A method for producing high-strength galvanized steel wire for bridge cables
By quenching and tempering hot-rolled wire rods, they are directly rolled into specifications of Φ5.0mm and above. Combined with fewer drawing passes and galvanizing, the problems of equipment wear and surface quality caused by multiple drawing passes are solved, and the efficient production of high-strength galvanized steel wire for bridge cables is realized.
Patent Information
- Application Number
- CN202110622950.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-06-04
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2041-06-04
AI Technical Summary
Existing technologies require multiple drawing processes when producing high-strength galvanized steel wire for bridge cables, resulting in high equipment wear, poor wire surface quality, and high energy consumption, making it difficult to meet the requirements of both high strength and plasticity.
Hot-rolled wire rods are directly rolled into specifications of Φ5.0mm and above through online or offline quenching and tempering heat treatment. By using fewer rounding drawing and galvanizing treatment, multiple drawing processes are avoided, thereby improving the strength of the steel wire and meeting the diameter requirements.
The production of high-strength galvanized steel wire for bridge cables has been achieved, with a tensile strength of ≥2000MPa and a torsion cycle of ≥15 times. This reduces the production process, improves production efficiency and the surface quality of the steel wire, and meets the needs of galvanized steel wire of different specifications.
Abstract
Description
Technical Field
[0001] The invention relates to the field of high-strength wire rod production, and in particular to a method for producing wire rods for high-strength galvanized steel wires for bridge cables. Background Art
[0002] Galvanized steel wire for bridge cables is used to manufacture main cables or inclined cables for long-span bridges. The galvanized steel wire used to manufacture the cable meets the high strength and strict requirements on torsion index. At present, it is produced by wire rod through multiple drawing and galvanizing. Due to the multiple drawing production, the raw material wire rod strength and plasticity are required to be more stringent. In order to achieve a better match of wire rod strength, plasticity and toughness, different wire rod manufacturers have different ways of toughening the wire rod.
[0003] At present, the domestic production of wire rods used to manufacture this type of galvanized steel wire generally adopts online stelmor air cooling, offline lead bath, offline salt bath or online salt bath, online water bath and other production processes. The diameter of the produced wire rods is mostly in the range of Φ12.0mm-Φ16.0mm. Due to the large diameter, the cooling capacity of the production equipment is high. At the same time, the subsequent drawing process requires multiple passes to obtain the final steel wire. Since the strength of the wire rod is continuously improved during the drawing process, the loss of the drawing die is particularly large, which will also affect the surface quality of the drawn steel wire and have a greater impact on the comprehensive performance of the finished steel wire.
[0004] The patent document currently published in China: Publication No. CN 104624680A involves the production of offline EDC. The wire rod needs to be reheated and austenitized before the material enters the EDC, which consumes a lot of energy. In addition, the finished product is steel wire for rope making, and the steel wire still adopts a multi-pass drawing method to produce high-strength steel wire.
[0005] The document with publication number CN 105803176 A relates to a method for improving the torsion performance of galvanized steel wire for bridge cables. The hot-rolled wire rod is pickled, phosphated, cold drawn, galvanized, and stabilized to obtain the finished galvanized steel wire. After cold drawing, the steel wire is subjected to low-temperature tempering treatment and then galvanized. The low-temperature tempering temperature is 200℃-260℃ and the time is 24-48 hours. This content is that the wire rod is subjected to low-temperature tempering after drawing, which is different from the production method designed by the inventor of the present application, which is to hot-roll the wire rod to a specified size and then perform online or offline quenching + tempering heat treatment, and then round the heat-treated wire rod for drawing. The inventor of the present application does not involve cold drawing. The patent document with publication number CN 107587071 A relates to a steel for bridge cables with a tensile strength ≥ 2100MPa and a production method. The hot-rolled wire rod is subjected to wire drawing and air cooling to room temperature. After drawing, galvanizing and heat stabilization treatment, the various performance indicators of the wire rod meet the technical requirements. The wire rod is also drawn into a high-strength steel wire through multiple passes. Summary of the invention
[0006] The present invention uses hot-rolled wire rods to undergo (online or offline) quenching + tempering heat treatment, and the heat-treated wire rods are then drawn through fewer passes to obtain steel wires, and the steel wire surfaces are cleaned and then galvanized to obtain bridge cable galvanized steel wires. The specifications of the wire rods after rolling are Φ5.0mm or above, and no diameter reduction drawing is required. The production diameter requirements of the galvanized steel wires can be achieved through fewer passes of drawing through fewer passes, and the various performance indicators of the galvanized steel wires meet customer requirements.
