Resin composition, multilayer structure, light conversion film and agricultural film
By using a combination of high-content EVOH and high-molecular-weight organic light conversion materials in the wavelength conversion film, the problem of degradation of existing film performance is solved, and the long-term maintenance of the light conversion function and environmentally friendly and efficient light conversion effect are achieved.
Patent Information
- Application Number
- CN202111159308.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-09-30
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2041-09-30
AI Technical Summary
The performance of existing wavelength conversion films is degraded after long-term use, especially the insufficient weather resistance of improved light conversion materials, which leads to a decline in the light conversion function, which may cause damage due to reaction with the molecules of the external environment under light excitation.
The combination of gas barrier resin ethylene-vinyl alcohol copolymer (EVOH) and an organic light conversion material with a molecular weight of 200 or more is adopted, and the EVOH content is 50 wt% or more and the organic light conversion material content is 0.01 wt% or more and less than 10 wt%. The weather resistance and anti-seepage properties of the material are enhanced through specific absorption and emission peak structures and metal complex designs.
It effectively maintains the long-term efficiency of the light conversion function, prevents the decomposition, damage and seepage of the light conversion materials, maintains a good appearance and environmental safety, and extends the service life of the film.
Smart Images

Figure FDA0005031222760000021 
Figure FDA0005031222760000031 
Figure FDA0005031222760000032
Abstract
Description
Technical Field
[0001] The present invention relates to a resin composition, a multilayer structure, a light conversion film and an agricultural film. Background Art
[0002] Facility cultivation, which is the cultivation of plants in greenhouses and other facilities, has achieved a leap in plant yield and quality compared to ground cultivation, and has therefore been widely used. In addition, in order to further improve the yield and quality of plants, adjust the harvest period, shorten the cultivation period, etc., attempts have recently been made to convert ultraviolet rays that are harmful to plants into blue or red light that is useful for photosynthesis, or to convert green to yellow light with low photosynthesis efficiency into orange to red light with high photosynthesis efficiency, using agricultural films used in greenhouses and other facilities.
[0003] Films that have the function of converting light of a specific wavelength into light of other wavelengths (hereinafter referred to as "light conversion function") may experience a decline in light conversion function or even fail to maintain their function when used for a long time. In order to solve this problem, Patent Document 1 proposes a wavelength conversion film comprising an inorganic ultraviolet blocking material and a wavelength conversion material.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent document 1: International Publication No. 2008 / 126766. Summary of the invention
[0007] Problem that the invention aims to solve
[0008] However, in order to suppress the degradation of the performance of the above-mentioned existing wavelength conversion (hereinafter referred to as "photoconversion") films due to long-term use, especially to improve the weather resistance of the photoconversion materials, although inorganic ultraviolet blocking materials are used, the weather resistance is still insufficient. It can be seen that the degradation of the photoconversion function over time is a difficult problem to overcome. The inventors of the present invention have found that the degradation of the photoconversion function may be caused by the photoconversion material being destroyed by reacting with other molecules (such as water vapor, oxygen, carbon dioxide, acid rain, pesticides, etc.) infiltrating the external environment under light excitation. Therefore, the present invention proposes a technical means to improve the weather resistance of the light conversion material by blending the gas barrier resin ethylene-vinyl alcohol copolymer (hereinafter referred to as "EVOH"). In addition, it is also found that if the photoconversion material is easy to seep out, it may also cause a reduction in the photoconversion function.
[0009] The present invention has been made based on the above circumstances, and an object of the present invention is to provide a resin composition, a multilayer structure, a light conversion film, and an agricultural film that can maintain a light conversion function for a long period of time.
[0010] Means used to solve problems
[0011] According to the present invention, the above object is achieved by providing the following solution.
