Titanium carbonitride nano coating on the surface of Cr-containing low-alloy steel and preparation method thereof

The titanium carbonitride nano-coating prepared by chemical vapor deposition method solves the problem of insufficient corrosion protection performance of Cr-containing low-alloy steel materials in high-temperature and high-pressure CO2 environments, achieves high density and good corrosion resistance, and is suitable for oil and gas field applications.

CN115478259BActive Publication Date: 2024-10-22CHINA NAT PETROLEUM CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110618230.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-05-31
Publication Date
2024-10-22
Estimated Expiration
2041-05-31

AI Technical Summary

Technical Problem

In the existing technology, the surface coating of Cr-containing low-alloy steel materials has poor corrosion protection performance in a high-temperature and high-pressure CO2 environment. The traditional titanium carbonitride coating has problems such as low density, many defects, and thermal expansion coefficient mismatch, leading to corrosion. , peeling and cracking occur frequently.

Method used

The chemical vapor deposition method is used to prepare titanium carbonitride nano-coatings. By controlling the proportion of nitrogen, carbon, and titanium elements, nanostructures and conical grain morphologies are formed, which enhances the density of the coating and the film-base bonding force, and reduces internal and external stresses. , improve the resistance to high temperature and high pressure CO2 corrosion.

Benefits of technology

Significantly improves the high-temperature and high-pressure CO2 corrosion resistance of Cr-containing low-alloy steel materials, enhances the density and uniformity of the coating, improves the thermal expansion coefficient matching with the base material, extends the service life of the coating, and reduces production costs low cost and suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115478259B_ABST
    Figure CN115478259B_ABST
Patent Text Reader

Abstract

The invention discloses a titanium carbonitride nano coating on the surface of Cr-containing low-alloy steel and a preparation method thereof. The method prepares the titanium carbonitride nano coating by chemical vapor deposition. The titanium carbonitride nano coating prepared by low-temperature chemical vapor deposition can effectively enhance the density of the coating and the bonding strength of the film substrate, reduce the internal stress and interface stress of the coating, reduce the structural defects of the coating, and effectively prevent the penetration of corrosion products into the coating under a high-temperature and high-pressure CO2 environment, thereby significantly improving the corrosion protection performance of the coating.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of metal corrosion protection coatings, and in particular relates to a titanium carbonitride nano coating on the surface of a Cr-containing low alloy steel and a preparation method thereof. Background Art

[0002] CO from oil metal pipes 2 Corrosion is one of the main corrosion problems faced by the oil and gas industry. 2 Oil recovery technology often produces high water content and high mineralization CO 2 The medium causes increasingly serious corrosion of metal pipes such as oil production equipment, oil casing, and transmission pipelines. Cr-containing low-alloy steel is currently the main material used in oil and gas fields to resist CO 2 Corroded metal pipes. 2 Under working conditions, the corrosion protection layer is formed by the Cr-rich corrosion product film generated on the surface of the Cr-containing low-alloy material. However, the corrosion resistance of this Cr-rich corrosion product film is very unstable. 2 Severe corrosion still occurs when used for a long time under working conditions.

[0003] Titanium carbonitride coatings have the advantages of friction and wear resistance, corrosion resistance and good chemical stability. They are often used as wear-resistant coatings on the surfaces of ceramics, carbon-based materials, hard alloys, high-speed steels and other cutting tools and molds to improve their wear resistance, cutting performance and service life. However, titanium carbonitride coatings prepared by traditional methods usually have disadvantages such as large stress at the film-base interface and inside the coating, low degree of crystallization, mismatch in thermal expansion coefficient, high defect density and poor density, which lead to corrosion, peeling and cracking of metal components, especially Cr-containing low-alloy steel materials, under high temperature and high pressure corrosion and wear conditions, and their corrosion protection ability for Cr-containing low-alloy steel materials is greatly weakened.

[0004] In view of the above shortcomings, there are currently three types of improvement methods: (1) Regulating the ratio of N, C, and Ti elements to prepare titanium carbonitride coatings with fibrous grain morphology. Titanium carbonitride coatings with fibrous grain morphology have good toughness and low internal stress in the coating, improved film-base bonding and enhanced friction and wear properties. However, fibrous titanium carbonitride coatings often have high porosity and low density, which leads to a significant decrease in their corrosion protection performance. (2) Add Al element to prepare TiAlN coating, and form a dense structure through the ternary compound system formed by Al element, N element and Ti element, as well as binary products such as TiAl, TiN and AlN, so as to improve the density and crystallization degree of the coating, and enhance the corrosion resistance and wear resistance of the coating; this method enhances the density of the coating to a certain extent, reduces the stress and number of defects in the coating, and improves the corrosion protection performance of the coating; however, the introduction of Al element is easy to cause lattice mismatch and increase the film-base interface stress; at the same time, the preparation temperature of TiAlN coating is generally higher than 900℃, which is easy to aggravate the thermal expansion coefficient mismatch between the coating and the alloy material, weaken the coating film-base bonding force and coating toughness, thus limiting the improvement of the coating wear resistance and corrosion resistance under high temperature and high pressure conditions. (3) Prepare composite coatings and multilayer coatings. Such as TiC / TiCN, TiCN / TiAlCN, TiCN / TiAlCN / TiN, etc. Although composite coatings and multilayer coatings have achieved good results in coating density, film-base bonding force and wear resistance and corrosion resistance. However, its anti-corrosion and wear-resistant properties are easily affected by the structure, interface bonding, phase composition and element distribution of each sub-coating. The coating preparation parameters and deposition process must be precisely controlled to obtain a coating structure with both good anti-corrosion and wear-resistant properties. The corresponding preparation process is difficult, complex and has high production costs, which is not conducive to its large-scale promotion and application in the field of metal pipelines in oil and gas fields.

[0005] Therefore, the field urgently needs to develop a new type of titanium carbonitride coating with high density, low defects and good corrosion and wear resistance on the surface of Cr-containing low alloy steel materials, so as to overcome the shortcomings of the existing technology and improve the performance of Cr-containing low alloy steel materials under high temperature and high pressure CO 2 Improve the corrosion resistance under low temperature and expand the application range of titanium carbonitride coating. Summary of the invention

[0006] The purpose of the present invention is to overcome the shortcomings of the above-mentioned prior art and provide a titanium carbonitride nano coating on the surface of Cr-containing low-alloy steel and a preparation method thereof, so as to solve the problem of poor corrosion resistance and wear resistance of a surface coating of a Cr-containing low-alloy steel material in the prior art.

