A weak curing agent and its preparation method, use method and application

By using weak curing agents of aluminum sulfate and cationic epichlorohydrin-polyethylene polyamine condensation polymer in offshore cementing fluid waste, the problem of offshore cementing fluid waste treatment technology is solved, and rapid solidification and Low-strength consolidation simplifies transportation and subsequent processing, and has little impact on the environment.

CN115502181BActive Publication Date: 2024-10-08CHINA OILFIELD SERVICES LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211290430.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-21
Publication Date
2024-10-08
Estimated Expiration
2042-10-21

AI Technical Summary

Technical Problem

Offshore cementing fluid waste treatment technology is not yet mature, making it difficult to achieve effective reduction and environmental protection. The existing storage technology has gelling phenomena, which increases the difficulty of subsequent processing.

Method used

A weak curing agent is used, including aluminum sulfate and cationic epichlorohydrin-polyethylene polyamine condensation polymer, which is prepared by uniform mixing and used to quickly form low-strength solidified bodies in offshore cementing fluid waste and simplify transportation. and subsequent processing.

Benefits of technology

It achieves rapid and weak solidification of cementing fluid waste, shortens the gelling time, reduces the difficulty and risk of transportation, and has a wide range of pharmaceutical sources with less environmental impact.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003901126900000071
    Figure BDA0003901126900000071
  • Figure BDA0003901126900000081
    Figure BDA0003901126900000081
  • Figure BDA0003901126900000091
    Figure BDA0003901126900000091
Patent Text Reader

Abstract

The present invention belongs to the field of petrochemical industry, and specifically relates to a weak curing agent and a preparation method, a use method and an application thereof, and in particular to a weak curing agent for offshore cementing fluid waste and a preparation method thereof. The weak curing agent of the present invention, by weight, comprises: 10-20 parts of aluminum sulfate, 0.3-1.0 parts of cationic epichlorohydrin-polyethylene polyamine polycondensate. The weak curing agent of the present invention is directed to the cementing fluid waste formed by two cement slurries and two drilling fluids commonly used at sea, and can quickly shorten the gelation time of the cementing fluid waste, so that it forms a solid body with lower strength in a short time, without free water, and can meet the requirements of bagging and transportation, reducing the difficulty and risk of transporting to land for further processing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of petrochemical industry, and specifically relates to a weak curing agent and a preparation method, a use method and an application thereof, and in particular to a weak curing agent for offshore cementing fluid waste and a preparation method thereof. Background Art

[0002] According to the needs of marine protection and national regulations, offshore oilfield operations must implement full waste recycling. According to statistics, during the drilling process of Bohai Oilfield, the average cementing fluid waste generated by a single well is about 600m 3 CNOOC has included the full recovery of cementing fluid waste in its service contract, but there is still no mature process solution for on-site reduction of cementing fluid waste. If the shortcomings of cementing fluid waste treatment technology are not improved, it will seriously affect the development of offshore drilling business. With the increasingly severe environmental protection situation and the implementation of zero emission policy in marine operations, it is urgent to study cementing fluid waste treatment technology suitable for offshore.

[0003] Offshore cementing fluid waste is mainly composed of cement slurry, drilling fluid, isolation fluid and other waste liquids. The treatment of cementing fluid waste has been explored for many years at home and abroad. Isolation fluid is mainly a seawater-based polymer solution. The treatment methods at home and abroad are similar, mainly physical, biological and chemical. Cementing cement slurry waste is mainly composed of oil well cement and different types of additives. It not only occupies a large amount of space on offshore platforms, but also easily causes secondary pollution. It generally needs to be sent back to land for treatment and is difficult to dispose of directly on offshore platforms. As a common working waste liquid in oil fields, drilling fluid has mature and diverse treatment methods, mainly direct discharge method, direct landfill method, pit sealing method, land cultivation method, destabilization and drying treatment method, injection into safe formations, etc.

