A high-performance crystal epoxy resin and its application

Through the formulation of composite epoxy resin and specific additives, the problems of poor aging resistance and insufficient toughness of materials in the preparation of traditional crystal diamonds are solved, and the preparation of high-performance crystal glue is realized. The product shows excellent durability under UV and high temperature conditions. and optical properties, reducing production costs.

CN115490991BActive Publication Date: 2024-10-29WUXI JIALIAN ELECTRONIC MATERIALS CO LTD

Patent Information

Application Number
CN202211144047.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-20
Publication Date
2024-10-29
Estimated Expiration
2042-09-20

AI Technical Summary

Technical Problem

In the traditional preparation process of crystal diamonds, the glass material is cumbersome to process at high temperatures, has high energy consumption and high cost, and the product has poor aging resistance and insufficient toughness, resulting in products that are prone to cracking and have bubbles and micropore defects.

Method used

Composite epoxy resin is used as the raw material. By formulating Agent A and Agent B, adding leveling agent, defoaming agent, curing accelerator and UV absorber to adjust the viscosity and defoaming properties, combined with hydrogenated bisphenol A type epoxy resin, Silicone-modified epoxy resin and low-viscosity epoxy resin are used to prepare high-performance crystal glue, which is cured after potting with a dispensing machine and vacuum degassing.

Benefits of technology

The aging resistance, toughness and defoaming properties of the crystal material are improved. The product shows excellent durability and optical properties under UV and high temperature conditions, extending the service life and reducing production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003854876480000061
    Figure BDA0003854876480000061
  • Figure BDA0003854876480000081
    Figure BDA0003854876480000081
Patent Text Reader

Abstract

The invention discloses a high-performance crystal glue and a crystal material prepared therefrom. The crystal glue comprises an agent A and an agent B, wherein the weight ratio of the agent A to the agent B is 100:90-120; the agent A comprises: 99.2-99.6wt% of a composite epoxy resin, 0.2-0.5wt% of a leveling agent, and 0.2-0.5wt% of a defoaming agent; the agent B comprises: 96.5-98.3wt% of a mixed acid anhydride, 1.5-3wt% of a curing accelerator, and 0.2-0.5wt% of an ultraviolet absorber; and the raw materials are scientifically matched to effectively solve the problems of poor aging resistance, poor toughness, bubbles, pinholes, and the like in the epoxy crystal glue.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of epoxy crystal glue, and in particular to a high-performance crystal glue drop and its application. Background Art

[0002] Epoxy resin is a general-purpose material, which is widely used in defense aviation, automobile field, shipbuilding, chemical industry and civil field. Epoxy resin has excellent insulation performance, electrical performance, mechanical performance, bonding performance, good processing performance, can be cured at low temperature, medium temperature and high temperature, and has a very wide range of adaptability. Epoxy resin has good light transmittance, good sealing, UV resistance and aging resistance, and is especially suitable for optical materials. It is widely used in LED lights, backlight sources, billboards, transparent accessories, etc. According to incomplete statistics, the share of epoxy resin in the field of optical material packaging is 40-60%, and epoxy resin occupies a pivotal position in this field.

[0003] Crystal diamonds are quite common in daily life, and are generally used for home decoration, pendant embellishment, toys, clothes and shoes decoration. The raw material used in the traditional process of preparing crystal diamonds is glass, and this process has many defects. First, the glass is melted at high temperature and then cast into shape. The preparation process is cumbersome, energy consumption is high, and production efficiency is low; secondly, glass is hard and brittle, easy to damage, and can cause harm to the human body; finally, the cost of using glass to prepare crystal diamonds is high, and the product price is high, which does not have a price advantage.