[0012] [1] a resin composition comprising an ethylene-vinyl alcohol copolymer (C) (hereinafter referred to as “EVOH (C)”) and an organic light conversion material (D) having a molecular weight of 200 or more (hereinafter referred to as “organic light conversion material (D)”), wherein the content of EVOH (C) is 50 wt % or more and 99.99 wt % or less, and the content of the organic light conversion material (D) is 0.01 wt % or more and less than 10 wt %;
[0013] [2] The resin composition according to [1], wherein the absorption spectrum and luminescence spectrum of the organic light conversion material (D) measured according to the method described in GB / T9721-2006 and JY / T 0571-2020 have at least one absorption peak in the range of 300nm to 600nm and at least one emission peak in the range of 400nm to 800nm;
[0014] [3] The resin composition according to [1] or [2], wherein the EVOH (C) has an ethylene unit content of 20 mol% to 60 mol% and a saponification degree of 90 mol% or more;
[0015] [4] The resin composition according to any one of [1] to [3], comprising 5 ppm or more and 200 ppm or less of the phosphate compound (a1) in terms of phosphate radical, and 10 ppm or more and 400 ppm or less of the alkali metal salt (a2) in terms of metal atom, wherein the phosphate radical-converted mass (W a1 ) and the mass (W) of the alkali metal salt (a2) in terms of metal atoms a2 ) mass ratio (W a1 / W a2 ) is greater than or equal to 0.01 and less than or equal to 2;
[0016] [5] The resin composition according to any one of [1] to [4], wherein the resin composition comprises 1 to 49.99 wt % of a thermoplastic resin (E) different from EVOH (C);
[0017] [6] The resin composition according to any one of [1] to [5], wherein the organic light conversion material (D) comprises at least one of an organic metal complex and an organic fluorescent dye;
[0018] [7] The resin composition according to [6], wherein the organometallic complex contains a rare earth element;
[0019] [8] The resin composition according to [7], wherein the rare earth element is europium or terbium;
[0020] [9] The resin composition according to [7] or [8], wherein the organometallic complex is A m Ln(La) x (Lb) y B n or A m Ln(Lc) z B n The metal complex shown, A is a positive monovalent counter cation, B is a negative monovalent counter anion, La is an anionic bidentate ligand, Lb is a neutral ligand, Lc is a tridentate ligand, and Ln is a positive trivalent rare earth metal ion; wherein x = any one of 0 to 4, y = any one of 0 to 4, and x+y = 4 or 5; z = any one of 1 to 3; m = any one of 0 to 3, and n = any one of 0 to 3;
[0021]
[10] The resin composition according to [9], wherein the organometallic complex is Ln(La) 3 (Lb) y The organometallic complex shown, y=1 or 2, La is at least one selected from the following general formulas I to III, Lb is at least one selected from the following general formulas VII to XI,
[0022]
[0023]
[0024]
[0025] In Formula I, R 1 , R 2 , R 3 , R 4 and R 5 are respectively a hydrogen atom, a halogen atom, a cyano group, an alkyl group and a haloalkyl group; in Formula II, R 1 and R 2 are aromatic groups, alkyl groups and halogenated alkyl groups respectively; in Formula III, R 1 , R 2 , R 3 and R 4 are respectively a hydrogen atom, a halogen atom, a cyano group, an alkyl group and a haloalkyl group; in Formula VII, Formula VIII, Formula IX and Formula XI, R 1 , R 2 , R 3 , R 4 and R 5 are alkyl or aromatic groups, respectively;
[0026]
[11] The resin composition according to [9], wherein the organometallic complex is Aln(La) 4 The organometallic complex shown in FIG. 1 is an alkali metal ion or an organic amine ion, and La is at least one selected from the following general formulas I to III.
