A method for producing hydrogen by electrolysis of water using a self-supporting carbon anode

The self-supporting carbon anode assisted water electrolysis hydrogen production method solves the problem of inefficient oxidation of carbon particles in traditional carbon-assisted electrolysis hydrogen production technology, achieves efficient and sustainable hydrogen production, reduces costs and improves stability.

CN115466969BActive Publication Date: 2024-10-18HARBIN INST OF TECH
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202211326102.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-27
Publication Date
2024-10-18
Estimated Expiration
2042-10-27

AI Technical Summary

Technical Problem

In traditional carbon-assisted electrolysis hydrogen production technology, the inefficient oxidation method of carbon particles leads to problems such as small current in the electrolysis system, slow hydrogen evolution rate, poor cycle stability, and inability to produce hydrogen sustainably.

Method used

The self-supporting carbon anode is used to assist the electrolysis of water to produce hydrogen. The self-supporting carbon anode is obtained through hydrothermal carbonization, tableting and high-temperature carbonization treatment. It serves as an anode and cathode to carry out oxidation reactions in the electrolyte, avoiding the need for carbon particles and carbon particles in the traditional system. Inefficient collision oxidation of the anode.

Benefits of technology

It achieves continuous low-energy hydrogen production, reduces the cost of the electrolysis system, avoids the wear of the proton exchange membrane, and improves the efficiency, sustainability and stability of hydrogen production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115466969B_ABST
    Figure CN115466969B_ABST
Patent Text Reader

Abstract

A method for producing hydrogen by electrolysis of water with the assistance of a self-supporting carbon anode, which relates to an implementation method for producing hydrogen by electrolysis of water with the assistance of carbon, and belongs to the technical field of hydrogen energy production. The purpose of the present invention is to solve the problem that in the traditional carbon-assisted electrolysis hydrogen production system, carbon particles can only be oxidized by colliding with the anode or reacting with other charge transfer carriers, and the carbon particles wear the proton exchange membrane, resulting in a small electrolysis current, a slow hydrogen evolution rate, poor cycle stability and inability to produce hydrogen for a long time. Methods: 1. Hydrothermal carbonization; 2. Tablet forming; 3. High-temperature carbonization; 4. Carbon anode-assisted electrolysis of water to produce hydrogen. The main advantage of the self-supporting carbon anode-assisted electrolysis of water to produce hydrogen in the present invention is that the self-supporting carbon as an anode can continuously undergo an oxidation reaction, thereby achieving continuous and low-energy hydrogen production. The present invention is suitable for the electrolysis of water to produce hydrogen.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an implementation method for producing hydrogen by carbon-assisted water electrolysis, belonging to the technical field of hydrogen energy production. Background Art

[0002] Hydrogen is a green and clean energy with the advantages of light weight, high calorific value, and pollution-free combustion. It is considered to be one of the most effective energy carriers. According to statistics, the global demand for hydrogen will reach 90 million tons in 2020, showing broad application prospects. However, hydrogen currently mainly comes from fossil energy and industrial by-product hydrogen, while causing a large amount of CO2 emissions. In contrast, water electrolysis hydrogen production technology has become the mainstream technical path for hydrogen production due to its simple process, environmental friendliness, high hydrogen production efficiency and purity. However, the current market share of this technology is only 2-4%, mainly due to the high cost of hydrogen production. Among them, electricity costs account for more than 80% of the cost of water electrolysis hydrogen production, which seriously limits the commercialization of water electrolysis hydrogen production technology.

[0003] At present, the power consumption of water electrolysis hydrogen production technology is 4.5~5.5kWh / Nm 3 H2 is mainly limited by the high energy consumption of the anode oxygen production reaction (>1.8V). Most carbon / hydrocarbon raw materials can provide the energy required for water electrolysis in the form of chemical energy. Therefore, carbon / hydrocarbon assisted electrolysis technology has a lower thermodynamic reaction limit and can undergo oxidation reaction at a voltage far lower than the decomposition voltage of water, 1.23V, while producing hydrogen at the cathode. In the carbon-assisted water electrolysis hydrogen production system, if biomass is used as the carbon source, the technology has the advantages of low cost and zero carbon emissions, and has engineering application prospects.

