface portion. Specifically, in the active material, the atomic ratio P of element M 1 relative to Nb obtained by X-ray photoelectron spectroscopy (XPS) (when the number of Nb atoms is 100, element M 1The ratio of the number of atoms. The same also applies to the atomic ratio Q) and the element M determined by inductively coupled plasma atomic emission spectroscopy (ICP-AES) 1 The atomic ratio Q to Nb preferably satisfies the relationship of P>Q. In this case, the effect of improving the energy density of the electrochemical device is further improved.

[0067] In the active material of this embodiment, the ratio of the oxide having a monoclinic crystal structure and represented by the general formula (1) in the total amount of the active material is preferably 20 mass % or more, more preferably 50 mass % or more, and may be 100 mass %.

[0068] The output of the active material of this embodiment is excellent, so it is not easily affected by the polarization caused by the diffusion of Li ions inside the active material due to the increase in the particle size of the active material particles. For the same reason, the primary particles of the active material can form agglomerates (secondary particles) with each other. However, from the perspective of improving the load characteristics and charge and discharge cycle characteristics of the electrochemical element, in the case of secondary particles, it is preferred that the primary particles of the active material are sintered to each other, and more preferably primary particles.

[0069] <Method for producing active material for electrochemical device>

[0070] The method for producing the active material of this embodiment is not particularly limited. For example, Nb, Al, and element M 1 The niobium oxide can be manufactured by a solid phase reaction method in which the precursors of active materials such as various metal oxides (the oxide represented by the above general formula (1)) are mixed and calcined; or a reaction method in which a mixture of metal compounds prepared by coprecipitating chlorides, nitrates and alkoxides of various metals in a liquid phase is used as a precursor to synthesize niobium oxide (the oxide represented by the above general formula (1)).

[0071] In the solid phase reaction method, from the viewpoint of improving the mutual diffusion of various metal ions, it is preferred to calcine at a temperature above 800°C, and more preferably calcine in the range of 900°C to 1400°C. The calcination time is not particularly limited, and can be carried out under conditions of 1 to 1000 hours. When the calcination temperature exceeds 1200°C, oxygen is slowly released from the sample, thereby producing a crystalline phase other than the monoclinic crystalline phase, or the composition becomes inconsistent with the above general formula (1), so the time maintained above 1200°C is more preferably within 10 hours. Regarding the cooling rate of the sample during calcination, there is no particular limitation as long as a monoclinic crystalline phase can be obtained, but in order to obtain a monoclinic crystalline phase that is stable at high temperatures, the cooling rate is preferably 15°C / minute to 60°C / minute (also including natural cooling). It is also possible to perform a rapid cooling treatment in the range of a cooling rate of 1°C / second to 1000°C / second.

[0072] In addition, as a method of reduction treatment, the above precursor may be placed in a carbon container and calcined in a vacuum atmosphere. As conditions for calcination, the temperature is preferably 800° C. to 1200° C., and the time is preferably 1 to 1000 hours, for example.

[0073] It should be noted that the “vacuum atmosphere” mentioned in the present specification means that the pressure in the firing furnace is lower than low vacuum (100 Pa to 31 kPa) in ISO3529-1, and more preferably lower than medium vacuum (0.1 Pa to 100 Pa).

[0074] <Method for determining the composition of active material for electrochemical device>

[0075] The composition of the active material of the present embodiment can be analyzed using, for example, ICP-AES. In the case where it is difficult to quantify using the above-mentioned ICP-AES due to the sintering of the active material of the present embodiment with the oxide-based solid electrolyte and the difficulty in separating the components, the composition can also be determined by combining various elemental analysis methods such as energy dispersive X-ray spectrometer (EDS) and wavelength dispersive X-ray spectrometer (WDS) with a scanning electron microscope (SEM) or a transmission electron microscope (TEM).

[0076] The oxygen deficiency amount δ contained in the active material of the present embodiment is determined by the oxygen deficiency amount δ of the element M determined by ICP-AES analysis. 1 Element M 2 It is determined by the molar amount of oxygen determined by the sum of the molar amounts of Al and Nb using an oxygen and nitrogen analyzer (ON736, etc.) manufactured by LECO Japan Contract Co., Ltd.

[0077] The Nb molar amount relative to the total Nb in the active material of this embodiment is4+ The molar amount Z (%) was determined from the area ratio of the peak attributed to Nb3d5 / 2 in the XPS spectrum.

[0078] <Method for Confirming Monoclinic Crystal Structure of Active Material for Electrochemical Device>

[0079] The crystal structure of the active material of the present embodiment can be determined by measuring the powder X-ray diffraction (powder XRD) pattern using Rigaku RINT2500VPC (X-ray used: CuKα ray) and comparing it with the Powder Diffraction File (PDF) database, or by analyzing it using the Rietveld method. When comparing the lattice size between different samples, when preparing the sample for powder XRD measurement, Si powder (Rigaku, 298.1K) was mixed. ) was used as an internal reference, and the spectrum was corrected so that the peak of X-ray diffraction attributable to the (111) plane of Si was 2θ=28.442 degrees. The lattice constant (d 010 ) can be obtained by setting the wavelength of the X-rays to The surface spacing obtained from the peak of diffraction attributable to the (020) plane is multiplied by 2 and calculated. In the case where the negative electrode contains the active material of the present embodiment as the negative electrode active material, the negative electrode of the electrochemical element (battery, etc.) after connecting a 1kΩ resistor and performing a constant resistance discharge for 100 hours is taken out, and the surface opposite to the surface bonded to the collector of the above-mentioned electrode is flatly processed in a manner parallel to the collector, and then fixed to a sample stand for powder XRD, thereby obtaining a powder XRD pattern of the electrode. In the case where the positive electrode contains the active material of the present embodiment as the positive electrode active material, after a constant current charge of 10μA is performed under the condition of an upper limit voltage of 3V, the positive electrode of the electrochemical element (battery, etc.) after further being maintained at a constant voltage state of 3V for 100 hours is taken out, and in the same manner as the negative electrode, the surface opposite to the surface bonded to the collector of the above-mentioned electrode is flatly processed in a manner parallel to the collector, and then fixed to a sample stand for powder XRD, thereby obtaining a powder XRD pattern of the electrode.

[0080] In the case where the active material of the present embodiment has a form sintered with a crystalline sulfide-based solid electrolyte or an oxide-based solid electrolyte, a sample piece is taken out from a molded body of a sample containing the active material of the present embodiment using focused ion beam (FIB) processing, mounted on a TEM sample stage, and then thin-filmed to form a thin sheet with a thickness of less than 100 nm. The selected area electron diffraction (SAD) pattern is obtained using TEM and analyzed, thereby confirming the monoclinic structure.

[0081] <Method for measuring absorbance of active material for electrochemical device>

[0082] The absorbance of the active material of this embodiment is obtained by dispersing 5 mg of the active material in 20 ml of water using an ultrasonic disperser into a 1 cm square test tube and measuring the absorbance at wavelengths of 500 nm, 600 nm and 700 nm using a near infrared-visible spectrophotometer.

[0083] <Method for Determining P and Q in Electrochemical Device Active Material>

[0084] The above P is attributed to element M according to the XPS spectrum. 1 The above Q is the ratio of the peak area of ​​​​the element M obtained by ICP-AES to the peak area attributable to Nb. 1 The ratio of the molar amount of to the molar amount of Nb.

[0085] <Electrode Materials for Electrochemical Devices>

[0086] The electrode material for electrochemical element of the present embodiment (hereinafter, sometimes referred to as "electrode material") contains the electrode active material for electrochemical element of the above embodiment, and may contain other materials for constituting the electrode for electrochemical element together with the above active material. As such materials, conductive additives such as carbon black, adhesives, solid electrolytes, etc. can be cited, and the electrode material can contain one or more of them together with the active material of the above embodiment as needed.

[0087] The electrode material may be a material having other materials attached to the surface of the active material, or may be a mixture of the active material and other materials, as long as the active material and other materials are present.

[0088] When the electrode material contains carbon black, examples of the carbon black include thermal black, furnace black, channel black, Ketjen black, acetylene black, etc. When the electrode material contains carbon black, the content of the carbon black in the electrode material can be set to 0.1 to 25 parts by mass relative to 100 parts by mass of the active material of the above embodiment.

[0089] When the electrode material contains a binder, examples of the binder include fluororesins such as polyvinylidene fluoride (PVDF). When the electrode material contains a binder, the content of the binder in the electrode material can be, for example, 0.1 to 25 parts by mass relative to 100 parts by mass of the active material of the above embodiment.

[0090] In the case where the electrode material contains a solid electrolyte, the solid electrolyte is not particularly limited as long as it has Li ion conductivity. For example, sulfide-based solid electrolytes, hydride-based solid electrolytes, halide-based solid electrolytes, oxide-based solid electrolytes, etc. can be used.

