A conductive Mxene nanocomposite organic hydrogel and its preparation method and application
By introducing components such as cyclodextrin modified chitosan and thermosensitive monomers into Mxene hydrogels, Mxene nanocomposite organic hydrogels with dynamic crosslinking network structures were prepared, and the detection of microscopic in the prior art was solved The problem of insufficient strain accuracy achieves high-precision temperature and strain sensing, and expands the detection range.
Patent Information
- Application Number
- CN202211037916.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-26
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2042-08-26
AI Technical Summary
The existing Mxene hydrogels have insufficient accuracy in detecting tiny strains such as saliva swallowing and pulse changes, which cannot meet the application needs of the medical field, and the sensor's detection range and accuracy are low.
Using cyclodextrin modified chitosan, Mxene suspension, thermosensitive monomer and benzaldehyde polyethylene glycol derivatives, Mxene with dynamic crosslinking network structure is prepared by ultrasonic mixing and initiator reaction. Nanocomposite organic hydrogel achieves the combination of conductivity and self-healing capabilities, enhancing temperature and strain sensing functions.
This method briefly prepares conductive hydrogels, with good mechanical properties and multiple dynamic crosslinking characteristics, realizes high-precision detection of tiny strains, expands the detection range and temperature adaptation range of the sensor, and solves the single sensor signal , the problem of low accuracy.
Smart Images

Figure CN115490884B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of biomedical engineering materials, and in particular to a conductive Mxene nanocomposite organic hydrogel and a preparation method and application thereof. Background Art
[0002] In recent years, flexible and wearable strain sensors have attracted great attention due to their numerous applications in electronic skin, personalized healthcare monitoring, and human-computer interaction. However, a major obstacle faced by these flexible and stretchable electronics is the mismatch between human tissue and traditional electronics in terms of mechanical and electrical properties. Human tissue is soft and conducts electrical signals through ions, while electronics are rigid and rely on electrons to conduct electricity. In this context, biomimetic functional materials have attracted considerable attention.
[0003] Hydrogel is a soft material with a unique 3D network structure formed by physical or chemical crosslinking of polymers. Hydrogels are mainly composed of water (>99%) and solvated molecules / polymers / inorganic particles (gelators). This means that hydrogels can maintain the same physicochemical properties as liquid water while exhibiting rheological behaviors similar to solids on a macro scale. Due to their highly designable structure and functionality, hydrogels have been widely used in bionic materials, flexible wearable devices, and soft robots.
[0004] Among the existing 2D nanomaterials, the transition metal carbide, nitride or carbonitride (MXene) family has attracted extensive attention due to its unique combination of metallic conductivity, solution processability, high aspect ratio and widely adjustable properties. MXene has shown very outstanding performance in a range of applications such as energy storage, sensing, optoelectronics, catalysis and biomedicine.
[0005] The prior art describes that an antifreeze, self-healing, and conductive Mxene nanocomposite organic hydrogel (MNOH) is prepared by immersing Mxene nanocomposite hydrogel (MNH) in an ethylene glycol (EG) solution to replace some water molecules. The prepared MNOH has excellent antifreeze performance (-40°C) and long-lasting moisturizing performance (8 days).
[0006] Prior art has disclosed multifunctional conductive organic hydrogels based on 2D MXene nanosheets and ZA fibers and then assembled wireless wearable sensors to track human motion. By introducing a ternary mixture, the organic hydrogel has ultra-low temperature (-81°C) and moisture retention. At the same time, the interaction between alginate chains and PAM induced by zinc ions gives the organic hydrogel superior mechanical properties.
[0007] The prior art (CN113603819A) also discloses a method for preparing a flexible wearable sensor based on MXene nanosheet composite polyelectrolyte hydrogel. The method synthesizes polyampholyte hydrogel by one-step random copolymerization of anionic and cationic monomers with MXene nanosheets. The synthesized hydrogel can sensitively and stably detect a full range of human activities (such as rotating the elbow, bending fingers, etc.) and writing.
