Colored polyamide resin composition and molded article thereof

By adding high melting point polyamide, inorganic filler materials, phosphinate and phosphite to the polyamide resin composition, and controlling the use of sulfur element and colorant, the flame retardancy of the polyamide resin composition after coloring is solved. Reduce the problem, achieve excellent performance in the reflow soldering process and meet the UL94V-0 standard.

CN115443309BActive Publication Date: 2024-10-29KURARAY CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202180027366.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-04-08
Publication Date
2024-10-29
Estimated Expiration
2041-04-08

AI Technical Summary

Technical Problem

The existing polyamide resin composition has reduced flame retardancy after coloring, making it difficult to meet the UL94V-0 standard, and lacks heat resistance, especially in the reflow soldering process.

Method used

A polyamide resin composition containing high melting point polyamide, inorganic filler materials, phosphinate and phosphite is used, and the flame retardancy and visual recognition of the composition are ensured by controlling the sulfur content and the type and amount of colorants. .

Benefits of technology

A halogen-free polyamide resin composition and its molded body with excellent flame retardancy and visual recognition in the reflow soldering process have been realized, which meet the UL94V-0 standard and have improved heat resistance and mechanical strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FDA0004838471960000011
    Figure FDA0004838471960000011
  • Figure GDA0003880257880000031
    Figure GDA0003880257880000031
  • Figure GDA0003880257880000032
    Figure GDA0003880257880000032
Patent Text Reader

Abstract

A polyamide resin composition and a molded article thereof, wherein the polyamide resin composition comprises 45 to 120 parts by mass of an inorganic filler (B), 25 to 40 parts by mass of at least one phosphinate (C) represented by a specific formula, 2 to 15 parts by mass of a phosphite (D), and a colorant (E) relative to 100 parts by mass of a specific polyamide (A), wherein the polyamide resin composition has a sulfur content of less than 220 ppm by mass, and ΔE represented by the following formula (1) is greater than 1. ΔE=〔(L * co1 ‑L * nat ) 2 +‑(a * col ‑a * nat ) 2 +(b * col ‑b * nat ) 2 〕 1 / 2 (1) In the formula, the symbols are as defined in the specification.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a colored polyamide resin composition and a molded article thereof, and more particularly to a colored halogen-free polyamide resin composition and a molded article thereof that can provide a molded article having excellent flame retardancy. Background Art

[0002] Polyamide has excellent mechanical properties and heat resistance, so it is often used in the field of automobile parts and electrical / electronic parts. In the field of electrical / electronic parts, surface mounting processes with high component mounting efficiency are becoming popular, and heat-resistant polyamides with high heat resistance and excellent strength are becoming popular as the preferred raw materials for forming these parts. In addition, in recent years, from the perspective of reducing environmental load, lead-free solders have been used as solders used in surface mounting processes, but the melting temperature of lead-free solders is relatively high, so it is necessary to set the temperature in the reflow soldering process of the surface mounting process to as high as about 260°C. Therefore, as heat-resistant polyamides for forming components for surface mounting processes, those with relatively high melting points even among heat-resistant polyamides are used.

[0003] Incidentally, in the field of electrical / electronic components, flame retardancy is mostly required for components, and in most cases, it is necessary to achieve the evaluation V-0 in the UL94 standard of UNDERWRITERS LABORATORIES. In the past, as heat-resistant polyamides for forming electrical / electronic components, materials with bromine-based flame retardants were generally used. However, due to the increase in environmental awareness in recent years, the use of several raw materials containing harmful lead, cadmium, etc. is being restricted. For halogen-containing compounds such as bromine-based flame retardants, there is a tendency to avoid their use regardless of the evaluation results of their safety, substantial environmental load, etc., and the demand for halogen-free flame-retardant polyamides is increasing.

[0004] Several halogen-free flame retardants for use with polyamides are known. However, flame retardants for use with heat-resistant polyamides having a high melting point are required to have, in addition to high flame retardancy, high heat resistance that can withstand high temperatures during melt kneading during the manufacture of polyamide resin compositions and during molding during the manufacture of molded products. This tendency is particularly pronounced for electrical / electronic components that undergo a reflow soldering process in a surface mounting process.

[0005] As a flame retardant having high flame retardancy and heat resistance and containing no halogen, phosphinates are known. For example, resin compositions containing specific semi-aromatic polyamide, polyphenylene ether and phosphinates are known (for example, Patent Documents 1 and 2).

[0006] Prior art literature

[0007] Patent Literature

[0008] Patent Document 1: Japanese Patent Application Publication No. 2007-182550

[0009] Patent Document 2: Japanese Patent Application Publication No. 2007-182551

[0010] Patent Document 3: Japanese Patent Application Publication No. 2015-120891

[0011] Patent Document 4: Japanese Patent Application Publication No. 2010-120983

[0012] Patent Document 5: Japanese Patent Application Publication No. 2014-521765

[0013] Patent Document 6: Japanese Patent Application Publication No. 2016-186080 Summary of the invention

[0014] Problems to be solved by the invention

[0015] Regarding the polyamide resin composition containing phosphinate as described above, it is sometimes used after being colored as a component for automobiles or for electrical / electronic components. However, there is a problem that the flame retardancy of the molded body obtained by using the polyamide resin composition containing phosphinate and having excellent visual recognition after coloring is sometimes reduced. For example, when the thickness of the test piece is 0.15 to 3.0 mm, there is a case where the test piece obtained by using the polyamide resin composition containing phosphinate and not using a colorant is suitable for the UL94V-0 standard, but the test piece obtained by using the polyamide resin composition containing phosphinate and a colorant is not suitable for the UL94V-0 standard.

[0016] On the other hand, Patent Document 3 discloses a flame retardant thermoplastic resin composition containing polyphenylene ether, a metal phosphinate and a colorant. However, Patent Document 3 does not mention the influence of the colorant on flame retardancy at all.

[0017] In addition, Patent Document 4 discloses a polyamide resin composition containing a metal phosphinate, a specific rubber, polyphosphate melamine as a flame retardant, and a white pigment. The polyamide resin composition contains polyphosphate melamine, which has poor heat resistance, and is difficult to be used as a resin composition used in a reflow soldering process. In addition, Patent Document 4 does not mention the effect of a colorant on flame retardancy.

[0018] Patent Documents 5 and 6 disclose flame-retardant polyamide compositions having excellent appearance, which contain specific polyamides, flame retardants containing metal phosphinates and colorants. However, Patent Documents 5 and 6 do not mention the influence of colorants on flame retardancy.

[0019] Therefore, an object of the present invention is to provide a halogen-free polyamide resin composition and a molded article thereof which can withstand a reflow process and has excellent flame retardancy and excellent visibility.

[0020] Means for solving problems

[0021] The present inventors have conducted intensive studies to solve the above-mentioned problems, and as a result, have come up with the present invention described below and have found that the problems can be solved.

[0022] That is, the present invention is as follows.

[0023] [1] A polyamide resin composition comprising 45 to 120 parts by mass of an inorganic filler (B), 25 to 40 parts by mass of at least one phosphinate (C) represented by the following formula (I) or (II), 2 to 15 parts by mass of a phosphite (D), and a colorant (E), based on 100 parts by mass of a polyamide (A) having a melting point of 280° C. or higher, wherein the polyamide resin composition has a sulfur content of less than 220 ppm by mass, ΔE represented by the following formula (1) is greater than 1,

[0024] [Chemical formula 1]

[0025]

[0026] [Chemical formula 2]

[0027]

[0028] [In formula (I) and formula (II), R 1 , R 2 , R 4 and R 5 Each independently represents a linear or branched alkyl group having 1 to 16 carbon atoms. 1 With R 2 and R 4 With R 5 They may be bonded to each other to form a ring. 3 represents a linear or branched alkylene group having 1 to 10 carbon atoms, an arylene group having 6 to 10 carbon atoms, an alkylarylene group having 7 to 20 carbon atoms, a cycloalkylene group having 3 to 10 carbon atoms, an arylalkylene group having 7 to 10 carbon atoms, or an arylalkylene group having 7 to 20 carbon atoms. M represents calcium, magnesium, aluminum or zinc. m is an integer of 1 to 4. n is an integer of 1 to 4. x is an integer of 1 to 4. In formula (II), m, x and n satisfy the relationship mx=2n.]

[0029] ΔE=〔(L * col -L * nat ) 2 +(a *col -a * nat ) 2 +(b * col -b * nat ) 2 〕 1 / 2 (1)

[0030] [In formula (1), ΔE is the * a * b * ) Color difference specified by the color system, L * col 、a * col and b * col The polyamide resin composition is * a * b * ) L specified in the color system * 、a * and b * , L * nat 、a * nat and b * nat The polyamide resin composition without colorant is defined by CIE1976 (L * a * b * ) L specified in the color system * 、a * and b * The above-mentioned polyamide resin composition not containing a colorant has the same composition as the above-mentioned polyamide resin composition except that it does not contain a colorant (E).]

