A flip-chip light-emitting diode chip and its preparation method
By using an initial current blocking layer and a low-viscosity positive photoresist to replace the high-viscosity photoresist in the flip-chip LED chip, the fluidity and uniformity problems in isolation trench preparation are solved, the cost is reduced, and the product quality is improved. Rate.
Patent Information
- Application Number
- CN202211007571.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-22
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-08-22
AI Technical Summary
When preparing isolation trenches for existing flip-chip LED chips, the high-viscosity photoresist has poor fluidity and high cost, resulting in a high product defect rate and poor uniformity, affecting production efficiency and cost.
The initial current blocking layer and low-viscosity positive photoresist are used as masks, and isolation grooves are formed through etching to replace the high-viscosity photoresist, improve fluidity and uniformity, and reduce costs.
It improves product yield, reduces production costs, solves the problem of poor fluidity and uniformity of high-viscosity photoresist, and improves preparation efficiency.
Smart Images

Figure CN115440867B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of light emitting diodes, and in particular to a flip-chip light emitting diode chip and a preparation method thereof. Background Art
[0002] A light emitting diode, or LED for short, is a commonly used light emitting device that emits light by releasing energy through the recombination of electrons and holes. Like an ordinary diode, a light emitting diode is composed of a PN junction and also has unidirectional conductivity.
[0003] In recent years, the LED industry has developed and upgraded rapidly. With its many advantages such as energy saving, high efficiency and high reliability, it is applied to general lighting, special lighting, plant lighting, landscape lighting, indoor display, outdoor display, backlight display, UV disinfection, UV curing and other scenarios. Flip-chip light-emitting diode chips have also been quickly recognized by the market, and their share has gradually increased.
[0004] Existing flip-chip light-emitting diode chips include isolation grooves. When preparing the isolation grooves, it is usually necessary to coat 10um of high-viscosity photoresist on the surface of the wafer as a mask to protect the areas that do not need to be etched. However, high-viscosity photoresist has poor fluidity and relatively poor uniformity, which can easily cause unclean development and lead to defective products. At the same time, high-viscosity photoresist is expensive, consumes a lot of money, and has high costs. Summary of the invention
[0005] Based on this, an object of the present invention is to provide a flip-chip light emitting diode chip and a method for preparing the same, so as to solve the above-mentioned deficiencies in the prior art.
[0006] To achieve the above-mentioned purpose, the present invention provides a flip-chip light-emitting diode chip, comprising a substrate and an epitaxial layer stacked in sequence, wherein the end of the epitaxial layer is etched to form a Mesa step, and the epitaxial layer and the Mesa step are both provided with an initial current layer and a positive photoresist stacked in sequence, and an isolation groove is formed by etching the initial current blocking layer and the positive photoresist located on at least a portion of the Mesa step to the substrate, and the viscosity of the positive photoresist is 50-400Cps.
[0007] The beneficial effects of the present invention are as follows: by using the initial current blocking layer and the low-viscosity positive photoresist together as a mask, the parts that do not need to be etched are protected to form isolation grooves by etching. Different from the prior art, the isolation grooves are prepared by replacing the high-viscosity photoresist with the low-viscosity positive photoresist, which can not only solve the problem that the high-viscosity photoresist has poor fluidity and relatively poor uniformity, resulting in unclean development and poor product quality, but also improve the product yield. At the same time, since the low-viscosity positive photoresist is cheaper than the high-viscosity photoresist, it can also effectively reduce the production cost.
[0008] Preferably, the flip-chip light-emitting diode chip also includes a target current blocking layer, a current expansion layer, a current transmission metal layer, a Bragg reflection layer and a bonding metal layer, and the target current blocking layer, the current expansion layer, the current transmission metal layer, the Bragg reflection layer and the bonding metal layer are sequentially stacked on the epitaxial layer.
[0009] Preferably, the Bragg reflection layer comprises SiO 2 and Ti 3 O 5 .