[0091] As sulfide-based solid electrolytes, in addition to particles such as Li2S-P2S5, Li2S-SiS2, Li2S-P2S5-GeS2, Li2S-B2S3-based glasses, etc., thio-LISICON-type materials (Li 10 GeP2S 12 、Li 9.54 Si 1.74 P 1.44 S 11.7 Cl 0.3 and other Li 12-12a-b+c+6d-e M 1 3+a-b-c- d M 2 b M 3 c M 4 d M 5 12-e X e (where M 1 is Si, Ge or Sn, M 2 is P or V, M 3 is Al, Ga, Y or Sb, M 4 is Zn, Ca or Ba, M 5 is S, or any one of S and O, X is F, Cl, Br or I, 0 ≤ a < 3, 0 ≤ b + c + d ≤ 3, 0 ≤ e ≤ 3), chalcogenide-type materials (Li6PS5Cl and other Li 7-f+g PS 6-x Cl x+y (where 0.05 ≤ f ≤ 0.9, -3.0f + 1.8 ≤ g ≤ -3.0f + 5.7), substances shown by Li 7-h PS 6-h Cl i Br j (where h = i + j, 0 < h ≤ 1.8, 0.1 ≤ i / j ≤ 10.0), etc.).

[0092] As the hydride-based solid electrolyte, for example, LiBH4, a solid solution of LiBH4 and the following alkali metal compound (for example, a solid solution with a molar ratio of LiBH4 to the alkali metal compound of 1:1 to 20:1), etc. can be cited. As the alkali metal compound in the above solid solution, at least one selected from the group consisting of lithium halides (LiI, LiBr, LiF, LiCl, etc.), rubidium halides (RbI, RbBr, RbF, RbCl, etc.), cesium halides (CsI, CsBr, CsF, CsCl, etc.), lithium amide, rubidium amide, and cesium amide can be cited.

[0093] As the halide-based solid electrolyte, for example, monoclinic LiAlCl4, defective spinel-type or layered LiInBr4, monoclinic Li 6-3m Y m X6 (where 0 < m < 2 and X = Cl or Br), etc. In addition, for example, known halide-based solid electrolytes described in International Publication No. 2020 / 070958 and International Publication No. 2020 / 070955 can also be used.

[0094] As the oxide-based solid electrolyte, for example, garnet-type Li7La3Zr2O 12 、NASICON-type Li 1+ O Al 1+O Ti 2-O (PO4)3、Li 1+p Al 1+p Ge 2-p (PO4)3、perovskite-type Li 3q La 2 / 3-q TiO3, etc.

[0095] Among these solid electrolytes, from the viewpoint of high Li ion conductivity, sulfide-based solid electrolytes are preferred, sulfide-based solid electrolytes containing Li and P are more preferred, and especially, thiogermanate-type sulfide-based solid electrolytes with high Li ion conductivity and high chemical stability are further preferred.

[0096] When the electrode material contains a solid electrolyte, the content of the solid electrolyte in the electrode material can be set to 0.1 to 500 parts by mass, for example, relative to 100 parts by mass of the active material in the above embodiment.

[0097] <Electrode for Electrochemical Element>

[0098] The electrode for an electrochemical element of this embodiment (hereinafter, sometimes simply referred to as "electrode") contains the active material of the above embodiment or the electrode material of the above embodiment, and is used as the positive electrode or negative electrode of an electrochemical element such as a secondary battery.

[0099] Examples of the electrode of this embodiment include a molded body (particles, etc.) obtained by molding an electrode mixture containing an active material and an electrode material, and an electrode having a structure in which a layer (electrode mixture layer) composed of a molded body of the electrode mixture is formed on a current collector.

[0100] In the electrode mixture constituting the electrode, when the active material of the above embodiment is used, the material required from the conductive auxiliary agent, binder, solid electrolyte, etc. is contained together with the above active material. In addition, in the electrode mixture constituting the electrode when the electrode material of the above embodiment is used, the material required from the conductive auxiliary agent, binder, solid electrolyte, etc. may be contained together with the above electrode material, but depending on the component composition of the above electrode material, the electrode mixture may also be composed of only the above electrode material.

[0101] As the conductive aid involved in the electrode mixture, various carbon blacks, graphites (natural graphite, artificial graphite), graphene, vapor-grown carbon fibers, carbon nanofibers, carbon nanotubes and other carbon materials previously exemplified as substances that can be used in electrode materials; powders or porous bodies of single substances or alloys of Cu, Ni, Al, Au, Pd, etc., which can be used alone or in combination of two or more. The content of the conductive aid in the electrode mixture (including the amount of carbon black when the electrode material used in the electrode mixture contains carbon black) is preferably 0 to 25% by mass.

[0102] As the binder involved in the electrode mixture, the same substance as the substance previously exemplified as the binder that can be used in the electrode material can be used. It should be noted that, for example, in the case where a sulfide-based solid electrolyte is contained in the electrode mixture (including the case where a sulfide-based solid electrolyte is contained in the electrode material constituting the electrode mixture), even if the binder is not used, the electrode material may not contain the binder in the case where good formability can be ensured in forming a molded body of the electrode mixture.

[0103] In the electrode mixture, when a binder is required, its content (including the amount of the binder when the electrode material used in the electrode mixture contains a binder) is preferably 15% by mass or less, and preferably 0.5% by mass or more. On the other hand, in the electrode mixture, when moldability can be obtained even without a binder due to the presence of a sulfide-based solid electrolyte, its content is preferably 0.5% by mass or less, more preferably 0.3% by mass or less, and further preferably 0% by mass (i.e., no binder).

[0104] In the solid electrolyte involved in the electrode mixture, one or more of the various sulfide solid electrolytes, hydride solid electrolytes, halide solid electrolytes and oxide solid electrolytes previously exemplified as substances that can be used in electrode materials can be used. In order to make the characteristics of the electrochemical element more excellent, it is preferred to contain a sulfide solid electrolyte, and more preferably to contain an argyrodite-type sulfide solid electrolyte.

[0105] It should be noted that from the perspective of reducing grain boundary resistance, the average particle size of the solid electrolyte is preferably greater than 0.1 μm, and more preferably greater than 0.2 μm. On the other hand, from the perspective of forming a sufficient contact interface between the active material and the solid electrolyte, it is preferably less than 10 μm, and more preferably less than 5 μm.

[0106] The average particle size of various particles (solid electrolyte, positive electrode active material, etc.) referred to in this specification refers to the value of the 50% diameter (D) in the volume-based integral fraction when the integral volume is obtained from the smallest particle using a particle size distribution measuring device (Microtrac particle size distribution measuring device "HRA9320" manufactured by Nikkiso Co., Ltd., etc.). 50 ).

[0107] When the electrode mixture contains a solid electrolyte, the content thereof (when the electrode material used in the electrode mixture contains a solid electrolyte, the amount of the solid electrolyte is also included) is preferably 4 to 80% by mass.

[0108] The content of the active material in the electrode mixture (the amount of the active material used in the electrode mixture or the active material derived from the electrode material) is preferably 20 to 95% by mass.

[0109] When the electrode has a current collector, the following materials can be used as the current collector. When the electrode is the positive electrode of the electrochemical element, the current collector can be made of a foil, punched metal, mesh, expanded metal, foamed metal of a metal such as aluminum, nickel, stainless steel, or a carbon sheet. When the electrode is the negative electrode of the electrochemical element, the current collector can be made of a foil, punched metal, mesh, expanded alloy, foamed metal, or a carbon sheet made of copper, nickel, or aluminum.

[0110] The molded body of the electrode mixture can be formed, for example, by mixing the active material of the above embodiment or the electrode material of the above embodiment with a conductive aid, a binder, a solid electrolyte, etc. added as needed to prepare the electrode mixture, and compressing the prepared electrode mixture by press molding or the like.

[0111] In the case of an electrode having a current collector, the electrode can be produced by laminating a molded body of the electrode mixture formed by the above-described method to a current collector by pressure bonding or the like.

[0112] Alternatively, the electrode mixture and solvent may be mixed to prepare an electrode mixture composition, which may be applied to a substrate such as a current collector or a solid electrolyte layer opposite to an electrode (in the case of forming a fully solid-state battery), dried, and then pressed to form a molded body of the electrode mixture.

[0113] The solvent containing the electrode mixture composition can use organic solvents such as water, N-methyl-2-pyrrolidone (NMP). It should be noted that the solvent when the electrode mixture composition also contains a solid electrolyte is preferably selected to be difficult to deteriorate the solid electrolyte. In particular, sulfide-based solid electrolytes and hydride-based solid electrolytes will react chemically due to trace amounts of moisture, so it is preferred to use non-polar aprotic solvents represented by hydrocarbon solvents such as hexane, heptane, octane, nonane, decane, decalin, toluene, and xylene. In particular, it is more preferred to use a super dehydrated solvent that makes the water content 0.001 mass % (10ppm) or less. In addition, it is also possible to use fluorine-based solvents such as "Vertrel (registered trademark)" made by Mitsui Dupont Fluorochemicals, "ZEORORA (registered trademark)" made by Japan Ruiong Company, "Novec (registered trademark)" made by Sumitomo 3M Company, and non-aqueous organic solvents such as methylene chloride and ether.