[0004] In order to make up for the shortcomings of traditional processes, researchers are looking for new materials and new processes to replace them. The light transmittance of epoxy resin is close to that of glass, making it suitable for making high-light-transmittance materials. There are some epoxy resin glues on the market for making crystal diamonds. Generally speaking, these glues have three problems: (1) The aging resistance of the glue is poor, and it will turn yellow and discolor after long-term use, affecting the appearance of the product; (2) The toughness of the product is poor, it is easy to crack and break, and the service life is short; (3) The fluidity of the glue is poor, and there are defects such as micropores and bubbles in the product. Summary of the invention

[0005] In view of the above problems existing in the prior art, the present invention provides a high-performance crystal glue and its application. The present invention scientifically matches the raw materials, which can effectively solve the problems of poor aging resistance, poor toughness, bubbles, pinholes and other defects of epoxy crystal glue.

[0006] The technical solution of the present invention is as follows:

[0007] The first object of the present invention is to provide a high-performance crystal glue, wherein the crystal glue comprises an agent A and an agent B, wherein the weight ratio of the agent A to the agent B is 100:90-120;

[0008] The composition of dose A is:

[0009] Composite epoxy resin 99.2-99.6wt%

[0010] Leveling agent 0.2-0.5wt%

[0011] Defoaming agent 0.2-0.5wt%;

[0012] The composition of agent B is:

[0013] Mixed anhydride 96.5-98.3wt%

[0014] Curing accelerator 1.5-3wt%

[0015] UV absorber 0.2-0.5wt%;

[0016] The composite epoxy resin comprises 40-75wt% of bisphenol A epoxy resin, 10-30wt% of hydrogenated bisphenol A epoxy resin, 10-20wt% of organosilicon-modified epoxy resin and 5-10wt% of low-viscosity epoxy resin;

[0017] The mixed acid anhydride is composed of 70-90 wt % of methyl hexahydrophthalic anhydride and 10-30 wt % of polypropylene glycol modified acid anhydride.

[0018] In one embodiment of the present invention, the epoxy equivalent of bisphenol A epoxy resin is 180-220 g / eq; the epoxy equivalent of hydrogenated bisphenol A epoxy resin is 200-300 g / eq; the epoxy equivalent of silicone modified epoxy resin is 200-1500 g / eq; and the epoxy equivalent of low viscosity epoxy resin is 150-500 g / eq.

[0019] In one embodiment of the present invention, the bisphenol A epoxy resin is one or more of R-139S, 850S, NPEL-128E, YN1826, YD-127, and GY 6010; the hydrogenated bisphenol A epoxy resin is one or more of EP-4080E, NPEK-113, and YX-8000; the silicone-modified epoxy resin is one or more of ALBIFLEX348, ALBIFLEX 296, EPSI-6862, EPSI-6878, and KR-470; the low-viscosity epoxy resin is one or more of 1,6-hexanediol diglycidyl ether, 1,4-butanediol diglycidyl ether, polypropylene glycol diglycidyl ether, and polyethylene glycol diglycidyl ether.

[0020] In one embodiment of the present invention, the leveling agent is one or more of BYK-358N, BYK-310, TEGO Glide 450, BYK-320, and Perenol S43.

[0021] In one embodiment of the present invention, the defoaming agent is one or more of BYK-A530, BYK-066N, TEGO Airex 900, Dow Corning 163, and Dow Corning 100F.

[0022] In one embodiment of the present invention, the polypropylene glycol modified anhydride is HP-08 produced by Shin Nippon Rika Chemical.

[0023] In one embodiment of the present invention, the curing accelerator is one or more of tetrabutyl phosphonium (ammonium) bromide, benzyl triphenyl phosphonium (ammonium) bromide, hexadecyl tributyl phosphonium (ammonium) bromide, triphenyl ethyl phosphonium (ammonium) bromide, triphenyl butyl phosphonium (ammonium) bromide, tetrabutyl-o,o-diethyl dithiophosphate phosphonium, U-CAT SA102 (DUB-modified zincate), PX-4ET (tetrabutyl phosphonium acetate), and 2E4MZ (2-ethyl-4-methylimidazole).