[0007] According to tests, the tensile strength of the galvanized steel wire for bridge cables produced by this method is ≥2000MPa, the number of torsion times is ≥15 times, and other performance indicators meet the use requirements of galvanized steel wire for bridge cables. Compared with the existing technology, the wire rod no longer needs to be drawn multiple times to increase the strength or reach the production diameter of the galvanized steel wire.
[0008] The technical solution of the present invention is: a method for producing wire rods for high-strength galvanized steel wires for bridge cables, wherein the steel billets are continuously rolled through high-speed wire rods to form wire rods with a size of ≥Φ5.0 mm, the size of the wire rods meeting the production requirements of galvanized steel wires, the hot-rolled wire rods undergo online or offline quenching + tempering heat treatment, the surface is treated and then a few passes of rounding drawing are performed to make the ovality of the wire rods meet the requirements of the steel wires, and then the galvanizing production is directly performed.
[0009] If the wire rod is subjected to offline heat treatment, the wire rod is unwound and unrolled after spinning and coiling, and passed through a heating device in a straight line state, the austenitizing heating temperature is 730℃-1100℃, the heating time is 2 seconds-30 minutes, and the austenite heating is followed by quenching to ensure that the cross section of the wire rod is 100% quenched martensite structure; after quenching, tempering treatment is directly carried out, the tempering temperature is 200℃-600℃, the tempering time is 2 seconds-30 minutes, and tempered sorbite with highly uniform cross section is obtained, and the wire is coiled after tempering.
[0010] If the wire rod adopts online heat treatment, the rolled piece is quenched and tempered before spinning and after final rolling. The final rolling temperature of the rolled piece is controlled at 730℃-1100℃. It is quenched immediately after final rolling to ensure that 100% of the cross section is quenched martensite structure. After quenching, the rolled piece is directly subjected to online tempering heat treatment. The tempering temperature is 200℃-600℃, and the tempering time is 2 seconds-30 minutes. After tempering, the rolled piece is directly fed into the spinning machine or the coiler for large coil collection.
[0011] The quenching heating method and the tempering heating method are selected from electromagnetic induction heating or gas heating furnace heating. Quenching is forced cooling in a water bath or other cooling medium.
[0012] The steel billet is heated to 1000℃~1200℃ and then rolling begins. The final rolling temperature is controlled at 730℃~1100℃ and the wire rod extrusion temperature is controlled at 730℃~1100℃. If offline quenching is adopted, the wire rod is put into the heat preservation hood for sufficient slow cooling after extrusion to form bainite structure.
[0013] Compared with the prior art, the advantages of the present invention are:
[0014] (1) The final rolling size of the hot-rolled wire rod of the present invention is ≥Φ5.0mm, and it is directly rolled into a diameter close to that of the finished steel wire. The wire rod does not need to be reduced in diameter and drawn in the subsequent process, thus avoiding the influence of multiple drawing passes on the surface quality of the steel wire. After a few rounding passes, the size meets the size requirements of galvanized steel wire.
[0015] (2) The strength of the wire rod is improved by online or offline quenching + tempering heat treatment. The heat treatment parameters can be adjusted according to the content of different chemical elements, and the conditions for producing steel wire for bridge cables with a strength level of 2000MPa or higher can be met.
[0016] (3) Since the process of reducing the diameter and drawing is saved, the production process is shortened, the production efficiency is improved, and the requirements of galvanized steel wire for different specifications and sizes can be met more flexibly. DETAILED DESCRIPTION
[0017] The following is a more detailed description of a method for producing ultra-high strength heat-treated wire rod for producing ≥2000MPa grade galvanized steel wire for bridge cables proposed by the present invention in combination with the preferred embodiments of the present invention.