[0031] [2] A molded article, which is a molded article of the polyamide resin composition according to [1].

[0032] Effects of the Invention

[0033] According to the present invention, a halogen-free polyamide resin composition and a molded article thereof which can withstand a reflow process and have excellent flame retardancy and excellent visibility can be provided. DETAILED DESCRIPTION

[0034] Hereinafter, description will be given based on an example of an embodiment of the present invention (hereinafter sometimes referred to as "this embodiment"). However, the embodiment described below is an example for embodying the technical idea of ​​the present invention, and the present invention is not limited to the following description.

[0035] In addition, in this specification, the preferred form of the embodiment is shown, but the form obtained by combining two or more independent preferred forms is also a preferred form. For matters shown in numerical ranges, when there are several numerical ranges, their lower limits and upper limits can be selectively combined to be set as a preferred form.

[0036] In addition, in this specification, when there is a description of a numerical range such as "XX to YY", it means "XX or more and YY or less".

[0037] <Polyamide resin composition>

[0038] The polyamide resin composition of the present embodiment is characterized in that, relative to 100 parts by mass of a specific polyamide (A), it contains 45 to 120 parts by mass of an inorganic filler (B), 25 to 40 parts by mass of at least one phosphinate (C) represented by a specific formula, 2 to 15 parts by mass of a phosphite (D), and a colorant (E), the sulfur content of the polyamide resin composition being less than 220 ppm by mass, and ΔE represented by the following formula (1) being greater than 1.

[0039] ΔE=〔(L * col -L * nat ) 2 +(a * col -a * nat ) 2 +(b * col -b * nat ) 2 〕 1 / 2 (1)

[0040] [In formula (1), ΔE is the * a * b * ) Color difference specified by the color system, L * col 、a * col and b * col The polyamide resin composition is * a * b * ) L specified in the color system * 、a * and b * , L * nat 、a* nat and b * nat The polyamide resin composition without colorant is defined by CIE1976 (L * a * b * ) L specified in the color system * 、a * and b * The above-mentioned polyamide resin composition not containing a colorant has the same composition as the above-mentioned polyamide resin composition except that it does not contain a colorant (E).]

[0041] The polyamide resin composition is a halogen-free polyamide resin composition that can withstand a reflow process and has excellent flame retardancy and excellent visual recognition.

[0042] The reason why a molded article of a polyamide resin composition containing a phosphinate and having excellent visibility after being colored also has excellent flame retardancy is not yet clear, but is considered to be as follows.

[0043] The main flame retardant mechanism of phosphinate is the formation of a carbonized layer caused by polyphosphoric acid generated by the decomposition of phosphinate during combustion, which inhibits heat conduction and hinders the thermal decomposition of resin and the combustion accompanying it. In addition, it is believed that in the present invention, not only phosphinate, but also phosphite contained in the polyamide resin composition of the present embodiment also contributes to the improvement of flame retardancy. Specifically, it is believed that phosphite decomposes / foams during combustion, thereby forming a heat insulation layer, which inhibits heat conduction and hinders the thermal decomposition of resin and the combustion accompanying it.

[0044] On the other hand, for colorants, if it is an organic colorant, sulfur is widely used to change the electronic state to adjust the color, and if it is an inorganic colorant, sulfur is widely used in the form of sulfide. In addition, there are cases where sulfur is mixed as an impurity during the manufacture of the colorant. In addition, there are cases where, in addition to the colorant, the catalyst used in the synthesis process of the polyamide resin, other additives, etc. also contain sulfur.

[0045] Considering the above, when sulfur is present in the polyamide resin composition containing phosphinate and phosphite, sulfur radicals are generated during combustion, and it is believed that the sulfur radicals deactivate polyphosphoric acid and phosphorous acid. In this case, it is believed that if the amount of sulfur is large, a sufficient carbonized layer and heat insulating layer cannot be formed, and as a result, the flame retardancy is reduced.

[0046] Therefore, it is considered that in the case of a polyamide resin composition containing a phosphinate and a colorant, by setting the sulfur element content to a specific value, a molded product having excellent flame retardancy can be provided.

[0047] [Polyamide (A)]

[0048] The melting point of the polyamide (A) is 280° C. or higher.

[0049] The melting point of the polyamide (A) is preferably 285° C. or higher, more preferably 295° C. or higher. When the melting point of the polyamide (A) is at least the above temperature, sufficient heat resistance can be maintained even when a molded article of a polyamide resin composition containing the polyamide (A) is used in an application exposed to a heating step such as a reflow step.

[0050] Preferably, the polyamide (A) contains diamine units, and 50 to 100 mol % of the diamine units are aliphatic diamine units having 4 to 18 carbon atoms.

[0051] In addition, the polyamide (A) preferably comprises a dicarboxylic acid unit and a diamine unit, wherein the dicarboxylic acid unit is mainly composed of a unit derived from terephthalic acid, and the diamine unit is mainly composed of a unit derived from at least one selected from aliphatic diamines having 4 to 12 carbon atoms. The melting point of the polyamide is often sufficiently high, and by using the polyamide, a polyamide resin composition can be prepared, and the polyamide resin composition can provide a molded body that can withstand a reflow process.

[0052] Here, "main component" means that other components may be included within the range that does not impair the effect of the present invention. "Main component of dicarboxylic acid unit" refers to preferably 50 to 100 mol%, more preferably 60 to 100 mol%, and further preferably 90 to 100 mol% of all dicarboxylic acid units. In addition, "main component of diamine unit" refers to preferably 50 to 100 mol%, more preferably 60 to 100 mol%, and further preferably 90 to 100 mol% of all diamine units.

[0053] Examples of the dicarboxylic acid units other than the units derived from terephthalic acid include aliphatic dicarboxylic acids such as oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, undecanedicarboxylic acid, dodecanedicarboxylic acid, dimethylmalonic acid, 2,2-diethylsuccinic acid, 2,2-dimethylglutaric acid, 2-methyladipic acid, and trimethyladipic acid; and 1,3-cyclopentanedicarboxylic acid, 1,3- The structural units include alicyclic dicarboxylic acids such as cyclohexanedicarboxylic acid, 1,4-cyclohexanedicarboxylic acid, cycloheptanedicarboxylic acid, cyclooctanedicarboxylic acid, and cyclodecanedicarboxylic acid; aromatic dicarboxylic acids such as isophthalic acid, 1,4-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, 2,7-naphthalenedicarboxylic acid, 2,2'-biphenyldicarboxylic acid, 4,4'-biphenyldicarboxylic acid, diphenylmethane-4,4'-dicarboxylic acid, and diphenylsulfone-4,4'-dicarboxylic acid. These units may be one or two or more.

[0054] Furthermore, the polyamide may contain a structural unit derived from a trivalent or higher-valent carboxylic acid such as trimellitic acid, trimesic acid, or pyromellitic acid within a range that allows melt molding, within a range that does not impair the effects of the present invention.

[0055] Examples of the aliphatic diamine unit having 4 to 18 carbon atoms include linear diamines derived from 1,4-butanediamine, 1,5-pentanediamine, 1,6-hexanediamine, 1,7-heptanediamine, 1,8-octanediamine, 1,9-nonanediamine, 1,10-decanediamine, 1,11-undecanediamine, 1,12-dodecanediamine, 1,13-tridecanediamine, 1,14-tetradecanediamine, 1,15-pentadecanediamine, 1,16-hexadecanediamine, 1,17-heptadecanediamine, 1,18-octadecanediamine, and the like. aliphatic diamines; 1-butyl-1,2-ethylenediamine, 1,1-dimethyl-1,4-butanediamine, 1-ethyl-1,4-butanediamine, 1,2-dimethyl-1,4-butanediamine, 1,3-dimethyl-1,4-butanediamine, 1,4-dimethyl-1,4-butanediamine, 2,3-dimethyl-1,4-butanediamine, 2-methyl-1,5-pentanediamine, 3-methyl-1,5-pentanediamine, 2,5-dimethyl-1,6-hexanediamine, 2,4-dimethyl-1,6-hexanediamine, 3,3-dimethyl-1,6-hexanediamine, 2,2-dimethyl-1,6-hexanediamine, 2,2,4-trimethyl-1,6-hexanediamine, 2,4,4-trimethyl-1,6-hexanediamine, 2,4-diethyl-1,6-hexanediamine, 2,2-dimethyl-1,7-heptanediamine, 2,3-dimethyl-1,7-heptanediamine, 2,4-dimethyl-1,7-heptanediamine, 2,5-dimethyl-1,7-heptanediamine, 2-methyl-1,8-octanediamine, 3-methyl-1,8-octanediamine The structural units include branched aliphatic diamines such as diamine, 4-methyl-1,8-octanediamine, 1,3-dimethyl-1,8-octanediamine, 1,4-dimethyl-1,8-octanediamine, 2,4-dimethyl-1,8-octanediamine, 3,4-dimethyl-1,8-octanediamine, 4,5-dimethyl-1,8-octanediamine, 2,2-dimethyl-1,8-octanediamine, 3,3-dimethyl-1,8-octanediamine, 4,4-dimethyl-1,8-octanediamine and 5-methyl-1,9-nonanediamine.