[0024] In one embodiment of the present invention, the ultraviolet absorber is one or more of N-(2-ethoxyphenyl)-N'-(4-ethylphenyl)oxalamide (UV-1033), 2-(2'-hydroxy-5'-tert-octylphenyl)benzotriazole (UV-329), 2-(2'-hydroxy-3',5'-di-tert-butylphenyl)-5-chlorobenzotriazole (UV-327), and 2-cyano-3,3-diphenyl ethyl acrylate (UV-335).

[0025] The second object of the present invention is to provide a method for preparing a crystal material by high-performance crystal glue dripping, comprising the following steps:

[0026] Preparation of Agent A: 99.2-99.6wt% of composite epoxy resin is put into a reaction kettle, the temperature is controlled at 70-80°C, vacuum stirred for 1-2h, then cooled to 50-60°C, 0.2-0.5wt% of leveling agent and 0.2-0.5wt% of defoamer are added, and stirring is continued for 30-60min to obtain Crystal Epoxy Agent A; the viscosity at 25°C is 10000-26000mpa·s;

[0027] Preparation of Agent B: Add 96.5-98.3wt% of mixed acid anhydride into a reaction kettle, control the temperature at 60-70°C, add 1.5-3wt% of curing accelerator and 0.2-0.5wt% of ultraviolet absorber, stir for 1-2h to obtain Agent B of crystal glue;

[0028] Agent A and agent B are mixed in a weight ratio of 100:90-120, vacuum degassed at 50-60° C. for 10-20 minutes, poured into a mold by a dispensing machine, cured at 80-120° C., and demolded after curing to obtain the crystal material.

[0029] The third object of the present invention is to provide an application of high-performance crystal glue for preparing crystal diamonds.

[0030] The existing epoxy resin composition for crystal diamonds has the problem of poor aging resistance, because the composition lacks yellowing-resistant raw materials; the existing epoxy resin composition for crystal diamonds has the problem of poor toughness, because the composition lacks flexible components; the existing epoxy resin composition for crystal diamonds has the problem of product defects, because the viscosity of the composition is high and the defoaming property is poor.

[0031] The present invention can solve the problems of yellowing resistance and poor toughness in the prior art by matching the types and amounts of raw materials.

[0032] The beneficial technical effects of the present invention are:

[0033] The present invention uses hydrogenated bisphenol A epoxy resin and organosilicon-modified epoxy resin as raw materials to improve the aging resistance of the composition; polypropylene glycol-modified acid anhydride and organosilicon-modified epoxy resin are compounded to improve the toughness of the product; in addition, the addition of low-viscosity epoxy resin can adjust the viscosity of the composition, and the use of special defoaming agents can improve the defoaming property of the composition. These adjustment schemes are highly targeted and solve practical problems. Experimental results show that these schemes achieve the expected effects.

[0034] The product of the invention has certain toughness, contains soft monomers such as silicone-modified epoxy resin and polypropylene glycol-modified acid anhydride, and can reduce the hardness of the product, thereby obtaining a product with better performance.

[0035] The crystal material prepared by the present invention has good optical properties, and the product has excellent UV resistance. It will not turn yellow after being used outdoors for 3 years, and the UV resistance effect is significantly improved compared with similar domestic products. The product also has good high temperature resistance, and does not change color after being baked at 150°C for 10 hours, which is a great advantage over similar domestic products. The product was tested at a current of 150mA for 100 hours, and the light decay was higher than 70%, which shows that the product has outstanding aging resistance and is better than similar domestic products. The product has high plane strain fracture toughness, high impact strength, and good toughness. In addition, the embodiment provided by the present invention has a glass transition temperature higher than 120°C, good toughness, and high hardness, and is suitable for use in the field of crystal diamonds. DETAILED DESCRIPTION

[0036] The present invention will be described in detail below in conjunction with the embodiments.