[0004] In traditional carbon-assisted electrolysis hydrogen production technology, carbon is added to the electrolyte in the form of solid particles. The traditional electrolysis system inevitably requires a catalyst as an anode to catalyze the oxidation of carbon particles. Since carbon particles will only be electrocatalytically oxidized when they hit the anode during stirring, the contact time ranges from a few milliseconds to tens of seconds, resulting in a small electrolysis current and a slow hydrogen evolution rate. In addition, carbon particles will aggravate the wear of the proton exchange membrane during stirring. Even if some researchers add a "charge transfer carrier" Fe 3+ / Fe 2+ cycle, so that the anode reaction to Fe 2+ However, Fe 3+ The oxidation capacity of Fe is limited, and it is usually necessary to heat the electrolysis system to enhance the 3+ In addition, when an inert oxygen-containing product layer is formed on the surface of carbon particles, Fe 3+ It is no longer possible to further oxidize the carbon particles, which hinders the Fe 2+The reduction and regeneration of carbon makes the current density of the system decay rapidly over time, and it is impossible to achieve sustained hydrogen production. Therefore, how to achieve efficient and sustainable deep oxidation of carbon is the key to the further development of carbon-assisted water electrolysis hydrogen production technology. Summary of the invention

[0005] The purpose of the present invention is to solve the problems in traditional carbon-assisted electrolysis hydrogen production systems, in which carbon particles can only be oxidized by colliding with the anode or reacting with other charge transfer carriers, and in which carbon particles wear the proton exchange membrane, resulting in small electrolysis current, slow hydrogen evolution rate, poor cycle stability and inability to produce hydrogen for a long time, and to provide a method for producing hydrogen by electrolysis of water using a self-supporting carbon anode.

[0006] A method for producing hydrogen by electrolyzing water with the assistance of a self-supporting carbon anode is accomplished by the following steps:

[0007] 1. Hydrothermal carbonization:

[0008] The carbon / hydrocarbon containing compound and deionized water are transferred to a reaction kettle, and then a hydrothermal reaction is carried out at 100°C to 220°C, and then filtered to obtain a solid reaction product; the solid reaction product is washed and then dried to obtain hydrothermally carbonized carbon;

[0009] 2. Tablet forming:

[0010] The hydrothermally carbonized carbon is filled into a mold, and pressure is applied by a tablet press, and the mold is released to obtain molded carbon;

[0011] 3. High temperature carbonization:

[0012] Under the protection of an inert gas atmosphere, the formed carbon is heated to 600°C to 1200°C, and then kept at 600°C to 1200°C to obtain a formed high-temperature carbonized product;

[0013] 4. Carbon anode assisted water electrolysis to produce hydrogen:

[0014] The formed high-temperature carbonization product is used as a self-supporting carbon anode, and the electrode that can undergo hydrogen evolution reaction is used as a cathode. The self-supporting carbon anode and the cathode are placed in an electrolytic cell, and then the electrolyte is added to the electrolytic cell to assemble a water electrolysis hydrogen production device, which is connected to a power supply to perform water electrolysis hydrogen production under constant current or constant voltage.

[0015] The principle of the present invention is as follows:

[0016] The present invention aims to solve the problems in traditional carbon-assisted electrolysis hydrogen production technology, in which the inefficient oxidation mode of carbon particles leads to a small current generated by the electrolysis system, a slow hydrogen evolution rate, poor cycle stability and an inability to produce hydrogen for a long time. Self-supporting carbon is used as an anode to undergo an oxidation reaction in an electrolyte, replacing the inefficient collision oxidation between carbon particles and the anode in the traditional system. Specifically, a compound containing carbon / hydrogen is first hydrothermally carbonized, and after a compression molding process, a high-temperature carbonization process is performed under an inert atmosphere to obtain self-supporting carbon. The self-supporting carbon is used as an anode and a cathode catalyst and immersed in an electrolyte to carry out self-supporting carbon anode-assisted water electrolysis to produce hydrogen.