[0114] The thickness of the formed body of the electrode mixture (in the case of an electrode with a collector, the thickness of the formed body of the electrode mixture on each side of the collector, the same below) is usually 50 μm or more, but from the perspective of high capacity of the electrochemical element, it is preferably 200 μm or more. It should be noted that the load characteristics of the electrochemical element are usually easily improved by thinning the positive electrode and the negative electrode, but according to the electrode of this embodiment, even when the formed body of the electrode mixture is thicker than 200 μm, its load characteristics can be improved. Therefore, in this embodiment, when the thickness of the formed body of the electrode mixture is, for example, more than 200 μm, the effect becomes more significant. In addition, the thickness of the formed body of the electrode mixture is usually less than 3000 μm.

[0115] In the case of an electrochemical device electrode produced by forming an electrode mixture layer on a current collector using an electrode mixture composition containing a solvent, the thickness of the electrode mixture layer is preferably 50 to 1000 μm.

[0116] <Electrochemical Components>

[0117] The electrochemical element of this embodiment has a positive electrode and a negative electrode. As long as either the positive electrode or the negative electrode is an electrode for the electrochemical element of the above embodiment, there are no special restrictions on other compositions and structures, and various compositions and structures used in electrochemical elements such as previously known secondary batteries can be applied.

[0118] The electrochemical element of this embodiment includes secondary batteries such as a secondary battery having a separator and an electrolyte between the positive electrode and the negative electrode, and an all-solid secondary battery having a solid electrolyte layer between the positive electrode and the negative electrode; and electrochemical elements such as supercapacitors. Below, a secondary battery as a representative form of the electrochemical element of this embodiment is described in detail.

[0119] A cross-sectional view schematically showing a secondary battery as an example of an electrochemical device according to the present embodiment is shown in FIG. Figure 1 . Figure 1 The secondary battery 1 shown has a positive electrode 10, a negative electrode 20, a separator (a solid electrolyte layer when the secondary battery is an all-solid secondary battery) 30 between the positive electrode 10 and the negative electrode 20, and an electrolyte (when the secondary battery is a secondary battery with an electrolyte) enclosed in an outer packaging body formed by an outer packaging can 40, a sealing can 50 and a resin gasket 60 interposed therebetween.

[0120] The sealing can 50 is fitted to the opening of the outer can 40 via the gasket 60 , and the opening end of the outer can 40 is tightened inward, whereby the gasket 60 and the sealing can 50 abut against each other, thereby sealing the opening of the outer can 40 and making the interior of the battery a sealed structure.

[0121] The outer can and the sealing can can be made of stainless steel. In addition, the raw materials of the gasket can be polypropylene, nylon, etc., and when heat resistance is required in connection with the use of the battery, fluororesins such as tetrafluoroethylene-perfluoroalkoxyethylene copolymer (PFA), polyphenylene ether (PEE), polysulfone (PSF), polyarylate (PAR), polyethersulfone (PES), polyphenylene sulfide (PPS), polyetheretherketone (PEEK) and other heat-resistant resins with a melting point exceeding 240°C can also be used. In addition, when the battery is used for applications requiring heat resistance, its seal can also be sealed with glass.

[0122] in addition, Figure 2 and Figure 3 2 is a diagram schematically showing another example of a secondary battery as an example of the electrochemical device according to the present embodiment. Figure 2 is a top view of a secondary battery. Figure 3 yes Figure 2 II line cross-sectional view.

[0123] Figure 2 and Figure 3 The secondary battery 100 shown in the figure houses the electrode body 200 in a laminated film outer package 500 composed of two metal laminated films, and the laminated film outer package 500 is sealed at its outer periphery by heat-sealing the upper and lower metal laminated films.

[0124] In the case where the secondary battery 100 is an all-solid secondary battery, the electrode body 200 is formed by stacking a positive electrode, a negative electrode, and a solid electrolyte layer therebetween. On the other hand, in the case where the secondary battery 100 is a secondary battery other than an all-solid secondary battery, the electrode body 200 is formed by stacking a positive electrode, a negative electrode, and a separator therebetween, and an electrolyte (electrolyte, etc.) is sealed together with the electrode body 200 in the laminated film outer package 500. Moreover, at least one of the positive electrode and the negative electrode of the electrode body 200 is an electrode of the above-mentioned embodiment.

[0125] It should be noted that in Figure 3 In order to avoid complicating the drawings, the layers constituting the laminated film outer package 500 and the components (positive electrode, negative electrode, etc.) constituting the electrode body 200 are not shown separately.

[0126] The positive electrode of the electrode body 200 is connected to the positive electrode external terminal 300 in the battery 100. Although not shown in the figure, the negative electrode of the electrode body 200 is also connected to the negative electrode external terminal 400 in the battery 100. In addition, one end side of the positive electrode external terminal 300 and the negative electrode external terminal 400 is led out to the outside of the laminated film outer packaging body 500 in a manner that can be connected to an external device or the like.

[0127] It should be noted that, when the secondary battery is a fully solid secondary battery, in the electrode of the above embodiment, an electrode whose electrode mixture contains a solid electrolyte is used. On the other hand, when the secondary battery is a non-aqueous electrolyte secondary battery, the electrode mixture involved in the electrode of the above embodiment may not contain a solid electrolyte.

[0128] In addition, when the electrode containing the active material of the above-mentioned embodiment is used as the positive electrode and the negative electrode containing no Li (Li ions) participating in the charge and discharge of the battery is used to manufacture the non-aqueous electrolyte secondary battery, it is necessary to pre-introduce the Li (Li ions) participating in the charge and discharge of the battery into the active material involved in the electrode of the above-mentioned embodiment. In this case, for example, the following method can be used: pre-doping (pre-doping outside the system) Li ions in the active material of the above-mentioned embodiment by conventional methods, and in addition, in the case where the non-aqueous electrolyte secondary battery has a non-aqueous electrolyte, a Li source (metal Li foil, Li alloy foil, etc.) is arranged at a position inside the non-aqueous electrolyte that can contact the non-aqueous electrolyte, and the active material of the electrode of the above-mentioned embodiment is doped (pre-doped in the system) with Li ions in the battery. It should be noted that in the case of pre-doping in the above-mentioned system, for example, a pre-doping electrode with a Li source attached to the surface of the collector and electrically connected to the negative electrode can be used.

[0129] <Negative Electrode of Secondary Battery Using the Electrode of the Embodiment as Positive Electrode>

[0130] In the case where the positive electrode involved in the non-aqueous electrolyte secondary battery is the electrode of the above-mentioned embodiment, the negative electrode may be, for example, a negative electrode consisting only of a molded body of a negative electrode mixture containing a negative electrode active material and a conductive aid, a negative electrode having a structure in which a layer (negative electrode mixture layer) consisting of a molded body of the negative electrode mixture is formed on a collector, and the like.

[0131] As the negative electrode active material, for example, one or a mixture of two or more carbon-based materials that can absorb and release lithium, such as graphite, pyrolytic carbon, coke, glassy carbon, sintered bodies of organic polymer compounds, mesocarbon microbeads (MCMB), and carbon fibers, can be used. In addition, single substances, compounds, and alloys of elements such as Al, Si, Sn, Ge, Bi, Sb, In, Zn, and P; compounds that can be charged and discharged at a low voltage close to that of lithium metal, such as lithium-containing nitrides or lithium-containing sulfides; and lithium metal can also be used as negative electrode active materials.

[0132] The content of the negative electrode active material in the negative electrode mixture is preferably 15 to 100% by mass.

[0133] The conductive aid of the negative electrode may be the same as those exemplified above as the conductive aid that can be used in the electrode of the above embodiment. The content of the conductive aid in the negative electrode mixture is preferably 0.1 to 15% by mass.

[0134] When the nonaqueous electrolyte secondary battery using the electrode of the above embodiment as the positive electrode is an all-solid secondary battery and the negative electrode active material is in a particulate form, the negative electrode mixture may contain a solid electrolyte.

[0135] The solid electrolyte of the negative electrode can use one or more of the various sulfide solid electrolytes, hydride solid electrolytes, halide solid electrolytes, and oxide solid electrolytes exemplified above as solid electrolytes that can be used as electrode materials in the above-mentioned embodiment. In order to make the battery characteristics more excellent, it is preferred to contain a sulfide solid electrolyte, and more preferably to contain an argyrodite-type sulfide solid electrolyte.

[0136] The content of the solid electrolyte in the negative electrode mixture is preferably 4 to 90% by mass.

[0137] The negative electrode mixture may contain a binder, but may not contain a binder if good moldability can be ensured even without the use of a binder, such as in the case of a negative electrode also containing a sulfide-based solid electrolyte. The binder may be the same substance as that previously exemplified as a binder that can be used in the electrode of the above embodiment.