[0008] In summary, the existing research focus on Mxene hydrogels is mainly on improving the mechanical properties, antifreeze properties and sensing stability of hydrogels. The smallest detection strain range of the existing technology is a bent finger, and the detection accuracy of small strains such as saliva swallowing is not enough. However, the detection of small strains such as saliva swallowing and pulse changes has great application potential in the medical field. Therefore, how to construct a hydrogel-based strain sensor with durability, efficient self-repair and low detection limit is a research trend in this field and a key scientific problem to be solved urgently. It is also a technical bottleneck that urgently needs to be broken through in the field of biomedical engineering. Summary of the invention
[0009] The purpose of the present invention is to overcome the above-mentioned deficiencies of the prior art and to provide a conductive Mxene nanocomposite organic hydrogel and a preparation method and application thereof.
[0010] The first object of the present invention is to provide a method for preparing a conductive Mxene nanocomposite organic hydrogel.
[0011] The second object of the present invention is to provide the Mxene nanocomposite organic hydrogel prepared by the above preparation method.
[0012] The third object of the present invention is to provide the use of the above-mentioned Mxene nanocomposite organic hydrogel in the preparation of a flexible temperature sensor.
[0013] The fourth object of the present invention is to provide the use of the above-mentioned Mxene nanocomposite organic hydrogel in the preparation of flexible strain sensors.
[0014] In order to achieve the above object, the present invention is implemented by the following scheme:
[0015] A method for preparing a conductive Mxene nanocomposite organic hydrogel comprises the following steps:
[0016] The cyclodextrin-modified chitosan, the Mxene suspension and the alcohol-water mixture are fully mixed, and then the thermosensitive monomer and the adamantyl-containing acrylic monomer are added, and after fully mixing, the initiator, the benzaldehyde-based polyethylene glycol derivative and N, N, N, N-tetramethylethylenediamine are added in sequence, and the Mxene nanocomposite organic hydrogel is obtained by fully reacting.
[0017] The structural formula of the cyclodextrin-modified chitosan is shown in formula (I), wherein x is an integer of 23 to 30, y is an integer of 217 to 272, and z is an integer of 3 to 8.
[0018]
[0019] The structural formula of the benzaldehyde-based polyethylene glycol derivative is shown in formula (II); wherein x is an integer of 70 to 85,
[0020]
[0021] The adamantyl-containing acrylic monomer is one or both of adamantyl acrylate and / or adamantyl methacrylate; the molar ratio of the temperature-sensitive monomer to the adamantyl-containing acrylic monomer is 200-400:1; and the alcohol-water mixture is a mixture of deionized water: glycerol = 1:0-1:1.
[0022] Preferably, the mass ratio of the cyclodextrin-modified chitosan to Mxene is 2-3:1-2.
[0023] More preferably, the mass ratio of the cyclodextrin-modified chitosan to Mxene is 2:1.
[0024] Preferably, the volume ratio of the Mxene to the alcohol-water mixture is 2-1:3-2.
[0025] Preferably, the method of fully mixing is ultrasonic mixing for 30 to 60 minutes.
[0026] Preferably, the initiator is ammonium persulfate and / or potassium persulfate.
[0027] Preferably, the temperature-sensitive monomer is one or more of N-isopropylacrylamide, N-propylacrylamide, N-cyclopropylacrylamide, N,N-diethylacrylamide, N-vinylisopropylamide, N-vinylpropionamide, N-vinylcaprolactam, N-vinylpyrrolidone, N-acryloylpyrrolidine, N-acryloyl-N-propopiperazine, N-(2,2-dimethyl-1,3-dioxane-5-ol)-acrylamide and / or N-(2-ethoxy-1,3-dioxane-5-ol)-acrylamide.
[0028] Preferably, an ice water bath is used throughout the entire process after the temperature-sensitive monomer is added.
[0029] Preferably, before adding the benzaldehyde-based polyethylene glycol derivative, the entire process is carried out under an ultrasonic environment.