[0027]
[0028] In Formula I, R 1 , R 2 , R 3 , R 4 and R 5 are respectively a hydrogen atom, a halogen atom, a cyano group, an alkyl group and a haloalkyl group; In formula II, R 1 and R 2 are aromatic groups, alkyl groups and halogenated alkyl groups respectively; in formula III and VI, R 1 , R 2 , R 3 and R 4 They are hydrogen atom, halogen atom, cyano group, alkyl group and haloalkyl group;
[0029]
[12] The resin composition according to [9], wherein the organometallic complex is Ln(Lc) 3 The organometallic complex shown, Lc is at least one selected from the following general formula XII or XIII;
[0030]
[0031]
[0032]
[13] The resin composition according to [6], wherein the organic fluorescent dye is a compound represented by the following general formula XIV to XXI:
[0033]
[0034]
[0035]
[0036]
[0037]
[0038] In Formula XVIII, R 1 and R 2 are respectively a hydrogen atom, a hydroxyl group, an amino group, an alkoxy group and an alkyl-substituted amino group,
[0039]
[0040] In Formula XIX, R 1 , R 2 , R 3 , R 4 , R 5 and R 6 are hydrogen atoms and alkyl groups,
[0041]
[0042] In formula XX, R 1 , R 2 and X are respectively a hydrogen atom, a halogen, a nitro group and an alkoxy group,
[0043]
[0044] In formula XX, R 1 , R 2 , R 3 , R 4 , R 5 , R 6 , R 7 , R 8 , R 9 , R 10 , R 11 and R 12 are hydrogen atoms, alkyl groups, and aromatic groups, respectively;
[0045]
[14] The resin composition according to any one of [1] to [5], wherein the organic light conversion material (D) is an organic metal complex or compound represented by the following general formula XXII to XXXI;
[0046]
[0047]
[0048]
[0049]
[0050]
[0051]
[0052]
[0053]
[0054]
[0055]
[0056]
[15] A multilayer structure comprising at least one layer (X) comprising the resin composition according to any one of [1] to
[14] (hereinafter referred to as “layer (X)”), and a layer (Y) comprising a thermoplastic resin (B) (hereinafter referred to as “layer (Y)”);
[0057]
[16] The multilayer structure according to
[15] , which has a structure in which a layer (Y) is laminated on at least one surface of the layer (X) via an adhesive layer (Z) containing an adhesive resin (F);
[0058]
[17] The multilayer structure according to
[16] , wherein the adhesive resin (F) is an acid-modified polyolefin resin, and the acid value of the acid-modified polyolefin resin is 1.5 mgKOH / g or more;
[0059]
[18] The multilayer structure according to
[15] , which has a structure in which layer (X) and layer (Y) are directly stacked;
[0060]
[19] The multilayer structure according to any one of
[15] to
[18] , wherein layer (Y) comprises an unmodified polyolefin resin;
[0061]
[20] The multilayer structure according to any one of
[15] to
[19] , wherein layer (Y) comprises an acid-modified polyolefin resin;
[0062]
[21] The multilayer structure according to any one of
[15] to
[20] , wherein the peel strength between layer (X) and a layer adjacent to layer (X) is 400 g / 15 mm or more;
[0063]
[22] The multilayer structure according to any one of
[15] to
[21] , wherein the oxygen permeability measured at a temperature of 20° C. and a humidity of 65% RH according to the method described in ISO 14663-2 is 100 cc / (m 2 ·day·atm) or less;
[0064]
[23] The multilayer structure according to any one of
[15] to
[22] , wherein the water vapor transmission rate at a temperature of 40°C and a humidity of 90% RH measured by the method described in ISO 15106-1:2003 is less than 20 g / (m 2 day);
[0065]
[24] A light conversion film comprising the multilayer structure described in any one of
[15] to
[23] ;
[0066]
[25] An agricultural film comprising the multilayer structure described in any one of
[15] to
[23] .
[0067] Effects of the Invention
[0068] According to the present invention, a resin composition, a multilayer structure, a light conversion film, and an agricultural film capable of maintaining light conversion efficiency for a long period of time can be provided. DETAILED DESCRIPTION
[0069] The resin composition of the present invention comprises EVOH (C) and an organic photoconversion material (D), wherein the content of EVOH (C) is more than 50wt% and less than 99.99wt%, and the content of the organic photoconversion material (D) is more than 0.01wt% and less than 10wt%. By using a resin composition comprising EVOH (C) and an organic photoconversion material (D), the decomposition and destruction of the organic photoconversion material (D) can be suppressed, so that the photoconversion efficiency can be maintained for a long time. In addition, the organic photoconversion material (D) is an organic photoconversion material with a molecular weight of more than 200, which can suppress the exudation of the organic photoconversion material (D), so that the photoconversion function can be maintained for a long time, and a good appearance can also be maintained, and soil pollution caused by the photoconversion material (D) can be suppressed. In addition, by using the above-mentioned EVOH (C) and the organic photoconversion material (D), a good photoconversion efficiency can be maintained for a long time. By using these structures, the resin composition provides a light conversion efficiency that can be maintained for a long time.