[0138] In the negative electrode mixture, when a binder is required, its content is preferably 15% by mass or less, and preferably 0.5% by mass or more. On the other hand, in the negative electrode mixture, from the viewpoint of formability, when a binder is not required, its content is preferably 0.5% by mass or less, more preferably 0.3% by mass or less, and further preferably 0% by mass (i.e., no binder is contained).

[0139] When a current collector is used for the negative electrode, the current collector similar to those exemplified above as the current collector that can be used when the electrode of the above embodiment is the negative electrode can be used.

[0140] The molded body of the negative electrode mixture can be formed, for example, by mixing a conductive aid, a binder, a solid electrolyte, etc., which are added as needed, with a negative electrode active material to prepare a negative electrode mixture, and compressing the prepared negative electrode mixture by press molding, etc. In the case of a negative electrode consisting only of a molded body of a negative electrode mixture, it can be manufactured by the above method.

[0141] In the case of a negative electrode having a current collector, the negative electrode can be produced by laminating a negative electrode mixture compact formed by the above-described method to a current collector by pressure bonding or the like.

[0142] In addition, in the case of a negative electrode having a collector, it can also be manufactured by the following method: a negative electrode mixture composition (paste, slurry, etc.) obtained by dispersing the above-mentioned negative electrode mixture in a solvent is applied to the collector, and after drying, pressure molding such as calendering is performed as needed to form a negative electrode mixture molded body (negative electrode mixture layer) on the surface of the collector.

[0143] The solvent of the negative electrode mixture composition can be water, an organic solvent such as NMP, etc. It should be noted that the solvent when the negative electrode mixture composition also contains a solid electrolyte is preferably selected from a solvent that is not easy to deteriorate the solid electrolyte, and preferably uses the same solvent as the various solvents previously exemplified as the solvent for the electrode mixture composition containing the solid electrolyte.

[0144] The thickness of the molded body of the negative electrode mixture (in the case of a negative electrode having a collector, the thickness of the molded body of the positive electrode mixture on each side of the collector, the same below) is usually 50 μm or more, but from the perspective of high capacity of the battery, it is preferably 200 μm or more. In addition, the thickness of the molded body of the negative electrode mixture is usually 2000 μm or less.

[0145] In addition, in the case of a negative electrode produced by forming a negative electrode mixture layer on a current collector using a negative electrode mixture composition containing a solvent, the thickness of the negative electrode mixture layer is preferably 50 to 1000 μm.

[0146] <Positive electrode of a secondary battery using the electrode of the above-described embodiment as the negative electrode>

[0147] When the negative electrode of the secondary battery is the electrode of the above-described embodiment, examples of the positive electrode include a positive electrode composed only of a molded body of a positive electrode mixture containing a positive electrode active material, a conductive assistant, etc., and a positive electrode having a structure in which a layer composed of a molded body of a positive electrode mixture (positive electrode mixture layer) is formed on a current collector.

[0148] The positive electrode active material is not particularly limited as long as it is a positive electrode active material used in a conventionally known secondary battery, i.e., an active material capable of occluding and releasing Li ions. Specific examples of the positive electrode active material include LiM r Mn 2-r O4 (where M is at least one element selected from the group consisting of Li, Na, K, B, Mg, Ca, Sr, Ba, Ti, V, Cr, Zr, Fe, Co, Ni, Cu, Zn, Al, Sn, Sb, In, Nb, Ta, Mo, W, Y, Ru, and Rh, 0 ≤ r ≤ 1) spinel-type lithium manganese composite oxide, Li r Mn (1-s-r) Ni s M t O (2-u) F v (where M is at least one element selected from the group consisting of Co, Mg, Al, B, Ti, V, Cr, Fe, Cu, Zn, Zr, Mo, Sn, Ca, Sr, and W, 0.8 ≤ r ≤ 1.2, 0 < s < 0.5, 0 ≤ t ≤ 0.5, u + v < 1, -0.1 ≤ u ≤ 0.2, 0 ≤ v ≤ 0.1) layered compound, LiCo 1-r M r O2 (where M is at least one element selected from the group consisting of Al, Mg, Ti, V, Cr, Zr, Fe, Ni, Cu, Zn, Ga, Ge, Nb, Mo, Sn, Sb, and Ba, 0 ≤ r ≤ 0.5) lithium cobalt composite oxide, LiNi 1-r M r O2 (where M is at least one element selected from the group consisting of Al, Mg, Ti, Zr, Fe, Co, Cu, Zn, Ga, Ge, Nb, Mo, Sn, Sb, and Ba, 0 ≤ r ≤ 0.5) lithium nickel composite oxide, Li 1+s M 1-r N r PO4F s(wherein M is at least one element selected from the group consisting of Fe, Mn and Co, N is at least one element selected from the group consisting of Al, Mg, Ti, Zr, Ni, Cu, Zn, Ga, Ge, Nb, Mo, Sn, Sb, V and Ba, 0≤r≤0.5, 0≤s≤1) olivine-type composite oxide, Li2M 1-r N r Pyrophosphate compounds such as P2O7 (wherein M is at least one element selected from the group consisting of Fe, Mn and Co, N is at least one element selected from the group consisting of Al, Mg, Ti, Zr, Ni, Cu, Zn, Ga, Ge, Nb, Mo, Sn, Sb, V and Ba, and 0≤r≤0.5) may be used alone or in combination of two or more.

[0149] In the case where the secondary battery is an all-solid secondary battery, the average particle size of the positive electrode active material is preferably 1 μm or more, more preferably 2 μm or more, and preferably 10 μm or less, more preferably 8 μm or less. It should be noted that the positive electrode active material can be a primary particle or a secondary particle formed by agglomeration of primary particles. If a positive electrode active material having an average particle size in the above range is used, more interfaces with the solid electrolyte contained in the positive electrode can be obtained, so the load characteristics of the battery are further improved.

[0150] When the secondary battery is an all-solid secondary battery, the positive electrode active material preferably has a reaction suppression layer on its surface for suppressing the reaction with the solid electrolyte contained in the positive electrode.

[0151] In the molded body of the positive electrode mixture, if the positive electrode active material is in direct contact with the solid electrolyte, the solid electrolyte will oxidize to form a resistance layer, and the ion conductivity in the molded body may be reduced. By providing a reaction inhibition layer that inhibits the reaction with the solid electrolyte on the surface of the positive electrode active material, direct contact between the positive electrode active material and the solid electrolyte is prevented, thereby suppressing the reduction of ion conductivity in the molded body caused by oxidation of the solid electrolyte.

[0152] The reaction inhibition layer can be made of a material having ion conductivity and capable of inhibiting the reaction between the positive electrode active material and the solid electrolyte. As materials that can constitute the reaction inhibition layer, for example, oxides containing Li and at least one element selected from the group consisting of Nb, P, B, Si, Ge, Ti and Zr can be cited. More specifically, Nb-containing oxides such as LiNbO3, Li3PO4, Li3BO3, Li4SiO4, Li4GeO4, LiTiO3, LiZrO3, Li2WO4, etc. can be cited. The reaction inhibition layer can contain only one of these oxides, or more than two, and further, a plurality of these oxides can also form a composite compound. Among these oxides, Nb-containing oxides are preferably used, and LiNbO3 is more preferably used.

[0153] The reaction suppression layer is preferably present on the surface in an amount of 0.1 to 1.0 parts by mass relative to 100 parts by mass of the positive electrode active material. Within this range, the reaction between the positive electrode active material and the solid electrolyte can be suppressed well.

[0154] Examples of a method for forming a reaction suppression layer on the surface of a positive electrode active material include a sol-gel method, a mechanofusion method, a CVD method, a PVD method, and an ALD method.

[0155] The content of the positive electrode active material in the positive electrode mixture is preferably 20 to 95% by mass.

[0156] As the conductive auxiliary agent of the positive electrode, the same substances as those exemplified above as the conductive auxiliary agents that can be used in the electrode of the above embodiment can be used. The content of the conductive auxiliary agent in the positive electrode mixture is preferably 0.1 to 15% by mass.

[0157] When the secondary battery is an all-solid secondary battery, a solid electrolyte is contained in the positive electrode mixture.

[0158] The solid electrolyte of the positive electrode can use one or more of the various sulfide solid electrolytes, hydride solid electrolytes, halide solid electrolytes, and oxide solid electrolytes exemplified above as solid electrolytes that can be used as electrode materials in the above-mentioned embodiment. In order to make the battery characteristics more excellent, it is preferred to contain a sulfide solid electrolyte, and more preferably to contain an argyrodite-type sulfide solid electrolyte.

[0159] The content of the solid electrolyte in the positive electrode mixture is preferably 4 to 80% by mass.

[0160] The positive electrode mixture may contain a binder, but may not contain a binder if good moldability can be ensured even without the use of a binder, such as in the case of a positive electrode that also contains a sulfide-based solid electrolyte. The binder may be the same substance as that previously exemplified as a binder that can be used in the electrode of the above embodiment.