[0017] Compared with the prior art, the present invention has the following beneficial effects:

[0018] The main advantage of the self-supporting carbon anode assisted water electrolysis hydrogen production of the present invention is that the self-supporting carbon as an anode can continuously undergo oxidation reaction, thereby achieving continuous low-energy hydrogen production. Since the self-supporting carbon is used as the anode, the system avoids the use of other anode catalysts, reducing the cost of the electrolysis system; at the same time, it avoids the wear of the proton exchange membrane by carbon particles, improving the safety of the system; the direct oxidation method of the self-supporting carbon anode can make the carbon particles uninterruptedly and deeply oxidized, and no additional stirring is required to promote carbon oxidation, thereby improving the efficiency, sustainability and stability of hydrogen production by carbon-assisted water electrolysis. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 Graph showing the effect of different carbonization temperatures on the oxidation of the self-supporting carbon anode, in which 600°C is the self-supporting carbon anode prepared in Example 1, 700°C is the self-supporting carbon anode prepared in Example 2, 800°C is the self-supporting carbon anode prepared in Example 3, 900°C is the self-supporting carbon anode prepared in Example 4, and 1000°C is the self-supporting carbon anode prepared in Example 5;

[0020] Figure 2 : are AC impedance spectra of the self-supporting carbon anodes at different carbonization temperatures, in which 600°C is the self-supporting carbon anode prepared in Example 1, 700°C is the self-supporting carbon anode prepared in Example 2, 800°C is the self-supporting carbon anode prepared in Example 3, 900°C is the self-supporting carbon anode prepared in Example 4, and 1000°C is the self-supporting carbon anode prepared in Example 5;

[0021] Figure 3 This is a comparison diagram of oxidation curves of the self-supporting carbon anode prepared in Example 6 and conventional carbon particles, in which 1 is the self-supporting carbon anode prepared in Example 6, and 2 is conventional carbon particles;

[0022] Figure 4 This is the constant current oxidation curve of the self-supporting carbon anode prepared in Example 6 at 20 mA;

[0023] Figure 5This is a performance diagram of the self-supporting carbon anode assisted water electrolysis prepared in Example 6;

[0024] Figure 6 This is the Faraday efficiency diagram of the self-supporting carbon anode assisted water electrolysis hydrogen production prepared in Example 6. The current density in Figure 1 is 200 mA / cm 2 , the current density of 2 is 100mA / cm 2 , the current density of 3 is 50mA / cm 2 ;

[0025] Figure 7 This is a test chart of the cycle stability of the self-supporting carbon anode prepared in Example 6 to assist in the electrolysis of water to produce hydrogen at a constant current of 15 mA. DETAILED DESCRIPTION

[0026] The following examples further illustrate the content of the present invention, but should not be construed as limiting the present invention. Without departing from the essence of the present invention, modifications and substitutions made to the methods, steps or conditions of the present invention all fall within the scope of the present invention.

[0027] Specific implementation method 1: In this implementation method, a method for producing hydrogen by electrolysis of water using a self-supporting carbon anode is completed by the following steps:

[0028] 1. Hydrothermal carbonization:

[0029] The carbon / hydrocarbon containing compound and deionized water are transferred to a reaction kettle, and then a hydrothermal reaction is carried out at 100°C to 220°C, and then filtered to obtain a solid reaction product; the solid reaction product is washed and then dried to obtain hydrothermally carbonized carbon;

[0030] 2. Tablet forming:

[0031] The hydrothermally carbonized carbon is filled into a mold, and pressure is applied by a tablet press, and the mold is released to obtain molded carbon;

[0032] 3. High temperature carbonization:

[0033] Under the protection of an inert gas atmosphere, the formed carbon is heated to 600°C to 1200°C, and then kept at 600°C to 1200°C to obtain a formed high-temperature carbonized product;

[0034] 4. Carbon anode assisted water electrolysis to produce hydrogen:

[0035] The formed high-temperature carbonization product is used as a self-supporting carbon anode, and the electrode that can undergo hydrogen evolution reaction is used as a cathode. The self-supporting carbon anode and the cathode are placed in an electrolytic cell, and then the electrolyte is added to the electrolytic cell to assemble a water electrolysis hydrogen production device, which is connected to a power supply to perform water electrolysis hydrogen production under constant current or constant voltage.