[0018] However, this embodiment is only a description of a preferred embodiment of the present invention and does not impose any limitation on the scope of the present invention.
[0019] Example 1
[0020] The high-speed wire rod factory produces wire rod XC40Si2CrNi2V for bridge cables. The billet is produced by vacuum smelting of molten steel + die casting. The billet is heated at high temperature to be opened into a 150 square billet. The surface of the billet is peeled and finished to ensure that the surface quality meets the rolling requirements. The billet melting composition wt% is as follows: C: 0.40%, Si: 1.80%, Mn: 0.95%, Cr: 0.80%, Ni: 1.70%, Mo: 0.40%, V: 0.10%, etc. The 150 square billet is heated in a high-speed wire heating furnace with a heating temperature ranging from 1000℃ to 1200℃, the final rolling temperature is controlled at 730℃-1100℃, the wire drawing temperature is controlled at 730℃-1100℃, and the wire drawing is put into a heat preservation cover for sufficient slow cooling after the wire drawing to ensure the formation of a bainite structure that is conducive to the subsequent offline wire drawing, and the wire rod is formed into a specified size. The nominal rolling size is Φ7.1mm, and the wire rod is hot rolled for use.
[0021] The hot-rolled wire rod is subjected to offline quenching + tempering heat treatment. After the wire rod is laid out, it is heated in an electromagnetic induction heating furnace, with an austenitizing temperature of 880°C and a heating time of 1-7 minutes. After the wire rod is heated, it is cooled in a water bath cooling device for 20 seconds. After quenching, the wire rod is directly heated in an electromagnetic induction heating furnace for tempering treatment, with a tempering temperature of 220°C-320°C and a tempering time of 4-7 minutes. After tempering, the surface of the wire rod is lubricated and rounded to Φ7.0mm, and then collected, packaged and sent to customers for galvanizing production.
[0022] After offline quenching + tempering heat treatment, the metallographic structure of the hot-rolled wire rod is tempered sorbite, the tensile strength of the heat-treated wire rod is Rm≥2050MPa, and the cross-sectional shrinkage rate Z≥20%. After surface treatment, the heat-treated wire rod is rounded, drawn and galvanized. The tensile strength of the galvanized steel wire is Rm≥2030MPa, and the number of torsion of the galvanized steel wire is ≥15 times. Other indicators meet the technical requirements.
[0023] Example 2
[0024] The high-speed wire rod factory hot-rolls and produces wire rod XC40Si3CrNi2V for bridge cables. The melting composition is as follows:
[0025] The chemical composition of the steel billet is 0.40% C, 2.40% Si, 0.30% Mn, 0.90% Cr, 1.80% Ni, 0.40% Mo, 0.20% V, etc. in wt%.
[0026] The nominal size of the rolled wire rod is Φ7.6mm. The billet is produced by 120-ton converter smelting + continuous casting. The continuous casting large square billet is rolled into 150 square small square billet after high-temperature uniform heating. The small square billet is heated in a high-speed wire heating furnace at a heating temperature of 1000℃ to 1200℃. After being taken out of the furnace, it is rolled in a high-speed rolling mill. The final rolling temperature is controlled at 720℃-1000℃, and the wire-spinning temperature is controlled at 720℃-950℃. After the wire rod is spun, it is put into a heat preservation hood for sufficient slow cooling to ensure the formation of a bainite structure that is conducive to the subsequent offline pay-off, and the specified size wire rod is formed. The rolling nominal size is Φ7.6mm, and the wire rod is ready for use after hot rolling.
[0027] The hot-rolled wire rod is subjected to offline quenching + tempering heat treatment. After the wire rod is laid out, it is heated in an electromagnetic induction heating furnace, with an austenitizing temperature of 830℃-900℃ and a heating time of 3 minutes to 10 minutes. After the wire rod is heated, it is cooled in a water bath cooling device for 15 seconds. After quenching, the wire rod is heated in an electromagnetic induction heating furnace for tempering treatment, with a tempering temperature of 200℃-420℃ and a tempering time of 5 minutes to 15 minutes. After tempering, the surface of the wire rod is lubricated and rounded to Φ7.5mm. The drawn steel wire is collected, packaged and sent to customers for galvanizing production.