[0070] (EVOH(C))
[0071] The oxygen permeability of EVOH (C) measured at a temperature of 20° C. and a humidity of 65% RH according to the method described in ISO 14663-2 is preferably 100 cc·20 μm / (m 2 ·day·atm) or less, more preferably 80cc·20μm / (m 2 ·day·atm) or less, more preferably 60cc·20μm / (m 2 ·day·atm) or less, more preferably 5.0cc·20μm / (m 2 ·day·atm), particularly preferably 1.0cc·20μm / (m 2 ·day·atm). The lower limit of the oxygen permeability may be no more than 0.005cc·20μm / (m 2 ·day·atm).
[0072] EVOH (C) is obtained by saponifying a copolymer containing ethylene and a vinyl ester using an alkali catalyst, etc. As the vinyl ester, vinyl acetate can be used as a representative substance, and other fatty acid vinyl esters (vinyl formate, vinyl propionate, vinyl valerate, vinyl caprate, vinyl laurate, vinyl stearate, vinyl benzoate, vinyl pivalate, vinyl versatate, etc.) can also be used.
[0073] The saponification degree of EVOH (C) is preferably 90 mol% or more, more preferably 95 mol% or more, further preferably 98 mol% or more, and particularly preferably 99 mol% or more. By setting the saponification degree to be above the above lower limit, the gas barrier properties of the resin composition of the present invention can be improved. In addition, the upper limit of the saponification degree can be 99.99 mol%. The saponification degree can be 1 It can be determined by a known method such as H-NMR measurement.
[0074] The ethylene unit content of EVOH (C) is preferably 20 mol% or more, more preferably 22 mol% or more, and further preferably 24 mol% or more. In addition, the ethylene unit content is preferably 60 mol% or less, more preferably 55 mol% or less, and further preferably 50 mol% or less. By setting the ethylene unit content to the above range, the melt moldability and gas barrier properties can be improved, and the light conversion efficiency of the resin composition of the present invention can be maintained for a long time. The ethylene unit content can be adjusted by 1 It can be determined by a known method such as H-NMR measurement.
[0075] In addition, EVOH (C) may have units derived from other monomers other than ethylene, vinyl esters and saponified products thereof without affecting the purpose of the present invention. In the case where EVOH (C) has the aforementioned other monomer units, the content of the aforementioned other monomer units relative to all structural units of EVOH (C) is preferably 30 mol% or less, more preferably 20 mol% or less, further preferably 10 mol% or less, and particularly preferably 5 mol% or less. In addition, in the case where EVOH (C) has the aforementioned units derived from other monomers, the lower limit may be 0.05 mol%, preferably 0.10 mol%. The above-mentioned other monomers include olefins such as propylene, butene, pentene, and hexene; 3-acyloxy-1-propylene, 3-acyloxy-1-butene, 4-acyloxy-1-butene, 3,4-diacyloxy-1-butene, 3-acyloxy-4-methyl-1-butene, 4-acyloxy-2-methyl-1-butene, 4-acyloxy-3-methyl-1-butene, 3,4-diacyloxy-2-methyl-1-butene, 4-acyloxy-1-pentene, 5-acyloxy-1-pentene, 4,5-diacyloxy-1-pentene, 4-acyloxy-1-hexene, 5-acyloxy-1-hexene, 6-acyloxy-1-hexene, 5,6-diacyloxy-1-hexene; Olefins having an ester group such as olefins, 1,3-diacetoxy-2-methylpropane, or saponified products thereof; unsaturated acids such as acrylic acid, methacrylic acid, crotonic acid, itaconic acid, or their anhydrides, salts, or mono- or di-alkyl esters; nitriles such as acrylonitrile and methacrylonitrile; amides such as acrylamide and methacrylamide; olefin sulfonic acids such as vinyl sulfonic acid, allyl sulfonic acid, and methyl allyl sulfonic acid, or their salts; vinyl silane compounds such as vinyl trimethoxysilane, vinyl triethoxysilane, vinyl tri(β-methoxy-ethoxy) silane, and γ-methacryloxypropyl methoxysilane; alkyl vinyl ethers, vinyl ketone, N-vinyl pyrrolidone, vinyl chloride, and vinylidene chloride.