[0004] Offshore cementing fluid waste generally exists on the platform in the form of slurry, which contains a certain amount of solid components such as oil well cement, barite, limestone, etc., as well as various chemical treatment agents added to cement slurry, drilling fluid, and spacer fluid, and its composition is extremely complex. The existing simple storage technology for cementing fluid waste on the platform may cause gelation if the storage time is prolonged, which increases the difficulty of subsequent treatment. Summary of the invention

[0005] The purpose of the present invention is to propose a weak curing agent and its preparation method, use method and application for cementing fluid waste mainly composed of cementing slurry and drilling fluid at sea. The present invention adopts a weak curing method to make the cementing fluid waste achieve the purpose of rapid weak curing, forming a solid or semi-solid with weak strength, and then transporting it back to land for further processing.

[0006] Specifically, the weak curing agent of the present invention comprises, by weight, 10-20 parts of aluminum sulfate and 0.3-1.0 parts of cationic epichlorohydrin-polyethylene polyamine condensation polymer.

[0007] The above-mentioned weak curing agent, by weight, includes: 13-17 parts of aluminum sulfate, and 0.4-0.6 parts of cationic epichlorohydrin-polyethylene polyamine condensation product.

[0008] The above-mentioned weak curing agent, by weight, includes: 15 parts of aluminum sulfate and 0.5 parts of cationic epichlorohydrin-polyethylene polyamine condensation product.

[0009] The weak curing agent mentioned above, the cationic epichlorohydrin-polyethylene polyamine condensation product has a molecular weight of 2000-3000.

[0010] On the other hand, the present invention provides a method for preparing the weak curing agent, comprising directly mixing aluminum sulfate and cationic epichlorohydrin-polyethylene polyamine condensation product in proportion and uniformly mixing them.

[0011] The preparation method of the above-mentioned weak curing agent, the cationic epichlorohydrin-polyethylene polyamine condensation polymer is prepared by the following method:

[0012] Add polyethylene polyamine and water into the reaction kettle, stir evenly, slowly add epichlorohydrin at 50-60°C, after the addition of epichlorohydrin, raise the system temperature to 70-80°C, react for 3-4h, cool down, and obtain cationic epichlorohydrin-polyethylene polyamine condensation product.

[0013] In the preparation method of the above-mentioned weak curing agent, the mass ratio of the polyethylene polyamine to the epichlorohydrin is (1-2): (3-5).

[0014] In yet another aspect, the present invention further provides the use of the above-mentioned weak curing agent in treating offshore cementing fluid waste.

[0015] In another aspect, the present invention further provides a method for using the weak curing agent, comprising: adding the weak curing agent to offshore cementing fluid waste for weak curing; when the free water in the cementing fluid waste is greater than 3 mL during the weak curing process, adding an organic silane cross-linked sulfonic acid water absorbent;

[0016] The mass fraction of the weak curing agent in the cementing fluid waste is 0.5%-3.0%, and the mass fraction of the organic silane cross-linked sulfonic acid water absorbent in the cementing fluid waste is 0-2%.

[0017] The technical solution of the present invention has the following beneficial effects:

[0018] (1) The weak curing agent of the present invention can quickly shorten the gelling time of cementing fluid waste formed by two kinds of cement slurries and two kinds of drilling fluids commonly used at sea, so that the waste cementing fluid can form a solid body with low strength in a short time without free water, which can meet the requirements of bagging and transportation, thereby reducing the difficulty and risk of transporting it to land for further processing;

[0019] (2) The weak curing agent of the present invention has a wide range of sources, is easily available, and has little impact on the environment. DETAILED DESCRIPTION

[0020] In order to fully understand the purpose, features and effects of the present invention, the present invention is described in detail through the following specific embodiments. Except for the following contents, the process method of the present invention adopts conventional methods or devices in the art. Unless otherwise specified, the following terms have the meanings commonly understood by those skilled in the art.