[0037] Example 1

[0038] A method for preparing a crystal material by high-performance crystal glue dripping comprises the following steps:

[0039] Preparation of Agent A: 56.5 parts of R-139S, 20 parts of EP-4080E, 15 parts of ALBIFLEX 348 and 8 parts of 1,4-butanediol diglycidyl ether were put into a reactor, the temperature was controlled at 70°C, vacuum stirred for 1.5 hours, then cooled to 50°C, 0.3 parts of BYK-310 and 0.2 parts of BYK-066N were added, and stirring was continued for 30 minutes to obtain Crystal Epoxy Agent A; the viscosity at 25°C was 15600mpa·s;

[0040] Preparation of Agent B: Put 77.2 parts of methyl hexahydrophthalic anhydride and 20 parts of HP-08 of Shin Nippon Chemical into a reactor, control the temperature at 60°C, add 2.5 parts of tetrabutylammonium bromide and 0.3 parts of UV-329, stir for 1 hour, and obtain Agent B of Crystal Epoxy;

[0041] Agent A and agent B were mixed at a weight ratio of 100:100, vacuum degassed at 50° C. for 15 minutes, poured into a mold by a dispensing machine, cured at 90° C. for 6 hours, and demolded after curing to obtain the crystal material.

[0042] Example 2

[0043] A method for preparing a crystal material by high-performance crystal glue dripping comprises the following steps:

[0044] Preparation of Agent A: 64.6 parts of YD-127, 15 parts of NPEK-113, 10 parts of EPSI-6862, and 10 parts of polyethylene glycol diglycidyl ether were put into a reactor, the temperature was controlled at 80°C, and vacuum stirred for 1.0h, then cooled to 60°C, and then 0.2 parts of TEGOGlide 450 and 0.2 parts of Dow Corning 163 were added, and stirring was continued for 30min to obtain Crystal Epoxy Agent A; the viscosity at 25°C was 13800mpa·s;

[0045] Preparation of Agent B: Put 86.8 parts of methyl hexahydrophthalic anhydride and 10 parts of HP-08 from Shin Nippon Chemical into a reactor, control the temperature at 70°C, add 3 parts of PX-4ET and 0.2 parts of UV-1033, stir for 1.5 hours, and obtain Agent B of Crystal Epoxy Glue;

[0046] Agent A and agent B were mixed in a weight ratio of 100:120, vacuum degassed at 60° C. for 10 minutes, poured into a mold by a dispensing machine, cured at 100° C. for 5 hours, and demolded after curing to obtain the crystal material.

[0047] Example 3

[0048] A method for preparing a crystal material by high-performance crystal glue dripping comprises the following steps:

[0049] Preparation of Agent A: 44.2 parts of NPEL-128E, 30 parts of YX-8000, 20 parts of EPSI-6878, and 5 parts of 1,6-hexanediol diglycidyl ether were put into a reactor, the temperature was controlled at 75°C, and vacuum stirred for 2 hours, then cooled to 60°C, and then 0.5 parts of BYK-358N and 0.3 parts of TEGO Airex 900 were added, and stirring was continued for 30 minutes to obtain Crystal Epoxy Agent A; the viscosity at 25°C was 23500mpa·s;

[0050] Preparation of Agent B: 67.5 parts of methyl hexahydrophthalic anhydride and 30 parts of HP-08 from Shin Nippon Chemical were put into a reactor, the temperature was controlled at 65°C, 2 parts of triphenylbutylphosphonium bromide and 0.5 parts of UV-327 were added, and stirred for 1.5 hours to obtain Agent B of Crystal Epoxy;

[0051] Agent A and agent B were mixed in a weight ratio of 100:110, vacuum degassed at 55° C. for 20 minutes, poured into a mold by a dispensing machine, cured at 120° C. for 6 hours, and demolded after curing to obtain the crystal material.

[0052] Comparative Example 1

[0053] On the basis of Example 1, the hydrogenated bisphenol A epoxy resin EP-4080E was replaced with bisphenol A epoxy resin R-139S. A crystal material was prepared according to the method of Example 1. The corresponding properties of the product were tested. The results are shown in Table 2.