[0076] EVOH (C) can be post-modified by methods such as urethanization, acetalization, cyanoethylation, and oxyalkyleneization.
[0077] The lower limit of the melt flow rate (MFR) of EVOH (C) measured at 210°C and 2160g load according to ISO1133 is preferably 0.5g / 10min, more preferably 1.0g / 10min, and further preferably 2.0g / 10min. On the other hand, the upper limit of MFR is preferably 100g / 10min, more preferably 50g / 10min, and further preferably 25g / 10min. When MFR is within the above range, melt moldability and processability can be improved.
[0078] EVOH (C) may be used alone or in combination of two or more.
[0079] (Organic photoconversion material (D))
[0080] The organic light conversion material (D) is an organic light conversion material with a molecular weight of 200 or more. The organic light conversion material (D) is a material that has different absorption wavelengths and luminescence wavelengths in the ultraviolet region or the visible light region, absorbs ultraviolet rays or visible rays, and emits light of different wavelengths. Therefore, materials that only absorb light of a specific wavelength, such as coloring pigments (white titanium oxide, phthalocyanine blue, etc.) are not included. In addition, the organic light conversion material (D) has a molecular weight of 200 or more, and the light conversion function can be maintained for a long time by suppressing the exudation of the organic light conversion material (D) from the resin composition, and further, it is possible to suppress the appearance of the organic light conversion material (D) and the pollution of the soil and the like caused by the organic light conversion material (D).
[0081] The organic light conversion material (D) preferably contains at least one of an organic metal complex and an organic fluorescent dye, more preferably at least one of an organic rare earth complex and an organic fluorescent dye, and even more preferably an organic fluorescent dye.
[0082] The metal element constituting the organometallic complex is not particularly limited, but is preferably a rare earth element, more preferably a lanthanoid element, and further preferably europium or terbium.
[0083] The organic rare earth complex is preferably A m Ln(La) x (Lb) y B n or A m Ln(Lc) z B n The metal complex shown, A is a positive monovalent counter cation, B is a negative monovalent counter anion, La is an anionic bidentate ligand, Lb is a neutral ligand, Lc is a tridentate ligand, Ln is a positive trivalent rare earth metal ion; wherein x = any one of 0 to 4, y = any one of 0 to 4, and x+y = 4 or 5; z = any one of 1 to 3; m = any one of 0 to 3, n = any one of 0 to 3, and the values of m and n can be determined by the staff in this field according to the charge balance.
[0084] For example, complex A m Ln(La) x (Lb) y B nIn the above formula, when La is a bidentate negative divalent anionic ligand and x = 3, the total negative charge is 6, Ln is a positive trivalent rare earth metal ion, and 3 positive monovalent counter cations are required to satisfy the charge balance, that is, m = 3, n = 0; when La is a bidentate negative monovalent anionic ligand and x = 4, the total negative charge is 4, Ln is a positive trivalent rare earth metal ion, and 1 positive monovalent counter cation is required to satisfy the charge balance, that is, m = 1, n = 0; when La is a bidentate negative monovalent anionic ligand and x = 3, the total negative charge is 3, Ln is a positive trivalent rare earth metal ion, and no counter cation or counter anion is required to satisfy the charge balance, that is, m = 0 and n = 0; when the complex does not contain anionic ligands (i.e. x = 0) and only contains neutral ligand Lb, Ln is a positive trivalent rare earth metal ion, and 3 negative monovalent counter anions are required to satisfy the charge balance, that is, m = 0, n = 3.
[0085] For example, complex A m Ln(Lc) z B n In the figure, when Lc is a tridentate negative divalent anionic ligand and z = 3, the total negative charge is 6, Ln is a positive trivalent rare earth metal ion, and 3 positive monovalent counter cations are required to satisfy the charge balance, that is, m = 3, n = 0; when Lc is a tridentate negative monovalent anionic ligand and z = 3, the total negative charge is 3, and no counter cations or counter anions are required to satisfy the charge balance, that is, m = 0 and n = 0; when Lc is a tridentate neutral ligand, Ln is a positive trivalent rare earth metal ion, and 3 negative monovalent counter anions are required to satisfy the charge balance, that is, m = 0, n = 3.
