Low thermal conductivity multilayer composite magnesium-aluminum spinel bricks for rotary kilns and their preparation method
By preparing low thermal conductivity multilayer composite magnesium-aluminum spinel bricks, the problem of high thermal conductivity of magnesium-aluminum spinel bricks was solved by utilizing the multilayer composite structure and specific materials. This resulted in a reduction in temperature in the transition zone of the rotary kiln, an improvement in equipment stability, an extension of service life, and energy saving.
Patent Information
- Application Number
- CN202211040984.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-29
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2042-08-29
AI Technical Summary
The high thermal conductivity of existing magnesium-aluminate spinel bricks leads to severe heat loss in the transition zone of rotary kilns, easy deformation of the kiln body, safety hazards, and energy waste. Furthermore, traditional materials contain highly toxic chromium compounds.
The preparation method of low thermal conductivity multilayer composite magnesium-aluminum spinel brick includes a working layer, a heat insulation layer and a heat insulation layer. It utilizes materials such as fused magnesia, fused magnesium-aluminum spinel particles and nano aerogel boards to reduce the thermal conductivity through a multilayer composite structure. Combined with binders such as urea-formaldehyde resin and low-sodium silica sol, it forms excellent high-temperature performance.
It significantly reduces the surface temperature of the cylinder by 50-80℃, reduces heat loss, extends service life, reduces equipment weight, improves equipment stability and safety, and saves energy and reduces consumption.
Smart Images

Figure CN115435597B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of refractory and energy-saving materials technology, specifically to low thermal conductivity multilayer composite magnesium-aluminate spinel bricks for rotary kilns and their preparation method. Background Technology
[0002] Rotary kilns are one of the main pieces of equipment in the production processes of cement, lime, and other materials. The following example uses a cement kiln. The transition zone of a cement rotary kiln is adjacent to the firing zone. The kiln lining is not as robust as in the firing zone, and the temperature fluctuates frequently. The flames enter and exit intermittently, causing the kiln lining to sag and fall off. The kiln lining material is often left unprotected, directly exposed to high-temperature radiation and the scouring effect of hot airflow. Therefore, the transition zone of a cement rotary kiln, especially the lower transition zone, is the section with the most demanding conditions for refractory materials. In the lower transition zone, there is intense scouring from granular clinker. Because the temperature fluctuations are much greater than in other sections, the hot plastic balls exchange heat with the cold air (approximately 1100-1200℃) from the grate cooler, resulting in a heat exchange temperature difference of about 400-500℃. Moreover, this heat exchange occurs between the clinker balls and the kiln lining and the secondary air from the grate cooler, leading to significant thermal stress. In addition, the clinker balls with 25%-30% liquid phase harden here, adhering to each other to form a kiln lining. Combined with the impact, collision, crushing, and grinding effects of the clinker balls and the kiln lining detached from the firing zone, the kiln lining in the lower transition zone is extremely unstable, making its workload the most severe. Therefore, the refractory material in this section, in addition to possessing the high refractoriness, high load softening temperature, and high strength of the refractory material in the firing zone, should also have good thermal shock resistance and kiln lining adhesion performance. Thus, the kiln lining material in this section is subjected to chemical erosion caused by clinker and alkali compounds, thermal stress caused by temperature changes leading to thermal shock spalling, scouring and abrasion from materials, and mechanical stress from mechanical vibration.
[0003] Previously, magnesia-chrome bricks were commonly used in transition zones, but because some of the chromium in magnesia-chrome bricks would precipitate from the "Cr" layer... 3+ "Transformed into highly toxic and carcinogenic Cr" 6+ "Gradually being phased out by rotary kilns, the mainstream material used in the transition zone of rotary kilns abroad is magnesia-alumina spinel brick. Although the performance of these materials is also very suitable for the working conditions of the transition zone, their thermal conductivity is much higher than that of magnesia-chrome brick. The thermal conductivity of magnesia-alumina spinel brick reaches 4.3 W / m·K at 500℃, which is a very important factor restricting the application of magnesia-alumina spinel brick. Unlike the firing zone, the transition zone does not have stable kiln skin protection. If the cylinder temperature is too high, the cylinder is prone to deformation, causing safety hazards. At the same time, excessive heat loss also results in a lot of energy waste. Therefore, this invention provides a method for preparing low thermal conductivity multilayer composite magnesia-alumina spinel bricks for rotary kilns." Summary of the Invention
[0004] (a) Technical problems to be solved
[0005] To address the shortcomings of existing technologies, this invention provides a method for preparing low thermal conductivity multilayer composite magnesium-aluminate spinel bricks for rotary kilns, thus solving the problems mentioned in the background section.