[0056] Among them, from the viewpoint of heat resistance to withstand the reflow process and flame retardancy of the molded article of the polyamide resin composition, a structural unit derived from at least two selected from 1,8-octanediamine, 2-methyl-1,8-octanediamine, 1,9-nonanediamine, 1,10-decanediamine, 1,11-undecanediamine and 1,12-dodecanediamine is preferred, and a structural unit derived from at least two selected from 1,9-nonanediamine, 2-methyl-1,8-octanediamine and 1,10-decanediamine is more preferred.

[0057] In particular, from the viewpoint of heat resistance to withstand the reflow process and flame retardancy of the molded product of the polyamide resin composition, it is preferred that the diamine unit contains a unit derived from an aliphatic diamine having 9 carbon atoms, more preferably the main component of the diamine unit is a unit derived from at least two types selected from aliphatic diamines having 9 carbon atoms, and further preferably the diamine unit contains 60 to 100 mol % of 1,9-nonanediamine units and 2-methyl-1,8-octanediamine units.

[0058] When the diamine units contain 60 to 100 mol% of the structural units derived from 1,9-nonanediamine and the structural units derived from 2-methyl-1,8-octanediamine in total, the molar ratio of the structural units derived from 1,9-nonanediamine to the structural units derived from 2-methyl-1,8-octanediamine is preferably in the range of 30:70 to 95:5 (structural units derived from 1,9-nonanediamine:structural units derived from 2-methyl-1,8-octanediamine), more preferably in the range of 50:50 to 90:10, and even more preferably in the range of 70:30 to 90:10. Within the above molar ratio range, the melting point of the polyamide (A) does not become too low, and it is particularly suitable to be set to a temperature that can withstand the reflow process.

[0059] The diamine units in the polyamide (A) may contain diamine units other than aliphatic diamine units having 4 to 18 carbon atoms, within the range not impairing the effects of the present invention. Examples of such diamine units include structural units derived from aliphatic diamines such as ethylenediamine, 1,2-propylenediamine, and 1,3-propylenediamine; alicyclic diamines such as cyclohexanediamine, methylcyclohexanediamine, isophoronediamine, norbornanedimethylamine, and tricyclodecanedimethyldiamine; and aromatic diamines such as p-phenylenediamine, m-phenylenediamine, p-phenylenediamine, m-phenylenediamine, 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenylsulfone, and 4,4'-diaminodiphenylether. These units may be one or more.

[0060] The polyamide (A) may contain an aminocarboxylic acid unit. Examples of the aminocarboxylic acid unit include units derived from lactams such as caprolactam and laurolactam; and aminocarboxylic acids such as 11-aminoundecanoic acid and 12-aminododecanoic acid. The content of the aminocarboxylic acid unit in the polyamide is preferably 40 mol% or less, more preferably 20 mol% or less, relative to 100 mol% of the total of the dicarboxylic acid unit and the diamine unit of the polyamide.

[0061] The polyamide (A) may contain units derived from a terminal blocking agent. The units derived from the terminal blocking agent are preferably 1.0 to 10 mol %, more preferably 2.0 to 7.5 mol %, and even more preferably 2.5 to 6.5 mol % relative to the diamine units.

[0062] The units derived from the end-capping agent can be made into the above-mentioned desired range by adding the end-capping agent in a manner that is within the above-mentioned desired range relative to the diamine when the polymerization raw materials are added. It should be noted that, considering that the monomer components volatilize during polymerization, it is desirable to slightly adjust the amount of the end-capping agent added when the polymerization raw materials are added so that the desired amount of units derived from the end-capping agent is introduced into the obtained resin.

[0063] As a method for obtaining the content of the unit derived from the end-capping agent in the polyamide (A), for example, there can be mentioned a method of measuring the solution viscosity, calculating the total terminal group amount from the relationship between the solution viscosity and the number average molecular weight, and subtracting the amino group amount and the carboxyl group amount obtained by titration from the solution viscosity as shown in Japanese Patent Application Laid-Open No. 07-228690; using 1 H-NMR, and a method of obtaining based on the integrated value of the signals corresponding to the diamine unit and the unit derived from the terminal blocking agent, etc.

[0064] As the end-capping agent, a monofunctional compound having reactivity with a terminal amino group or a terminal carboxyl group can be used. Specifically, monocarboxylic acids, acid anhydrides, monoisocyanates, monoacyl halides, monoesters, monoalcohols, monoamines, etc. can be cited. From the viewpoints of reactivity and stability of the end-capping, monocarboxylic acids are preferred as the end-capping agent for the terminal amino group, and monoamines are preferred as the end-capping agent for the terminal carboxyl group. In addition, from the viewpoints of ease of handling, monocarboxylic acids are more preferred as the end-capping agent.

[0065] The monocarboxylic acid used as the end-capping agent is not particularly limited as long as it is reactive with an amino group, and examples thereof include aliphatic monocarboxylic acids such as acetic acid, propionic acid, butyric acid, valeric acid, caproic acid, caprylic acid, lauric acid, tridecanoic acid, myristic acid, palmitic acid, stearic acid, pivalic acid, and isobutyric acid; alicyclic monocarboxylic acids such as cyclopentanecarboxylic acid and cyclohexanecarboxylic acid; aromatic monocarboxylic acids such as benzoic acid, toluic acid, α-naphthoic acid, β-naphthoic acid, methylnaphthoic acid, and phenylacetic acid; and any mixture thereof. Among these, at least one selected from the group consisting of acetic acid, propionic acid, butyric acid, valeric acid, caproic acid, caprylic acid, lauric acid, tridecanoic acid, myristic acid, palmitic acid, stearic acid, and benzoic acid is preferred in terms of reactivity, stability of the end-capping, price, and the like.

[0066] The monoamine used as the end-capping agent is not particularly limited as long as it is reactive with the carboxyl group, and examples thereof include aliphatic monoamines such as methylamine, ethylamine, propylamine, butylamine, hexylamine, octylamine, decylamine, stearylamine, dimethylamine, diethylamine, dipropylamine, and dibutylamine; alicyclic monoamines such as cyclohexylamine and dicyclohexylamine; aromatic monoamines such as aniline, toluidine, diphenylamine, and naphthylamine; and any mixtures thereof. Among these, at least one selected from butylamine, hexylamine, octylamine, decylamine, stearylamine, cyclohexylamine, and aniline is preferred in terms of reactivity, high boiling point, stability of the end-capping, and price.

[0067] The polyamide (A) can be produced by any method known as a method for producing polyamides, for example, by a solution polymerization method or an interfacial polymerization method using an acid chloride and a diamine as raw materials, a melt polymerization method using a dicarboxylic acid and a diamine as raw materials, a solid phase polymerization method, or a melt extrusion polymerization method.

[0068] Polyamide (A) can be produced, for example, by the following method: first, after adding diamine, dicarboxylic acid, and, if necessary, a catalyst and a capping agent together to produce a nylon salt, heat polymerization is carried out at a temperature of 200 to 250° C. to prepare a prepolymer, and further solid phase polymerization is carried out, or polymerization is carried out using a melt extruder. In the case of the final stage of polymerization by solid phase polymerization, it is preferably carried out under reduced pressure or under the flow of an inert gas. If the polymerization temperature is in the range of 200 to 280° C., the polymerization rate is large, the productivity is excellent, and coloring and gelation can be effectively suppressed. As the polymerization temperature in the final stage of polymerization by a melt extruder, it is preferably 370° C. or less. If polymerization is carried out under such conditions, a polyamide with little decomposition and little deterioration can be obtained.

[0069] Examples of the catalyst that can be used in the production of polyamide (A) include phosphoric acid, phosphorous acid, hypophosphorous acid, and salts or esters thereof. Examples of the salts or esters include salts of phosphoric acid, phosphorous acid or hypophosphorous acid with a metal such as potassium, sodium, magnesium, vanadium, calcium, zinc, cobalt, manganese, tin, tungsten, germanium, titanium, antimony, etc.; ammonium salts of phosphoric acid, phosphorous acid or hypophosphorous acid; and ethyl, isopropyl, butyl, hexyl, isodecyl, octadecyl, decyl, stearyl, phenyl, etc., of phosphoric acid, phosphorous acid or hypophosphorous acid.

[0070] The polyamide (A) may contain any of crystalline polyamide, amorphous polyamide, and a mixture thereof within a range not impairing the effects of the present invention.