[0030] The present invention also claims protection for the Mxene nanocomposite organic hydrogel prepared by any of the above preparation methods.
[0031] The present invention also seeks to protect the use of the above-mentioned Mxene nanocomposite organic hydrogel in the preparation of a flexible temperature sensor.
[0032] The present invention also seeks to protect the use of the above-mentioned Mxene nanocomposite organic hydrogel in the preparation of flexible strain sensors.
[0033] Compared with the prior art, the present invention has the following beneficial effects:
[0034] The invention discloses a method for preparing a conductive Mxene nanocomposite organic hydrogel. The preparation method is simple and quick, and the gel can be obtained by a one-pot method. Mxene is taken as a conductive material, and an ultrasonic method is used to promote the conductive material to be evenly distributed in the hydrogel to form a conductive hydrogel.
[0035] The Mxene nanocomposite organic hydrogel prepared by the preparation method includes a first unit (cyclodextrin-modified chitosan), a second unit (benzaldehyde-based polyethylene glycol derivative) and a third unit (thermosensitive polymer). The amino group on the chitosan chain of the first unit reacts with the terminal aldehyde group of the second unit to form a first layer of dynamically cross-linked network. The first unit and the second unit are connected based on the self-assembly of the host and guest of adamantane-cyclodextrin to form a second layer of dynamically cross-linked network. Mxene is dispersed between the interpenetrating double network hydrogel as a conductive material. Mxene, as a layered conductive material, forms abundant hydrogen bonds with the hydroxyl groups on the first unit and the second unit. The double network structure gives the hydrogel good mechanical properties, and the multiple dynamic cross-linking characteristics give the hydrogel excellent self-healing ability. The hydrogel with both temperature sensitivity and conductivity has dual sensing functions of temperature and strain, and the phase change enhancement effect of the thermosensitive polymer based on the host-guest dynamic cross-linking gives the hydrogel extremely high strain sensing accuracy.
[0036] The dispersion medium in the Mxene nanocomposite organic hydrogel prepared by the preparation method of the present invention introduces an alcohol-water mixed solvent so that the prepared conductive hydrogel has good antifreeze properties and a wider temperature adaptability range, and has a lower detection limit, and can sense even small strains, thereby expanding the detection range of the hydrogel sensor and solving the technical defects of the existing conductive hydrogel, such as narrow application range, single sensing signal and low sensing accuracy. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 The resistance change sensing diagram of the Mxene nanocomposite organic hydrogel prepared in Example 1 at different temperatures;
[0038] Figure 2 This is a compressive strain resistance change sensor diagram of the Mxene nanocomposite organic hydrogel prepared in Example 1;
[0039] Figure 3 The resistance change sensing diagram of the Mxene nanocomposite organic hydrogel prepared in Example 1 under different strains;
[0040] Figure 4 This is a compressive strain resistance change sensor diagram of the hydrogel prepared in Comparative Example 1;
[0041] Figure 5 This is the compressive strain resistance change sensor diagram of the hydrogel prepared in Comparative Example 2. DETAILED DESCRIPTION
[0042] The present invention is further described in detail below in conjunction with the accompanying drawings and specific examples of the specification. The examples are only used to explain the present invention and are not used to limit the scope of the present invention. The test methods used in the following examples are conventional methods unless otherwise specified; the materials and reagents used are reagents and materials that can be obtained from commercial channels unless otherwise specified.
[0043] Example 1 Preparation and detection of Mxene nanocomposite organic hydrogel
[0044] The structural formula of cyclodextrin modified chitosan (HPCS-CD) is shown in formula (I), wherein x is an integer of 23 to 30, y is an integer of 217 to 272, and z is an integer of 3 to 8.
[0045]
[0046] The structural formula of the benzaldehyde-based polyethylene glycol derivative (PEGFA) is shown in formula (II), wherein x is an integer of 70 to 85,
[0047]
[0048] The alcohol-water mixture is a mixture of glycerol: deionized water = 1:1.