[0054] Comparative Example 2

[0055] On the basis of Example 1, the organosilicon-modified epoxy resin ALBIFLEX 348 was replaced with bisphenol A epoxy resin R-139S. A crystal material was prepared according to the method of Example 1. The corresponding properties of the product were tested. The results are shown in Table 2.

[0056] Comparative Example 3

[0057] On the basis of Example 1, HP-08 of Shin Nippon Rika Chemical was replaced with methyl hexahydrophthalic anhydride, and a crystal material was prepared according to the method of Example 1. The corresponding properties of the product were tested, and the results are shown in Table 2.

[0058] Performance Test:

[0059] (1) Table 1 lists the performance test results of Examples 1-3 of the present invention and commercially available epoxy resin products.

[0060] Table 1

[0061]

[0062] From the data in the table we can see that:

[0063] The light transmittance of the products of the embodiments of the present invention is higher than 96%, and the refractive index is ≥1.51. It is not difficult to see that the products provided by the present invention have excellent light transmittance and transparency, which are similar to the indicators of glass and are more suitable for application in the field of crystal diamonds.

[0064] The flexural strength of the products in the three embodiments is greater than 135 MPa, and the products have high strength and good mechanical properties.

[0065] The plane strain fracture toughness of the products in the three examples is greater than 1.30 MPa·m 1 / 2 , the impact strength is less than 12MPa, indicating that the product has good toughness.

[0066] It is worth mentioning that the product of the present invention has outstanding performance in aging resistance. The product's UV resistance test shows that the product will not change color until 12 hours later. Using a UV lamp with a power of 150w for the experiment, the energy of 1 hour is equivalent to 0.3 years of outdoor natural light irradiation, which means that the embodiment provided by the present invention will not change color when used outdoors for at least 3 years. The product's high temperature resistance is also excellent. When baked at a temperature of 150°C, the product's color change time exceeds 10 hours. In addition, the product's light decay test effect is also ideal. A current of 150mA is passed and the test is performed for 100 hours. The light decay of the product is greater than 72%. The above data show that the product of the present invention has a good effect in aging resistance.

[0067] The glass transition temperature of the products of the present invention is higher than 120° C., the hardness is relatively high, and they are suitable for use in crystal diamonds.

[0068] Example 1 has a high cost-effectiveness and is a general-purpose material. Example 2 has good comprehensive performance and a low price. Example 3 has outstanding aging resistance, high light transmittance and transparency, and the best performance. Customers can make a reasonable choice according to different usage requirements.

[0069] The present invention selects a commercially available product for comparison, and the results show that the product of the present invention has excellent performance and obvious advantages. Taking Example 1 as an example, the transmittance and refractive index of Example 1 are equivalent to those of commercially available products, but Example 1 changes color in 15 hours in the UV test, changes color in 13 hours in the 150°C high temperature test, and the transmittance after 100 hours of light decay test is 76.2%, while the corresponding indicators of commercially available products are 5 hours, 6 hours and 55.6%, respectively. From this comparison, it is not difficult to see that Example 1 has outstanding aging resistance, can be used for a long time under UV and high temperature conditions, and has a long service life, which is the key to the present invention being superior to commercially available products.

[0070] The glass transition temperature of the commercially available product is 82.9°C, and the indicators of the embodiments provided by the present invention are all higher than 120°C. It can be inferred that the commercially available product may use an amine curing agent, while the present invention uses an anhydride curing agent. The anhydride curing agent has outstanding performance in terms of aging resistance, light transmittance, glass transition temperature, etc., which is also an innovation of the present invention.

[0071] In addition, the plane strain fracture toughness of the product of Example 1 is 1.35 MPa·m 1 / 2 The index of commercially available products is 0.83MPa·m 1 / 2 This shows that Example 1 has better toughness, can resist external forces, reduce product cracking and damage, and extend service life. The impact strength of Example 1 is 12.6MPa, and the index of the commercially available product is 10.7MPa, which is evidence of the good toughness of Example 1.