[0021] The terms "the", "said", "one" and "an" as used herein do not indicate a limitation of quantity, but rather indicate the presence of at least one of the referenced object. The terms "preferred", "more preferred" and the like refer to embodiments of the present invention that may provide certain benefits in certain circumstances. However, other embodiments may also be preferred under the same or other circumstances. In addition, the description of one or more embodiments does not imply that other embodiments are not applicable, nor is it intended to exclude other embodiments from the scope of the present invention.

[0022] When a numerical range is disclosed herein, the above range is considered to be continuous and includes the minimum and maximum values ​​of the range, as well as every value between such minimum and maximum values. Further, when a range refers to an integer, every integer between the minimum and maximum values ​​of the range is included. In addition, when multiple ranges are provided to describe a feature or characteristic, the ranges can be combined. In other words, unless otherwise indicated, all ranges disclosed herein should be understood to include any and all subranges included therein.

[0023] Offshore cementing fluid waste generally exists on the platform in the form of slurry. The slurry contains a certain amount of solid components such as oil well cement, barite, limestone, etc., and also contains various chemical treatment agents added to cement slurry, drilling fluid, and spacer fluid. The composition is extremely complex and it is difficult to effectively treat it on the offshore platform. Therefore, a weak curing agent for offshore cementing fluid waste and a preparation method thereof are proposed. The weak curing agent is added to the cementing fluid waste stored on the offshore platform, so that the cementing fluid waste can be quickly and weakly solidified in a short time to form a low-strength consolidated body without free water, which can meet the requirements of bagging and transportation, and then transported to land for further treatment.

[0024] Specifically, the weak curing agent provided by the present invention comprises, by weight, 10-20 parts of aluminum sulfate and 0.3-1.0 parts of cationic epichlorohydrin-polyethylene polyamine condensation polymer.

[0025] Among them, after the aluminum sulfate is dissolved in the cementing fluid waste, a large amount of aluminum ions and sulfate ions are generated, which promotes the formation of ettringite. The ettringite is in a rod-like or columnar morphology in the system. The rapid generation of ettringite combines into a network, thereby achieving a rapid setting effect.

[0026] When the weight proportion of aluminum sulfate in the weak curing agent is less than 10 parts, the cementing fluid waste cannot be solidified; when the weight proportion of aluminum sulfate is greater than 20 parts, the strength of the cementing fluid waste after solidification is high, and the difficulty of subsequent treatment of the solidified material increases.

[0027] Preferably, when the weight portion of aluminum sulfate in the weak curing agent is 13-17 parts, the quick-setting effect is better, and when the weight portion of aluminum sulfate in the weak curing agent is 15 parts, the quick-setting effect is the best.

[0028] The cationic epichlorohydrin-polyethylene polyamine polycondensate has good adsorption performance on solid phase particles of cementing fluid waste, forms a network structure with multiple solid phase particles, and causes the cementing fluid waste to quickly lose fluidity.

[0029] When the weight portion of the cationic epichlorohydrin-polyethylene polyamine condensation product in the weak curing agent is less than 0.3 parts, the cementing fluid waste loses fluidity for too long and cannot achieve the purpose of quickly losing fluidity; when the weight portion of the cationic epichlorohydrin-polyethylene polyamine condensation product is greater than 1.0 parts, the cementing fluid waste loses fluidity for too short a time and may lose fluidity in the mixing tank.

[0030] Preferably, when the weight proportion of the cationic epichlorohydrin-polyethylene polyamine condensation product in the weak curing agent is 0.4-0.6 parts, the adsorption performance of the weak curing agent on solid particles is better, and when its weight proportion is 0.5 parts, the adsorption performance on solid particles is the best.

[0031] In some preferred embodiments, the cationic epichlorohydrin-polyethylene polyamine condensation polymer is prepared by the following method:

[0032] Add polyethylene polyamine and water into the reaction kettle, stir evenly, slowly add epichlorohydrin at 50-60°C, after the addition of epichlorohydrin, raise the system temperature to 70-80°C, react for 3-4h, cool down, and obtain cationic epichlorohydrin-polyethylene polyamine condensation product.