[0010] Preferably, the current transmission metal layer includes an N-type current transmission metal layer and a P-type current transmission metal layer, the bonding metal layer includes an N-type bonding metal layer and a P-type bonding metal layer, the P-type bonding metal layer is electrically connected to the P-type current transmission metal layer, and the N-type bonding metal layer is electrically connected to the N-type current transmission metal layer.
[0011] To achieve the above object, the present invention further provides a method for preparing a flip-chip light-emitting diode chip, which is used to prepare the above flip-chip light-emitting diode chip, comprising the following steps:
[0012] Obtaining a substrate, and depositing an epitaxial layer on the substrate;
[0013] Coating a first positive photoresist on the epitaxial layer, and sequentially performing exposure, development and etching to form a Mesa step on the epitaxial layer;
[0014] Removing the first positive photoresist, and depositing an initial current blocking layer with a first preset thickness on the surface of the Mesa step and the epitaxial layer;
[0015] A second positive photoresist with a second preset thickness is coated on the initial current blocking layer, and after exposure and development in sequence, the second positive photoresist is etched to the substrate to form an isolation groove;
[0016] Coating a third positive photoresist on the surfaces of the etched initial current blocking layer and the isolation groove, and sequentially forming a target current blocking layer through exposure, development and corrosion;
[0017] A current spreading layer, a current transmission metal layer, a Bragg reflection layer and a bonding metal layer are sequentially prepared on the surface of the target current blocking layer.
[0018] Preferably, the step of sequentially exposing and developing and then etching the substrate to form an isolation groove comprises:
[0019] removing a portion of the second positive photoresist by sequentially exposing and developing to expose a portion of the initial current blocking layer;
[0020] Using a BOE solution to etch the exposed initial current blocking layer to obtain a target etching area and expose a portion of the Mesa step;
[0021] A photo-induced coupled plasma etching process is used to etch and expose a portion of the Mesa step until the substrate is etched to form an isolation groove, and the second positive photoresist and a portion of the initial current blocking layer are etched away to obtain an intermediate current blocking layer with a third preset thickness.
[0022] Preferably, the step of sequentially forming the target current blocking layer by exposure, development and corrosion comprises:
[0023] removing a portion of the second positive photoresist by sequentially exposing and developing to expose a portion of the intermediate current blocking layer;
[0024] The exposed middle current blocking layer is etched away using the BOE etching solution, and the third positive photoresist is removed to obtain a target current blocking layer with a fourth preset thickness.
[0025] Preferably, the first preset thickness is 2um, the second thickness is 2.3um, and the third preset thickness and the fourth preset thickness are both 0.3um.
[0026] Preferably, the viscosity of the first positive photoresist, the second positive photoresist and the third positive photoresist are all between 50-400 Cps.
[0027] Preferably, the material of the target current blocking layer is SiO 2 、SiN、AlO 2 , Ti 3 O 5 At least one of .
[0028] Additional aspects and advantages of the present invention will be given in part in the following description and in part will be obvious from the following description, or will be learned through practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 A schematic structural diagram of a flip-chip light-emitting diode chip provided in the first embodiment of the present invention;
[0030] Figure 2 A flow chart of a method for preparing a flip-chip light-emitting diode chip provided in accordance with a second embodiment of the present invention;
[0031] Figure 3 A schematic diagram of the process of preparing a flip-chip light-emitting diode chip after step S203 is completed in the second embodiment of the present invention;
[0032] Figure 4 A schematic diagram of the process of preparing a flip-chip light-emitting diode chip according to the second embodiment of the present invention after step S204 is completed;
[0033] Figure 5 A schematic diagram of the process of preparing a flip-chip light-emitting diode chip according to the second embodiment of the present invention after step S205 is completed;
[0034] Figure 6 A schematic diagram of the process of preparing a flip-chip light-emitting diode chip according to the second embodiment of the present invention after step S206 is completed;
[0035] Figure 7 A schematic diagram of the process of preparing a flip-chip light-emitting diode chip according to the second embodiment of the present invention after step S207 is completed;
[0036] Figure 8 A schematic diagram of the process of preparing a flip-chip light-emitting diode chip after completing step S208 in the second embodiment of the present invention;
[0037] Fig. 9 This is a schematic diagram of the process of preparing a flip-chip light-emitting diode chip after step S209 is completed in the second embodiment of the present invention.