[0007] In order to achieve the above object, the present invention adopts the following technical solutions:

[0008] A method for preparing a titanium carbonitride nano-coating on the surface of a Cr-containing low-alloy steel comprises the following steps:

[0009] Step 1, under vacuum conditions, introducing a first auxiliary gas into a chemical vapor deposition chamber to preheat a substrate; the substrate is a Cr-containing low alloy steel;

[0010] Step 2, introducing a nitrogen source, a carbon source and a titanium source into a chemical vapor deposition chamber; the nitrogen source is introduced through a second auxiliary gas, the titanium source is introduced through a third auxiliary gas, and the introduced reactants are chemically reacted and deposited on the surface of the substrate to obtain a process coating; the deposition temperature is 650-850° C., the deposition time is 300-800 min, and the deposition pressure is 0.02-0.05 MPa;

[0011] Step 3, after the coating is cooled, a titanium carbonitride nano-coating is obtained.

[0012] A further improvement of the present invention is:

[0013] Preferably, the flow rate of the carbon source is 300-600 sccm.

[0014] Preferably, the first auxiliary gas is a mixed gas of hydrogen and nitrogen; the second auxiliary gas is hydrogen, and the third auxiliary gas is hydrogen and nitrogen.

[0015] Preferably, in step 1, the preheating vacuum is 0.5-1Pa, the preheating temperature is 50-80°C, the hydrogen flow rate in the first auxiliary gas is 100-200sccm, and the nitrogen flow rate is 100-300sccm; the flow rate of the second auxiliary gas is 500-1000sccm; the flow rate of hydrogen in the third auxiliary gas is 500-1000sccm, and the flow rate of argon is 500-1000sccm.

[0016] Preferably, in step 2, the nitrogen source is nitrogen, acetonitrile, ammonia, or a combination thereof; the titanium source is titanium dichloride, titanium trichloride, titanium tetrachloride, butyl titanate, titanium powder or a combination thereof; and the carbon source is methane, ethane, propane, ethylene, propylene, acetylene, or a combination thereof.

[0017] Preferably, in step 3, the cooling process is:

[0018] (3-1) First stage cooling process: stop introducing the titanium source and the third auxiliary gas, the flow rate of the first auxiliary gas is 100-300 sccm, the flow rate of the second auxiliary gas is 100-300 sccm, the cooling rate is 5-10°C / min, and the temperature is cooled to 300-500°C;

[0019] (3-2) Second stage cooling process: when the temperature drops to 300-500°C, stop introducing the second auxiliary gas; when the temperature drops to 100-200°C, stop introducing the first auxiliary gas, and then cool to room temperature to obtain a titanium carbonitride nano-coating on the surface of a Cr-containing low-alloy steel material.

[0020] The titanium carbonitride nano coating on the surface of Cr-containing low-alloy steel prepared by the above preparation method is attached to the surface of a substrate, and the substrate is Cr-containing low-alloy steel; the coating has an atomic percentage of 20-30% nitrogen, 30-50% carbon, and 30-40% titanium, and the sum of the atomic percentages of the three elements is ≤100%.

[0021] Preferably, the coating is composed of titanium carbonitride nano-grains, the nano-grains have a cone-shaped morphology, and the average diameter of the nano-grains is 20-200 nm.

[0022] Preferably, the coating has a thickness of 10-45 μm.

[0023] Preferably, the friction coefficient of the coating is 0.25-0.31; the self-corrosion potential of the coating is -121.8mv, and the self-corrosion current density is 3.883×10 -6 (mA cm).

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] The present invention relates to a method for preparing a titanium carbonitride nano coating on the surface of a Cr-containing low alloy steel. The method prepares the titanium carbonitride nano coating by chemical vapor deposition. The titanium carbonitride nano coating prepared by low-temperature chemical vapor deposition can effectively enhance the density of the coating and the bonding strength of the film substrate, reduce the internal stress and interface stress of the coating, reduce the structural defects of the coating, and effectively prevent the high temperature and high pressure CO 2 The corrosion products in the environment can penetrate into the coating, thereby significantly improving the corrosion protection performance of the coating.

[0026] The present invention also discloses a titanium carbonitride nano coating on the surface of Cr-containing low alloy steel. The coating has a nano structure, and the grains are in a cone-shaped morphology. The nano structure of the coating of the present invention can effectively block the high temperature and high pressure CO in oil and gas fields. 2 HCO in corrosive environments 3- Ion penetration into the coating significantly improves the resistance of Cr-containing low alloy steel to high temperature and high pressure CO 2The nano-titanium carbonitride coating prepared by low-temperature chemical vapor deposition has high density, good uniformity and circumferential plating performance. The nanostructure can effectively improve the thermal expansion coefficient mismatch between the titanium carbonitride coating and the Cr-containing low-alloy steel material, and improve the density of the coating. At the same time, a metallurgical bond is formed between the coating and the Cr-containing low-alloy steel substrate, thereby significantly enhancing the film-based bonding between the coating and the Cr-containing low-alloy steel material, and realizing high-temperature and high-pressure CO in oil and gas fields. 2 Long-term protection for Cr-containing low-alloy steel materials in corrosive environments. The coating has little effect on the dimensional accuracy of the substrate and good biocompatibility, making it suitable for precision machinery, biomedical facilities and other fields. At the same time, the coating has low production cost, simple process, strong controllability, and is suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 A Cr-containing low alloy steel material prepared in Example 1 has a surface resistance to high temperature and high pressure CO 2 XRD test pattern of corroded titanium carbonitride nanocoating.

[0028] Figure 2 A Cr-containing low alloy steel material prepared in Example 1 has a surface resistance to high temperature and high pressure CO 2 Surface SEM test image of corroded titanium carbonitride nanocoating.

[0029] Figure 3 A Cr-containing low alloy steel material prepared in Example 1 has a surface resistance to high temperature and high pressure CO 2 Cross-sectional SEM image of corroded titanium carbonitride nanocoating.

[0030] Figure 4 A Cr-containing low alloy steel material prepared in Example 1 has a surface resistance to high temperature and high pressure CO 2 EDS test image of corroded titanium carbonitride nanocoating.

[0031] Figure 5 This is a SEM image of the titanium carbonitride crystal coating on the surface of the composite prepared in Comparative Example 1 and the Cr-containing low-alloy steel for oil and gas field surface pipelines.

[0032] Figure 6 The titanium carbonitride crystal coating on the surface of the Cr-containing low alloy steel for oil and gas field surface pipeline prepared in Comparative Example 1 in the friction performance test of the present invention (referred to as the coating prepared in Comparative Example 1) and the Cr-containing low alloy steel material surface resistance to high temperature and high pressure CO prepared in Example 1 are compared. 2 Electrochemical performance-polarization curve test diagram of the corroded titanium carbonitride nanocoating (referred to as the coating prepared in Example 1).