[0033] More preferably, the mass ratio of the polyethylene polyamine to the epichlorohydrin is (1-2):(3-5).

[0034] More preferably, the molecular weight of the cationic epichlorohydrin-polyethylene polyamine condensation product is 2000-3000.

[0035] In a second aspect, the present invention also provides a method for preparing the weak curing agent, comprising directly mixing aluminum sulfate and cationic epichlorohydrin-polyethylene polyamine condensation product in proportion and uniformly mixing them.

[0036] In a third aspect, the present invention provides the use of the weak curing agent in treating offshore cementing fluid waste.

[0037] The weak curing agent of the present invention is used to treat the mixed slurry of offshore cementing fluid waste formed by two commonly used cement slurries, two drilling fluids and an isolation fluid. The weak curing time is less than 4 hours, and the free water of the cementing fluid waste after weak curing is less than 3 mL, which is convenient for transportation back to land for further treatment.

[0038] In a fourth aspect, the present invention also provides a method for using the weak curing agent, wherein the weak curing agent is added to offshore cementing fluid waste for weak curing; when the free water content of the cementing fluid waste is greater than 3 mL during the weak curing process, an organic silane cross-linked sulfonic acid water absorbent is added.

[0039] Preferably, the mass fraction of the weak curing agent in the cementing fluid waste is 0.5%-3.0%, and the mass fraction of the organosilane cross-linked sulfonic acid water absorbent in the cementing fluid waste is 0-2%.

[0040] When the organosilane cross-linked sulfonic acid water absorbent is added to the cementing fluid waste, its polymer chains are entangled with each other to form an interpenetrating network type of high-performance water absorbent, which improves the absorption capacity of highly mineralized brine. The organosilane cross-linked sulfonic acid water absorbent is an interpenetrating network type cross-linked polymer, which overcomes the defect that a single network can only absorb fresh water, seals the water molecules, and restricts the free movement of water molecules in the cement slurry. It can not only absorb highly mineralized brine, but also has a high absorption capacity for seawater.

[0041] Preferably, the organosilane cross-linked sulfonic acid water absorbent includes: polyacrylamide water absorbent, polyacrylic acid water absorbent, etc., which are cross-linked by organosilane and contain sulfonic acid groups.

[0042] According to practice, the weak curing agent of the present invention can quickly gel the cementing fluid waste in a short time to form a weaker strength, and then transport it back to land for further processing.

[0043] Example

[0044] The present invention is further described below by way of examples, but the present invention is not limited to the scope of the examples. The experimental methods without specific conditions in the following examples are based on conventional methods and conditions.

[0045] Example 1 Evaluation of weak curing properties of Biodrill drilling fluid, cement slurry and spacer fluid in a volume ratio of 1:1:1

[0046] Preparation of weak curing agent: Take 15 parts of aluminum sulfate and 0.6 parts of cationic epichlorohydrin-polyethylene polyamine condensation product by weight, mix them evenly and set aside.

[0047] Preparation of Biodrill drilling fluid: water + 0.3% NaOH + 0.2% Na2CO3 + 0.4% PF-BIOVIS + 1.2% PF-FLOTROL + 0.4% PF-BIOCAP + 3% PF-BIOTROL + 2% PF-LUBE + 0.2% PF-PAC-LV + 12% NaCl + 15% barite. According to the mass ratio, various drilling fluid treatment agents are added in sequence under stirring, and then stirred at high speed for 2 hours, cured at 45℃ for 24 hours, stirred at high speed for 2 hours in the middle, and set aside. The main components of Biodrill drilling fluid are NaCl, barite, polyanionic cellulose and various soluble biopolymers. There are many hydrophilic solid phase components, high viscosity, strong water absorption, and can reduce the free water in the system.