[0049] 1. Preparation of MXene nanocomposite organic hydrogel
[0050] 0.6 g of cyclodextrin-modified chitosan (HPCS-CD) was dissolved in 2 mL of Mxene suspension and alcohol-water mixture, and 50 μL of adamantyl acrylate (ADMA) was added after ultrasonic treatment for 30 min, followed by 0.35 g of N-isopropylacrylamide (NIPAM) and ultrasonic treatment for 60 min.
[0051] Then, 0.005-0.01 g of ammonium persulfate (APS) was added and ultrasonicated for 5 min, followed by 1-2 mL of PEGFA and 200-500 μL of N,N,N,N-tetramethylethylenediamine (TEMED). The mixture was magnetically stirred evenly and the magnet was removed within 1 min. The mixture was allowed to stand to obtain the Mxene nanocomposite organic hydrogel.
[0052] 2. Identification of MXene Nanocomposite Organic Hydrogel
[0053] The two ends of the Mxene nanocomposite organic hydrogel prepared in step 2 are tightly fixed to the electrochemical workstation sensor with two layers of conductive copper sheets and copper wires. The hydrogel is placed on a temperature control table. The temperature of the Mxene nanocomposite organic hydrogel prepared in step 2 is changed to observe the change in its resistance, thereby reflecting the temperature sensitivity of the hydrogel.
[0054] The experimental results are as follows Figure 1 As shown, at different temperatures, the corresponding ΔR / R0 (ΔR=R-R0, R and R0 are the original resistance and the resistance under a certain deformation, respectively) are different and have obvious differences, indicating that the hydrogel has temperature sensing ability.
[0055] The two ends of the Mxene nanocomposite organic hydrogel prepared in step 2 are tightly fixed to the electrochemical workstation sensor with two layers of conductive copper sheets and copper wires. The hydrogel is fixed on a press. The Mxene nanocomposite organic hydrogel prepared in step 2 is compressed to observe its resistance change, thereby reflecting the sensing accuracy.
[0056] The experimental results are as follows Figure 2 As shown, in the process of continuous compression of the hydrogel, the corresponding ΔR / R0 gradually decreases from 0 to 75%, and there is a resistance change when the strain is very small, with a sensitivity of 0.426% and high sensing accuracy.
[0057] The two ends of the Mxene nanocomposite organic hydrogel prepared in step 2 were tightly fixed to the electrochemical workstation sensor with two layers of conductive copper sheets and copper wires, and 1%, 2% and 5% strains were applied to the hydrogel respectively to test the resistance change of the Mxene nanocomposite organic hydrogel under different strains.
[0058] The results are as follows Figure 3 As shown, when 1%, 2% and 5% strains are applied, ΔR / R0 changes significantly, and has the ability to detect different strains.
[0059] Example 2 Preparation of Mxene Nanocomposite Organic Hydrogel
[0060] The materials used in this embodiment are consistent with those in Embodiment 1.
[0061] 0.6 g of HPCS-CD was dissolved in 2 mL of Mxene suspension and alcohol-water mixture, and 50 μL of adamantyl acrylate (ADMA) was added after ultrasonic treatment for 30 min, followed by 0.35 g of N-propylacrylamide and ultrasonic treatment for 60 min.
[0062] Then, 0.005-0.01 g of ammonium persulfate (APS) was added and ultrasonicated for 5 min, followed by 1-2 mL of PEGFA and 200-500 μL of N,N,N,N-tetramethylethylenediamine (TEMED). The mixture was magnetically stirred evenly and the magnet was removed within 1 min. The mixture was allowed to stand to obtain the Mxene nanocomposite organic hydrogel.
[0063] Example 3 Preparation of Mxene Nanocomposite Organic Hydrogel
[0064] The materials used in this embodiment are consistent with those in Embodiment 1.
[0065] 0.6 g of HPCS-CD was dissolved in 2 mL of Mxene suspension and alcohol-water mixture, and 50 μL of adamantyl acrylate (ADMA) was added after ultrasonic treatment for 30 min, followed by 0.35 g of N-cyclopropylacrylamide and ultrasonic treatment for 60 min.