[0033] Figure 7This is a test graph of uniform corrosion rate of the titanium carbonitride crystal coating on the surface of Cr-containing low-alloy steel for oil and gas field surface pipelines prepared in Comparative Example 1 in the friction performance test of the present invention (referred to as the coating prepared in Comparative Example 1) and a titanium carbonitride nano coating on the surface of a Cr-containing low-alloy steel material prepared in Example 1 that is resistant to high temperature and high pressure CO2 corrosion (referred to as the coating prepared in Example 1).

[0034] Figure 8 This is a friction coefficient test graph of the titanium carbonitride crystal coating on the surface of Cr-containing low-alloy steel for oil and gas field surface pipelines prepared in Comparative Example 1 in the friction performance test of the present invention (referred to as the coating prepared in Comparative Example 1) and a titanium carbonitride nano coating on the surface of a Cr-containing low-alloy steel material resistant to high temperature and high pressure CO2 corrosion prepared in Example 1 (referred to as the coating prepared in Example 1).

[0035] Fig. 9 The titanium carbonitride crystal coating on the surface of the Cr-containing low alloy steel for oil and gas field surface pipeline prepared in Comparative Example 1 in the friction performance test of the present invention (referred to as the coating prepared in Comparative Example 1) and the Cr-containing low alloy steel material surface resistance to high temperature and high pressure CO prepared in Example 1 are compared. 2 Average wear rate test chart of corroded titanium carbonitride nano-coating (referred to as coating prepared in Example 1). DETAILED DESCRIPTION

[0036] The present invention is further described in detail below in conjunction with the accompanying drawings:

[0037] In a first aspect of the present invention, a titanium carbonitride nano-coating is provided. The coating contains titanium carbonitride formed by nitrogen, carbon and titanium, and the titanium carbonitride in the coating is a nano-structure.

[0038] In another preferred embodiment, the coating is titanium carbonitride formed by nitrogen, carbon and titanium.

[0039] In another preferred embodiment, the total content of N, C and Ti in the coating is ≥96%, preferably ≥98%, more preferably ≥99%, or ≥99.5%, and most preferably ≥99.9%, based on the total weight of the coating.

[0040] In another preferred embodiment, the atomic percentage of nitrogen in the coating is 20-30%, the atomic percentage of carbon is 30-50%, and the atomic percentage of titanium is 30-40%, calculated based on the total number of atoms in the coating.

[0041] In another preferred embodiment, the coating is composed of nano-crystals.

[0042] In another preferred embodiment, the nano-grains of the coating have a cone-shaped morphology.

[0043] In another preferred embodiment, the total volume V of the nanocrystals is 1 The volume V of the coating 0 Ratio (V 1 / V 0 )≥80%, preferably ≥90%, more preferably ≥95%, and most preferably ≥99%.

[0044] In another preferred embodiment, the size of the nanocrystal particles is 20-200 nm, preferably 50-120 nm;

[0045] In another preferred embodiment, the thickness of the coating is 10-45 μm, preferably 15-40 μm, and more preferably 25-35 μm.

[0046] As used in the present invention, the term "nanostructure" means that the size of the grains in the coating is ≤ 1×10 -6 m.

[0047] As used in the present invention, the term "micrometer scale" means that the grain size of the coating is in the range of 1×10 -6 m~1×10 -9 m.

[0048] As used herein, the term "tapered" refers to providing a linear profile feature of grains in the coating.

[0049] In another preferred embodiment, the coating comprises one or more features selected from the following group:

[0050] (1) The friction coefficient of the coating is 0.25-0.31;

[0051] (2) The average wear rate of the coating is 1.5×10 -7 -2.1×10 -7 mm 3 N -1 m -1 .

[0052] (3) The self-corrosion potential of the coating is -121.8mv, and the self-corrosion current density is 3.883×10 -6 (mA cm -2 ).

[0053] (4) The uniform corrosion rate of the coating is 0.00015 mm / a.

[0054] In a second aspect, the present invention provides a method for preparing a Cr-containing low alloy steel material surface resistant to high temperature and high pressure CO as described in the first aspect of the present invention. 2 A method for corroding a titanium carbonitride nanocoating, the method comprising the steps of:

[0055] (1) providing a substrate;

[0056] (2) By low-temperature chemical vapor deposition, in the presence of a nitrogen source, a carbon source and a titanium source, chemical reaction and vapor deposition growth are carried out on the surface of the substrate, thereby forming the coating on the surface of the substrate.

[0057] As used in the present invention, the term "nitrogen source" refers to a raw material that provides nitrogen in the coating.

[0058] As used in the present invention, the term "carbon source" refers to a raw material that provides carbon elements in the coating.

[0059] As used in the present invention, the term "titanium source" refers to a raw material that provides the titanium element in the coating.

[0060] In another preferred embodiment, the steel material is a Cr-containing low alloy steel.

[0061] In another preferred embodiment, in the step (1), the substrate includes an untreated or pretreated substrate.

[0062] In another preferred embodiment, in the step (1), the substrate is a pretreated substrate, and the pretreatment comprises the steps of: (a) performing surface cleaning, sandblasting, surface cleaning, surface polishing and drying treatments on the surface of the substrate in sequence.

[0063] In another preferred embodiment, in step (a), the cleaning agent used for surface cleaning is selected from the following group: water, alcohol, acetone, or a combination thereof.

[0064] In another preferred embodiment, the water is selected from the following group: tap water, distilled water, deionized water, or a combination thereof.

[0065] In another preferred embodiment, the ultrasonic cleaning time is 20-30 minutes.

[0066] In another preferred embodiment, in the step (a), the following materials are selected for sandblasting: brown corundum sand (aluminum oxide sand), quartz sand, white corundum sand, or a combination thereof.

[0067] In another preferred embodiment, the particle size of the white corundum sand is 200-300 mesh.

[0068] In another preferred embodiment, in the step (a), the surface roughness of the substrate after surface polishing is Ra<0.2, preferably 0.05-0.2.

[0069] In another preferred embodiment, in the step (a), the drying temperature is 60-80°C.

[0070] In another preferred embodiment, in the step (a), the drying time is 4-8 hours.

[0071] In another preferred embodiment, the method further comprises the step of: (b) before the following step (2) is performed, introducing a first auxiliary gas under vacuum conditions to preheat the substrate.

[0072] In another preferred embodiment, in the step (b), the first auxiliary gas is selected from the following group: nitrogen, helium, argon, hydrogen, or a combination thereof.

[0073] In another preferred embodiment, in the step (b), the flow rate of the first auxiliary gas is 200-500 sccm.

[0074] In another preferred embodiment, in the step (b), the first auxiliary gas is hydrogen and nitrogen.

[0075] In another preferred embodiment, the flow rate of hydrogen is 100-200 sccm.

[0076] In another preferred embodiment, the flow rate of the nitrogen gas is 100-300 sccm.

[0077] In another preferred embodiment, the purity of the hydrogen is 99.99%.