[0072] From the data in the above table, it can be seen that the crystal material of the present invention has obvious advantages in UV resistance, high temperature resistance, light decay test, etc., and can meet the special requirements of crystal diamond materials, and is expected to be widely used in the crystal diamond field.

[0073] (2) Table 2 lists the performance test results of the products of Example 1 and Comparative Examples 1-3 of the present invention.

[0074] Table 2

[0075]

[0076] From the data in Table 2, it can be seen that the transmittance, refractive index, bending strength, glass transition temperature, plane strain fracture toughness, impact strength, and hardness of Example 1 in the present invention are similar to those of Comparative Example 1, and Example 1 has advantages in UV resistance, high temperature resistance, and light decay test. This shows that the role of hydrogenated bisphenol A epoxy resin in the present invention is irreplaceable.

[0077] Compared with the comparative example 2, the transmittance, refractive index, bending strength and hardness of the embodiment 1 of the present invention are not much different. The embodiment 1 shows obvious advantages in UV resistance, high temperature resistance and light decay test. In addition, the plane strain fracture toughness and impact strength of the comparative example 2 are significantly reduced, which indicates that the toughness of the product is greatly reduced. From these data, it is not difficult to see that the organosilicon-modified epoxy resin plays an important role in the present invention, and the use of this material plays a key role in improving the performance of the product.

[0078] Compared with Example 3, the transmittance, refractive index, bending strength, glass transition temperature, and hardness of Example 1 in the present invention are similar. Example 1 has advantages in UV resistance, high temperature resistance, and light decay test. The plane strain fracture toughness of Example 3 is reduced to 1.26 MPa·m 1 / 2 , the impact strength is reduced to 11.5MPa. These two data show that the toughness of Example 3 is significantly reduced, which shows that polypropylene glycol modified anhydride has an outstanding effect in aging resistance, toughness, etc., and is an irreplaceable raw material.

[0079] In summary, the present invention uses raw materials such as bisphenol A epoxy resin, hydrogenated bisphenol A epoxy resin, silicone modified epoxy resin, low viscosity epoxy resin to form component A, and raw materials such as methyl hexahydrophthalic anhydride and polypropylene glycol modified acid anhydride to form component B, and combines appropriate preparation processes to obtain a series of high-performance crystal diamond materials. Compared with commercially available products, the products of the present invention have obvious advantages in aging resistance, optical properties, glass transition temperature, etc., and have broad market application prospects.

Claims

1. A high-performance crystal glue, characterized in that: The crystal glue comprises agent A and agent B, and the weight ratio of agent A to agent B is 100:90-120; The composition of dose A is: Composite epoxy resin 99.2-99.6wt% Leveling agent 0.2-0.5wt% Defoaming agent 0.2-0.5wt%; The composition of agent B is: Mixed anhydride 96.5-98.3wt% Curing accelerator 1.5-3wt% UV absorber 0.2-0.5wt%; The composite epoxy resin comprises 40-75wt% of bisphenol A epoxy resin, 10-30wt% of hydrogenated bisphenol A epoxy resin, 10-20wt% of organosilicon-modified epoxy resin and 5-10wt% of low-viscosity epoxy resin; The mixed acid anhydride is composed of 79.42wt% methyl hexahydrophthalic anhydride and 20.58wt% polypropylene glycol modified acid anhydride; The bisphenol A epoxy resin is one or more of R-139S, 850S, NPEL-128E, YN1826, YD-127, and GY 6010; the hydrogenated bisphenol A epoxy resin is one or more of EP-4080E, NPEK-113, and YX-8000; the silicone-modified epoxy resin is one or more of ALBIFLEX348, ALBIFLEX 296, EPSI-6862, EPSI-6878, and KR-470; the low-viscosity epoxy resin is one or more of 1,6-hexanediol diglycidyl ether, 1,4-butanediol diglycidyl ether, polypropylene glycol diglycidyl ether, and polyethylene glycol diglycidyl ether.