[0066] Then, 0.005-0.01 g of ammonium persulfate (APS) was added and ultrasonicated for 5 min, followed by 1-2 mL of PEGFA and 200-500 μL of N,N,N,N-tetramethylethylenediamine (TEMED). The mixture was magnetically stirred evenly and the magnet was removed within 1 min. The mixture was allowed to stand to obtain the Mxene nanocomposite organic hydrogel.
[0067] Comparative Example 1 Preparation and Detection of a Hydrogel
[0068] The materials used in this embodiment are consistent with those in Embodiment 1.
[0069] 1. Preparation of Hydrogel
[0070] 0.6 g of HPCS-CD was dissolved in 2 mL of the Mxene suspension and alcohol-water mixture, and ultrasonicated for 30 min. Then, 0.35 g of N-isopropylacrylamide (NIPAM) was added and ultrasonicated for 60 min.
[0071] Then, 0.005-0.01 g of ammonium persulfate (APS) was added and ultrasonicated for 5 min, and then 1-2 mL of PEGFA was added. The mixture was magnetically stirred evenly and the magnet was removed within 1 min. The hydrogel was obtained by standing.
[0072] 2. Identification of Hydrogels
[0073] The two ends of the hydrogel prepared in step 1 are tightly fixed to the electrochemical workstation sensor with two layers of conductive copper sheets and copper wires. The hydrogel is fixed on a press and the hydrogel is compressed to observe the change in its resistance, thereby reflecting the sensing accuracy.
[0074] The experimental results are as follows Figure 4As shown, during the continuous compression of the hydrogel, the corresponding ΔR / R0 gradually decreased by 60% from 0. The volume of the hydrogel decreased by less than 10%, and the sensitivity was 0.995%. The sensing accuracy and change rate were not as good as those of the Mxene nanocomposite organic hydrogel prepared in Example 1.
[0075] Comparative Example 2 Preparation and Detection of a Hydrogel
[0076] The materials used in this embodiment are consistent with those in Embodiment 1.
[0077] 1. Preparation of Hydrogel
[0078] Take 0.6 g of HPCS-CD and dissolve it in 2 mL of Mxene suspension and alcohol-water mixture. After ultrasonic treatment for 30 minutes, add 50 μL of adamantane acrylate (ADMA) and stir, then add 0.1-0.2 g of acrylamide monomer and stir, then add 0.005-0.01 g of ammonium persulfate (APS) and ultrasonicate for 5 minutes, stir evenly with a magnetic stir, remove the magnet within 1 minute, and let it stand to obtain the hydrogel.
[0079] 2. Identification of Hydrogels
[0080] The two ends of the hydrogel prepared in step 1 are tightly fixed to the electrochemical workstation sensor with two layers of conductive copper sheets and copper wires. The hydrogel is fixed on a press and the hydrogel is compressed to observe the change in its resistance, thereby reflecting the sensing accuracy.
[0081] The experimental results are as follows Figure 5 As shown in the figure, during the continuous compression of the hydrogel, the corresponding ΔR / R0 gradually decreases from 0 to 60% (ΔR=R-R0, R and R0 are the original resistance and the resistance under a certain deformation, respectively). The volume of the hydrogel is reduced by less than 10%, and the sensitivity is 9.21%. The sensing accuracy and change rate are not as good as those of the Mxene nanocomposite organic hydrogel prepared in Example 1.
[0082] Comparative Example 3 Preparation of a hydrogel
[0083] The materials used in this embodiment are consistent with those in Embodiment 1.
[0084] 0.6 g of HPCS-CD was dissolved in 2 mL of an alcohol-water mixture, and after ultrasonication for 30 min, 50 μL of adamantyl acrylate (ADMA) was added, followed by 0.35 g of N-isopropylacrylamide (NIPAM) and ultrasonication for 60 min.