[0078] In another preferred embodiment, the flow rate of the nitrogen gas is 99.99% sccm

[0079] In another preferred embodiment, in the step (b), in the preheating step, the heating rate is 5-8°C / min.

[0080] In another preferred embodiment, in the step (b), the preheating temperature is 50-80°C.

[0081] In another preferred embodiment, in the step (2), the low-temperature chemical vapor deposition method includes the steps of: introducing a nitrogen source, a carbon source, a titanium source and a second and a third auxiliary gas to obtain the coating on the surface of the substrate through chemical reaction and deposition growth.

[0082] In another preferred embodiment, in the step (2), the nitrogen source is introduced using the second auxiliary gas as a carrier.

[0083] In another preferred embodiment, the second auxiliary gas is selected from the following group: argon, nitrogen, helium, hydrogen, or a combination thereof.

[0084] In another preferred example, the second auxiliary gas is hydrogen.

[0085] In another preferred embodiment, the flow rate of the second auxiliary gas is 500-1000 sccm.

[0086] In another preferred embodiment, in the step (2), the nitrogen source is selected from the following group: nitrogen, acetonitrile, ammonia, or a combination thereof.

[0087] In another preferred embodiment, in the step (2), the titanium source is introduced using a third auxiliary gas as a carrier.

[0088] In another preferred embodiment, the third auxiliary gas is selected from the following group: hydrogen, argon, nitrogen, helium, or a combination thereof.

[0089] In another preferred embodiment, the third auxiliary gas is hydrogen and argon.

[0090] In another preferred example, the flow rate of the third auxiliary gas is 1000-2000 sccm.

[0091] In another preferred embodiment, the flow rate of hydrogen is 500-1000 sccm.

[0092] In another preferred embodiment, the flow rate of the argon gas is 500-1000 sccm.

[0093] In another preferred embodiment, in the step (2), the titanium source is selected from the following group: titanium dichloride, titanium trichloride, titanium tetrachloride, butyl titanate, titanium powder, or a combination thereof.

[0094] In another preferred embodiment, in the step (2), heating to the deposition temperature is performed at a rate of 5-10°C / min.

[0095] In another preferred embodiment, in the step (2), the deposition conditions include: the deposition temperature is 650-850°C.

[0096] In another preferred embodiment, in the step (2), the deposition conditions further include: the deposition time is 300-800 min, preferably 400-700 min, and more preferably 500-600 min.

[0097] In another preferred embodiment, in the step (2), the deposition conditions further include: the deposition pressure is 0.02-0.05 MPa.

[0098] In another preferred embodiment, any two or three of the first auxiliary gas, the second auxiliary gas and the third auxiliary gas are the same or different.

[0099] In another preferred embodiment, in the step (2), the carbon source is a gas source, and the flow rate of the carbon source is 300-600 sccm.

[0100] In another preferred embodiment, the carbon source is selected from the group consisting of methane, ethane, propane, ethylene, propylene, acetylene, or a combination thereof. In another preferred embodiment, the purity of the methane is 99.99%.

[0101] In another preferred embodiment, the method further comprises step (3): cooling the coating obtained in step (2), wherein the cooling step comprises:

[0102] (3-1) First stage cooling process: stop introducing the titanium source and the third auxiliary gas, adjust the flow rate of the first auxiliary gas to 100-300 sccm, adjust the flow rate of the second auxiliary gas to 100-300 sccm, and cool the temperature to 300-500 ℃ at a cooling rate of 5-10 ℃ / min.

[0103] (3-2) Second stage cooling process: when the temperature drops to 300-500°C, stop introducing the second auxiliary gas; when the temperature drops to 100-200°C, stop introducing the first auxiliary gas, and then cool to room temperature to obtain a titanium carbonitride nano-coating on the surface of a Cr-containing low-alloy steel material.

[0104] As used in the present invention, the term "Cr-containing low alloy steel" refers to alloy steel with a total amount of alloying elements such as Cr less than 5%, a relatively low carbon content, generally less than 0.20%, and a generally ferrite + pearlite structure. The Cr-containing low alloy steel corresponds to the Cr-containing low alloy steel in the American standard ASTM A749 "Definition of Terms" and the Japanese standard JIS G0203 "Iron and Steel Terms".

[0105] As used herein, the term "CVD furnace" refers to a chemical vapor deposition furnace.

[0106] As used in the present invention, the term "low temperature chemical vapor deposition" means that the coating preparation temperature range is 500°C to 900°C.

[0107] As used herein, the term "sccm" is a unit of volume flow, ie, standard-state cubic centimeter per minute.

[0108] As used in the present invention, the term "min" is a time unit, namely, minute in English.

[0109] As used herein, the term "assistant gas" refers to a gas having a purity of 99.9%.

[0110] In a preferred embodiment of the present invention, the surface of the Cr-containing low alloy steel material is resistant to high temperature and high pressure CO 2 The method for preparing the corroded titanium carbonitride nanocoating comprises the following steps:

[0111] 1. Place the substrate in a CVD device, evacuate to a vacuum degree of 0.5-1Pa, and introduce the first auxiliary gas (such as a mixture of hydrogen and nitrogen, with a hydrogen flow rate of 100-200sccm and a nitrogen flow rate of 100-300sccm). Start the gas system preheating program, with a preheating temperature of 50-80°C and a heating rate of 5-8°C / min;

[0112] 2. Heat to 650-850°C at a rate of 5-10°C / min, and introduce a nitrogen source, a carbon source, a titanium source and a second and a third auxiliary gas, wherein the nitrogen source is introduced as the second auxiliary gas, and the titanium source is introduced as the third auxiliary gas as a carrier gas. The second auxiliary gas flow rate is 500-1000sccm, and the third auxiliary gas flow rate is 1000-2000sccm, wherein the hydrogen flow rate is 500-1000sccm, and the argon flow rate is 500-1000sccm; the carbon source flow rate is 300-600sccm; the deposition time is 500-600min, and the deposition pressure is 0.02-0.05MPa; the second auxiliary gas is hydrogen, and the third auxiliary gas is hydrogen and nitrogen.

[0113] 3. After the deposition is completed, enter the controllable cooling program, stop introducing the titanium source and the third auxiliary gas, adjust the flow rate of the first auxiliary gas to 100-300sccm, adjust the flow rate of the second auxiliary gas to 100-300sccm, and the cooling rate is 5-10℃ / min. Cool down to 300-500℃. When the temperature drops to 300-500℃, stop introducing the second auxiliary gas; when the temperature drops to 100-200℃, stop introducing the first auxiliary gas, and then cool to room temperature to obtain a titanium carbonitride nano coating on the surface of a Cr-containing low-alloy steel material.