[0161] In the positive electrode mixture, when a binder is required, its content is preferably 15% by mass or less, and preferably 0.5% by mass or more. On the other hand, in the positive electrode mixture, from the viewpoint of formability, when a binder is not required, its content is preferably 0.5% by mass or less, more preferably 0.3% by mass or less, and further preferably 0% by mass (i.e., no binder is contained).

[0162] When a current collector is used for the positive electrode, the current collector similar to those exemplified above as the current collector that can be used when the electrode of the above embodiment is the positive electrode can be used.

[0163] The molded body of the positive electrode mixture can be formed, for example, by further mixing a binder, a solid electrolyte, etc. added as needed with the positive electrode active material and the conductive aid to prepare the positive electrode mixture, and compressing the prepared positive electrode mixture by press molding, etc. In the case of a positive electrode consisting only of a molded body of the positive electrode mixture, it can be manufactured by the above method.

[0164] In the case of a positive electrode having a current collector, the positive electrode can be produced by laminating the resulting body of the positive electrode mixture formed by the above-mentioned method and the current collector by pressure bonding or the like.

[0165] In addition, in the case of a positive electrode having a current collector, it can also be manufactured by the following method: a positive electrode mixture composition (paste, slurry, etc.) obtained by dispersing the above-mentioned positive electrode mixture in a solvent is applied to the current collector, and after drying, pressure molding such as calendering is performed as needed to form a positive electrode mixture molded body (positive electrode mixture layer) on the surface of the collector.

[0166] The solvent of the positive electrode mixture composition can use an organic solvent such as NMP. It should be noted that the solvent when the positive electrode mixture composition also contains a solid electrolyte is preferably selected from a solvent that is not easy to deteriorate the solid electrolyte, and preferably uses the same solvent as the various solvents previously exemplified as the solvent for the electrode mixture composition containing a solid electrolyte.

[0167] The thickness of the molded body of the positive electrode mixture (in the case of a positive electrode having a collector, the thickness of the molded body of the positive electrode mixture on each side of the collector, the same below) is usually 50 μm or more, but from the viewpoint of high capacity of the battery, it is preferably 200 μm or more. In addition, the thickness of the molded body of the positive electrode mixture is usually 2000 μm or less.

[0168] In addition, in the case of a positive electrode produced by forming a positive electrode mixture layer on a current collector using a positive electrode mixture composition containing a solvent, the thickness of the positive electrode mixture layer is preferably 50 to 1000 μm.

[0169] (Solid Electrolyte Layer)

[0170] In the case where the secondary battery is an all-solid secondary battery, the solid electrolyte in the solid electrolyte layer between the positive electrode and the negative electrode can use one or more of the various sulfide-based solid electrolytes, hydride-based solid electrolytes, halide-based solid electrolytes, and oxide-based solid electrolytes previously exemplified as solid electrolytes that can be used in the electrode materials of the above-mentioned embodiments. Among them, in order to make the battery characteristics more excellent, it is preferred to contain a sulfide-based solid electrolyte, and more preferably contain a sulfide-based solid electrolyte of argyrodite type. Moreover, it is further preferred that the positive electrode, the negative electrode, and the solid electrolyte layer all contain a sulfide-based solid electrolyte, and it is further preferred to contain a sulfide-based solid electrolyte of argyrodite type.

[0171] The solid electrolyte layer may have a porous body such as a resin nonwoven fabric as a support.

[0172] The solid electrolyte layer can be formed by the following methods, etc.: a method of compressing the solid electrolyte by pressure molding, etc.; a method of dispersing the solid electrolyte in a solvent to prepare a composition for forming a solid electrolyte layer, applying it to a substrate, a positive electrode, and a negative electrode and drying it, and performing pressure molding such as pressing treatment as needed.

[0173] The solvent used in the solid electrolyte layer-forming composition is preferably a solvent that does not easily deteriorate the solid electrolyte, and preferably the same solvents as those exemplified above as solvents for the electrode mixture composition containing the solid electrolyte.

[0174] The thickness of the solid electrolyte layer is preferably 10 to 500 μm.

[0175] (Diaphragm)

[0176] In the case where the secondary battery is a battery other than an all-solid-state secondary battery, the separator between the positive electrode and the negative electrode is preferably a separator that has sufficient strength and can retain a large amount of non-aqueous electrolyte. From this point of view, a microporous membrane, non-woven fabric, etc. including polyethylene, polypropylene or ethylene-propylene copolymer with a thickness of 10 to 50 μm and an opening ratio of 30 to 70% is preferably used.

[0177] (Non-aqueous electrolyte)

[0178] In the case where the secondary battery is a battery other than an all-solid secondary battery, the electrolyte generally uses a non-aqueous liquid electrolyte (hereinafter referred to as a "non-aqueous electrolyte"). Moreover, as the non-aqueous electrolyte, a non-aqueous electrolyte in which an electrolyte salt such as a lithium salt is dissolved in an organic solvent is used. As the organic solvent, there is no particular limitation, and examples thereof include chain esters such as dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, and methyl propyl carbonate; cyclic esters with high dielectric constants such as ethylene carbonate, propylene carbonate, butylene carbonate, and vinylene carbonate; mixed solvents of chain esters and cyclic esters, etc., and are particularly suitable for mixed solvents of chain esters as the main solvent and cyclic esters.

[0179] As electrolyte salts to be dissolved in an organic solvent when preparing a non-aqueous electrolyte solution, for example, LiPF6, LiBF4, LiAsF6, LiSbF6, LiCF3SO3, LiC4F9SO3, LiCF3CO2, Li2C2F4(SO3)2, LiC n F 2n+1 SO3 (n ≥ 2), LiN (RfSO2) (Rf'SO2), LiC (RfSO2) 3, LiN (RfOSO2) 2 (herein, Rf, Rf' are fluoroalkyl groups) are used alone or in combination of two or more. The concentration of the electrolyte salt in the non-aqueous electrolyte is not particularly limited, but is preferably 0.3 mol / l or more, more preferably 0.4 mol / l or more, and preferably 1.7 mol / l or less, more preferably 1.5 mol / l or less.

[0180] In the secondary battery, in addition to the above-mentioned nonaqueous electrolyte, a gel electrolyte obtained by gelling the above-mentioned nonaqueous electrolyte with a gelling agent composed of a polymer or the like may be used as the nonaqueous electrolyte.

[0181] (Aqueous Electrolyte)

[0182] When the negative electrode of the secondary battery is the electrode of the above embodiment, an aqueous electrolyte may be used. For example, an aqueous electrolyte may be a composition obtained by mixing more than 4 to 15 mol of water with 1 mol of an alkali metal salt containing an organic anion having a fluoroalkyl group as a constituent.

[0183] (Electrode body)

[0184] The positive electrode and the negative electrode can be used in a battery in the form of a stacked electrode body in which the positive electrode and the negative electrode are stacked with a solid electrolyte layer or a separator interposed therebetween, and in the form of a wound electrode body in which the stacked electrode body is wound.

[0185] When forming an electrode body having a solid electrolyte layer, it is preferred to perform pressure molding in a stacked state of the positive electrode, the negative electrode, and the solid electrolyte layer from the viewpoint of improving the mechanical strength of the electrode body.

[0186] (Battery form)

[0187] Secondary batteries have Figure 1 As shown in the figure, the battery has an outer packaging body composed of an outer can, a sealing can and a gasket (i.e., a form generally referred to as a coin-shaped battery or a button-shaped battery), Figure 2 and Figure 3 In addition to the form of an outer packaging body composed of a resin film or a metal-resin laminate film as shown, an outer packaging body may also have an outer packaging body having a metal outer can with a bottomed cylindrical shape (cylindrical shape, square cylindrical shape) and a sealing structure for sealing its opening.

[0188] Example

[0189] Hereinafter, the present invention will be described in detail based on examples. However, the following examples do not limit the present invention.

[0190] Example 1

[0191] <Synthesis of Active Substance>

[0192] The active material was synthesized by a solid phase reaction method using powders of various metal oxides (all obtained from Kojundo Chemical Co., Ltd.) as starting materials. 14.507 g, 427.6 mg and 80.3 mg of Nb2O5 (purity: >99.9%), α-Al2O3 (purity: >99.99%) and ZnO (purity: >99.99%) were weighed and mixed respectively. The mixture of the above starting materials was added to a zirconia container with an internal volume of 500 ml together with 15 g of ethanol and 120 g of YSZ balls with a diameter of 5 mm, and a planetary ball mill ("planetarymill pulverisette" manufactured by FRITSCH) was used. 5 (trade name)) was mixed at 250 rpm for 3 hours, and the zirconium oxide balls were separated from the mixed sample. The slurry thus obtained was dried to obtain a precursor powder of the active material. The above-mentioned precursor powder was transferred to an alumina crucible, heated to 1150°C at a heating rate of 16°C / min in an atmospheric atmosphere, kept as it was for 8 hours, and naturally cooled to room temperature. The obtained powder was crushed in a mortar for 5 minutes, and passed through a sieve with a mesh of 150 μm, thereby obtaining a crude product of the active material. 4 g of the above-mentioned crude product of the active material was added together with 4 g of ethanol and 30 g of YSZ balls with a diameter of 5 mm into a zirconium oxide container with an internal volume of 12.5 ml, and crushed at 250 rpm for 3 hours using the above-mentioned planetary ball mill. The obtained slurry was vacuum dried at 60°C overnight to obtain Zn 0.1 Al 0.85 Nb 11.05 O 29 . Determination of the obtained Zn 0.1 Al 0.85 Nb 11.05 O 29 The powder XRD pattern confirmed that the active material had a monoclinic crystal structure.