[0036] Specific embodiment 2: This embodiment differs from specific embodiment 1 in that: the hydrothermal reaction time in step 1 is 6h to 48h; in step 1, the solid reaction product is washed 3 to 5 times with deionized water, and then dried at 40°C to 90°C to obtain hydrothermally carbonized carbon. The other steps are the same as those in specific embodiment 1.

[0037] Specific implementation method 3: This implementation method is different from specific implementation method 1 or 2 in that the mass ratio of the carbon / hydrocarbon containing compound described in step 1 to the volume ratio of deionized water is (5g-20g): (50mL-200mL). The other steps are the same as specific implementation method 1 or 2.

[0038] Specific embodiment 4: This embodiment differs from specific embodiments 1 to 3 in that the carbon / hydrocarbon-containing compound in step 1 is one or a mixture of corn cobs, straw, grapefruit peel, watermelon peel, lignin and coal. The other steps are the same as those of specific embodiments 1 to 3.

[0039] Specific embodiment 5: This embodiment differs from specific embodiments 1 to 4 in that: the three-dimensional structure of the mold described in step 2 is one or more of a cube, a cuboid, a cylinder and a prism; the tablet press described in step 2 is one or more of a single punch tablet press, a rotary tablet press, a basket tablet press, a sub-high-speed rotary tablet press, a fully automatic high-speed tablet press and a rotary core tablet press. The other steps are the same as specific embodiments 1 to 4.

[0040] Specific implementation method 6: This implementation method is different from specific implementation methods 1 to 5 in that the pressure in step 2 is 20 MPa to 30 MPa. The other steps are the same as those in specific implementation methods 1 to 5.

[0041] Specific embodiment 7: This embodiment differs from specific embodiments 1 to 6 in that: the inert gas in step 3 is nitrogen or argon; the heating rate in step 3 is 2°C / min to 20°C / min; the insulation time in step 3 is 1h to 6h. The other steps are the same as those in specific embodiments 1 to 6.

[0042] Specific implementation eight: This implementation differs from specific implementations one to seven in that: the constant current in step four is 10 mA to 2000 mA; the constant voltage in step four is 0.1 V to 3 V. The other steps are the same as those in specific implementations one to seven.

[0043] Specific embodiment 9: This embodiment differs from specific embodiments 1 to 8 in that: the cathode described in step 4 is a Pt mesh, a Pt sheet, a Ni electrode, a carbon cloth, a graphite felt, or a cathode catalyst supported on a carrier, wherein the cathode catalyst is a catalyst having a hydrogen evolution function, and the carrier is a Pt mesh, a Pt sheet, a Ni electrode, a carbon cloth, or a graphite felt. The other steps are the same as those of specific embodiments 1 to 8.

[0044] Specific embodiment 10: This embodiment differs from specific embodiments 1 to 9 in that the electrolyte described in step 4 is 1 mol / L KOH solution, 1 wt% to 50 wt% KOH solution, 0.5 mol / L to 10 mol / L H2SO4 or PBS buffer. The other steps are the same as those of specific embodiments 1 to 9.

[0045] The following examples are used to verify the beneficial effects of the present invention:

[0046] Example 1: A method for preparing a self-supporting carbon anode is completed by the following steps:

[0047] 1. Hydrothermal carbonization:

[0048] 5.0 g of a compound containing carbon / hydrogen and 50 mL of deionized water were transferred to a reactor, and then subjected to a hydrothermal reaction at 220° C. for 24 h, followed by filtration to obtain a solid reaction product; the solid reaction product was washed three times with deionized water, and then dried to obtain hydrothermally carbonized carbon;

[0049] The carbon / hydrogen containing compound in step 1 is corn cob;

[0050] 2. Tablet forming:

[0051] 0.4 g of hydrothermally carbonized carbon was filled into a cylindrical mold with a diameter of 13 mm, and a pressure of 10 MPa was applied by a tablet press, and the mold was demolded to obtain molded carbon;

[0052] The tablet press described in step 2 is a single punch tablet press;

[0053] 3. High temperature carbonization:

[0054] Under the protection of nitrogen atmosphere, the formed carbon is heated to the carbonization temperature at a heating rate of 10°C / min, and then kept at the carbonization temperature for 4 hours to obtain a formed high-temperature carbonization product, which is a self-supporting carbon anode;

[0055] The carbonization temperature described in step 3 is 600°C.