[0006] (II) Technical Solution To achieve the above objectives, the present invention provides the following technical solution: a method for preparing low thermal conductivity multilayer composite magnesia-alumina spinel bricks for rotary kilns, comprising a working layer, a heat insulation layer, and a heat insulation layer, wherein the working layer and the heat insulation layer are connected, and a notch is provided at one end of the heat insulation layer away from the working layer, and the heat insulation layer is located within the notch; the working layer is made of a first aggregate, powder, and a composite binder, wherein the sum of the aggregate and powder is 100wt%, the first aggregate accounts for 60-65wt%, and the powder accounts for 35-40wt%; the composite binder accounts for 6-8wt% of the sum of the aggregate and powder; the first aggregate includes 5-1 molten magnesia particles with a particle size of 0-1mm. The powder comprises 0 wt%, 10-15 wt% fused magnesia-alumina spinel particles with a particle size of 0-1 mm, 25-30 wt% fused magnesia particles with a particle size of 1-3 mm, and 15-20 wt% fused magnesia particles with a particle size of 3-5 mm. The powder also includes 5-10 wt% fused magnesia-alumina spinel fine powder with a particle size <0.074 mm, 15-20 wt% fused magnesia fine powder with a particle size <0.074 mm, 1-2 wt% metallic aluminum powder with a particle size <0.045 mm, 5 wt% defective spinel fine powder with a particle size <0.003 mm, and 1-2 wt% yttrium oxide fine powder with a particle size <0.045 mm.
[0007] Preferably, the composite binder is composed of urea-formaldehyde resin and sulfite pulp, and the mass ratio of urea-formaldehyde resin to sulfite pulp in the composite binder is 3:1.
[0008] Preferably, the main chemical component of the fused magnesia particles is MgO, with a content of 97-97.5 wt%; the main chemical components of the magnesium aluminum spinel particles are: MgO content of 32-33 wt% and Al2O3 content of 64-65 wt%; and the Al2O3 content in the defective spinel fine powder is greater than 90 wt%.
[0009] Preferably, the insulation layer is made of a second aggregate, mixed fine powder, high-temperature reinforcing agent, binder, and pore-forming agent, wherein the sum of the second aggregate, mixed fine powder, and high-temperature reinforcing agent is 100 wt%, the second aggregate accounts for 55-60 wt%, the mixed fine powder accounts for 37-40 wt%, the high-temperature reinforcing agent accounts for 3-5 wt%, the pore-forming agent accounts for 1-2 wt% of the sum of the three, and the binder accounts for 3-5 wt% of the sum of the second aggregate, mixed fine powder, and high-temperature reinforcing agent. The second aggregate includes 15-20 wt% porous magnesia particles with a particle size of 0-1 mm, 25-30 wt% olivine particles with a particle size of 1-3 mm, and 15-20 wt% olivine particles with a particle size of 3-5 mm. The mixed fine powder includes 30-35 wt% olivine fine powder with a particle size <0.074 mm and 10-15 wt% porous magnesia fine powder with a particle size <0.074 mm.
[0010] Preferably, the high-temperature reinforcing agent is a high-temperature reinforcing agent for refractory materials disclosed in Chinese Patent ZL201410488950.3, the pore-forming agent is polyethylene fiber of 0.3 mm and 0.5 mm, and the binder is low-sodium silica sol with a chemical composition mass percentage of Na2O < 0.006% and SiO2 > 30%.
[0011] Preferably, the heat insulation layer is a nano-aerogel plate with a thermal conductivity of <0.02W / (m·K) and a maximum operating temperature of 1150~1250℃. The notch cross-section is trapezoidal or rectangular.