[0071] Examples of the crystalline polyamide include polycaproamide (polyamide 6), polyhexamethylene adipamide (polyamide 66), polytetramethylene adipamide (polyamide 46), polyhexamethylene sebacamide (polyamide 610), polyhexamethylene dodecanedioic acid (polyamide 612), polyundecamethylene adipamide (polyamide 116), polybis(4-aminocyclohexyl)methane dodecanamide (polyamide PACM12), polybis(3-methyl-4-aminocyclohexyl)methane dodecanamide (polyamide dimethyl PACM12), polyundecamethylene terephthalamide (polyamide 11T), Polyhexahydroterephthalamide undecaprylidene (polyamide 11T (H)), polyundecamide (polyamide 11), polydodecanamide (polyamide 12), polytrimethylhexamethylene terephthalamide (polyamide TMDT), polymethylene adipamide (polyamide MXD6), polyhexamethylene terephthalamide (polyamide 6T), polyhexamethylene isophthalamide (polyamide 6I), copolymers of polyamide 6I and polyamide 6T (polyamide 6I / 6T), and copolymers of polyamide 6T and polyundecamide (polyamide 11) (polyamide 6T / 11), as well as copolymers and mixtures thereof. It should be noted that the above-mentioned crystalline polyamide also includes substances obtained by replacing the benzene rings of terephthalic acid and / or isophthalic acid with alkyl groups or halogen atoms. The crystalline polyamide can be used alone or in combination of multiple types.

[0072] Examples of the amorphous polyamide include condensates of terephthalic acid / isophthalic acid / hexamethylenediamine, condensates of terephthalic acid / isophthalic acid / hexamethylenediamine / bis(3-methyl-4-aminocyclohexyl)methane, condensates of terephthalic acid / 2,2,4-trimethyl-1,6-hexamethylenediamine / 2,4,4-trimethyl-1,6-hexamethylenediamine, and condensates of isophthalic acid / hexamethylenediamine / bis(3-methyl-4-aminocyclohexyl)methane. Formic acid / bis(3-methyl-4-aminocyclohexyl)methane / ω-laurolactam condensation product, isophthalic acid / 2,2,4-trimethyl-1,6-hexanediamine / 2,4,4-trimethyl-1,6-hexanediamine condensation product, terephthalic acid / isophthalic acid / 2,2,4-trimethyl-1,6-hexanediamine / 2,4,4-trimethyl-1,6-hexanediamine condensation product, etc. It should be noted that the above-mentioned amorphous polyamide also includes substances obtained by replacing the benzene ring of terephthalic acid and / or isophthalic acid with an alkyl group or a halogen atom. Amorphous polyamides can be used alone or in combination.

[0073] [Inorganic filler (B)]

[0074] Examples of the inorganic filler (B) include various clay minerals such as carbon nanotubes, fullerenes, talc, wollastonite, zeolite, sericite, mica, kaolin, clay, pyrophyllite, silicon dioxide, bentonite, aluminum silicate, silicon oxide, magnesium oxide, aluminum oxide, magnesium carbonate, dolomite, calcium sulfate, calcium hydroxide, magnesium hydroxide, aluminum hydroxide, milled fibers, glass powder, ceramic beads, boron nitride, silicon carbide, halloysite, vermiculite, and glass fibers. These inorganic fillers may be used alone or in combination of two or more.

[0075] From the viewpoint of the molding processability of the polyamide resin composition and the mechanical strength of the molded body of the polyamide resin composition, the inorganic filler (B) is preferably at least one selected from glass fibers having a circular cross-section or glass fibers having a non-circular cross-section (hereinafter, they may be simply referred to as glass fibers).

[0076] The cross-sectional shape of the glass fiber having a circular cross section may be, for example, a true circle or a substantially circular shape. The cross-sectional shape of the glass fiber having a non-circular cross section may be, for example, a cocoon shape in which the central portion of the long side direction of the cross section becomes thinner, an oblong shape having substantially parallel portions at positions symmetrical to the center of gravity of the cross section, or an ellipse.

[0077] In view of the moldability of the polyamide resin composition and the mechanical strength of a molded product of the polyamide resin composition, the inorganic filler (B) is preferably glass fiber having a circular cross section or glass fiber having a non-circular cross section.

[0078] When the above-mentioned inorganic filler (B) is a glass fiber with a circular cross-section and a glass fiber with a non-circular cross-section, the outer circumferential length of the cross-section of the glass fiber with the non-circular cross-section is preferably: 1.05 to 1.8 times the outer circumferential length of the glass fiber with a circular cross-section having the same cross-sectional area as the glass fiber with the non-circular cross-section.

[0079] In addition, when the above-mentioned inorganic filler (B) is glass fiber with a circular cross-section and glass fiber with a non-circular cross-section, the ratio of their contents is not particularly limited, but the mass ratio of glass fiber with a circular cross-section / glass fiber with a non-circular cross-section is preferably 20 / 80 to 80 / 20, more preferably 30 / 70 to 60 / 40, and further preferably 30 / 70 to 50 / 50.

[0080] The average fiber length of the glass fiber is preferably 1.0 to 10 mm, more preferably 1.0 to 7.0 mm, and further preferably 2.0 to 4.0 mm.

[0081] From the viewpoint of flame retardancy, mechanical strength, and appearance of a molded article of the polyamide resin composition, the average fiber diameter of the glass fiber is preferably 6 to 20 μm, more preferably 7 to 16 μm, and even more preferably 8 to 14 μm.

[0082] The average fiber length and average fiber diameter of the glass fibers can be determined by measuring the fiber length and fiber diameter of each of 400 randomly selected glass fibers by image analysis using electron microscopy and calculating the weight average values ​​of the respective fiber lengths and fiber diameters.

[0083] The polyamide resin composition contains 45 to 120 parts by mass of inorganic filler (B) relative to 100 parts by mass of polyamide (A). If the above-mentioned content of the inorganic filler (B) is 45 parts by mass or more, the molded body of the polyamide resin composition can obtain sufficient strength, and can obtain practical strength that can withstand connectors, etc. In addition, if the above-mentioned content is 120 parts by mass or less, the fluidity of the polyamide resin composition becomes good, the molding processability is excellent, and the composite productivity is also excellent. The above-mentioned content of the inorganic filler (B) is preferably 48 parts by mass or more, and more preferably 50 parts by mass or more. In addition, the above-mentioned content of the inorganic filler (B) is preferably 100 parts by mass or less, and more preferably 80 parts by mass or less.

[0084] [Phosphinate (C)]

[0085] The polyamide resin composition contains 25 to 40 parts by mass of the phosphinate (C) based on 100 parts by mass of the polyamide (A), thereby making it a halogen-free polyamide resin composition that can provide a molded article having excellent flame retardancy.

[0086] The phosphinate (C) is at least one of the following formula (I) or (II). That is, the phosphinate (C) is a phosphinate represented by the following formula (I), a diphosphinate represented by the following formula (II), or a mixture thereof.

[0087] [Chemical formula 3]

[0088]

[0089] [Chemical formula 4]

[0090]

[0091] In formula (I) and formula (II), R 1 , R 2 , R 4 and R 5Each independently represents a linear or branched alkyl group having 1 to 16 carbon atoms. Among them, an alkyl group having 1 to 8 carbon atoms is preferred, and a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, a tert-butyl group, an n-pentyl group, and an n-octyl group is more preferred, and an ethyl group is further preferred. 1 With R 2 and R 4 With R 5 They may be bonded to each other to form a ring.

[0092] R 3 It represents a linear or branched alkylene group having 1 to 10 carbon atoms, an arylene group having 6 to 10 carbon atoms, an alkylarylene group having 7 to 20 carbon atoms, a cycloalkylene group having 3 to 10 carbon atoms, an aralkylene group having 7 to 10 carbon atoms, or an arylalkylene group having 7 to 20 carbon atoms.

[0093] Examples of the linear or branched alkylene group having 1 to 10 carbon atoms include methylene, ethylene, n-propylene, isopropylene, isopropylidene, n-butylene, tert-butylene, n-pentylene and n-octylene.

[0094] Examples of the arylene group having 6 to 10 carbon atoms include a phenylene group and a naphthylene group.

[0095] Examples of the alkylarylene group having 7 to 10 carbon atoms include methylphenylene, ethylphenylene, tert-butylphenylene, methylnaphthylene, ethylnaphthylene and tert-butylnaphthylene.

[0096] Examples of the cycloalkylene group having 3 to 10 carbon atoms include cyclohexylene and cyclohexanedimethylene.

[0097] Examples of the aralkylene group having 7 to 10 carbon atoms include phenylenemethylene, phenyleneethylene and xylylene.

[0098] Examples of the arylalkylene group having 7 to 20 carbon atoms include phenylmethylene, phenylethylene, phenylpropylene and phenylbutylene.

[0099] M represents calcium, aluminum, magnesium or zinc, preferably aluminum or zinc, more preferably aluminum.