[0193] <Formation of Solid Electrolyte Layer>

[0194] A sulfide-based solid electrolyte (Li 5.4 PS 4.2 Cl 0.8 Br 0.8 )80mg, using a press at 1000kgf / cm 2 The solid electrolyte layer is formed by molding under pressure.

[0195] <Production of positive electrode>

[0196] The synthesized Zn 0.1 Al 0.85 Nb 11.05 O 29(active material), the same sulfide solid electrolyte as that used in the solid electrolyte layer, and graphene (conductive aid) were mixed at a mass ratio of 60:33:7 and fully kneaded to prepare a positive electrode mixture. Next, 15 mg of the positive electrode mixture was placed on the solid electrolyte layer in the reinforced resin cylinder and pressed at 4000 kgf / cm 2 The positive electrode composed of the positive electrode mixture compact is formed on the solid electrolyte layer by molding under a pressure of , thereby producing a laminated body in which the positive electrode and the solid electrolyte layer are laminated.

[0197] <Assembly of Sheet-Shaped All-Solid State Secondary Batteries>

[0198] On the solid electrolyte layer side of the above-mentioned stack, a material made by laminating a lithium metal plate with a diameter of 10 mm and a thickness of 100 μm and an indium metal plate with a diameter of 10 mm and a thickness of 100 μm was placed as the negative electrode, and then a SUS circular plate with a diameter of 10 mm and a thickness of 1 mm was placed on the positive electrode side and the negative electrode side respectively and fixed, thereby making a stacked electrode body. Using the above-mentioned stacked electrode body, a stacked electrode body with the same structure as the above-mentioned structure was made. Figure 2 The present invention is a sheet-shaped all-solid battery similar to the battery shown in the figure. On the surface of the aluminum laminate film constituting the laminate film outer packaging body that becomes the inner side of the outer packaging body, the positive electrode collector foil (SUS foil) and the negative electrode collector foil (SUS foil) are pasted in a horizontal arrangement with a certain degree of spacing therebetween. Each of the above-mentioned collector foils is cut into a shape having a main body portion facing the positive electrode side surface or the negative electrode side surface of the above-mentioned stacked electrode body and a portion that becomes the positive electrode external terminal 300 and the negative electrode external terminal 400 protruding from the above-mentioned main body toward the outside of the battery.

[0199] The above-mentioned stacked electrode body is placed on the negative electrode collector foil of the above-mentioned laminated film outer packaging body, and the above-mentioned stacked electrode body is wrapped with the above-mentioned laminated film outer packaging body in a manner that the positive electrode collector foil is arranged on the positive electrode of the above-mentioned laminated film outer packaging body. The remaining three sides of the above-mentioned laminated film outer packaging body are sealed by heat welding under vacuum to obtain a sheet-shaped all-solid-state secondary battery.

[0200] Example 2

[0201] In addition to changing the active material to monoclinic Zn 0.2 Al 0.7 Nb 11.1 O 29 A sheet-shaped all-solid secondary battery was produced in the same manner as in Example 1 except for the above. It was confirmed in the same manner as in Example 1 that the active material used in the positive electrode was a monoclinic crystal.

[0202] Example 3

[0203] In addition to changing the active material to monoclinic Zn0.3 Al 0.55 Nb 11.15 O 29 A sheet-shaped all-solid secondary battery was produced in the same manner as in Example 1 except for the above. It was confirmed in the same manner as in Example 1 that the active material used in the positive electrode was a monoclinic crystal.

[0204] Example 4

[0205] In addition to changing the active material to monoclinic Cu 0.1 Al 0.85 Nb 11.05 O 29 A sheet-shaped all-solid secondary battery was produced in the same manner as in Example 1 except for the above. It was confirmed in the same manner as in Example 1 that the active material used in the positive electrode was a monoclinic crystal.

[0206] Example 5

[0207] In addition to changing the active material to monoclinic Cu 0.2 Al 0.7 Nb 11.1 O 29 A sheet-shaped all-solid secondary battery was produced in the same manner as in Example 1 except for the above. It was confirmed in the same manner as in Example 1 that the active material used in the positive electrode was a monoclinic crystal.

[0208] Example 6

[0209] In addition to changing the active material to monoclinic Cu 0.3 Al 0.55 Nb 11.15 O 29 A sheet-shaped all-solid secondary battery was produced in the same manner as in Example 1 except for the above. It was confirmed in the same manner as in Example 1 that the active material used in the positive electrode was a monoclinic crystal.

[0210] Comparative Example 1

[0211] In addition to changing the active material to monoclinic AlNb 11 O 29 A sheet-shaped all-solid secondary battery was produced in the same manner as in Example 1 except for the above. It was confirmed in the same manner as in Example 1 that the active material used in the positive electrode was a monoclinic crystal.

[0212] Comparative Example 2

[0213] In addition to changing the active material to monoclinic Zn 0.67 Nb 11.33 O 29 (Zn2Nb 34 O87 ) were carried out in the same manner as in Example 1 to produce a sheet-shaped all-solid secondary battery. It should be noted that, in the same manner as in Example 1, it was confirmed that the active material used in the positive electrode was a monoclinic crystal.

[0214] Comparative Example 3

[0215] In addition to changing the active material to monoclinic Zn 0.566 Al 0.1 Nb 11.31 O 29 A sheet-shaped all-solid secondary battery was produced in the same manner as in Example 1 except for the above. It was confirmed in the same manner as in Example 1 that the active material used in the positive electrode was a monoclinic crystal.

[0216] Comparative Example 4

[0217] In addition to changing the active material to monoclinic Ti2Nb 10 O 29 A sheet-shaped all-solid secondary battery was produced in the same manner as in Example 1 except for the above. It was confirmed in the same manner as in Example 1 that the active material used in the positive electrode was a monoclinic crystal.

[0218] Comparative Example 5

[0219] A sheet-shaped all-solid secondary battery was produced in the same manner as in Example 1 except that the active material was changed to monoclinic TiNb2O7. It should be noted that, in the same manner as in Example 1, it was confirmed that the active material used in the positive electrode was a monoclinic crystal.

[0220] The following evaluations were performed on each of the sheet-shaped all-solid secondary batteries of Examples and Comparative Examples.

[0221] [Load characteristics evaluation]

[0222] For each sheet-shaped all-solid secondary battery of the embodiment and the comparative example, a pressure of 1000 kg / cm 2 The battery was constrained by a pressure of 0.05C, and constant current discharge was performed at a current value of 0.38V, followed by constant voltage discharge until the current value reached 0.01C, and then constant current charging was performed at a current value of 0.05C until the voltage reached 1.88V, and the charging capacity (initial capacity) was measured. Then, for each battery, constant current discharge, constant voltage discharge, and constant current charging were performed under the same conditions as when the initial capacity was measured, and constant current discharge and constant voltage discharge were performed again under the same conditions as when the initial capacity was measured, and constant current charging was performed at a current value of 0.24C until the voltage reached 1.88V, and the charging capacity (0.24C charging capacity) was measured. Then, for each battery, the 0.24C charging capacity was divided by the initial capacity to obtain the capacity retention rate, thereby evaluating the load characteristics.

[0223] [Charge and discharge cycle characteristics]

[0224] For each sheet-like all-solid secondary battery of the embodiment and the comparative example, after 2 cycles of charge and discharge under the same conditions as the load characteristic evaluation, the 0.24C charge capacity was measured, and after the open end voltage was measured for 1 hour, constant current charging was performed at a current value of 0.1C until the voltage reached 1.88V, and after the open end voltage was measured for 1 hour again, step charging was performed at a current value of 0.05C under constant current conditions until the voltage reached 1.88V. Then, the sum of all the constant current step charge capacities of the above 0.24C, 0.1C, and 0.05C (0.05C charge capacity) was calculated. Then, for each battery, the value obtained by dividing the 0.05C charge capacity by the initial capacity was expressed as a percentage, and the capacity retention rate was calculated, thereby evaluating the charge and discharge cycle characteristics.

[0225] The above evaluation results are shown in Table 1 together with the composition and physical properties of the active material. The "α" in the column of the active material in Table 1 refers to the value of α in the above general formula (1). 010 ” refers to the value of the interplanar spacing of the (010) plane determined by X-ray diffraction method (the same applies to Table 3 described later).