[0012] Preferably, the preparation method of the composite magnesium-aluminum spinel brick is as follows: Step 1, Ingredients: Working layer: Place granules no smaller than 0.074mm into a mixing mill, add the composite binder, and mix for 5 minutes. Then add the remaining powder and mix for 10 minutes. Insulation layer: Place granules no smaller than 0.074mm and a pore-forming agent into a mixing mill, add the binder, and mix for 5 minutes. Then add the remaining powder sequentially and mix for 10 minutes.
[0013] The second step is to divide the mold into two parts after the ingredients are prepared, and add the clay for the working layer and the insulation layer into the two compartments respectively. After removing the partition, the mold is formed using a press.
[0014] The third step is to let the brick blanks air dry for 24 hours, and then dry them at 110℃ for 24 hours.
[0015] The fourth step is to load the kiln and keep it at 1510℃~1530℃ for 4~8 hours, then cool it down. The fifth step is to bond the nano-aerogel plate to the notch of the cooled product to obtain a low thermal conductivity multilayer composite magnesium aluminum spinel brick for rotary kilns.
[0016] (III) Beneficial Effects
[0017] Compared with the prior art, the present invention provides a method for preparing low thermal conductivity multilayer composite magnesium-aluminate spinel bricks for rotary kilns, which has the following beneficial effects: The preparation method of the low thermal conductivity multilayer composite magnesium-aluminum spinel brick for rotary kilns of the present invention has the following advantages: the product of the present invention has excellent high-temperature performance due to the advantages of the multilayer composite structure, and its thermal conductivity is much lower than that of similar products. Tests have shown that when used in the transition zone of cement kilns, it can greatly reduce the surface temperature of the cylinder, which is 50-80°C lower than that of similar products on the market. Attached Figure Description
[0018] Figure 1 This is a schematic diagram of the preparation method of low thermal conductivity multilayer composite magnesium-aluminate spinel bricks for rotary kilns proposed in this invention. Figure 2 This is a cross-sectional view of the structure of the method for preparing low thermal conductivity multilayer composite magnesium-aluminate spinel bricks for rotary kilns proposed in this invention.
[0019] In the diagram: 1. Working layer; 2. Insulation layer; 3. Heat insulation layer. Detailed Implementation
[0020] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0021] Example 1
[0022] like Figure 1As shown in Figure 2, a low thermal conductivity multilayer composite magnesium-aluminum spinel brick for rotary kilns includes a working layer 1, a heat insulation layer 2, and a heat insulation layer 3. The working layer 1 and the heat insulation layer 2 are connected. A notch is provided on the heat insulation layer 2 at one end away from the working layer, and the heat insulation layer 3 is located in the notch. Working layer 1 is made of first aggregate, powder and composite binder, and is formulated according to the following weight ratio: First aggregate 65wt%, of which 5wt% are fused magnesia particles with a particle size of 0-1mm, 10wt% are fused magnesia-alumina spinel particles with a particle size of 0-1mm, 30wt% are fused magnesia particles with a particle size of 1-3mm, and 20wt% are fused magnesia particles with a particle size of 3-5mm; Powder 35wt%, of which 10wt% are fused magnesia-alumina spinel fine powder with a particle size <0.074mm, 17wt% are fused magnesia fine powder with a particle size <0.074mm, 2% are metallic aluminum powder with a particle size <0.045mm, 5wt% are defective spinel fine powder with a particle size <0.003mm, and 1% are yttrium oxide fine powder with a particle size <0.045mm. The insulation layer 2 is composed of a second aggregate, mixed fine powder, high-temperature reinforcing agent, pore-forming agent, and external binder in the following weight ratio: the second aggregate accounts for 60 wt%, the mixed fine powder accounts for 36 wt%, the high-temperature reinforcing agent accounts for 4 wt%, the pore-forming agent accounts for 1.5 wt% of the sum of the aggregate, powder, and high-temperature reinforcing agent, and the binder accounts for 3-5 wt% of the sum of the second aggregate, mixed fine powder, and high-temperature reinforcing agent. The second aggregate includes 20 wt% porous magnesia particles with a particle size of 0-1 mm, 25 wt% olivine particles with a particle size of 1-3 mm, and 15 wt% olivine particles with a particle size of 3-5 mm. The fine powder includes 30 wt% olivine fine powder with a particle size <0.074 mm and 10 wt% porous magnesia fine powder with a particle size <0.074 mm. The pore-forming agent is polyethylene fiber, with 50% of the fibers being 0.3 mm and 50% being 0.5 mm in length. The insulation layer 3 is a nano-aerogel board. The high-temperature reinforcing agent is a refractory material high-temperature reinforcing agent disclosed in Chinese Patent ZL201410488950.3, composed of the following raw materials in the indicated mass percentages: 15-20% synthetic mullite with a particle size <0.045mm, 55-60% alumina micro powder with a particle size <0.045mm, 15-20% silica micro powder with a particle size <0.045mm, and 5-10% special additives; the special additives are sodium carboxymethyl cellulose or sodium lignosulfonate. The materials are taken in proportion, mixed, and co-ground until the average particle size is <0.002mm.