[0100] m is an integer of 1 to 4. n is an integer of 1 to 4. x is an integer of 1 to 4. In formula (II), m, x, and n satisfy the relationship of mx=2n (ie, the product of m and x is equal to the product of 2 and n).

[0101] Examples of the phosphinic acid constituting the phosphinic acid salt (C) include dimethylphosphinic acid, methylethylphosphinic acid, diethylphosphinic acid, methyl-n-propylphosphinic acid, methylisobutylphosphinic acid, methyloctylphosphinic acid, methylphenylphosphinic acid and diphenylphosphinic acid. Among them, diethylphosphinic acid is preferred.

[0102] Specific examples of the phosphinate represented by the above formula (I) include calcium dimethylphosphinate, magnesium dimethylphosphinate, aluminum dimethylphosphinate, zinc dimethylphosphinate, calcium methylethylphosphinate, magnesium methylethylphosphinate, aluminum methylethylphosphinate, zinc methylethylphosphinate, calcium diethylphosphinate, magnesium diethylphosphinate, aluminum diethylphosphinate, zinc diethylphosphinate, calcium methyl-n-propylphosphinate, magnesium methyl-n-propylphosphinate, aluminum methyl-n-propylphosphinate, zinc methyl-n-propylphosphinate, calcium methylphenylphosphinate, magnesium methylphenylphosphinate, aluminum methylphenylphosphinate, zinc methylphenylphosphinate, calcium diphenylphosphinate, magnesium diphenylphosphinate, aluminum diphenylphosphinate, and zinc diphenylphosphinate.

[0103] Examples of the diphosphinic acid constituting the diphosphinate include methanedi(methylphosphinic acid) and benzene-1,4-di(methylphosphinic acid).

[0104] Specific examples of the diphosphinate represented by the above formula (II) include calcium methanedi(methylphosphinate), magnesium methanedi(methylphosphinate), aluminum methanedi(methylphosphinate), zinc methanedi(methylphosphinate), calcium benzene-1,4-di(methylphosphinate), magnesium benzene-1,4-di(methylphosphinate), aluminum benzene-1,4-di(methylphosphinate), and zinc benzene-1,4-di(methylphosphinate).

[0105] The phosphinate (C) may be used alone or in combination of two or more.

[0106] As the phosphinate (C), from the viewpoint of further excellent flame retardancy, aluminum diethylphosphinate, zinc diethylphosphinate, aluminum methanedi(methylphosphinate), and zinc methanedi(methylphosphinate) are preferred. Among them, aluminum diethylphosphinate is more preferred.

[0107] From the viewpoint of flame retardancy, mechanical strength, and appearance of the molded body of the polyamide resin composition, the number average particle size of the phosphinate (C) is preferably 100 μm or less, more preferably 50 μm or less, and further preferably 40 μm or less. The lower limit of the number average particle size is preferably 1 μm or more, more preferably 5 μm or more, and further preferably 10 μm or more. By using a powder having a number average particle size in the above range, not only higher flame retardancy can be exhibited, but also the mechanical strength of the obtained molded body can be further improved.

[0108] In addition, the number average particle size is a particle size value at a weight accumulation of 50% when the particle size distribution is measured using a particle size distribution measuring device such as a laser scattering particle size analyzer.

[0109] The polyamide resin composition contains 25 to 40 parts by mass of phosphinate (C) relative to 100 parts by mass of polyamide (A). If the above content of the phosphinate (C) is 25 parts by mass or more, the molded body of the polyamide resin composition has excellent flame retardancy. In addition, if the above content is 40 parts by mass or less, the molding processability of the polyamide resin composition is excellent, and the mechanical strength of the molded body of the polyamide resin composition is excellent. The above content of the phosphinate (C) is preferably 26 parts by mass or more, and more preferably 27 parts by mass or more. In addition, the above content of the phosphinate (C) is preferably 38 parts by mass or less, and more preferably 35 parts by mass or less.

[0110] [Phosphite (D)]

[0111] The polyamide resin composition contains 2 to 15 parts by mass of the phosphite (D) based on 100 parts by mass of the polyamide (A), thereby exhibiting excellent flame retardancy and improving melt kneading and molding processability of the polyamide resin composition.

[0112] The phosphite (D) is not particularly limited, and examples thereof include sodium phosphite, potassium phosphite, calcium phosphite, zinc phosphite, ammonium phosphite, aluminum phosphite, and aluminum hydrogen phosphite. From the viewpoint of exerting further excellent flame retardancy, aluminum phosphite and aluminum hydrogen phosphite are preferred. The phosphite (D) may be used alone or in combination of multiple types.

[0113] The polyamide resin composition contains 2 to 15 parts by mass of phosphite (D) relative to 100 parts by mass of polyamide (A). If the above content of phosphite (D) is 2 parts by mass or more, the molded body of the polyamide resin composition has excellent flame retardancy. In addition, if the above content is 15 parts by mass or less, the molding processability of the polyamide resin composition is excellent, and the mechanical strength of the molded body of the polyamide resin composition is excellent. The above content of phosphite (D) is preferably 2.5 parts by mass or more, and more preferably 3 parts by mass or more. The above content of phosphite (D) is preferably 13 parts by mass or less, and more preferably 10 parts by mass or less.

[0114] In the polyamide resin composition, the sum of the above-mentioned phosphinate (C) and the above-mentioned phosphite (D) is preferably 16 to 25% by mass relative to 100% by mass of the polyamide resin composition. If the sum of the above-mentioned contents of phosphinate (C) and phosphite (D) is 16% by mass or more, the molded body of the polyamide resin composition has excellent flame retardancy. In addition, if the sum of the above-mentioned contents is 25% by mass or less, the molding processability of the polyamide resin composition is excellent, and the mechanical strength of the molded body of the polyamide resin composition is excellent. The sum of the above-mentioned contents is preferably 16.5% by mass or more, more preferably 17% by mass or more. In addition, the sum of the above-mentioned contents is preferably 23% by mass or less, more preferably 22.5% by mass or less.

[0115] In the polyamide resin composition, the mass ratio (C) / (D) of the phosphinate (C) to the phosphite (D) is preferably 70 / 30 to 94 / 6. If the mass ratio is within the above range, the molded article of the polyamide resin composition has excellent flame retardancy. The mass ratio is preferably 75 / 25 to 93 / 7, and more preferably 80 / 20 to 92 / 8.

[0116] [Colorant (E)]

[0117] By adding a colorant (E) to the polyamide resin composition, various colors can be exhibited, and visual recognition and decorative properties can be imparted. The colorant (E) is not particularly limited, and examples thereof include organic colorants such as organic dyes and organic pigments, and inorganic colorants such as inorganic pigments. It should be noted that the colorant (E) does not include carbon black.

[0118] In one aspect of the present invention, the colorant (E) contains an organic colorant. The colorant (E) may also be an organic colorant.

[0119] In another aspect of the present invention, the colorant (E) contains an inorganic colorant. The colorant (E) may also be an inorganic colorant.

[0120] Examples of organic dyes include anthraquinone dyes, perinone dyes, anthrapyridone dyes, formaldehyde dyes, azine dyes, azo dyes, azomethine dyes, phthalocyanine dyes, quinoneimine dyes, quinoline dyes, nitro dyes, indigo dyes, and oxazine dyes.

[0121] Among these, anthraquinone dyes, perinone dyes, anthrapyridone dyes and phthalocyanine dyes are preferred from the viewpoint of heat resistance to withstand the reflow process, color development and compatibility, and anthraquinone dyes, perinone dyes and anthrapyridone dyes are more preferred.

[0122] Specific examples of the anthraquinone-based dye include Solvent Red 169, Solvent Red 172, Solvent Orange 63, Solvent Blue 101, Solvent Blue 102, Solvent Yellow 98, and the like.

[0123] Specific examples of the perinone-based dye include Solvent Red 179 and the like.

[0124] Specific examples of the anthrapyridone dye include Solvent Red 52 and the like.

[0125] Specific examples of the formazan-based dye include nigrosine compounds such as Solvent Black 5.

[0126] Specific examples of the phthalocyanine dye include Solvent Blue 38 and the like.

[0127] Among these, Solvent Red 52, Solvent Red 169, Solvent Red 172, Solvent Red 179, and Solvent Blue 101 are preferred, and Solvent Red 52 and Solvent Red 179 are more preferred, from the viewpoint of flame retardancy of a molded article of the polyamide resin composition.

[0128] Examples of the organic pigment include azo pigments such as azo lake pigments, insoluble monoazo pigments, insoluble disazo pigments, and chelated azo pigments; phthalocyanine pigments, perylene pigments, perinone pigments, anthraquinone pigments, quinacridone pigments, dioxazine pigments, thioindigo pigments, isoindolinone pigments, quinophthalone pigments, diketopyrrolopyrrole pigments, benzimidazolone pigments, and slen pigments.