[0056] Example 2: The difference between this example and Example 1 is that the carbonization temperature in step 3 is 700° C. The other steps and parameters are the same as those in Example 1.

[0057] Example 3: The difference between this example and Example 1 is that the carbonization temperature in step 3 is 800° C. The other steps and parameters are the same as those in Example 1.

[0058] Example 4: This example is different from Example 1 in that the carbonization temperature in step 3 is 900° C. The other steps and parameters are the same as those in Example 1.

[0059] Example 5: This example is different from Example 1 in that the carbonization temperature in step 3 is 1000° C. The other steps and parameters are the same as those in Example 1.

[0060] Example 6: The difference between this example and Example 5 is that in step 2, 6 g of hydrothermally carbonized carbon is filled into a 4 cm×8 cm×5 cm rectangular parallelepiped mold, a tablet press is applied with a pressure of 20 MPa, and the mold is released to obtain molded carbon. The other steps and parameters are the same as those in Example 5.

[0061] In a three-electrode system, the self-supporting carbon obtained in Examples 1 to 5 was used as the working electrode, the Pt sheet was used as the counter electrode, and the mercury / mercury oxide electrode was used as the reference electrode. The polarization curve of the working electrode was recorded by a BioLogic-VMP3 electrochemical workstation.

[0062] Figure 1 Graph showing the effect of different carbonization temperatures on the oxidation of the self-supporting carbon anode, in which 600°C is the self-supporting carbon anode prepared in Example 1, 700°C is the self-supporting carbon anode prepared in Example 2, 800°C is the self-supporting carbon anode prepared in Example 3, 900°C is the self-supporting carbon anode prepared in Example 4, and 1000°C is the self-supporting carbon anode prepared in Example 5;

[0063] from Figure 1 It can be seen that the self-supporting carbon prepared by carbonization at 1000°C in Example 5 has excellent oxidation activity, which can reach 80 mA cm at a potential of 1.6 V (vs. RHE). -2 of current density.

[0064] In the three-electrode system ( Figure 1 The carbon anode was subjected to AC impedance test at open circuit voltage using a BioLogic-VMP3 electrochemical workstation with a frequency range of 0.01–10 5 Hz, with an amplitude of 5mV.

[0065] Figure 2: are AC impedance spectra of the self-supporting carbon anodes at different carbonization temperatures, in which 600°C is the self-supporting carbon anode prepared in Example 1, 700°C is the self-supporting carbon anode prepared in Example 2, 800°C is the self-supporting carbon anode prepared in Example 3, 900°C is the self-supporting carbon anode prepared in Example 4, and 1000°C is the self-supporting carbon anode prepared in Example 5;

[0066] from Figure 2 It can be seen that as the carbonization temperature increases, the conductivity of the carbon anode increases, and the self-supporting carbon anode prepared by carbonization at 1000° C. in Example 5 has the best electron transfer ability.

[0067] Test conditions such as Figure 1 The working electrode is the self-supporting carbon anode (2.6 g) prepared in Example 6, and the polarization curve (No. 1) of the working electrode is recorded using an electrochemical workstation.

[0068] The carbon particles in the conventional carbon-assisted water electrolysis system are powders obtained by grinding the self-supporting carbon anode prepared in Example 6. 2.6 g of the obtained carbon powder was weighed and placed in 1 M KOH (80 mL) electrolyte, with Pt sheets as working electrodes and counter electrodes, respectively, and mercury / mercuric oxide electrode as reference electrode, and the polarization curve of the Pt sheet working electrode (No. 2) was recorded using a BioLogic-VMP3 electrochemical workstation at a stirring speed of 500 rpm / min.