[0023] Preparation method: Step 1, Ingredients: Working layer: Place granules no smaller than 0.074mm into a mixing mill, add the composite binder, and mix for 5 minutes. Then add the remaining powder and mix for 10 minutes. Insulation layer: Place granules no smaller than 0.074mm and a pore-forming agent into a mixing mill, add the binder, and mix for 5 minutes. Then add the remaining powder sequentially and mix for 10 minutes.
[0024] The second step is to divide the mold into two parts after the ingredients are prepared, and add the clay for the working layer and the heat insulation layer into the two compartments respectively. After removing the partition, the mold is formed using a press.
[0025] The third step is to let the brick blanks air dry for 24 hours, and then dry them at 110℃ for 24 hours.
[0026] The fourth step is firing.
[0027] After the shaped brick blank is removed and dried at 110℃ for 24 hours, it is loaded into the kiln and kept at 1510℃ for 5 hours before cooling. The nano aerogel board is then bonded to the notch of the cooled product to obtain a low thermal conductivity multilayer composite magnesium aluminum spinel brick for rotary kilns.
[0028] Implementation results:
[0029]
[0030] Example 1: When the product is used in the transition zone of a cement rotary kiln, the cylinder temperature is reduced by 83°C compared to traditional magnesium-aluminate spinel bricks. Specific Implementation Example 2
[0032] like Figure 1As shown in Figure 2, a low thermal conductivity multilayer composite magnesium-aluminum spinel brick for rotary kilns includes a working layer 1, a heat insulation layer 2, and a heat insulation layer 3. The working layer 1 and the heat insulation layer 2 are connected. A notch is provided on the heat insulation layer 2 at one end away from the working layer, and the heat insulation layer 3 is located in the notch. Working layer 1 is composed of aggregate, powder, and composite binder in the following weight ratios: aggregate 65wt%, including 5wt% fused magnesia particles with a particle size of 0-1mm, 10wt% fused magnesia-alumina spinel particles with a particle size of 0-1mm, 30wt% fused magnesia particles with a particle size of 1-3mm, and 20wt% fused magnesia-alumina particles with a particle size of 3-5mm; powder 35wt%, including 10wt% fused magnesia-alumina spinel fine powder with a particle size <0.074mm, 17wt% fused magnesia fine powder with a particle size <0.074mm, 2% metallic aluminum powder with a particle size <0.045mm, 5wt% defective spinel fine powder with a particle size <0.003mm, and 1.5% yttrium oxide fine powder with a particle size <0.045mm. The insulation layer 2 is composed of aggregate, mixed fine powder, high-temperature reinforcing agent, pore-forming agent, and external binder in the following weight ratio: aggregate 60wt%, mixed fine powder 36wt%, high-temperature reinforcing agent 4wt%, pore-forming agent 2wt% of the sum of aggregate, powder, and high-temperature reinforcing agent, and binder 3-5wt% of the sum of aggregate, mixed fine powder, and high-temperature reinforcing agent. The aggregate consists of: 20wt% porous magnesia particles with a particle size of 0-1mm, 25wt% olivine particles with a particle size of 1-3mm, and 15wt% olivine particles with a particle size of 3-5mm. The fine powder consists of: 30wt% olivine fine powder with a particle size <0.074mm and 10wt% porous magnesia fine powder with a particle size <0.074mm. The pore-forming agent is polyethylene fiber, with 50% of the fibers being 0.3mm and 50% being 0.5mm in length. The insulation layer 3 is a nano-aerogel board.