[0129] Among these, from the viewpoints of heat resistance to withstand a reflow process, color development, and compatibility, azo pigments and phthalocyanine pigments are preferred, and phthalocyanine pigments are more preferred.

[0130] Specific examples of the phthalocyanine pigment include Pigment Blue 15, and Pigment Blue 15 is preferred from the viewpoint of flame retardancy of a molded article of the polyamide resin composition.

[0131] From the viewpoint of obtaining a polyamide resin composition having excellent visibility, the content of the organic colorant in the colorant (E) is preferably 0.01 to 100% by mass, and more preferably 1 to 100% by mass.

[0132] Examples of inorganic pigments include metal oxides such as titanium oxide (TiO, Ti2O3, TiO2), zinc oxide (Pb3O4), iron oxide (Fe2O3), antimony oxide, and zirconium oxide, ultramarine (Pigment Blue 29), zinc sulfide, zinc phosphate, barium sulfate, manganese phosphate, cobalt aluminate, cobalt stannate, cobalt zincate, antimony oxide, antimony sulfide, cerium sulfide, lanthanum sulfide, chromium oxide, zinc chromate, and composite metal oxides containing a plurality of oxides of nickel, bismuth, vanadium, molybdenum, cadmium, titanium, zinc, manganese, cobalt, iron, chromium, antimony, magnesium, and aluminum. Specific examples of composite metal oxides include Pigment Yellow 53, Pigment Green 50, Pigment Brown 24, Pigment Blue 28, and Pigment Blue 36.

[0133] Among these, metal oxides and composite metal oxides are preferred. From the viewpoint of flame retardancy of a molded article of the polyamide resin composition, titanium oxide (TiO, Ti2O3, TiO2), iron oxide (Fe2O3), Pigment Yellow 53, Pigment Green 50, and Pigment Brown 24 are preferred.

[0134] From the viewpoint of obtaining a polyamide resin composition having excellent visibility, the content of the inorganic colorant in the colorant (E) is preferably 20 to 100% by mass, more preferably 30 to 100% by mass, and even more preferably 50 to 100% by mass.

[0135] The colorant (E) may be used alone or in combination of two or more. However, from the viewpoint of providing a polyamide resin composition having a rich color variation, the colorant (E) preferably contains an organic colorant and an inorganic colorant. When the colorant (E) contains an organic colorant and an inorganic colorant, the weight ratio of the organic colorant to the inorganic colorant is preferably 1 / 1 to 1 / 30, and more preferably 1 / 1 to 1 / 15.

[0136] The colorant (E) may be used in any form of powder, liquid or masterbatch. In order to improve dispersibility, wax may be added or mixed in advance.

[0137] From the viewpoint of flame retardancy, color development and mechanical strength of the molded article of the polyamide resin composition, the content of the colorant (E) is preferably 0.001 to 5.0% by mass, more preferably 0.01 to 3.0% by mass, for an organic colorant, and preferably 0.01 to 5.0% by mass, more preferably 0.05 to 5.0% by mass, for an inorganic colorant, relative to 100% by mass of the polyamide resin composition.

[0138] [Other ingredients]

[0139] The polyamide resin composition may contain other components such as a resin other than the polyamide (A), an antioxidant, and a release agent, within a range not impairing the effects of the present invention.

[0140] As resins other than polyamide (A), for example, polycarbonate; modified polyphenylene ether; polyphenylene ether; polyacetal; polyphenylene sulfide (PPS); polysulfone (Japanese: ポリサルホン); polyethersulfone; polysulfone; polyarylate; cyclic polyolefin; polyetherimide; syndiotactic polystyrene; brominated polystyrene; polyamideimide; polyimide; liquid crystal polymers such as aromatic polyesters and aromatic polyester amides; polyaminobismaleimide; aromatic polyetherketones such as polyetheretherketone and polyetherketone, etc.

[0141] Examples of the antioxidant include hindered phenol compounds, phosphorus compounds, lactone compounds, and hydroxy compounds.

[0142] Examples of the release agent include silicone-based, fluorine-based, long-chain alkyl-based, and fatty acid amide-based release agents.

[0143] The polyamide resin composition may further contain other components such as a heat stabilizer, a light stabilizer, a styrene-maleic anhydride copolymer (SMA), a lubricant, a nucleating agent, a crystallization delaying material, an anti-hydrolysis agent, an antistatic agent, a free radical inhibitor, a matting agent, an ultraviolet absorber, an anti-drip agent, and a slip imparting agent as needed.

[0144] The content of other components in the polyamide resin composition may be within a range that does not impair the effects of the present invention, and is preferably 10% by mass or less, more preferably 5% by mass or less, from the viewpoint of flame retardancy of a molded article of the polyamide resin composition.

[0145] [Sulfur content]

[0146] The sulfur content in the polyamide resin composition of the present invention is less than 220 mass ppm. From the viewpoint of flame retardancy of a molded article of the polyamide resin composition, the sulfur content in the polyamide resin composition is preferably less than 210 mass ppm, more preferably less than 200 mass ppm. In addition, from the viewpoint of ease of manufacture, it is preferably 20 mass ppm or more, more preferably 50 mass ppm or more, and further preferably 70 mass ppm or more.

[0147] The total content of the polyamide (A), the inorganic filler (B), the phosphinate (C), the phosphite (D) and the colorant (E) is preferably 90 to 99.9% by mass, more preferably 95 to 99.9% by mass, and further preferably 95 to 99.7% by mass relative to 100% by mass of the polyamide resin composition. If the total content is within the above range, it is suitable as a polyamide resin composition for providing a molded body having better flame retardancy.

[0148] Regarding the strength of the polyamide resin composition, considering the use as connectors and structural parts of automobiles and electric / electronic parts, the tensile strength at break in a tensile test according to ISO 527 is 80 MPa or more, preferably 90 MPa or more, and more preferably 100 MPa or more.

[0149] The polyamide resin composition of the present invention has ΔE represented by the following formula (1) greater than 1. When ΔE is greater than 1, the polyamide resin composition has excellent visibility. In addition, the inorganic filler (B) and the colorant (E) can be selected so as to satisfy the above requirements.

[0150] ΔE=〔(L * col -L * nat ) 2 +(a * col -a * nat ) 2 +(b * col -b * nat ) 2 〕 1 / 2 (1)

[0151] In formula (1), ΔE is the CIE1976 (L * a * b * ) represents the color difference specified in the color system.

[0152] L * col 、a * col and b * col The polyamide resin composition of the present invention is * a * b * ) L specified in the color system * 、a * and b *That is, the polyamide resin composition of the present invention is * a * b * ) L specified in the color system * For L * col , a * for a * col , b * for b * col .

[0153] L * nat 、a * nat and b * nat The polyamide resin composition without colorant having the same composition as the above polyamide resin composition except that the colorant (E) is not contained is a polyamide resin composition without colorant having the same composition as the above polyamide resin composition according to CIE1976 (L * a * b * ) L specified in the color system * 、a * and b * That is, the polyamide resin composition without colorant having the same composition as the above polyamide resin composition except that the colorant (E) is not contained is measured by CIE1976 (L * a * b * ) L specified in the color system * For L * nat , a * for a * nat , b * for b * nat .

[0154] In the polyamide resin composition of the present invention, ΔE represented by formula (1) is preferably greater than 3, more preferably greater than 10, and even more preferably greater than 30, from the viewpoint of improving visibility.

[0155] [Method for producing polyamide resin composition]

[0156] The method for producing the polyamide resin composition is not particularly limited, and a known method can be used. For example, the obtained polyamide resin composition can contain 45 to 120 parts by mass of an inorganic filler (B), 25 to 40 parts by mass of at least one phosphinate (C) represented by the above formula (I) or the above formula (II), 2 to 15 parts by mass of a phosphite (D), and a colorant (E) relative to 100 parts by mass of a polyamide (A) having a melting point of 280°C or more, and the sulfur content is less than 220 parts by mass, and the ΔE represented by the above formula (1) is greater than 1, and a mixture obtained by dry-mixing polyamide (A), inorganic filler (B), phosphinate (C), phosphite (D), colorant (E), and other components as required is melt-kneaded, thereby producing a polyamide resin composition.

[0157] The method of melt mixing is not particularly limited, and the method that can evenly mix the above-mentioned components can be preferably adopted. For example, preferably a single-screw extruder, a twin-screw extruder, a kneader, a Banbury mixer etc., from the viewpoint of good dispersibility of flame retardant and colorant and industrial productivity, a twin-screw extruder is more preferred.

[0158] <molded body>

[0159] After the polyamide resin composition is produced, for example, the pelletized polyamide resin composition can be supplied to various molding methods to obtain a molded body. The molding method of the molded body can be appropriately selected according to the application, and injection molding, extrusion molding, hollow molding, compression molding, press molding, calendering molding and the like can be used.

[0160] In particular, the polyamide resin composition of the present embodiment can not only withstand the reflow process but also provide a molded article having excellent flame retardancy, and is therefore suitable as an injection molded article used in applications having a surface mounting process.