[0038] Substrate 10 Isolation slot 60 Epitaxial layer 20 Third positive photoresist 32 Buffer layer 21 Target current blocking layer 51 N-type semiconductor layer 22 Current spreading layer 70 Active layer 23 Current carrying metal layer 71 P-type semiconductor layer 24 Bragg reflector 72 Mesa Steps 40 Bonding metal layer 73 Initial current blocking layer 50 Flip-chip LED chips 100 Second positive photoresist 31
[0039] The following specific implementation manner will further illustrate the present invention in conjunction with the above-mentioned drawings. DETAILED DESCRIPTION
[0040] In order to facilitate the understanding of the present invention, the present invention will be described more fully below with reference to the relevant drawings. Several embodiments of the present invention are given in the drawings. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present invention more thorough and comprehensive.
[0041] It should be noted that when an element is referred to as being "fixed to" another element, it may be directly on the other element or there may be a central element. When an element is considered to be "connected to" another element, it may be directly connected to the other element or there may be a central element at the same time. The terms "vertical", "horizontal", "left", "right" and similar expressions used herein are for illustrative purposes only.
[0042] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which the present invention belongs. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more of the related listed items.
[0043] like Figure 1 and Figure 4 As shown, the first embodiment of the present invention provides a flip-chip light emitting diode chip. The flip-chip light emitting diode chip 100 includes a substrate 10 , an epitaxial layer 20 , a Mesa step 40 and an isolation trench 60 .
[0044] Among them, the end of the epitaxial layer 20 is etched to form a Mesa step 40, and the isolation groove 60 is located below the Mesa step 40. The epitaxial layer 20 and the Mesa step 40 are both provided with an initial current blocking layer 50 and a positive photoresist stacked in sequence. The isolation groove 60 is formed by etching the initial current blocking layer 50 and the positive photoresist located on at least part of the Mesa step 40 to the substrate 10. It should be noted that the viscosity of the positive photoresist is 50-400Cps.
[0045] It can be understood that by using the initial current blocking layer 50 and the low-viscosity positive photoresist together as a mask, the parts that do not need to be etched are protected to etch and form the isolation groove 60. Different from the prior art, the low-viscosity positive photoresist is used to replace the high-viscosity photoresist to prepare the isolation groove 60. It can not only solve the problem that the high-viscosity photoresist has poor fluidity and relatively poor uniformity, which causes unclean development and leads to defective products, but also improve the product yield. At the same time, since the low-viscosity positive photoresist is cheaper than the high-viscosity photoresist, it can also effectively reduce the production cost.
[0046] In some of the embodiments, the flip-chip light-emitting diode chip further includes a target current blocking layer 51, a current expansion layer 70, a current transmission metal layer 71, a Bragg reflection layer 72 and a bonding metal layer 73. The target current blocking layer 51, the current expansion layer 70, the current transmission metal layer 71, the Bragg reflection layer 72 and the bonding metal layer 73 are sequentially stacked on the epitaxial layer 20. The current expansion layer 70 covers the target current blocking layer 51. The target current blocking layer 51 is formed by corroding and thinning the initial current blocking layer 50. The thickness of the target current blocking layer 51 is 0.3 um, and the thickness of the initial current blocking layer 50 is 2 um.