[0048] Preparation of early strength cement slurry for surface cementing: 100g oil well cement + 86g water + 3.6g early strength agent PC-A90S + 2.4g early strength agent PC-A90L + 1g defoamer PC-X60L, stir evenly at high speed and set aside. The main additives of early strength cement slurry for surface cementing are early strength agent PC-A90S (main components are aluminum sulfate, USZ, lithium chloride, polymerized alumina, triethanolamine, etc.), early strength agent PC-A90L (main components are triethanolamine, alumina) and defoamer organic phosphate, etc., which can promote the hydration reaction and strength formation of oil well cement and increase the curing speed of oil well cement.

[0049] Preparation of liner cementing slurry: 100g oil well cement + 41.6g water + 6.9g fluid loss agent PC-G81L + 2.5g gas channeling control agent PC-GS12S + 0.8g retarder PC-H21L + 0.9g defoamer PC-X60L, stir evenly at high speed and set aside. The main additives of liner cementing slurry are organic high molecular polymer (fluid loss agent PC-G81L), alkali, silica (gas channeling control agent PC-GS12S), sulfonated aldehyde ketone condensate (retarder PC-H21L), polyol phosphate ester and organic phosphate ester (defoamer PC-X60L), etc., which have good dispersibility and retarding properties while reducing water loss.

[0050] Preparation of isolation liquid: 228.8g water + 1.5g polysaccharide isolation agent PC-S11S + 1g organophosphate defoamer PC-X60L + 100g barite. Add various treatment agents in sequence while stirring, then stir at high speed for 2h, cure at 45℃ for 12h, and set aside.

[0051] Preparation of cementing fluid waste slurry: The volume ratio of Biodrill drilling fluid, cement slurry and spacer fluid was fixed at 1:1:1, and the two cement slurry systems were changed and stirred evenly. Slurry A: The volume ratio of Biodrill drilling fluid, surface cementing early strength cement slurry and spacer fluid was 1:1:1, and slurry B: The volume ratio of Biodrill drilling fluid, liner cementing cement slurry and spacer fluid was 1:1:1. Different mass fractions of the above-mentioned uniformly mixed weak curing agent and organosilane cross-linked sulfonic acid water absorbent were added to evaluate the fluidity and free water under different curing times, as shown in Table 1.

[0052] Table 1 Biodrill drilling fluid, cement slurry, and spacer fluid in a 1:1:1 ratio. Weak curing properties of slurry A

[0053]

[0054] For slurry A, since the water-cement ratio of the surface cementing early-strength cement slurry is 0.86, no water absorbent is added, and free water is generated during the weak curing process. After adding 1% of the water absorbent, the free water content is controlled below 3%. For slurry B, since the water-cement ratio of the tail pipe cementing cement slurry is 0.42, no free water is precipitated after adding 0.5% of the weak curing agent and 0.5% of the water absorbent. The two slurry systems lose fluidity within 4 hours when the mass fraction of the weak curing agent is 0.5%-2.0%, and the weak curing time is short.

[0055] Example 2 PEM drilling fluid, cement slurry, and spacer fluid volume ratio of 1:1:1 slurry weak curing performance evaluation Preparation of PEM drilling fluid: water + 0.3% NaOH + 0.3% Na2CO3 + 3% bentonite, high-speed stirring for 2h, curing and aging at 45°C for 24h, adding various treatment agents in sequence under stirring, 0.6% PF-PAC-LV + 0.6% PF-VIF + 3% PF-JLX-C + 1.5% PF-LPF + 1.5% PF-LSF + 0.6% PF-PLH + 6% KCl + 12% NaCl, then high-speed stirring for 2h, curing for 24h, and high-speed stirring for 2h in the middle for standby. The main components of PEM drilling fluid are NaCl, KCl, bentonite and soluble polymers, there are more hydrophilic solid phase components, high inorganic salt content, bentonite is in a state of moderate flocculation and moderate dispersion, high viscosity, and a certain amount of free water will be generated.

[0056] The preparation of surface cementing early strength cement slurry, tail pipe cementing cement slurry and isolation fluid is the same as above.