[0161] <Purpose>

[0162] The polyamide resin composition of the present embodiment has heat resistance that can withstand the reflow process and provides a molded body with excellent flame retardancy. Therefore, it is useful as external connection terminals such as FPC connectors, BtoB connectors, card connectors, SMT connectors, coaxial connectors, and memory card connectors; SMT relays; SMT bobbins; slots such as memory slots and CPU slots; switches such as command switches and SMT switches; sensors such as rotation sensors and acceleration sensors; IGBT module parts of inverters, ECU housings, insulating parts, vehicle-mounted connectors, engine brackets, intercoolers, bearing retainers and other automotive parts, etc. Among them, it is useful as SMT connectors, SMT relays, and IGBT module parts for automobiles and electronic equipment, and is particularly useful as SMT connectors.

[0163] The molded article obtained from the polyamide resin composition of the present embodiment exhibits excellent flame retardancy and can be suitably used for applications such as SMT connectors and SMT relays.

[0164] Examples of electronic devices including a molded article obtained from the polyamide resin composition of the present embodiment include portable electronic devices such as smartphones and personal computers, and automobiles, but are not limited thereto.

[0165] Example

[0166] Hereinafter, the present invention will be described in more detail with reference to Examples and Comparative Examples, but the present invention is not limited thereto.

[0167] In addition, the melting point and glass transition temperature of the polyamide (A) used in the examples and comparative examples were measured according to the method shown below.

[0168] (Melting point and glass transition temperature of polyamide (A))

[0169] The melting point of the polyamide (PA9T described below) used as the polyamide (A) was determined by using a differential scanning calorimeter (DSC7020) manufactured by Hitachi High-Tech Science Co., Ltd., and setting the peak temperature of the melting peak that appeared when the temperature was raised from 30°C to 360°C at a rate of 10°C / min in a nitrogen atmosphere as the melting point (°C). In addition, when there are multiple melting peaks, the peak temperature of the melting peak on the highest temperature side is set as the melting point.

[0170] After that, the sample was completely melted by keeping the temperature 30°C higher than the melting point for 10 minutes, then cooled to 40°C at a rate of 10°C / min and kept at 40°C for 10 minutes. When the temperature was raised to 30°C higher than the melting point at a rate of 10°C / min again, the midpoint where the DSC curve became step-shaped was defined as the glass transition temperature.

[0171] [Examples 1 to 9 and Comparative Examples 1 to 5]

[0172] The polyamide (A) and other components (antioxidant-1, antioxidant-2, mold release agent, and lubricant) in the compounding amounts shown in Table 1 were supplied to a twin-screw extruder (screw diameter: 32 mm φ, L / D = 30, rotation speed: 150 rpm, discharge amount: 10 kg / hour) manufactured by the Plastics Engineering Institute through a hopper at the uppermost upstream part. Further, the inorganic filler (B), phosphinate (C), phosphite (D), and colorant (E) in the compounding amounts shown in Table 1 were supplied through a side feeder, and melt-kneading was performed. The melt-kneaded polyamide resin composition was extruded into a raw filament shape, cooled, and then cut to obtain pellets of the polyamide resin composition.

[0173] The compounding amounts of the polyamide (A), inorganic filler (B), phosphinate (C), phosphite (D), and colorant (E) in Table 1 all mean "parts by mass".

[0174] Using the pellets obtained above, the molded articles were evaluated [flame retardancy, mechanical strength, sulfur content, color value] by the following method. The results are shown in Table 2.

[0175] [Flame Retardancy]

[0176] Using an injection molding machine UH-1000 manufactured by Nissei Plastic Industrial Co., Ltd., pellets of the polyamide resin composition obtained in each example or comparative example were injection molded into plate-like test pieces (thickness: 0.40 mm, 0.75 mm, 3.0 mm) with a width of 12.5 mm and a length of 125 mm at a maximum barrel temperature of 320°C, a mold temperature of 140°C, and an injection speed of 750 to 150 mm / second as test pieces. The flame retardancy of the test pieces with each thickness was evaluated according to the regulations of the UL94 standard shown below.

[0177] <UL94 Standard / Flame Retardancy Test>

[0178] The upper end of the above-mentioned test piece is fixed with a clamp so that the test piece is fixed vertically, and a predetermined flame is brought into contact with the lower end for 10 seconds and then separated, and the burning time of the test piece is measured (first time). When the fire is extinguished, the flame is brought into contact with the lower end again for 10 seconds and then separated, and the burning time of the test piece is measured (second time). The same measurement is repeated for 5 pieces, and 10 data of 5 first burning time data and 5 second burning time data are obtained. The total of the 10 data is set as T, and the maximum value of the 10 data is set as M. If T is less than 50 seconds, M is less than 10 seconds, and the fixture is not burned, and the molten material with flames does not fall and the dry cotton placed 12 inches below is ignited, it is "V-0"; if T is less than 250 seconds, M is less than 30 seconds, and other conditions are met as V-0, it is "V-1"; when T is less than 250 seconds, M is less than 30 seconds, and the fixture is not burned, the molten material with flames falls and the cotton 12 inches below is ignited, it is "V-2".

[0179] 〔Mechanical strength〕

[0180] The pellets of the polyamide resin composition obtained in each example and comparative example were injection molded into dumbbell-shaped tensile test pieces (ISO1A dumbbell) at a maximum cylinder temperature of 320°C, a mold temperature of 140°C, and an injection speed of 150 to 50 mm / sec using an injection molding machine UH-1000 manufactured by Nissei Plastic Industry Co., Ltd. as test pieces.

[0181] The test pieces prepared by the above method were measured for tensile breaking strength and tensile breaking strain at 23° C. in accordance with ISO 527 using a tensile testing machine INSTRON 5969 (manufactured by Instron Japan Company Limited).

[0182] 〔Sulfur content〕

[0183] The sulfur content (ppm by mass) of the polyamide resin composition obtained in each of the Examples and Comparative Examples was measured by the following apparatus and conditions.

[0184] In addition, the pellets of the polyamide resin composition obtained in each Example and Comparative Example were spread all over an aluminum cup and measured as a sample.

[0185] Measuring device: Scanning fluorescence X-ray analyzer ZSX Primusμ manufactured by Rigaku Corporation

[0186] X-ray tube: Rh 3.0kW

[0187] ·Analysis diameter: φ30mm

[0188] Atmosphere: Vacuum

[0189] Sample rotation:

[0190] ·Measurement mode: FP method

[0191] ·Filter (Japanese: フイルタ): OUT

[0192] ·Analytical window film: 0.7μm PET

[0193] Slit: Standard

[0194] ·Spectral crystal: Ge

[0195] Detector: proportional counter

[0196] Color value (L * a * b * , ΔE)〕

[0197] The color value of the polyamide resin composition obtained in each embodiment and comparative example is L * a * b * The measurement was carried out using the following apparatus and conditions.

[0198] In addition, the dumbbell-shaped tensile test piece of the polyamide resin composition obtained in each Example and Comparative Example, that is, ISO 1A dumbbell was used as a sample for measurement.

[0199] Measuring device: RAL COLORCATCH NANO colorimeter manufactured by RAL gGmbH

[0200] Light source: CIE standard light source D65

[0201] Sensor: CCD camera (224×224 pixels)

[0202] Measuring geometry: 45° / 0° Software: RAL iCOLOURS (Version 3.7.2)

[0203] Device used: Use the software on iPhone8 (iOS 13.3)

[0204] According to the obtained L * a * b * , calculate ΔE represented by the following formula (1).

[0205] ΔE=〔(L * col -L * nat ) 2 +(a * col-a * nat ) 2 +(b * col -b * nat ) 2 〕 1 / 2 (1)

[0206] It should be noted that in formula (1), L * col 、a * col and b * col The polyamide resin composition obtained in each example is measured by CIE1976 (L * a * b * ) L specified in the color system * 、a * and b * , L * nat 、a * nat and b * nat The polyamide resin composition without colorant is defined by CIE1976 (L * a * b * ) L specified in the color system * 、a * and b * The above-mentioned polyamide resin composition not containing a colorant has the same composition as the above-mentioned polyamide resin composition except that it does not contain a colorant (E).

[0207] The components shown in Table 1 are as follows.

[0208] 〔Polyamide (A)〕

[0209] ·PA9T: "Genestar GC51010" (manufactured by KURARAY Co., Ltd., PA9T (polyamide in which the dicarboxylic acid unit is a terephthalic acid unit and the diamine unit is a 1,9-nonanediamine unit and a 2-methyl-1,8-octanediamine unit (molar ratio 85 / 15)), melting point 305°C, glass transition temperature 125°C)

[0210] [Inorganic filler (B)]

[0211] Glass fiber: "ECS03T-262H" (manufactured by Nippon Electric Glass Co., Ltd., cross-sectional shape: round, 3 mm chopped strands, fiber diameter 10.5 μm)

[0212] 〔Phosphinate (C)〕

[0213] Aluminum phosphinate: "Exolit OP 1230" (manufactured by Clariant Chemicals, aluminum diethylphosphinate, number average particle size 25 μm)

[0214] 〔Phosphite (D)〕

[0215] · Aluminum phosphite: "APA-100" (manufactured by Taihei Chemical Industry Co., Ltd.)