[0086] The counter cation is preferably an alkali metal ion or an organic ammonium ion, and the organic ammonium ion is preferably a quaternary ammonium ion, a 1,3-dialkyl-substituted imidazolium ion or an N-alkyl-substituted pyridinium ion; the counter anion is preferably a chloride ion, a bromide ion, a nitrate ion, an acetate ion, or a sulfonate ion.
[0087] The organic rare earth complex is preferably Ln(La) 3 (Lb) y The metal complex shown is preferably y=1 or 2, La is at least one of the following general formulas I to III, and Lb is at least one of the following general formulas VII to XI. When La is the following general formulas I to III, the organic rare earth complex is the structure of the following general formulas IVa to VIa.
[0088]
[0089]
[0090]
[0091]
[0092] In Formula I and Formula IVa, R 1 , R 2 , R 3 , R 4 , R 5 Each independently represents a hydrogen atom, a halogen atom, a cyano group, an alkyl group, or a halogen-substituted alkyl group; wherein the halogen atom refers to F, Cl, Br, I, etc.; the alkyl group is preferably a C1-C18 straight-chain or branched-chain alkyl group, more preferably a C1-C4 straight-chain or branched-chain alkyl group, including a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a sec-butyl group, and a tert-butyl group, and particularly preferably a methyl group, an ethyl group, and a tert-butyl group; the halogen-substituted alkyl group is preferably a halogen-substituted C1-C18 straight-chain or branched-chain alkyl group, more preferably a halogen-substituted C1-C4 straight-chain or branched-chain alkyl group, such as a trifluoromethyl group and a pentafluoroethyl group;
[0093] In Formula II and Formula Va, R 1 , R 2 Each is independently an aromatic group, an alkyl group, or a halogen-substituted alkyl group; wherein the aromatic group includes phenyl, naphthyl, thienyl, furyl, pyridyl, and derivatives thereof; the alkyl group is preferably a C1-C18 straight-chain or branched-chain alkyl group, more preferably a C1-C4 straight-chain or branched-chain alkyl group, including methyl, ethyl, propyl, isopropyl, butyl, isobutyl, sec-butyl, tert-butyl, and particularly preferably a methyl, ethyl, and tert-butyl group; the halogen-substituted alkyl group is preferably a halogen-substituted C1-C18 straight-chain or branched-chain alkyl group, more preferably a halogen-substituted C1-C4 straight-chain or branched-chain alkyl group, such as trifluoromethyl and pentafluoroethyl.
[0094] In Formula III and Formula VIa, R 1 , R 2 , R 3 , R 4 Each independently represents a hydrogen atom, a halogen atom, a cyano group, an alkyl group, or a halogen-substituted alkyl group; wherein the halogen atom refers to F, Cl, Br, I, etc.; the alkyl group is preferably a C1-C18 straight-chain or branched-chain alkyl group, and more preferably a C1-C4 straight-chain or branched-chain alkyl group, including a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a sec-butyl group, and a tert-butyl group, and particularly preferably a methyl group, an ethyl group, and a tert-butyl group; the halogen-substituted alkyl group is preferably a halogen-substituted C1-C18 straight-chain or branched-chain alkyl group, and more preferably a halogen-substituted C1-C4 straight-chain or branched-chain alkyl group, such as a trifluoromethyl group and a pentafluoroethyl group.
[0095] In Formula VII, R 1 , R 2 , R 3Each is independently an alkyl group or an aromatic group; wherein the alkyl group is preferably a C1-C18 straight-chain or branched alkyl group, and particularly preferably a methyl group, ethyl group, n-propyl group, isopropyl group, n-butyl group, tert-butyl group, n-octyl group, n-dodecyl group, n-hexadecyl group, and n-octadecyl group; the aromatic group is a phenyl group, a naphthyl group, or a phenyl group substituted by a C1-C18 alkyl group.
[0096] In Formula VIII, Formula IX and Formula XI, R 1 , R 2 , R 3 , R 4 , R 5 Each is independently a hydrogen atom, a methyl group or a phenyl group.