[0047] In some embodiments, the epitaxial layer 20 includes a buffer layer 21, an N-type semiconductor layer 22, an active layer 23 and a P-type semiconductor layer 24 from bottom to top, the Mesa step 40 is located on a portion of the N-type semiconductor layer 22, the isolation trench 60 includes two trench walls, and the two trench walls of the isolation trench 60 are respectively attached to the side wall of the substrate 10 and the side wall of the epitaxial layer 20, the target current blocking layer 51 is located on the P-type semiconductor layer 24, and the target current blocking layer 51 includes SiO 2 、Al 2 O 3 、Ti 3 O 5 The target current blocking layer 51 is used to play the role of current blocking, the current expansion layer 70 is located on the target current blocking layer 51, and the current expansion layer 70 covers the target current blocking layer 51, the current transmission metal layer 71 is located on the current expansion layer 70, and the current transmission metal layer 71 includes an N-type current transmission metal layer and a P-type current transmission metal layer, and the Bragg reflection layer 72 is located on the current transmission metal layer 71, and the Bragg reflection layer 72 includes SiO2 alternately stacked in a preset period. 2 and Ti 3 O 5 The Bragg reflection layer 72 includes a P-type Bragg reflection layer through hole and an N-type Bragg reflection layer through hole, and the bonding metal layer 73 includes an N-type bonding metal layer and a P-type bonding metal layer.
[0048] It can be understood that the P-type bonding metal layer is electrically connected to the P-type current transmission metal layer through the P-type Bragg reflection layer through hole, and the N-type bonding metal layer is electrically connected to the N-type current transmission metal layer through the N-type Bragg reflection layer through hole.
[0049] It should be noted that the above implementation process is only to illustrate the feasibility of the present application, but it does not mean that the flip-chip LED chip of the present application has only the above-mentioned implementation process. On the contrary, as long as the flip-chip LED chip of the present application can be implemented, it can be included in the feasible implementation plan of the present application.
[0050] The second embodiment of the present invention provides a method for preparing a flip-chip light emitting diode chip, which is used to prepare the flip-chip light emitting diode chip 100 in the first embodiment. The flow chart of the preparation method of this embodiment is as follows: Figure 2 As shown, the process includes the following steps:
[0051] Step S101, obtaining a substrate 10, and depositing an epitaxial layer 20 on the substrate 10;
[0052] Specifically, the substrate 10 includes Si, SiC, GaN, Al 2 O 3, and the epitaxial layer 20 includes a buffer layer 21, an N-type semiconductor layer 22, an active layer 23 and a P-type semiconductor layer 24 from bottom to top.
[0053] Step S102, coating a first positive photoresist on the epitaxial layer 20, and sequentially performing exposure, development and etching to form a Mesa step 40 on the epitaxial layer 20;
[0054] Specifically, after coating a first positive photoresist with a viscosity of 50-400 Cps on the P-type semiconductor layer 24, an exposure and development process is performed to expose a preliminary etching area, and then a portion of the P-type semiconductor layer 24, the active layer 23 and the N-type semiconductor layer 22 are etched away in the preliminary etching area using an inductively coupled plasma etching process to form the Mesa step 40.
[0055] Step S103, removing the first positive photoresist, and depositing an initial current blocking layer 50 with a first preset thickness on the surface of the Mesa step 40 and the epitaxial layer 20;
[0056] Specifically, the first positive photoresist is removed, and the initial current blocking layer 50 with a thickness of 2 um is prepared on the surface of the P-type semiconductor layer 24 and the Mesa step 40 by using a PECVD process. The initial current blocking layer 50 includes SiO2, Al2O3, and Ti3O5.
[0057] Step S104, coating the initial current blocking layer 50 with a second positive photoresist 31 of a second preset thickness, and after sequentially exposing and developing, etching to the substrate 10 to form an isolation groove 60;
[0058] Specifically, a second positive photoresist 31 with a thickness of 2.5um and a viscosity of 50-400Cps is coated on the surface of the initial current blocking layer 50, and then an exposure and development process is performed to expose a portion of the initial current blocking layer 50; the exposed initial current blocking layer 50 is then etched away using a BOE etching solution to expose a portion of the Mesa step 40; and then the exposed portion of the Mesa step 40 is etched away using an inductively coupled plasma etching process until the substrate 10 is visible, thereby obtaining the isolation groove 60.