[0069] Figure 3 This is a comparison diagram of oxidation curves of the self-supporting carbon anode prepared in Example 6 and conventional carbon particles, in which 1 is the self-supporting carbon anode prepared in Example 6, and 2 is conventional carbon particles;

[0070] from Figure 3 It can be seen that the oxidation efficiency of the self-supporting carbon anode is much higher than the efficiency of carbon particles being oxidized by colliding with the Pt anode.

[0071] Test conditions such as Figure 1 The working electrode is the self-supporting carbon anode (2.6 g) prepared in Example 6, and a BioLogic-VMP3 electrochemical workstation is used to apply a constant current of 20 mA to the working electrode to record the curve of voltage change over time.

[0072] Figure 4 This is the constant current oxidation curve of the self-supporting carbon anode prepared in Example 6 at 20 mA;

[0073] from Figure 4 It can be seen that after the self-supporting carbon anode prepared in Example 6 was oxidized at a current of 20 mA for 93 h, the electrode potential reached 1.4 V (vs. RHE), proving that the self-supporting carbon anode can be stably oxidized at a low potential.

[0074] The formed high-temperature carbonization product prepared in Example 6 was used as a self-supporting carbon anode, a Pt electrode (1*1 cm) was used as a cathode, and a 1 mol / L KOH solution was used as an electrolyte. The self-supporting carbon anode and the Pt cathode were placed in an electrolytic cell, and the electrolyte was added to the electrolytic cell to assemble a water electrolysis hydrogen production device, which was connected to a power supply. Water electrolysis was performed to produce hydrogen at a cell voltage of 0-1.6 V. The electrode polarization curve is shown in FIG. Figure 5 As shown;

[0075] Figure 5 This is a performance diagram of the self-supporting carbon anode assisted water electrolysis prepared in Example 6;

[0076] from Figure 5 It can be seen that the self-supporting carbon anode assisted water electrolysis to produce hydrogen can significantly reduce the power consumption of water electrolysis. When driven by a voltage of 1.6V, the current of water electrolysis can reach 102mA.

[0077] The formed high-temperature carbonization product prepared in Example 6 was used as a self-supporting carbon anode, a Pt electrode (1*1 cm) was used as a cathode, and a 1 mol / L KOH solution was used as an electrolyte. The self-supporting carbon anode and the cathode were placed in an electrolytic cell, and the electrolyte was added to the electrolytic cell to assemble a water electrolysis hydrogen production device, and a power supply was connected to control the current density of the cathode to 50 mA / cm 2 , 100mA / cm 2 , 200mA / cm 2 Electrolysis of water to produce hydrogen, such as Figure 6 As shown;

[0078] Figure 6 This is the Faraday efficiency diagram of the self-supporting carbon anode assisted water electrolysis hydrogen production prepared in Example 6. The current density in Figure 1 is 200 mA / cm 2 , the current density of 2 is 100mA / cm 2 , the current density of 3 is 50mA / cm 2 ;

[0079] from Figure 6 It can be seen that the self-supporting carbon anode assisted water electrolysis to produce hydrogen has a Faraday efficiency greater than 98% at different current densities and can produce high-purity hydrogen.

[0080] The formed high-temperature carbonization product prepared in Example 6 was used as a self-supporting carbon anode, a Pt electrode (1*1 cm) was used as a cathode, and a 1 mol / L KOH solution was used as an electrolyte. The self-supporting carbon anode and the cathode were placed in an electrolytic cell, and then the electrolyte was added to the electrolytic cell to assemble a water electrolysis hydrogen production device, connect a power supply, and test it at a constant current of 15 mA, as shown in Figure 7.

[0081] Figure 7This is a test diagram of the cycle stability of the self-supporting carbon anode assisted water electrolysis hydrogen production prepared in Example 6 at a constant current of 15 mA;

[0082] from Figure 7 It can be seen that after the self-supporting carbon anode assisted water electrolysis to produce hydrogen ran at a current of 15 mA for 18 hours, the voltage slowly rose to 1.6 V, proving that the self-supporting carbon anode can continuously assist water electrolysis to produce hydrogen at a low voltage.