2. The crystal glue according to claim 1, characterized in that: The epoxy equivalent of bisphenol A epoxy resin is 180-220 g / eq; the epoxy equivalent of hydrogenated bisphenol A epoxy resin is 200-300 g / eq; the epoxy equivalent of silicone modified epoxy resin is 200-1500 g / eq; the epoxy equivalent of low viscosity epoxy resin is 150-500 g / eq.

3. The crystal glue according to claim 1, characterized in that: The leveling agent is one or more of BYK-358N, BYK-310, TEGO Glide 450, BYK-320, and Perenol S43.

4. The crystal glue according to claim 1, characterized in that: The defoaming agent is one or more of BYK-A530, BYK-066N, TEGO Airex 900, Dow Corning 163, and Dow Corning 100F.

5. The crystal glue according to claim 1, characterized in that: The polypropylene glycol modified anhydride is HF-08 produced by Shin Nippon Rika Chemical.

6. The crystal glue according to claim 1, characterized in that: The curing accelerator is one or more of tetrabutylphosphonium bromide, tetrabutylammonium bromide, benzyltriphenylphosphonium bromide, benzyltriphenylammonium bromide, hexadecyltributylphosphonium bromide, hexadecyltributylammonium bromide, triphenylethylphosphonium bromide, triphenylethylammonium bromide, triphenylbutylphosphonium bromide, triphenylbutylammonium bromide, tetrabutyl-o,o-diethylphosphonium dithiophosphate, U-CAT SA102, PX-4ET, and 2E4MZ.

7. The crystal glue according to claim 1, characterized in that: The ultraviolet absorber is one or more of N-(2-ethoxyphenyl)-N'-(4-ethylphenyl)oxalamide, 2-(2'hydroxy-5'tert-octylphenyl)benzotriazole, 2-(2'-hydroxy-3',5'-di-tert-butylphenyl)-5-chlorobenzotriazole, and 2-cyano-3,3-diphenyl ethyl acrylate.

8. A method for preparing crystal material by using high-performance crystal glue as claimed in claim 1, characterized in that: The method comprises the following steps: Preparation of Agent A: Add 99.2-99.6wt% of composite epoxy resin into a reaction kettle, control the temperature to 70-80°C, stir under vacuum for 1-2h, then cool to 50-60°C, add 0.2-0.5wt% of leveling agent and 0.2-0.5wt% of defoaming agent, and continue stirring for 30-60min to obtain Crystal Epoxy Agent A; Preparation of Agent B: Add 96.5-98.3wt% of mixed acid anhydride into a reaction kettle, control the temperature at 60-70°C, add 1.5-3wt% of curing accelerator and 0.2-0.5wt% of ultraviolet absorber, stir for 1-2h to obtain Agent B of crystal glue; Agent A and agent B are mixed in a weight ratio of 100:90-120, vacuum degassed at 50-60° C. for 10-20 minutes, poured into a mold by a dispensing machine, cured at 80-120° C., and demolded after curing to obtain the crystal material.

9. An application of the high-performance crystal glue according to claim 1, characterized in that: Used to prepare crystal diamonds.

Citation Information

Patent Citations

  • Method for constructing basins for the nuclear industry, and basins realized according to this method

    EP0010053A1

  • Cold-proof and damp-proof epoxy resin main agent for crystal glue drip and preparation method thereof

    CN103045147A

  • UV-resistant aging-resistant high-performance LED epoxy resin composition and preparation method thereof

    CN113999492A

  • Epoxy resin composition, cured product, transparent sealing material, and photosemiconductor device

    JP2013133339A

Cited By

  • High-quality insect crystal specimen model and manufacturing method thereof

    CN122337087A