[0059] Step S105, coating a third positive photoresist 32 on the surfaces of the etched initial current blocking layer 50 and the isolation trench 60, and sequentially forming a target current blocking layer 51 by exposure, development and etching;
[0060] Specifically, in step S105, while etching is performed by an inductively coupled plasma etching process until the substrate 10 is formed to obtain the isolation groove 60, the second positive photoresist 31 above the initial current blocking layer 50 will also be completely etched away, and the initial current blocking layer 50 will also be etched and thinned, leaving an initial current blocking layer 50 with a thickness of 0.3um; then, a third positive photoresist 32 with a viscosity of 50-400Cps is coated on the initial current blocking layer 50 after etching and thinning, and then an exposure and development process is performed to expose a portion of the initial current blocking layer 50 after etching and thinning; finally, a BOE etching solution is used to etch away the exposed initial current blocking layer 50 after etching and thinning, and the third positive photoresist 32 is removed to obtain the target current blocking layer 51.
[0061] Step S106 , sequentially preparing a current spreading layer 70 , a current transmission metal layer 71 , a Bragg reflection layer 72 and a bonding metal layer 73 on the surface of the target current blocking layer 51 .
[0062] In a specific embodiment, when preparing the isolation groove 60, the initial current blocking layer 50 and the positive low-viscosity photoresist are used together as a mask to protect the parts that do not need to be etched. Different from the prior art, it can not only solve the problem that the high-viscosity photoresist has poor fluidity, but also relatively poor uniformity, which causes unclean development and leads to defective products, thereby improving the product yield. At the same time, since the low-viscosity positive photoresist is cheaper than the high-viscosity photoresist, it can also effectively reduce the production cost. In addition, this method is simple to operate, has strong applicability, and is easy to promote widely.
[0063] In some embodiments, the step of sequentially exposing and developing and then etching the substrate 10 to form the isolation groove 60 includes:
[0064] removing a portion of the second positive photoresist 31 by exposure and development in sequence to expose a portion of the initial current blocking layer 50;
[0065] The exposed initial current blocking layer 50 is etched using a BOE solution to obtain a target etching area and expose a portion of the Mesa step 40;
[0066] A photo-induced coupled plasma etching process is used to etch and expose a portion of the Mesa step 40 until the substrate 10 is etched to form an isolation groove 60, and the second positive photoresist 31 and a portion of the initial current blocking layer 50 are etched away to obtain an intermediate current blocking layer of a third preset thickness.
[0067] In some embodiments, the steps of sequentially forming the target current blocking layer 51 by exposure, development and corrosion include:
[0068] removing a portion of the second positive photoresist 31 by sequentially exposing and developing to expose a portion of the intermediate current blocking layer;
[0069] The exposed middle current blocking layer is etched away using the BOE etching solution, and the third positive photoresist 32 is removed to obtain a target current blocking layer 51 with a fourth preset thickness.
[0070] In some embodiments, the first preset thickness is 2um, the second thickness is 2.3um, and the third preset thickness and the fourth preset thickness are both 0.3um.
[0071] In some embodiments, the viscosity of the first positive photoresist, the second positive photoresist 31 and the third positive photoresist 32 are all between 50-400 Cps.
[0072] In some embodiments, the material of the target current blocking layer 51 is SiO 2 、SiN、AlO 2 , Ti 3 O 5 At least one of .
[0073] In some embodiments, the etching gas used in the inductively coupled plasma etching process includes Cl 2 , BCl 3 CF 4 .
[0074] In some embodiments, the Bragg reflection layer 72 includes SiO 2 and Ti 3 O 5 alternately stacked in a preset period.