[0114] Example 1

[0115] A Cr-containing low alloy steel material surface resistant to high temperature and high pressure CO 2 Preparation of Corroded Titanium Carbonitride Nanocoating

[0116] 1. Clean and polish the surface of a Cr-containing low-alloy steel substrate with a size of 100mm*100mm*50mm, sandblast the surface with white corundum sand, clean it with alcohol ultrasonic wave after polishing, dry it at 80℃ for 6 hours and place it in a CVD device.

[0117] 2. Vacuum the CVD device to 10 -1 Pa, introduce the first auxiliary gas hydrogen and nitrogen, the hydrogen flow rate is 200sccm, and the nitrogen flow rate is 200sccm. Start the gas system preheating program, set the preheating temperature to 70°C, and the preheating rate to 5°C / min.

[0118] 3. Start the heating program of the CVD system, set the heating temperature to 850°C and the heating rate to 8°C / min, and continuously introduce a hydrogen flow rate of 200sccm and a nitrogen flow rate of 300sccm. The CVD device is heated to 850°C to enter the deposition program, and methane, titanium dichloride and acetonitrile are introduced into the reaction chamber as the carbon source, titanium source and nitrogen source respectively. Among them, the methane flow rate is 600sccm; acetonitrile is first heated to 90°C, and then loaded into the CVD device with the second auxiliary gas as the carrier gas, and the flow rate of the second auxiliary gas hydrogen is 800sccm; titanium dichloride is first heated to 65°C, and then loaded into the CVD device with the third auxiliary gas as the carrier gas, and the hydrogen flow rate in the third auxiliary gas is 800sccm, and the argon flow rate is 500sccm; the deposition time is 540min; the deposition pressure is 0.03MPa

[0119] 4. After the deposition is completed, the CVD device enters a controllable cooling mode, stops introducing titanium dichloride and the third auxiliary gas, adjusts the hydrogen flow rate in the first auxiliary gas to 100 sccm, and the nitrogen flow rate to 100 sccm; adjusts the hydrogen flow rate of the second auxiliary gas to 200 sccm, and cools the temperature to 500 ℃ at a cooling rate of 8 ℃ / min; then stops introducing the second auxiliary gas; after the temperature drops to 200 ℃, stops introducing the first auxiliary gas, enters a natural cooling stage, and cools to room temperature to obtain a Cr-containing low alloy steel material with surface resistance to high temperature and high pressure CO 2 Corrosion of titanium carbonitride nanocoatings.

[0120] Determination

[0121] The surface resistance of a Cr-containing low alloy steel material to high temperature and high pressure CO obtained in Example 1 2 The corroded titanium carbonitride nanocoating was subjected to XRD, SEM and EDS tests. The results are as follows: Figure 1-5 shown.

[0122] Figure 1 The surface resistance of a Cr-containing low alloy steel material to high temperature and high pressure CO obtained in Example 1 2 XRD test pattern of corroded titanium carbonitride nanocoating. Figure 1 Display: The surface of a Cr-containing low alloy steel material obtained in Example 1 is resistant to high temperature and high pressure CO 2 The corroded titanium carbonitride nano-coating is composed of titanium carbonitride, has a face-centered cubic structure, and has a preferred growth orientation of (111) plane.

[0123] Figure 2 The surface resistance of a Cr-containing low alloy steel material to high temperature and high pressure CO obtained in Example 1 2 SEM test image of the corroded titanium carbonitride nanocoating surface. Figure 2 Display: The surface of a Cr-containing low alloy steel material obtained in Example 1 is resistant to high temperature and high pressure CO2 The surface of the corroded titanium carbonitride nano-coating is dense and uniform, and the coating is composed of nano-scale cone-shaped grains; the size of the nano-grains is 60-120nm.

[0124] Figure 3 The surface resistance of a Cr-containing low alloy steel material to high temperature and high pressure CO obtained in Example 1 2 Cross-sectional SEM image of corroded titanium carbonitride nanocoating. Figure 4 Display: The surface of a Cr-containing low alloy steel material obtained in Example 1 is resistant to high temperature and high pressure CO 2 The corroded titanium carbonitride nano-coating is tightly bonded to the substrate, and the coating thickness is 30-32 μm.

[0125] Figure 4 The surface resistance of a Cr-containing low alloy steel material to high temperature and high pressure CO obtained in Example 1 2 EDS test image of corroded titanium carbonitride nano-coating surface. Figure 2 Display: The surface of a Cr-containing low alloy steel material obtained in Example 1 is resistant to high temperature and high pressure CO 2 The corroded titanium carbonitride nano coating is mainly composed of nitrogen, carbon, nitrogen and titanium, wherein the atomic percentage of carbon is 35.38%, the atomic percentage of nitrogen is 25.96%, and the atomic percentage of titanium is 38.66%.

[0126] Figure 5 This is a SEM test image of the titanium carbonitride crystal coating on the surface of the Cr-containing low-alloy steel material obtained in Comparative Example 1. Figure 5 It shows that the titanium carbonitride crystal coating on the surface of the Cr-containing low-alloy steel material obtained in Comparative Example 1 is mainly composed of long plate-like grains, and the length of the long plate-like grains is 1.5-2 μm and the width is 1.2 μm.

[0127] According to calculations, the surface resistance of a Cr-containing low alloy steel material obtained in Example 1 to high temperature and high pressure CO 2 The elements of the corroded titanium carbonitride nanocoating are nitrogen, carbon and titanium. The nitrogen content accounts for about 25.96% by mole, the carbon content accounts for about 35.38% by mole, and the titanium content accounts for about 38.66% by mole. The atomic percentages of nitrogen, carbon and titanium are shown in Table 1.

[0128] Table 1 shows the atomic percentage of each element in the titanium carbonitride nanocoating prepared in Example 1

[0129]

[0130] Performance Testing

[0131] High temperature and high pressure CO 2 Corrosion performance test

[0132] Method: The surface of a Cr-containing low alloy steel material prepared in Example 1 is resistant to high temperature and high pressure CO 2 Corrosion of Titanium Carbonitride Nanocoatings by High-temperature and High-pressure CO 2 Corrosion resistance test under corrosion.

[0133] Coating in high temperature and high pressure CO 2 Anti-corrosion performance test method under corrosion: using an electrochemical tester, at 80°C, 0.5Mpa saturated CO 2 The corresponding polarization curves, self-corrosion potential and self-corrosion current density values ​​were obtained by immersing the samples in the solution for different time periods. Each sample was tested 3 times and the average value of the results was taken.

[0134] result:

[0135] A Cr-containing low alloy steel material obtained in Example 1 has a surface resistance to high temperature and high pressure CO 2 The self-corrosion potential of the corroded titanium carbonitride nanocoating is -121.8mv, and the self-corrosion current density is 3.883×10 -6 (mA cm -2 ),like Figure 6 shown.

[0136] Corrosion resistance test

[0137] Method: The surface of a Cr-containing low alloy steel material prepared in Example 1 is resistant to high temperature and high pressure CO 2 The corrosion performance of the titanium carbonitride nanocoating was compared.