[0033] Preparation method: Step 1, Ingredients: Working layer: Place granules no smaller than 0.074mm into a mixing mill, add the composite binder, and mix for 5 minutes. Then add the remaining powder and mix for 10 minutes. Insulation layer: Place granules no smaller than 0.074mm and a pore-forming agent into a mixing mill, add the binder, and mix for 5 minutes. Then add the remaining powder sequentially and mix for 10 minutes.
[0034] The second step is to divide the mold into two parts after the ingredients are prepared, and add the clay for the working layer and the heat insulation layer into the two compartments respectively. After removing the partition, the mold is formed using a press.
[0035] The third step is to let the brick blanks air dry for 24 hours, and then dry them at 110℃ for 24 hours.
[0036] The fourth step is firing.
[0037] After the shaped brick blank is removed and dried at 110℃ for 24 hours, it is placed in a kiln and kept at 1510℃ for 5 hours before cooling. The nano aerogel board is then bonded to the gap of the cooled product to obtain this product.
[0038] Implementation results:
[0039]
[0040] Example 2: When the product is used in the transition zone of a cement rotary kiln, the cylinder temperature is reduced by 93°C compared to traditional magnesium-aluminate spinel bricks.
[0041] As can be seen from Examples 1 and 2 above, the thermal conductivity of the product of this invention is much lower than that of common magnesium-aluminate spinel bricks on the market. The porous magnesia and olivine used achieve a lower bulk density, thereby reducing the weight of thermal equipment. This reduced weight effectively lowers the load on the motor, the operating current, and the power consumption per ton of product, while also improving the stability of motor operation, reducing maintenance frequency, and ensuring long-term stable operation of the equipment. The lower thermal conductivity also reduces heat loss, and the higher softening temperature and thermal shock stability ensure the safety and longer service life of the product. Replacing existing ordinary magnesium-aluminate spinel bricks, this invention significantly extends the service life while achieving energy savings and reduced consumption.
[0042] In summary, the preparation method of the low thermal conductivity multilayer composite magnesium-aluminum spinel brick for rotary kilns of this invention and its preparation method have the following advantages: the product of this invention relies on the advantages of its multilayer composite structure and has excellent high-temperature performance. At the same time, its thermal conductivity is much lower than that of similar products. Tests have shown that when used in the transition zone of cement kilns, it can greatly reduce the surface temperature of the cylinder, which is 50-80°C lower than that of similar products on the market.
[0043] It should be noted that, in this document, relational terms such as "first" and "second" are used only to distinguish one entity or operation from another, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Furthermore, the terms "comprising," "including," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such a process, method, article, or apparatus. Without further limitations, an element defined by the phrase "comprising one..." does not exclude the presence of other identical elements in the process, method, article, or apparatus that includes said element.
[0044] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.
Claims
1. A low thermal conductivity multilayer composite magnesium-aluminate spinel brick for rotary kilns, comprising a working layer, a heat insulation layer, and a thermal insulation layer, characterized in that: The working layer and the insulation layer are connected. A notch is provided on the insulation layer at one end away from the working layer, and the heat insulation layer is located within the notch. The working layer is made of a first aggregate, powder, and a composite binder. The sum of the first aggregate and the powder is 100 wt%, with the first aggregate accounting for 60-65 wt% and the powder accounting for 35-40 wt%. The composite binder accounts for 6-8 wt% of the sum of the first aggregate and powder. Based on 100wt% of the sum of the first aggregate and powder, the first aggregate comprises: 5-10wt% fused magnesia particles with a particle size of 0-1mm, 10-15wt% fused magnesia-alumina spinel particles with a particle size of 0-1mm, 25-30wt% fused magnesia particles with a particle size of 1-3mm, and 15-20wt% fused magnesia particles with a particle size of 3-5mm; based on 100wt% of the sum of the first aggregate and powder, the powder comprises: 5-10wt% fused magnesia-alumina spinel fine powder with a particle size <0.074mm, 15-20wt% fused magnesia fine powder with a particle size <0.074mm, 1-2wt% metallic aluminum powder with a particle size <0.045mm, 5wt% defective spinel fine powder with a particle size <0.003mm, and 1-2wt% yttrium oxide fine powder with a particle size <0.045mm.
2. The low thermal conductivity multilayer composite magnesium-aluminate spinel brick for rotary kilns according to claim 1, characterized in that: The composite binder is composed of urea-formaldehyde resin and sulfite pulp, with a mass ratio of urea-formaldehyde resin to sulfite pulp of 3:
1.