[0075] In some embodiments, the current transmission metal layer 71 includes an N-type current transmission metal layer and a P-type current transmission metal layer, the bonding metal layer 73 includes an N-type bonding metal layer and a P-type bonding metal layer, the P-type bonding metal layer is electrically connected to the P-type current transmission metal layer, and the N-type bonding metal layer is electrically connected to the N-type current transmission metal layer.
[0076] In some embodiments, the Bragg reflection layer 72 includes a P-type Bragg reflection layer through hole and an N-type Bragg reflection layer through hole, the P-type bonding metal layer is electrically connected to the P-type current transmission metal layer through the P-type Bragg reflection layer through hole, and the N-type bonding metal layer is electrically connected to the N-type current transmission metal layer through the N-type Bragg reflection layer through hole.
[0077] In some embodiments, the steps of sequentially preparing a current spreading layer 70, a current transmission metal layer 71, a Bragg reflection layer 72 and a bonding metal layer 73 on the surface of the target current blocking layer 51 include:
[0078] An ITO (indium tin oxide) layer is prepared on the target current blocking layer 51 by a magnetron sputtering process, a pattern is formed on the ITO layer by a photolithography process, and a portion of the ITO layer is exposed, and the exposed portion of the ITO layer is corroded to form a current spreading layer 70;
[0079] A negative photoresist is coated on the current spreading layer 70, and metal is evaporated on the current spreading layer 70 coated with the negative photoresist. After the evaporation is completed, a part of the metal is stripped off and the negative photoresist is removed to form a current transmission metal layer 71;
[0080] Depositing a Bragg reflection layer 72 on the current transmission metal layer 71 by electron beam evaporation process;
[0081] The negative photoresist is coated on the surface of the Bragg reflection layer 72 , and then subjected to evaporation and lift-off processes to form a bonding metal layer 73 .
[0082] In a preferred embodiment of the present application, the preparation process of the flip-chip light emitting diode chip 100 is as follows:
[0083] Step S201, providing a substrate 10;
[0084] Step S202, depositing an epitaxial layer 20 on the substrate 10, wherein the epitaxial layer 20 includes a buffer layer 21, an N-type semiconductor layer 22, an active layer 23 and a P-type semiconductor layer 24 from top to bottom;
[0085] Step S203, coating the P-type semiconductor layer 24 with a first positive photoresist, then performing exposure and development processes to expose the portion to be etched, and then etching away a portion of the P-type semiconductor layer 24, the active layer 23, and the N-type semiconductor layer 22 using an inductively coupled plasma etching process to form a Mesa step 40, and then removing the first positive photoresist to complete this step. Figure 3 As shown;
[0086] Step S204: Prepare an initial current blocking layer 50 on the surface of the P-type semiconductor layer 24 and the Mesa step 40 by using a PECVD process. The initial current blocking layer 50 includes SiO 2 、Al 2 O 3 、Ti 3 O 5 The initial thickness of the current blocking layer 50 is 2 um. Figure 4 As shown;
[0087] Step S205, coating the surface of the initial current blocking layer 50 with a second positive photoresist 31 having a thickness of 2.5 μm, and then performing exposure and development processes to expose a portion of the initial current blocking layer 50. The structure after completing this step is as follows: Figure 5 As shown;
[0088] Step S206, using BOE etching solution to etch away the exposed portion of the initial current blocking layer 50 to expose a portion of the Mesa step 40. The structure after completing this step is as follows: Figure 6 As shown;
[0089] Step S207, using a photo-inductively coupled plasma etching process to etch away the exposed portion of the Mesa step 40 until the substrate 10 is exposed to obtain the isolation groove 60. At the same time, the second positive photoresist 31 above the initial current blocking layer 50 will be completely etched away, and the initial current blocking layer 50 will also be etched and thinned, leaving a relatively thin initial current blocking layer 50. At this time, the thickness of the etched initial current blocking layer 50 is 0.3 um. The structure after completing this step is as follows: Figure 7 As shown;