[0028] After the hot-rolled wire rod of the present invention is subjected to offline quenching + tempering heat treatment, the metallographic structure is tempered troostite, the tensile strength Rm of the heat-treated wire rod is ≥2150MPa, the cross-sectional shrinkage Z is ≥25%, the heat-treated wire rod is subjected to surface treatment and then rounded, drawn and galvanized to produce Φ7.5mm, the tensile strength Rm of the galvanized steel wire is ≥2130MPa, the number of torsion of the galvanized steel wire is ≥15 times, and other indicators meet the technical requirements.
[0029] In addition to the above embodiments, the present invention also includes other implementation modes. Any technical solutions formed by equivalent transformation or equivalent replacement should fall within the protection scope of the claims of the present invention.
Claims
1. A method for producing high-strength galvanized steel wire for bridge cables, characterized in that: The steel billet is continuously rolled by high-speed wire rod and directly rolled into a diameter close to that of the finished steel wire. The wire rod does not need to be reduced and drawn in the subsequent process, and is rolled into a wire rod with a size of ≥Φ5.0mm. The size of the wire rod meets the production requirements of galvanized steel wire. The hot-rolled wire rod is subjected to online or offline quenching + tempering heat treatment, and after the surface is treated, a few rounding drawing is performed to make the ovality of the wire rod meet the requirements of the steel wire, and then the galvanizing production is directly carried out; If the wire rod adopts offline heat treatment, the wire rod after spinning and winding is unwound and unwound, and passes through a heating device in a straight state, the austenitizing heating temperature is 730°C-1100°C, the heating time is 2 seconds-30 minutes, and the austenite heating is followed by quenching to ensure that the cross section of the wire rod is 100% quenched martensite structure; after quenching, tempering treatment is directly performed, the tempering temperature is 200°C-600°C, the tempering time is 2 seconds-30 minutes, and the cross section is highly uniform tempered sorbite, and the wire is wound into a coil after tempering; If the wire rod adopts online heat treatment, the rolled piece shall be quenched and tempered before spinning and after final rolling. The final rolling temperature of the rolled piece shall be controlled at 730℃-1100℃. The rolled piece shall be quenched immediately after final rolling to ensure that 100% of the cross section is quenched martensite structure. After quenching, the rolled piece shall be directly subjected to online tempering heat treatment. The tempering temperature is 200℃-600℃ and the tempering time is 2 seconds-30 minutes. After tempering, the rolled piece shall be directly fed into the spinning machine or the coiler for large coil collection. The steel billet is heated to 1000℃~1200℃ and then rolling begins. The final rolling temperature is controlled at 730℃~1100℃ and the wire rod extrusion temperature is controlled at 730℃~1100℃. If offline quenching is adopted, the wire rod is put into the heat preservation hood for sufficient slow cooling after extrusion to form bainite structure.
2. The production method according to claim 1, characterized in that: The quenching heating method and the tempering heating method are selected from electromagnetic induction heating or gas heating furnace heating.
3. The production method according to claim 1, characterized in that: The tempering heating method is selected from electromagnetic induction heating or gas heating furnace heating.
4. The production method according to claim 1, characterized in that: The quenching is to quench the wire rod in water.
Citation Information
Patent Citations
Method for producing significant-purpose steel wire for manufacturing rope
CN104624680A
Method for improving torsional property of galvanized steel wire used for bridge cable rope
CN105803176A
Steel with tensile strength of no less than 2100 MPa and for bridge cable, and production method thereof
CN107587071A
Hot-rolled steel wire rod for large bridge cable rope zinc-plated steel wire over 2000 MPa level and production method
CN109468530A
High-strength and high-toughness bridge cable steel and preparation method thereof
CN110144521A