[0138] Corrosion performance test method: Before the test, the sample weight was weighed using an electronic balance; then the sample resistance to CO was tested using a high-temperature autoclave device. 2 Corrosion performance. The test parameters are: temperature: 60℃, CO 2 The pressure is 0.1MPa, and the test time is 360 hours. After the test, the surface corrosion products are removed by ultrasonic cleaning with chemical cleaning solution (500mL hydrochloric acid + 3.5 hexamethylenetetramine + 500mL deionized water), and then the surface is cleaned with 10% NaOH solution, deionized water and anhydrous ethanol for 20 minutes in sequence, and then the surface is dried with cold air and weighed with an electronic balance.

[0139] The calculation formula for uniform corrosion is:

[0140]

[0141] in,

[0142] CR: uniform corrosion rate (mm / a); W: mass loss (mg); A: sample surface area (mm 2); D: coating density (mg / cm 3 ); t: experimental time (h)

[0143] result:

[0144] Example 1: Surface resistance of a Cr-containing low alloy steel material to high temperature and high pressure CO 2 The uniform corrosion rate of the corroded titanium carbonitride nanocoating is 0.00015 mm / a. Figure 7 shown.

[0145] Friction performance test

[0146] Method: The surface of a Cr-containing low alloy steel material prepared in Example 1 is resistant to high temperature and high pressure CO 2 The friction performance of the corroded titanium carbonitride nanocoating was compared.

[0147] Friction performance test method: Rtec friction and wear tester was used to test the wear resistance of the sample. Test mode: 6mm SiC ball was used to perform XY bidirectional linear non-lubricated reciprocating friction on the sample at room temperature. The specific test parameters were: normal load 5-20N, friction speed 20mm / s, friction distance 5mm, time 20min, frequency 2Hz. Each sample was tested 3 times and the average value of the results was taken.

[0148] result:

[0149] A Cr-containing low alloy steel material obtained in Example 1 has a surface resistance to high temperature and high pressure CO 2 The friction coefficient of the corroded titanium carbonitride nanocoating is 0.26, as Figure 8 shown.

[0150] Wear performance test

[0151] Method: The wear performance comparison test was conducted on the titanium carbonitride anti-corrosion and wear-resistant coating on the surface of 316L stainless steel for oil and gas field surface pipelines prepared in Example 1.

[0152] Wear performance test method: Based on the friction performance test, firstly, the wear scar volume test is carried out by the surface profiler to obtain the wear scar volume data; secondly, the wear scar volume data is integrated and calculated by the analysis software to obtain the wear scar volume value; finally, the wear rate is calculated according to the wear rate calculation formula:

[0153]

[0154] in,

[0155] W: volume wear rate; V: wear volume; S: load size; L: total friction distance.

[0156] result:

[0157] Example 1: Surface resistance of a Cr-containing low alloy steel material to high temperature and high pressure CO 2 The average wear rate of the corroded titanium carbonitride nanocoating is 1.5×10 -7 mm 3 N -1 m -1 ,like Fig. 9 shown.

[0158] Example 2

[0159] The method is the same as in Example 1, except that the nitrogen source in step 1 is ammonia (NH 4 ).

[0160] The results show that the coating shows nanostructure and conical grain morphology, the ratio of nanostructure V1 to the volume V0 of the coating (V1 / V0) is 96%; the size of the nanograins is 200nm; the atomic percentage of nitrogen in the coating is 22.65%, the atomic percentage of carbon is 37.23%, and the atomic percentage of titanium is 42.12%; the self-corrosion potential of the coating is -134.2mv, and the self-corrosion current density is 4.646×10 -6 (mA cm -2 ), the friction coefficient of the coating is 0.29, and the average wear rate is 2.0×10 - 7 mm 3 N -1 m; the uniform corrosion rate of the coating is 0.0002mm / a,

[0161] Example 3

[0162] The method is the same as that of Example 1, except that in step 3, the carbon source is propylene.

[0163] The results show that the coating exhibits nanostructure and conical grain morphology, the ratio of the nanostructure V1 to the volume V0 of the coating (V1 / V0) is 97%; the size of the nanograins is 2200nm; the atomic percentage of nitrogen in the coating is 25.83%, the atomic percentage of carbon is 38.52%, and the atomic percentage of titanium is 35.65%; the self-corrosion potential of the coating is -138.6mv, and the self-corrosion current density is 4.763×10 -6 (mA cm -2 ), the friction coefficient of the coating is 0.30, and the average wear rate is 2.1×10 - 7 mm 3 N -1 m. The uniform corrosion rate of the coating is 0.0002mm / a.

[0164] Example 4

[0165] The method is the same as that of Example 1, except that in step 3, the titanium source is titanium tetrachloride.

[0166] The results show that the coating exhibits nanostructure and conical grain morphology, the ratio of the nanostructure V1 to the volume V0 of the coating (V1 / V0) is 97%; the size of the nanograins is 190nm; the atomic percentage of nitrogen in the coating is 27.02%, the atomic percentage of carbon is 36.28%, and the atomic percentage of titanium is 36.70%; the self-corrosion potential of the coating is -140.3mv, and the self-corrosion current density is 4.905×10 -6 (mA cm -2 ), the friction coefficient of the coating is 0.31, and the average wear rate is 2.1×10 - 7 mm 3 N -1 m. The uniform corrosion rate of the coating is 0.0002mm / a.

[0167] Example 5

[0168] The method is the same as that of Example 1, except that in step 3, the deposition temperature is 830°C.

[0169] The results show that the coating exhibits nanostructure and conical grain morphology, the ratio of the nanostructure V1 to the volume V0 of the coating (V1 / V0) is 96%; the size of the nanograins is 190nm; the atomic percentage of nitrogen in the coating is 27.02%, the atomic percentage of carbon is 36.28%, and the atomic percentage of titanium is 36.70%; the self-corrosion potential of the coating is -146.6mv, and the self-corrosion current density is 4.816×10 -6 (mA cm -2 ), the friction coefficient of the coating is 0.30, and the average wear rate is 1.9×10 - 7 mm 3 N -1 m. The uniform corrosion rate of the coating is 0.0002mm / a.

[0170] Example 6

[0171] The method is the same as that of Example 1, except that the third auxiliary gas is argon.

[0172] The results show that the coating exhibits nanostructure and conical grain morphology, the ratio of the nanostructure V1 to the volume V0 of the coating (V1 / V0) is 97%; the size of the nanograins is 230nm; the atomic percentage of nitrogen in the coating is 29.03%, the atomic percentage of carbon is 32.44%, and the atomic percentage of titanium is 38.53%; the self-corrosion potential of the coating is -143.2mv, and the self-corrosion current density is 4.881×10 -6 (mA cm -2 ), the friction coefficient of the coating is 0.29, and the average wear rate is 2.0×10 - 7 mm 3 N -1 m. The uniform corrosion rate of the coating is 0.0002mm / a.