[0085] Next, 0.005-0.01 g of ammonium persulfate (APS) was added and ultrasonicated for 5 min, followed by 1-2 mL of PEGFA and 200-500 μL of N,N,N,N-tetramethylethylenediamine (TEMED). The mixture was stirred evenly with a magnetic stirrer, the magnet was removed within 1 min, and the hydrogel was obtained by standing.
[0086] Comparative Example 4 Preparation of a hydrogel
[0087] The materials used in this embodiment are consistent with those in Embodiment 1.
[0088] 0.6 g of HPCS-CD was dissolved in 2 mL of Mxene suspension and alcohol-water mixture, and 50 μL of adamantyl acrylate (ADMA) was added after ultrasonic treatment for 30 min, followed by 0.35 g of N-isopropylacrylamide (NIPAM) and ultrasonic treatment for 60 min.
[0089] Then, 0.005-0.01 g of ammonium persulfate (APS) was added and ultrasonicated for 5 min, and then 1-2 mL of PEGFA was added. The mixture was magnetically stirred evenly and the magnet was removed within 1 min. The hydrogel was obtained by standing.
[0090] Comparative Example 5 Preparation of a hydrogel
[0091] The materials used in this embodiment are consistent with those in Embodiment 1.
[0092] Take 0.6 g of HPCS-CD and dissolve it in 2 mL of Mxene suspension and alcohol-water mixture. After ultrasonic treatment for 30 minutes, add 50 μL of adamantane acrylate (ADMA), then add 0.35 g of N-isopropylacrylamide (NIPAM) and stir for 60 minutes. After stirring, add 0.005-0.01 g of ammonium persulfate (APS) and ultrasonicate for 5 minutes. Stir magnetically evenly and remove the magnet within 1 minute. Let it stand to obtain hydrogel.
[0093] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit the protection scope of the present invention. For ordinary technicians in this field, other different forms of changes or modifications can be made based on the above descriptions and ideas. It is not necessary and impossible to list all the implementation methods here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.
Claims
1. A method for preparing a conductive Mxene nanocomposite organic hydrogel, characterized in that: The following steps are involved: The cyclodextrin-modified chitosan, the Mxene suspension and the alcohol-water mixture are fully mixed, and then the temperature-sensitive monomer and the adamantyl-containing acrylic monomer are added, and after being fully mixed, the initiator, the benzaldehyde-based polyethylene glycol derivative and N, N, N, N-tetramethylethylenediamine are added in sequence, and the Mxene nanocomposite organic hydrogel is obtained by fully reacting; the initiator is ammonium persulfate, and the temperature-sensitive monomer is N-isopropylacrylamide; The structural formula of the cyclodextrin-modified chitosan is shown in formula (I), wherein x is an integer of 23 to 30, y is an integer of 217 to 272, and z is an integer of 3 to 8. The structural formula of the benzaldehyde-based polyethylene glycol derivative is shown in formula (II); wherein x is an integer of 70 to 85, The adamantyl-containing acrylic monomer is one or both of adamantyl acrylate and / or adamantyl methacrylate; the molar ratio of the temperature-sensitive monomer to the adamantyl-containing acrylic monomer is 200-400:1; and the alcohol-water mixture is a mixture of deionized water: glycerol = 1:0-1:
1.
2. The preparation method according to claim 1, characterized in that: The mass ratio of the cyclodextrin modified chitosan to Mxene is 2-3:1-2.
3. The preparation method according to claim 1, characterized in that: The volume ratio of the Mxene to the alcohol-water mixture is 2-1:3-2.
4. The preparation method according to claim 1, characterized in that: The method for fully mixing is ultrasonic mixing for 30 to 60 minutes.
5. The preparation method according to claim 1, characterized in that: After adding the temperature-sensitive monomer, keep the mixture in an ice-water bath.
6. The Mxene nanocomposite organic hydrogel prepared by the preparation method according to any one of claims 1 to 5.
7. Use of the Mxene nanocomposite organic hydrogel according to claim 6 in the preparation of a flexible temperature sensor.
8. Use of the Mxene nanocomposite organic hydrogel according to claim 6 in the preparation of a flexible strain sensor.