Claims

1. A method for producing hydrogen by electrolysis of water assisted by a self-supporting carbon anode, characterized in that A method for producing hydrogen by electrolysis of water using a self-supporting carbon anode is accomplished by the following steps:

1. Hydrothermal carbonization: The carbon / hydrocarbon containing compound and deionized water are transferred to a reaction kettle, and then a hydrothermal reaction is carried out at 100°C to 220°C, and then filtered to obtain a solid reaction product; the solid reaction product is washed and then dried to obtain hydrothermally carbonized carbon; The carbon / hydrocarbon-containing compound in step 1 is one or a mixture of several of corn cobs, straw, grapefruit peel, watermelon peel, lignin and coal; 2. Tablet forming: The hydrothermally carbonized carbon is filled into a mold, and pressure is applied by a tablet press, and the mold is released to obtain molded carbon; 3. High temperature carbonization: Under the protection of an inert gas atmosphere, the formed carbon is heated to 600°C to 1200°C, and then kept at 600°C to 1200°C to obtain a formed high-temperature carbonized product; The insulation time described in step 3 is 1h to 6h; 4. Carbon anode assisted water electrolysis to produce hydrogen: The formed high-temperature carbonization product is used as a self-supporting carbon anode, and an electrode capable of generating hydrogen evolution reaction is used as a cathode. The self-supporting carbon anode and the cathode are placed in an electrolytic cell, and then an electrolyte is added to the electrolytic cell to assemble a water electrolysis hydrogen production device, which is connected to a power source to perform water electrolysis hydrogen production under a constant current or constant voltage; The cathode described in step 4 is a Pt mesh, a Pt sheet, a Ni electrode, a carbon cloth, a graphite felt or a cathode catalyst supported on a carrier, wherein the cathode catalyst is a catalyst having a hydrogen evolution function, and the carrier is a Pt mesh, a Pt sheet, a Ni electrode, a carbon cloth, or a graphite felt; The electrolyte described in step 4 is 1 mol / L KOH solution, 1wt%-50wt% KOH solution, 0.5mol / L-10mol / L H2SO4 or PBS buffer.

2. A method for producing hydrogen by electrolysis of water using a self-supporting carbon anode according to claim 1, characterized in that The time of the hydrothermal reaction in step one is 6h to 48h; in step one, the solid reaction product is washed 3 to 5 times with deionized water, and then dried at 40°C to 90°C to obtain hydrothermally carbonized carbon.

3. The method for producing hydrogen by electrolysis of water using a self-supporting carbon anode according to claim 1, characterized in that The volume ratio of the carbon / hydrocarbon containing compound described in step 1 to deionized water is (5g-20g):(50mL-200mL).

4. The method for producing hydrogen by electrolysis of water using a self-supporting carbon anode according to claim 1, characterized in that The three-dimensional structure of the mold described in step 2 is one or more of a cube, a cuboid, a cylinder and a prism; the tablet press described in step 2 is one or more of a single punch tablet press, a rotary tablet press, a basket tablet press, a sub-high-speed rotary tablet press, a fully automatic high-speed tablet press and a rotary core tablet press.

5. The method for producing hydrogen by electrolysis of water using a self-supporting carbon anode according to claim 1, characterized in that The pressure described in step 2 is 20MPa to 30MPa.

6. The method for producing hydrogen by electrolysis of water using a self-supporting carbon anode according to claim 1, characterized in that The inert gas described in step three is nitrogen or argon; the heating rate described in step three is 2°C / min to 20°C / min.

7. The method for producing hydrogen by electrolysis of water using a self-supporting carbon anode according to claim 1, characterized in that The constant current described in step 4 is 10mA to 2000mA; the constant voltage described in step 4 is 0.1V to 3V.

Citation Information

Cited By

  • Function sequence integrated carbon anode assisted water electrolysis hydrogen production method

    CN119465224A

  • Preparation method and application of carbon-based anode material

    CN119571357A

  • Preparation method of membrane electrode for acidic iron ion circulation auxiliary electrolytic hydrogen production system and application of membrane electrode in low-power-consumption hydrogen production