[0173] Example 7

[0174] The method is the same as that of Example 1, except that in step 3, the second auxiliary gas is 1500 sccm.

[0175] The results show that the coating exhibits nanostructure and conical grain morphology, the ratio of the nanostructure V1 to the volume V0 of the coating (V1 / V0) is 98%; the size of the nanograins is 160nm; the atomic percentage of nitrogen in the coating is 26.18%, the atomic percentage of carbon is 33.72%, and the atomic percentage of titanium is 40.10%; the self-corrosion potential of the coating is -136.7mv, and the self-corrosion current density is 3.921×10 -6 (mA cm -2 ), the friction coefficient of the coating is 0.28, and the average wear rate is 2.0×10 - 7 mm 3 N -1 m. The uniform corrosion rate of the coating is 0.0002mm / a.

[0176] Example 8

[0177] The method is the same as that of Example 1, except that in step 3, the methane flow rate is 300 sccm.

[0178] The results show that the coating exhibits nanostructure and conical grain morphology, the ratio of the nanostructure V1 to the volume V0 of the coating (V1 / V0) is 96%; the size of the nanograins is 210nm; the atomic percentage of nitrogen in the coating is 23.49%, the atomic percentage of carbon is 38.41%, and the atomic percentage of titanium is 38.10%; the self-corrosion potential of the coating is -147.5mv, and the self-corrosion current density is 4.876×10 -6 (mA cm -2), the friction coefficient of the coating is 0.31, and the average wear rate is 2.0×10 - 7 mm 3 N -1 m. The uniform corrosion rate of the coating is 0.0002mm / a.

[0179] Comparative Examples 1-6

[0180] Preparation of Titanium Carbonitride Crystalline Coating Composited on Surface of Cr-Containing Low Alloy Steel

[0181] The titanium carbonitride crystal coatings described in Comparative Examples 1-6 were prepared in a similar manner to that of Example 1, except that the parameters in the coating preparation process were changed as shown in Table 2, and the grain morphology, grain size, and element percentage of the coatings were characterized. 2 Corrosion, friction and wear test methods are used to determine the corrosion resistance, friction coefficient and average wear rate.

[0182] Among them, the SEM image of the titanium carbonitride crystal coating on the surface of the composite and Cr-containing low alloy steel obtained in Comparative Example 1 is as follows Figure 6 As shown. Figure 6 It can be seen that the grains of the titanium carbonitride crystal coating prepared in Comparative Example 1 are in the shape of long flakes, and the length of the long flake grains is 1.5-2 μm and the width is 1.2 μm.

[0183] Table 2 Characterization and performance test of titanium carbonitride crystal coating prepared in Comparative Examples 1-6

[0184]

[0185]

[0186] Comparison of Examples 1-8 and Comparative Examples 1-6

[0187] The corrosion performance and friction and wear performance of the coatings prepared in Example 1 and Comparative Examples 1-6 are compared. The comparison results are shown in Figure 6 , Figure 7 , Figure 8 and Fig. 9 .

[0188] from Figure 6 , Figure 7 , Figure 8 and Fig. 9It can be seen that the self-corrosion potential of the titanium carbonitride nano-coating on the surface of the Cr-containing low-alloy steel prepared in Example 1 is -121.8 mv, which is significantly lower than the self-corrosion potential of the titanium carbonitride crystal coating prepared in Comparative Examples 1-6 (such as the self-corrosion potential of Comparative Example 1 is -231.4 mv); the self-corrosion current density of the titanium carbonitride nano-coating on the surface of the Cr-containing low-alloy steel prepared in Example 1 is 3.883×10 -6 (mA cm -2 ), which is significantly smaller than the titanium carbonitride crystal coatings prepared in Comparative Examples 1-6 (e.g., the self-corrosion current density of Comparative Example 1 is 1.135×10 -4 (mA cm -2 )). The average corrosion rate of the titanium carbonitride nano-coating on the surface of the Cr-containing low-alloy steel prepared in Example 1 is 0.00015 mm / a, which is significantly lower than the titanium carbonitride crystal coating prepared in Comparative Examples 1-6 (such as the average corrosion rate of Comparative Example 1 is 0.0021 mm / a). The friction coefficient of the titanium carbonitride nano-coating on the surface of the Cr-containing low-alloy steel prepared in Example 1 is 0.26, which is significantly lower than the titanium carbide crystal coating prepared in Comparative Examples 1-6 (such as the friction coefficient of Comparative Example 1 can reach 0.37). The average wear rate of the titanium carbonitride nano-coating on the surface of the Cr-containing low-alloy steel prepared in Example 1 is 1.5×10 - 7 mm 3 N -1 m -1 , which is significantly smaller than that of Comparative Examples 1-6 (for example, in Comparative Example 6, the average wear rate is 2.1×10 -6 mm 3 N -1 m). Therefore, it is shown that the titanium carbonitride nanocoating prepared in Example 1 has better resistance to high temperature and high pressure CO than the titanium carbonitride crystal coatings prepared in Comparative Examples 1-6. 2 Corrosion and friction and wear resistance.

[0189] In addition, the self-corrosion potential, self-corrosion current density, average corrosion rate, friction coefficient and average wear rate of Examples 1-8 are significantly lower than those of Comparative Examples 1-6, indicating that the titanium carbonitride nano-coating on the surface of the Cr low alloy steel material prepared in Examples 1-8 has excellent resistance to high temperature and high pressure CO 2 Corrosion and friction and wear resistance.

[0190] discuss

[0191] In the titanium carbonitride nano-coating prepared in the embodiment of the present invention, the ratio of the volume V1 of the nano-grain structure to the volume V0 of the coating (V1 / V0) is ≥90%, or even ≥95%.

[0192] Example 7

[0193] The nitrogen source is nitrogen, the titanium source is titanium dichloride, the carbon source is methane, and the other steps not involved are the same as those in Example 1.

[0194] Example 8

[0195] The nitrogen source is acetonitrile, the titanium source is titanium trichloride, the carbon source is ethane, and the other steps not involved are the same as those in Example 1.

[0196] Example 9

[0197] The titanium source is butyl titanate, the carbon source is propane, and the other steps not involved are the same as those in Example 1.

[0198] Example 10

[0199] The titanium source is titanium powder, the carbon source is ethylene, and the other steps not involved are the same as those in Example 1.

[0200] Embodiment 11

[0201] The carbon source is a mixed gas of propane and acetylene, and the remaining steps not involved are the same as those in Example 1.