[0057] Preparation of cementing fluid waste slurry: The volume ratio of PEM drilling fluid, spacer fluid and cement slurry was fixed at 1:1:1, and the two cement slurry systems were changed and stirred evenly. Slurry C: The volume ratio of PEM drilling fluid, surface cementing early strength cement slurry and spacer fluid was 1:1:1, and slurry D: The ratio of PEM drilling fluid, liner cementing cement slurry and spacer fluid was 1:1:1. Different mass fractions of the above-mentioned uniformly mixed weak curing agent and organosilane cross-linked sulfonic acid water absorbent were added to evaluate the fluidity and free water under different curing times, as shown in Table 2.

[0058] Table 2 Weak curing properties of slurry with a ratio of 1:1:1 for PEM drilling fluid, cement slurry and spacer fluid

[0059]

[0060]

[0061] For slurry C, since the water-cement ratio of the surface cementing early-strength cement slurry is 0.86, after adding 2.5% weak curing agent and 1.0% water absorbent, it loses fluidity within 2 hours, the weak curing time is short, and the free water content is controlled below 3%. For slurry D, since the water-cement ratio of the tail pipe cementing cement slurry is 0.42, after adding 1.0% weak curing agent and 0.5% water absorbent, it loses fluidity within 2 hours, the weak curing time is short, and the free water content is controlled below 3%.

[0062] The present invention has been disclosed above with preferred embodiments, but those skilled in the art should understand that these embodiments are only used to describe the present invention and should not be understood as limiting the scope of the present invention. It should be noted that all changes and substitutions equivalent to these embodiments should be deemed to be included in the scope of the claims of the present invention. Therefore, the scope of protection of the present invention should be based on the scope defined in the claims.

Claims

1. A weak curing agent for treating offshore cementing fluid waste, It is characterized in that The composition is as follows by weight: 10-20 parts of aluminum sulfate and 0.3-1.0 parts of cationic epichlorohydrin-polyethylene polyamine condensation product with a molecular weight of 2000-3000.

2. The weak curing agent according to claim 1, It is characterized in that The composition is as follows by weight: 13-17 parts of aluminum sulfate and 0.4-0.6 parts of cationic epichlorohydrin-polyethylene polyamine condensation product.

3. The weak curing agent according to claim 2, It is characterized in that The composition is as follows by weight: 15 parts of aluminum sulfate and 0.5 parts of cationic epichlorohydrin-polyethylene polyamine condensation product.

4. A method for preparing a weak curing agent according to any one of claims 1 to 3, It is characterized in that The method comprises directly mixing aluminum sulfate and cationic epichlorohydrin-polyethylene polyamine condensation polymer in proportion and uniformly.

5. The method for preparing the weak curing agent according to claim 4, It is characterized in that The cationic epichlorohydrin-polyethylene polyamine condensation product is prepared by the following method: Add polyethylene polyamine and water into the reaction kettle, stir evenly, slowly add epichlorohydrin at 50-60°C, after the addition of epichlorohydrin, raise the system temperature to 70-80°C, react for 3-4h, cool down, and obtain cationic epichlorohydrin-polyethylene polyamine condensation product.

6. The method for preparing the weak curing agent according to claim 5, It is characterized in that The mass ratio of the polyethylene polyamine to the epichlorohydrin is (1-2):(3-5).

7. Use of the weak curing agent according to any one of claims 1 to 3 in treating offshore cementing fluid waste.

8. A method for using the weak curing agent according to any one of claims 1 to 3, It is characterized in that A weak curing agent is added to the offshore cementing fluid waste for weak curing; when the free water in the offshore cementing fluid waste is greater than 3 mL during the weak curing process, an organic silane cross-linked sulfonic acid water absorbent is added; The mass fraction of the weak curing agent in the cementing fluid waste is 0.5%-3.0%, and the mass fraction of the organosilane cross-linked sulfonic acid water absorbent in the cementing fluid waste is 0-2%.