[0226] [Table 1]

[0227]

[0228] As shown in Table 1, the sheet-like all-solid-state secondary batteries of Examples 1 to 6 having a positive electrode with the oxide represented by the above general formula (1) as the active material have high capacity retention rates during load characteristic evaluation and high capacity retention rates during charge and discharge cycle characteristic evaluation, and have excellent load characteristics and charge and discharge cycle characteristics.

[0229] In contrast, the use of 1 The battery of Comparative Example 1 using an oxide of Al as the positive electrode active material, the battery of Comparative Examples 2, 4, and 5 using an oxide not containing Al as the positive electrode active material, and the battery using an oxide of element M 1 The battery of Comparative Example 3, in which an inappropriate amount of oxide is used as the positive electrode active material, has a capacity retention rate during load characteristic evaluation and a capacity retention rate during charge and discharge cycle characteristic evaluation that are lower than those of the battery of the embodiment, and has poor load characteristics and charge and discharge cycle characteristics.

[0230] Example 7

[0231] <Preparation of positive electrode material>

[0232] 0.86 g of lithium and 38.7 g of pentaethoxyniobium were mixed in 394 g of dehydrated ethanol to prepare a coating solution for forming a reaction inhibition layer. Next, a coating device using a rotating fluidized bed was used to coat 1000 g of the positive electrode active material (LiNi 0.5 Mn 1.5 The reaction inhibiting layer forming coating solution was applied to the surface of the positive electrode material at a rate of 2 g per minute. The obtained powder was heat treated at 350° C., thereby obtaining a positive electrode material having a reaction inhibiting layer formed on the surface thereof, which was composed of 2 parts by mass of LiNbO3 relative to 100 parts by mass of the positive electrode active material.

[0233] The above positive electrode material, vapor-grown carbon fiber (conductive aid) and Li 5.8 PS 4.6 Cl 1.6 (sulfide-based solid electrolyte) to prepare a positive electrode mixture. The mixing ratio of the above positive electrode material, conductive additive and sulfide-based solid electrolyte is 67:4:29 by mass ratio. 102 mg of the positive electrode mixture is put into a powder molding mold with a diameter of 7.5 mm and pressed at 1000 kgf / cm 2 The positive electrode is formed by molding under a pressure of to produce a positive electrode composed of a cylindrical positive electrode mixture molded body.

[0234] <Formation of Solid Electrolyte Layer>

[0235] 17 mg of the same sulfide-based solid electrolyte as used in the positive electrode was added to the solid electrolyte layer in the powder molding die, and a press was used at 1000 kgf / cm 2 The positive electrode mixture is molded under a pressure of , thereby forming a solid electrolyte layer on the positive electrode mixture molded body.

[0236] <Production of negative electrode>

[0237] The monoclinic Zn 0.1 Al 0.85 Nb 11.05 O 29 (negative electrode active material), sulfide-based solid electrolyte (Li 5.4 PS 4.2 Cl 0.8 Br 0.8 ) and graphene (conductive aid) were mixed in a mass ratio of 60:33:7 and fully kneaded to prepare a negative electrode mixture. Next, 67 mg of the negative electrode mixture was placed on the solid electrolyte layer in the powder molding die and pressed at 10000 kgf / cm 2 The anode material is molded by pressing a pressure of , and a cathode composed of the cathode mixture molded body is formed on the solid electrolyte layer, thereby manufacturing a laminated electrode body in which the cathode, the solid electrolyte layer, and the cathode are laminated.

[0238] <Assembly of all-solid-state batteries>

[0239] Two flexible graphite sheets "PERMA-FOIL (product name)" (thickness: 0.1 mm, apparent density: 1.1 g / cm) manufactured by Toyo Tan Co., Ltd. were prepared. 3 ) is punched into a sheet having the same size as the stacked electrode body, and one of the sheets is placed on the inner bottom surface of a stainless steel sealing can in which a polypropylene ring gasket is embedded. Next, the stacked electrode body is overlapped on the graphite sheet with the negative electrode on the graphite sheet side, and another graphite sheet is placed thereon, and then a stainless steel outer can is covered, and the open end of the outer can is tightened inwardly to seal, thereby making a flat all-solid secondary battery with a diameter of about 9 mm, in which the graphite sheets are respectively placed between the inner bottom surface of the sealing can and the stacked body and between the inner bottom surface of the outer can and the stacked electrode body.

[0240] Example 8

[0241] In addition to changing the negative electrode active material to monoclinic Cu 0.1 Al 0.85 Nb 11.05 O 29 Other than that, the same operation as in Example 7 was carried out to produce a flat all-solid secondary battery.

[0242] Comparative Example 6

[0243] In addition to changing the negative electrode active material to monoclinic AlNb 11 O 29 Other than that, the same operation as in Example 7 was carried out to produce a flat all-solid secondary battery.

[0244] The flat all-solid secondary batteries of Examples 7 and 8 and Comparative Example 6 were subjected to the following evaluations.

[0245] [Load characteristics]

[0246] For the all-solid batteries of Example 7, Example 8 and Comparative Example 6, constant current charging is performed at a current value of 0.07C until the voltage reaches 3.8V, followed by constant voltage charging until the current value reaches 0.005C, and then constant current discharge is performed at a current value of 0.07C until the voltage reaches 1.5V to determine the initial capacity. Constant current charging and constant voltage charging are performed again, and then constant current step discharge is performed to measure the discharge capacity (constant current step discharge capacity) at each current value. The above-mentioned constant current step discharge is performed as follows: for the charged battery, constant current discharge is performed at a current value of 0.6C until the voltage reaches 1.5V, followed by constant current discharge at a current value of 0.3C until the voltage reaches 1.5V, and then constant current discharge is performed at a current value of 0.1C until the voltage reaches 1.5V. Then, the sum of all the constant current step discharge capacities of 0.6C to 0.1C (0.1C discharge capacity) was calculated, and the 0.6C discharge capacity (the same as the step discharge capacity at 0.6C during constant current step discharge) was divided by the 0.1C discharge capacity to evaluate the load characteristics.

[0247] [Charge and discharge cycle characteristics]

[0248] For the all-solid batteries of Example 7, Example 8 and Comparative Example 6, constant current charging is performed at a current value of 0.07C until the voltage reaches 3.8V, followed by constant voltage charging until the current value reaches 0.005C, and then constant current discharge is performed at a current value of 0.07C until the voltage reaches 1.5V to obtain the initial capacity. Constant current charging is performed again at a current value of 0.07C until the voltage reaches 3.8V, followed by constant voltage charging until the current value reaches 0.005C, and then constant current step discharge is performed to measure the discharge capacity (constant current step discharge capacity) at each current value. The above-mentioned constant current step discharge is performed as follows: for the charged battery, constant current discharge is performed at a current value of 0.6C until the voltage reaches 1.5V, followed by constant current discharge at a current value of 0.3C until the voltage reaches 1.5V, and then constant current discharge is performed at a current value of 0.1C until the voltage reaches 1.5V. Then, the sum of all the constant current step discharge capacities of 0.6C to 0.1C was calculated (0.1C discharge capacity). Next, for each of the above batteries, constant current charging was performed at a current value of 0.3C until it reached 3.8V, constant voltage charging was performed until it reached 0.005C, and then constant current step discharge of 0.6C to 0.1C was performed under the same conditions as above to measure the 0.1C discharge capacity.

[0249] In the above series of charge and discharge operations, the operation during the initial capacity measurement was taken as the first cycle, and the final operation of constant voltage charging at a current value of 0.3C followed by constant current step discharge was taken as the third cycle. The 0.1C discharge capacity of the third cycle was divided by the 0.1C discharge capacity of the charge and discharge cycle (second cycle) in which constant current charging was performed at a current value of 0.1C to evaluate the charge and discharge cycle characteristics.

[0250] The above evaluation results in the all-solid batteries of Example 7, Example 8, and Comparative Example 6 are shown in Table 2 as relative values ​​when the result of the all-solid battery of Comparative Example 6 is set to 100.

[0251] [Table 2]

[0252]

[0253] As shown in Table 2, the flat all-solid secondary batteries of Examples 7 and 8 having a negative electrode with the oxide represented by the above general formula (1) as the active material have high capacity retention rates during load characteristic evaluation and high capacity retention rates during charge and discharge cycle characteristic evaluation, and have excellent load characteristics and charge and discharge cycle characteristics.

[0254] In contrast, the use of 1 The battery of Comparative Example 6, in which the oxide of the negative electrode is used as the active material, has a capacity retention rate during load characteristic evaluation and a capacity retention rate during charge-discharge cycle characteristic evaluation lower than those of the battery of the embodiment, and has poor load characteristics and charge-discharge cycle characteristics.

[0255] Example 9

[0256] In addition to changing the active material to monoclinic Cu 0.21 Al 0.74 Nb 11.05 O 27.89 A sheet-shaped all-solid secondary battery was produced in the same manner as in Example 1. It should be noted that the active material was confirmed to be a monoclinic crystal in the same manner as in Example 1. The composition of the active material was determined by ICP-AES measurement and measurement using an oxygen and nitrogen analyzer.