3. The low thermal conductivity multilayer composite magnesium-aluminate spinel brick for rotary kilns according to claim 1, characterized in that: The main chemical component of the fused magnesia particles is magnesium oxide, with a content of 97-97.5 wt%; the main chemical components of the fused magnesia-alumina spinel particles are magnesium oxide with a content of 32-33 wt% and aluminum oxide with a content of 64-65 wt%; the aluminum oxide content in the defective spinel fine powder is greater than 90 wt%.
4. The low thermal conductivity multilayer composite magnesium-aluminate spinel brick for rotary kilns according to claim 1, characterized in that: The insulation layer is made of a second aggregate, mixed fine powder, high-temperature reinforcing agent, binder, and pore-forming agent. The total weight of the second aggregate, mixed fine powder, and high-temperature reinforcing agent is 100 wt%, with the second aggregate accounting for 55-60 wt%, the mixed fine powder accounting for 37-40 wt%, the high-temperature reinforcing agent accounting for 3-5 wt%, the pore-forming agent accounting for 1-2 wt% of the sum of the second aggregate, mixed fine powder, and high-temperature reinforcing agent, and the binder accounting for 3-5 wt% of the sum of the second aggregate, mixed fine powder, and high-temperature reinforcing agent. Based on the sum of the second aggregate, mixed fine powder, and high-temperature reinforcing agent being 100wt%, the second aggregate comprises: 15-20wt% porous magnesia particles with a particle size of 0-1mm, 25-30wt% olivine particles with a particle size of 1-3mm, and 15-20wt% olivine particles with a particle size of 3-5mm; based on the sum of the second aggregate, mixed fine powder, and high-temperature reinforcing agent being 100wt%, the mixed fine powder comprises: 30-35wt% olivine fine powder with a particle size <0.074mm, and 10-15wt% porous magnesia fine powder with a particle size <0.074mm.
5. The low thermal conductivity multilayer composite magnesium-aluminate spinel brick for rotary kilns according to claim 4, characterized in that: The high-temperature reinforcing agent is a high-temperature reinforcing agent for refractory materials disclosed in Chinese Patent ZL201410488950.
3. The pore-forming agent is polyethylene fiber with a diameter of 0.3 mm and 0.5 mm. The binder is low-sodium silica sol, and its chemical composition by mass percentage is sodium oxide < 0.006% and silica > 30%.
6. The low thermal conductivity multilayer composite magnesium-aluminate spinel brick for rotary kilns according to claim 4, characterized in that: The insulation layer is a nano-aerogel board with a thermal conductivity of <0.02W / (m·K) and a maximum operating temperature of 1150~1250℃. The notch cross-section is trapezoidal or rectangular.
7. The method for preparing low thermal conductivity multilayer composite magnesium-aluminate spinel bricks for rotary kilns according to claim 6, characterized in that: The preparation method of the composite magnesium-aluminum spinel brick is as follows: Step 1, Ingredient preparation: Working layer: Put granules no smaller than 0.074mm into a mixer, add a composite binder and mix for 5 minutes, then add the remaining powder and mix for 10 minutes for later use; Insulation layer: Put granules no smaller than 0.074mm and a pore-forming agent into a mixer, add a binder and mix for 5 minutes, then add the remaining powder in sequence and mix for 10 minutes for later use. The second step is to divide the mold into two parts after the ingredients are prepared, and add the clay for the working layer and the insulation layer into the two compartments respectively. After removing the partition, the mold is formed using a press. The third step is to let the brick blanks air dry for 24 hours, and then dry them at 110℃ for 24 hours. The fourth step is to load the kiln and keep it at 1510℃~1530℃ for 4~8 hours, then cool it down. The fifth step is to bond the nano-aerogel plate to the notch of the cooled product to obtain a low thermal conductivity multilayer composite magnesium aluminum spinel brick for rotary kilns.
Citation Information
Patent Citations
High-temperature reinforcing agent for refractory materials and preparation method of high-temperature reinforcing agent
CN104230361A
Modified high-purity magnesium aluminate spinel composite brick and preparation method thereof
CN106278324A
Silicon carbide composite refractory product containing rare earth oxide
CN111620709A