[0216] 〔Colorant (E)〕

[0217] E-1: "Solvent Red 52" (red organic colorant, CAS No. 81-39-0)

[0218] E-2: "Solvent Red 179" (red organic colorant, CAS No. 6829-22-7)

[0219] ·E-3: “Iron (III) oxide” (red inorganic colorant, CAS No. 1309-37-1)

[0220] ·E-4: “Pigment Yellow 53” (yellow inorganic colorant, CAS No. 8007-18-9)

[0221] ·E-5: "Pigment Blue 15" (blue organic colorant, CAS No. 147-14-8)

[0222] ·E-6: “Pigment Green 50” (green inorganic colorant, CAS No. 68186-85-6)

[0223] ·E-7: “Pigment Brown 24” (brown inorganic colorant, CAS No. 68186-90-3)

[0224] E-8: "Solvent Yellow 98" (yellow organic colorant, CAS No. 27870-92-4)

[0225] E-9: "Solvent Orange 63" (orange organic colorant, CAS No. 16924-75-0)

[0226] E-10: "Ultramarine (Pigment Blue 29)" (blue inorganic colorant, CAS No. 57455-37-5)

[0227] ·E-11: “Zinc sulfide” (white inorganic colorant, CAS No. 1314-98-3)

[0228] [Other ingredients]

[0229] · Antioxidant-1: "Irganox 1098" (manufactured by BASF JAPAN Co., Ltd.)

[0230] · Antioxidant-2: "Irgafos 168" (manufactured by BASF JAPAN Co., Ltd.)

[0231] Release agent: High-density polyethylene "HI WAX NP055" (Mitsui Chemicals, Inc.)

[0232] · Lubricant: Calcium stearate "CALCIUM STEARATE S" (manufactured by NOF Corporation)

[0233] Nucleating agent: Talc "Micron White #5000S" (produced by Hayashi Chemical Industry Co., Ltd.)

[0234] In Table 1, "(C) + (D)" means the total amount (mass %) of the contents of the phosphinate (C) and the phosphite (D) relative to 100 mass % of the polyamide resin composition.

[0235] In addition, in Table 1, "(C) / (D)" means the mass ratio of the phosphinate (C) to the phosphite (D).

[0236] [Table 1]

[0237]

[0238] [Table 2]

[0239]

[0240] As shown in Table 1, the colored polyamide resin composition molded article of the present embodiment has excellent flame retardancy by comparison between the examples and the comparative examples. In addition, the polyamide resin composition of the present embodiment has heat resistance that can withstand the reflow process because the polyamide (A) having a melting point of 280°C or more is used.

[0241] Industrial Applicability

[0242] The colored polyamide resin composition of the present embodiment has heat resistance that can withstand the reflow process and provides a molded body with excellent flame retardancy, and is therefore useful as external connection terminals such as FPC connectors, BtoB connectors, card connectors, SMT connectors, coaxial connectors, and memory card connectors; SMT relays; SMT bobbins; slots such as memory slots and CPU slots; switches such as command switches and SMT switches; sensors such as rotation sensors and acceleration sensors; IGBT module components of inverters, ECU housings, insulators, vehicle-mounted connectors, engine brackets, intercoolers, bearing retainers, and other automotive parts.

Claims

1. A polyamide resin composition, comprising, relative to 100 parts by mass of a polyamide (A) having a melting point of 280° C. or higher, 45 to 120 parts by mass of an inorganic filler (B), 25 to 40 parts by mass of at least one phosphinate (C) represented by the following formula (I) or (II), 2 to 15 parts by mass of a phosphite (D), and a colorant (E), wherein the colorant (E) does not contain carbon black, the polyamide resin composition contains sulfur and the sulfur content is less than 220 ppm by mass, ΔE represented by the following formula (1) is greater than 1, In formula (I) and formula (II), R 1 , R 2 , R 4 and R 5 Each independently represents a linear or branched alkyl group having 1 to 16 carbon atoms, and R 1 With R 2 and R 4 With R 5 optionally bonded to each other to form a ring, R 3 represents a linear or branched alkylene group having 1 to 10 carbon atoms, an arylene group having 6 to 10 carbon atoms, an alkylarylene group having 7 to 20 carbon atoms, a cycloalkylene group having 3 to 10 carbon atoms, an aralkylene group having 7 to 10 carbon atoms, or an arylalkylene group having 7 to 20 carbon atoms, M represents calcium, magnesium, aluminum or zinc, m is an integer of 1 to 4, n is an integer of 1 to 4, and x is an integer of 1 to 4. In formula (II), m, x and n satisfy the relationship of mx=2n. ΔE=〔(L * col -L * nat ) 2 +(a * col -a * nat ) 2 +(b * col -b * nat ) 2 〕 1 / 2 (1) In formula (1), ΔE is the CIE1976 (L * a * b * ) Color difference specified by the color system, L * col 、a * col and b * col The polyamide resin composition is * a * b * ) L specified in the color system * 、a * and b * , L * nat 、a * nat and b * nat The polyamide resin composition without colorant having the same composition as the polyamide resin composition except that the polyamide resin composition does not contain the colorant (E) is a polyamide resin composition without colorant having the same composition as the polyamide resin composition except that the polyamide resin composition does not contain the colorant (E) according to CIE1976 (L * a * b * ) L specified in the color system * 、a * and b * .

2. The polyamide resin composition according to claim 1, in, The colorant (E) contains an organic colorant, and the organic colorant is at least one selected from anthraquinone dyes, perinone dyes, anthrapyridone dyes, and phthalocyanine dyes.

3. The polyamide resin composition according to claim 1, in, The colorant (E) contains an organic colorant, and the organic colorant is a phthalocyanine pigment.

4. The polyamide resin composition according to claim 1, in, The colorant (E) contains an inorganic colorant, and the inorganic colorant is at least one selected from metal oxides and composite metal oxides.

5. The polyamide resin composition according to claim 2 or 3, in, The content of the organic colorant is 0.001% by mass to 5.0% by mass relative to 100% by mass of the polyamide resin composition.

6. The polyamide resin composition according to claim 4, in, The content of the inorganic colorant is 0.01% by mass to 5.0% by mass relative to 100% by mass of the polyamide resin composition.

7. The polyamide resin composition according to any one of claims 1 to 4, in, The phosphite (D) is aluminum phosphite or aluminum hydrogen phosphite, the total amount of the phosphinate (C) and the phosphite (D) is 16% to 25% by mass relative to the polyamide resin composition, and the mass ratio of the phosphinate (C) to the phosphite (D), (C) / (D), is 70 / 30 to 94 / 6.

8. The polyamide resin composition according to any one of claims 1 to 4, in, The polyamide (A) comprises diamine units, and 50 mol% to 100 mol% of the diamine units are aliphatic diamine units having 4 to 18 carbon atoms.

9. The polyamide resin composition according to any one of claims 1 to 4, in, The polyamide (A) comprises a dicarboxylic acid unit and a diamine unit, wherein the dicarboxylic acid unit is mainly a unit derived from terephthalic acid, and the diamine unit is mainly a unit derived from at least one selected from aliphatic diamines having 4 to 12 carbon atoms.

10. The polyamide resin composition according to any one of claims 1 to 4, in, The inorganic filler (B) is at least one selected from glass fibers having a circular cross section or glass fibers having a non-circular cross section.

11. The polyamide resin composition according to any one of claims 1 to 4, in, The inorganic filler (B) is glass fiber with a circular cross-section and glass fiber with a non-circular cross-section, and the outer circumference of the cross-section of the glass fiber with the non-circular cross-section is 1.05 to 1.8 times the outer circumference of the glass fiber with the circular cross-section having the same cross-sectional area as the non-circular cross-section.

12. A method for producing the polyamide resin composition according to any one of claims 1 to 4, The method comprises the step of melt-kneading a polyamide (A), an inorganic filler (B), a phosphinate (C), a phosphite (D), a colorant (E), and other components as required. 13 . A molded product, which is a molded product of the polyamide resin composition according to claim 1 . 14 . The molded article according to claim 13 , which is an injection molded article used in an application having a surface mounting process.

Citation Information

Patent Citations

  • Polyamide

    JP1995228690A

  • Heat-resistant resin composition

    JP2007182550A

  • Excellently heat-resistant resin composition

    JP2007182551A

  • Flame-retardant polyamide resin composition and molded article obtained by using the same

    JP2010120983A

  • Flame-retardant polyamide composition

    JP2014521765A