[0257] Example 10

[0258] A mixture of various metal oxide powders (all obtained from Kojundo Chemical Co., Ltd.) was placed in a carbon container and calcined at 1000°C for 4 hours in a vacuum atmosphere with a pressure of 100 Pa or less to obtain monoclinic Cu 0.14 Al 0.73 Nb 11.13 O 28.00 In addition to changing the active material to the above-mentioned monoclinic Cu0.14 Al 0.73 Nb 11.13 O 28.00 A sheet-shaped all-solid secondary battery was produced in the same manner as in Example 1. It should be noted that the active material was confirmed to be a monoclinic crystal in the same manner as in Example 1. The composition of the active material was determined by ICP-AES measurement and measurement using an oxygen and nitrogen analyzer.

[0259] Embodiment 11

[0260] In addition to changing the active material to monoclinic Fe 0.20 Al 0.83 Nb 10.97 O 28.23 A sheet-shaped all-solid secondary battery was produced in the same manner as in Example 1. It should be noted that the active material was confirmed to be a monoclinic crystal in the same manner as in Example 1. The composition of the active material was determined by ICP-AES measurement and measurement using an oxygen and nitrogen analyzer.

[0261] Comparative Example 7

[0262] In addition to changing the active material to monoclinic Al 0.87 Nb 11.13 O 28.47 A sheet-shaped all-solid secondary battery was produced in the same manner as in Example 1. It should be noted that the active material was confirmed to be a monoclinic crystal in the same manner as in Example 1. The composition of the active material was determined by ICP-AES measurement and measurement using an oxygen and nitrogen analyzer.

[0263] For the sheet-like all-solid secondary batteries of Examples 9 to 11 and Comparative Example 7, the same operations as the battery of Example 1 were carried out, except that the lower limit discharge voltage was changed to 0.18 V, and the load characteristics and charge and discharge cycle characteristics were evaluated. The energy density per unit weight of the active material was calculated by dividing the weight of the active material contained in the electrode by the battery capacity.

[0264] Regarding the sheet-shaped all-solid secondary batteries of Examples 9 to 11 and Comparative Example 7, the compositions and physical properties of the active materials are shown in Tables 3 and 4, and the above-mentioned evaluation results are shown in Table 5. It should be noted that in the "With or Without Reduction Treatment" column of Table 3, "○" indicates that the reduction treatment was performed, and "×" indicates that the reduction treatment was not performed.

[0265] [Table 3]

[0266]

[0267] [Table 4]

[0268]

[0269] [Table 5]

[0270]

[0271] As shown in Tables 3 to 5, the sheet-shaped all-solid-state secondary batteries of Examples 9 to 11 having the oxide represented by the above general formula (1) as the active material have high capacity retention rates during load characteristic evaluation and capacity retention rates during charge-discharge cycle characteristic evaluation, and have excellent load characteristics and charge-discharge cycle characteristics. In contrast, for the battery of Comparative Example 7 having a positive electrode with an aluminum niobium composite oxide without element M 1 as the active material, the capacity retention rate during load characteristic evaluation and the capacity retention rate during charge-discharge cycle characteristic evaluation are both poor.

[0272] In addition, for the battery of Example 10 having a positive electrode with the above oxide that has been subjected to a reduction treatment in a carbon container, where the value of Z is appropriate, the absorbances A1, A2, and A3 satisfy the relationship A1 < A2 and A3 < A2, and the atomic ratio P and the atomic ratio Q satisfy the relationship P > Q as the active material, compared with the batteries of Examples 9 and 11 having a positive electrode with the above oxide without the reduction treatment and the battery of Comparative Example 7 having a positive electrode with an aluminum niobium composite oxide without element M 1 as the active material, the energy density increases.

[0273] Within the scope not departing from the gist of the present invention, it can also be implemented in ways other than the above. The embodiments disclosed in this application are examples, and the present invention is not limited to these embodiments. The scope of the present invention is preferably interpreted based on the description in the appended claims compared with the description in the above specification, and all changes within the scope equivalent to the claims are included in the claims.

[0274] Industrial Applicability

[0275] The electrochemical element of the present invention can be applied to the same uses as conventional secondary batteries having non-aqueous electrolytes (non-aqueous electrolytic solutions, gel electrolytes), secondary batteries having aqueous electrolytes, all-solid-state secondary batteries, and supercapacitors. In addition, the electrode for the electrochemical element of the present invention can constitute the electrochemical element of the present invention, and the active material for the electrochemical element of the present invention and the electrode material for the electrochemical element of the present invention can constitute the electrode for the electrochemical element of the present invention.

[0276] It should be noted that the electrochemical element of the present invention has excellent load characteristics and is therefore suitable for many uses that require such characteristics, such as power sources for industrial equipment and mobile bodies (electric vehicles, hybrid vehicles, electric motorcycles and other vehicles, ships, submarines, radio control, rockets, flying bodies such as artificial satellites, drones, etc.). In addition, among mobile bodies, there are mobile bodies that use regenerative energy to charge the batteries used, such as hybrid vehicles, but in this case, there are situations where the charging current and voltage are unstable, so dendrites of element A are easily generated in the battery, which may cause battery degradation. However, since the electrochemical element of the present invention uses an oxide that is difficult to generate dendrites of element A as an active material, it is possible to suppress the deterioration caused by the dendrites of element A even if it is charged using regenerative energy, and it can also be preferably applied to mobile bodies that sometimes perform such charging.

[0277] Explanation of symbols

[0278] 1.100: electrochemical components (secondary batteries),

[0279] 10: positive electrode,

[0280] 20: negative electrode,

[0281] 30: solid electrolyte layer or diaphragm,

[0282] 40: outer can,

[0283] 50: Sealing jar,

[0284] 60: gasket,

[0285] 200: Electrode body,

[0286] 300: Positive external terminal,

[0287] 400: Negative external terminal,

[0288] 500: Laminated film outer packaging body.

Claims

1. An electrode active material for an electrochemical element, characterized in that An oxide having a monoclinic crystal structure and satisfying the following general formula (1) A y M 1 α Al x-α Nb 12-x-z M 2 z O 29-δ (1) In the general formula (1), A is at least one element selected from Li and Na, and M 1 is at least one element selected from the group consisting of Fe, Mn, Zn, Cu, Ag, Mg, Ca, Sr, Ba, Co, Eu, Y, Bi, La, Ce, Nd, Sm and Gd, M 2 is at least one element selected from the group consisting of K, Ti, Ni, Zr, V, Mo, Ta and W, <x≤1.1,0≤y≤24,0≤z≤2,-1≤δ≤2,0<α≤0.4x。 2. The electrode active material for an electrochemical element according to claim 1, wherein In the general formula (1), the element M 1 It is at least one element selected from the group consisting of Fe, Zn and Cu, and 0<δ≤2.

3. The electrode active material for an electrochemical element according to claim 1 or 2, wherein The Nb in the oxide represented by the general formula (1) 4+ The ratio Z of the total Nb in terms of atomic % is 3.5≤Z≤30.

4. The electrode active material for an electrochemical element according to claim 1 or 2, wherein When the absorbance at a wavelength of 500 nm is set as A1, the absorbance at a wavelength of 600 nm is set as A2, and the absorbance at a wavelength of 700 nm is set as A3, the relationship A1 < A2 is satisfied, and the relationship A3 < A2 is satisfied.

5. The electrode active material for an electrochemical device according to any one of claims 1 to 4, wherein Element M determined by X-ray photoelectron spectroscopy 1 The atomic ratio P relative to Nb and the element M determined by inductively coupled plasma emission spectrometry 1 The atomic ratio Q relative to Nb satisfies the relationship of P>Q.

6. The electrode active material for an electrochemical element according to claim 1, wherein The oxide represented by the general formula (1) satisfies the following general formula (2). M 1 α Al 1-1.5α Nb 11+0.5α O 29-δ (2) In the general formula (2), M 1 It is at least one element selected from Zn and Cu, 0<α≤0.4, 0≤δ≤0.5α.

7. A method for producing an electrode active material for an electrochemical device, which is a method for producing an electrode active material for an electrochemical device according to any one of claims 1 to 6, characterized in that: The oxide represented by the general formula (1) or its precursor is fired in a carbon container under a vacuum atmosphere.

8. An electrode material for an electrochemical element, characterized in that: Contains the electrode active material for an electrochemical element according to any one of claims 1 to 6.

9. The electrode material for an electrochemical element according to claim 8, which further contains a solid electrolyte.

10. An electrode for an electrochemical element, characterized in that: Contains the electrode active material for an electrochemical element according to any one of claims 1 to 6, or contains the electrode material for an electrochemical element according to claim 8 or 9.

11. An electrochemical element, characterized in that: Having a positive electrode and a negative electrode, and either the positive electrode or the negative electrode is the electrode for an electrochemical element according to claim 10.