[0202] Example 12

[0203] In the step 2, evacuate to a vacuum degree of 0.5 Pa, introduce the first auxiliary gases hydrogen and nitrogen, the hydrogen flow rate is 100 sccm, the nitrogen flow rate is 300 sccm, set the preheating temperature to 50°C, the heating rate to 6°C / min, and the other steps not involved are the same as those in Example 1.

[0204] Example 13

[0205] In the step 2, evacuate to a vacuum degree of 0.8 Pa, introduce the first auxiliary gases hydrogen and nitrogen, the hydrogen flow rate is 150 sccm, the nitrogen flow rate is 100 sccm, set the preheating temperature to 80°C, the heating rate to 8°C / min, and the other steps not involved are the same as those in Example 1.

[0206] Embodiment 14

[0207] In step 3, the CVD system heating program is started, the heating temperature is set to 650°C, the heating rate is set to 8°C / min, the flow rate of the second auxiliary gas is set to 800sccm, the flow rate of hydrogen in the third auxiliary gas is set to 1000sccm, and the flow rate of argon is set to 1000sccm; the deposition time is 580min; the deposition pressure is set to 0.02MPa, and the other steps not involved are the same as those in Example 1.

[0208] Embodiment 15

[0209] In the step 3, the CVD system heating program is started, the heating temperature is set to 700°C, the heating rate is set to 8°C / min, the flow rate of the second auxiliary gas is set to 1000sccm, the flow rate of hydrogen in the third auxiliary gas is set to 500sccm, and the flow rate of argon is set to 800sccm; the deposition time is 500min; the deposition pressure is set to 0.05MPa, and the other steps not involved are the same as those in Example 1.

[0210] Example 16

[0211] In the step 3, the CVD system heating program is started, the heating temperature is set to 850°C, the heating rate is set to 8°C / min, the flow rate of the second auxiliary gas is set to 500sccm, the flow rate of hydrogen in the third auxiliary gas is set to 800sccm, and the flow rate of argon is set to 500sccm; the deposition time is 600min; the deposition pressure is set to 0.03MPa, and the other steps not involved are the same as those in Example 1.

[0212] Embodiment 17

[0213] In step 4, the hydrogen flow rate in the first auxiliary gas is adjusted to 200 sccm; the hydrogen flow rate of the second auxiliary gas is adjusted to 100 sccm, the cooling rate is 7°C / min, and the temperature is cooled to 400°C; then the introduction of the second auxiliary gas is stopped; when the temperature drops to 150°C, the introduction of the first auxiliary gas is stopped, and the other steps not involved are the same as those in Example 1.

[0214] Embodiment 18

[0215] In step 4, the hydrogen flow rate in the first auxiliary gas is adjusted to 300 sccm; the hydrogen flow rate of the second auxiliary gas is adjusted to 1000 sccm, the cooling rate is 7°C / min, and the temperature is cooled to 300°C; then the introduction of the second auxiliary gas is stopped; when the temperature drops to 100°C, the introduction of the first auxiliary gas is stopped, and the other steps not involved are the same as those in Example 1.

[0216] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a titanium carbonitride nano-coating on the surface of a Cr-containing low alloy steel, characterized in that: The following steps are involved: Step 1, under vacuum conditions, introducing a first auxiliary gas into a chemical vapor deposition chamber to preheat a substrate; the substrate is a Cr-containing low alloy steel; Step 2, introducing a nitrogen source, a carbon source and a titanium source into a chemical vapor deposition chamber; the nitrogen source is introduced through a second auxiliary gas, and the titanium source is introduced through a third auxiliary gas, and the introduced reactants undergo chemical reaction deposition on the surface of the substrate to obtain a process coating; The deposition temperature is 650-850°C, the deposition time is 300-800 min, and the deposition pressure is 0.02-0.05 MPa; In step 2, the nitrogen source is nitrogen, acetonitrile, ammonia, or a combination thereof; the titanium source is titanium dichloride, and the carbon source is methane; The flow rate of the carbon source is 300-600 sccm; Step 3, cooling the coating to obtain a titanium carbonitride nano coating; In the coating, the total content of N, C and Ti is ≥ 96%; The titanium carbonitride nano-coating is composed of titanium carbonitride nano-grains, the nano-grains have a cone-shaped morphology, and the average diameter of the nano-grains is 20-200nm; The ratio of the total volume V1 of the titanium carbonitride nanocrystals to the volume V0 of the coating (V1 / V0) is ≥80%; The cooling process is: (3-1) First stage cooling process: stop introducing the titanium source and the third auxiliary gas, the flow rate of the first auxiliary gas is 100-300 sccm, the flow rate of the second auxiliary gas is 100-300 sccm, the cooling rate is 5-10°C / min, and the temperature is cooled to 300-500°C; (3-2) Second stage cooling process: when the temperature drops to 300-500°C, stop introducing the second auxiliary gas; when the temperature drops to 100-200°C, stop introducing the first auxiliary gas, and then cool to room temperature to obtain a titanium carbonitride nano-coating on the surface of a Cr-containing low alloy steel material; The coating is attached to the surface of a substrate, which is a Cr-containing low alloy steel; the coating has, in atomic percentage, 20-30% nitrogen, 30-50% carbon, and 30-40% titanium, and the sum of the atomic percentages of the three elements is ≤100%.

2. The method for preparing a titanium carbonitride nano-coating on the surface of a Cr-containing low alloy steel according to claim 1, characterized in that: The first auxiliary gas is a mixed gas of hydrogen and nitrogen; the second auxiliary gas is hydrogen, and the third auxiliary gas is hydrogen and nitrogen.

3. The method for preparing a titanium carbonitride nano-coating on the surface of a Cr-containing low alloy steel according to claim 2, characterized in that: In step 1, the preheating vacuum is 0.5-1Pa, the preheating temperature is 50-80°C, the hydrogen flow rate in the first auxiliary gas is 100-200sccm, and the nitrogen flow rate is 100-300sccm; the flow rate of the second auxiliary gas is 500-1000sccm; the flow rate of hydrogen in the third auxiliary gas is 500-1000sccm, and the flow rate of argon is 500-1000sccm.

4. The titanium carbonitride nano-coating on the surface of Cr-containing low alloy steel prepared by the preparation method according to claim 1 is characterized in that: The coating is attached to the surface of a substrate, which is a Cr-containing low alloy steel; the coating has, in atomic percentage, 20-30% nitrogen, 30-50% carbon, and 30-40% titanium, and the sum of the atomic percentages of the three elements is ≤100%.

5. The titanium carbonitride nano coating on the surface of Cr-containing low alloy steel according to claim 4, characterized in that: The coating has a thickness of 10-45 μm.

6. The titanium carbonitride nano coating on the surface of Cr-containing low alloy steel according to claim 4, characterized in that: The friction coefficient of the coating is 0.25-0.31; the self-corrosion potential of the coating is -121.8mv, and the self-corrosion current density is 3.883×10 -6 (mA cm).