[0090] Step S208, coating the third positive photoresist 32 on the surface of the isolation groove 60 and the etched initial current blocking layer 50, and then performing exposure and development processes to expose a portion of the etched initial current blocking layer 50. The structure after completing this step is as follows: Figure 8 As shown;
[0091] Step S209, using BOE etching solution to etch away the exposed initial current blocking layer 50 after etching, and then removing the third positive photoresist 32 to obtain a target current blocking layer 51, the thickness of the target current blocking layer 51 is 0.3um, and the target current blocking layer 51 plays a role of current blocking in the flip-chip light-emitting diode chip 100. The structure after completing this step is as follows: Fig. 9 As shown;
[0092] Step S210, an ITO (indium tin oxide) layer is prepared on the surface of the target current blocking layer 51, the Mesa step 40, the epitaxial layer 20 and the isolation groove 60 by using a magnetron sputtering process, and then a pattern is formed on the surface of the ITO layer by a photolithography process, and a part of the ITO layer is exposed, and then an ITO etching solution is used to remove the exposed ITO layer, and then the photoresist is removed to form a current spreading layer 70;
[0093] Step S211, coating negative photoresist on the surfaces of the current spreading layer 70, the P-type semiconductor layer 24, the Mesa step 40 and the isolation groove 60, then performing exposure and development processes to form a pattern, then using electron beam evaporation process to evaporate metal Cr, Al, Ti, Pt, Ti, Pt, Au, Pt, Ti, then using Lift-Off process to strip off part of the metal, and then removing the negative photoresist to form a current transmission metal layer 71, the current transmission metal layer 71 includes an N-type current transmission metal layer and a P-type current transmission metal layer;
[0094] Step S212, using electron beam evaporation technology to evaporate the Bragg reflection layer 72 on the surface of the current transmission metal layer 71, the current expansion layer 70, the P-type semiconductor layer 24, the Mesa step 40 and the isolation groove 60, and then photolithography to form a pattern on the surface of the Bragg reflection layer 72, and then using an electric discharge coupled plasma etching process to etch to form a Bragg reflection layer 72 through hole, the Bragg reflection layer 72 includes SiO2 and Ti3O5 alternately stacked in a preset period, and the Bragg reflection layer 72 through hole includes an N-type Bragg reflection layer through hole and a P-type Bragg reflection layer through hole;
[0095] Step S213, negative photoresist is then coated on the surface of the Bragg reflector 72, and then exposure and development processes are performed to form a pattern, metal Al, Ti, Pt, Ti, Ni, and Au are evaporated using an electron beam evaporation process, and then a portion of the metal is stripped off using a Lift-Off process, and then the negative photoresist is removed to form a bonding metal layer 73, the bonding metal layer 73 includes an N-type bonding metal layer and a P-type bonding metal layer. After completing this step, Figure 1 , which is a schematic structural diagram of the flip-chip light emitting diode chip 100 finally prepared.
[0096] In the specific implementation, when preparing the isolation groove 60, the initial current blocking layer 50 and the positive low-viscosity photoresist are used together as a mask to protect the parts that do not need to be etched. Different from the existing technology, this solves the problem of using expensive high-adhesion photoresist as a mask to prepare the isolation groove 60, reduces the preparation cost of the flip-chip light-emitting diode chip 100, and at the same time, this method is simple to operate, has strong applicability, and is easy to promote widely.
[0097] The third embodiment of the present invention provides a method for preparing a flip-chip light-emitting diode chip. The steps of the method for preparing a flip-chip light-emitting diode chip shown in this embodiment are basically the same as those of the method for preparing a flip-chip light-emitting diode chip shown in the second embodiment, except that:
[0098] The exposed portion of the initial current blocking layer 50 is etched away by an ICP etching process to expose a portion of the Mesa step 40 .
[0099] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.
[0100] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the patent of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A method for preparing a flip-chip light-emitting diode chip, characterized in that: Used for preparing a flip-chip light-emitting diode chip, the flip-chip light-emitting diode chip comprises a substrate and an epitaxial layer stacked in sequence, characterized in that a Mesa step is formed at the end of the epitaxial layer by etching, an initial current blocking layer and a positive photoresist stacked in sequence are provided on the epitaxial layer and the Mesa step, an isolation groove is formed by etching the initial current blocking layer and the positive photoresist located on at least part of the Mesa step to the substrate, and the viscosity of the positive photoresist is 50-400 Cps; The method comprises the following steps: Obtaining a substrate, and depositing an epitaxial layer on the substrate; Coating a first positive photoresist on the epitaxial layer, and sequentially performing exposure, development and etching to form a Mesa step on the epitaxial layer; Removing the first positive photoresist, and depositing an initial current blocking layer with a first preset thickness on the surface of the Mesa step and the epitaxial layer; A second positive photoresist with a second preset thickness is coated on the initial current blocking layer, and after exposure and development in sequence, the second positive photoresist is etched to the substrate to form an isolation groove; Coating a third positive photoresist on the surface of the etched initial current blocking layer and the isolation groove, and sequentially forming a target current blocking layer by exposure, development and etching, wherein the viscosity of the first positive photoresist, the second positive photoresist and the third positive photoresist is between 50-400 Cps; A current spreading layer, a current transmission metal layer, a Bragg reflection layer and a bonding metal layer are sequentially prepared on the surface of the target current blocking layer.
2. The method for preparing a flip-chip light-emitting diode chip according to claim 1, characterized in that: The flip-chip light-emitting diode chip also includes a target current blocking layer, a current spreading layer, a current transmission metal layer, a Bragg reflection layer and a bonding metal layer, and the target current blocking layer, the current spreading layer, the current transmission metal layer, the Bragg reflection layer and the bonding metal layer are sequentially stacked on the epitaxial layer.
3. The method for preparing a flip-chip light emitting diode chip according to claim 2, characterized in that: The Bragg reflection layer includes SiO2 and Ti3O5 alternately stacked in a preset period.
4. The method for preparing a flip-chip light emitting diode chip according to claim 2, characterized in that: The current transmission metal layer includes an N-type current transmission metal layer and a P-type current transmission metal layer, the bonding metal layer includes an N-type bonding metal layer and a P-type bonding metal layer, the P-type bonding metal layer is electrically connected to the P-type current transmission metal layer, and the N-type bonding metal layer is electrically connected to the N-type current transmission metal layer.
5. The method for preparing a flip-chip light emitting diode chip according to claim 1, characterized in that: The step of etching the substrate to form an isolation groove after sequentially exposing and developing comprises: removing a portion of the second positive photoresist by sequentially exposing and developing to expose a portion of the initial current blocking layer; Using a BOE solution to etch the exposed initial current blocking layer to obtain a target etching area and expose a portion of the Mesa step; A photo-induced coupled plasma etching process is used to etch and expose a portion of the Mesa step until the substrate is etched to form an isolation groove, and the second positive photoresist and a portion of the initial current blocking layer are etched away to obtain an intermediate current blocking layer with a third preset thickness.
6. The method for preparing a flip-chip light emitting diode chip according to claim 5, characterized in that: The step of forming the target current blocking layer by sequentially exposing, developing and etching comprises: removing a portion of the second positive photoresist by sequentially exposing and developing to expose a portion of the intermediate current blocking layer; The exposed middle current blocking layer is etched away using the BOE solution, and the third positive photoresist is removed to obtain a target current blocking layer with a fourth preset thickness.
7. The method for preparing a flip-chip light emitting diode chip according to claim 6, characterized in that: The first preset thickness is 2um, the second preset thickness is 2.3um, and the third preset thickness and the fourth preset thickness are both 0.3um.
8. The method for preparing a flip-chip light emitting diode chip according to claim 1, characterized in that: The material of the target current blocking layer is at least one of SiO2, SiN, AlO2, and Ti3O5.