[0097] The organic rare earth complex is preferably Aln(La) 4 In the metal complex shown, the cation A is preferably an alkali metal ion or an organic ammonium ion, and La is at least one of the following general formulas I to III. The organic ammonium ion is preferably a quaternary ammonium ion, a 1,3-dialkyl-substituted imidazolium ion or an N-alkyl-substituted pyridinium ion; the quaternary ammonium ion structure is N + R 1 R 2 R 3 R 4 , the aforementioned R 1 , R 2 , R 3 , R 4 Each is independently an alkyl group or an aromatic group, wherein the alkyl group is preferably a C1-C18 straight chain or branched alkyl group, and is particularly preferably a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, a tert-butyl group, an n-octyl group, an n-dodecyl group, an n-hexadecyl group, and an n-octadecyl group; the aromatic group is a phenyl group, a naphthyl group, or a substituted phenyl group. In addition, when La is the following general formula I to III, the organometallic complex is the following general formula IVb to VIb.
[0098]
[0099]
[0100] In Formula I and Formula IVb, R 1 , R 2 , R 3 , R 4 , R 5Each independently represents a hydrogen atom, a halogen atom, a cyano group, an alkyl group, or a halogen-substituted alkyl group; wherein the halogen atom refers to F, Cl, Br, I, etc.; the alkyl group is preferably a C1-C18 straight-chain or branched-chain alkyl group, and more preferably a C1-C4 straight-chain or branched-chain alkyl group, including a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a sec-butyl group, and a tert-butyl group, and particularly preferably a methyl group, an ethyl group, and a tert-butyl group; the halogen-substituted alkyl group is preferably a halogen-substituted C1-C18 straight-chain or branched-chain alkyl group, and more preferably a halogen-substituted C1-C4 straight-chain or branched-chain alkyl group, such as a trifluoromethyl group and a pentafluoroethyl group.
[0101] In Formula II and Formula Vb, R 1 , R 2 Each is independently an aromatic group, an alkyl group, or a halogen-substituted alkyl group; wherein the aromatic group is preferably a phenyl group, a thienyl group, a naphthyl group, a furyl group, a pyridyl group, and derivatives thereof; the alkyl group is preferably a C1-C18 straight-chain or branched-chain alkyl group, more preferably a C1-C4 straight-chain or branched-chain alkyl group, including a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a sec-butyl group, and a tert-butyl group, and particularly preferably a methyl group, an ethyl group, and a tert-butyl group; the halogen-substituted alkyl group is preferably a halogen-substituted C1-C18 straight-chain or branched-chain alkyl group, more preferably a halogen-substituted C1-C4 straight-chain or branched-chain alkyl group, such as a trifluoromethyl group and a pentafluoroethyl group.
[0102] In Formula III and Formula VIb, R 1 , R 2 , R 3 , R 4 Each independently represents a hydrogen atom, a halogen atom, a cyano group, an alkyl group, or a halogen-substituted alkyl group; wherein the halogen atom refers to F, Cl, Br, I, etc.; the alkyl group is preferably a C1-C18 straight-chain or branched-chain alkyl group, and more preferably a C1-C4 straight-chain or branched-chain alkyl group, including a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a sec-butyl group, and a tert-butyl group, and particularly preferably a methyl group, an ethyl group, and a tert-butyl group; the halogen-substituted alkyl group is preferably a halogen-substituted C1-C18 straight-chain or branched-chain alkyl group, and more preferably a halogen-substituted C1-C4 straight-chain or branched-chain alkyl group, such as a trifluoromethyl group and a pentafluoroethyl group.
[0103] The organic rare earth complex is also preferably A m Ln(Lc) 3 B n In the rare earth complex shown, Lc is preferably at least one of the following general formulas XII or XIII; A is preferably a positive monovalent alkali metal ion or an organic ammonium ion, and B is preferably a negative monovalent chloride ion, bromide ion, nitrate ion, acetate ion or sulfonate ion; m = 0 or 3, n = 0 or 3, and the values of m and n satisfy the charge balance of the complex.
[0104]
[0105]
[0106] In Formula XII, R 1 , R 2 , R 3 Each is independently the structure shown in the figure; wherein R 4 , R 5 Each is independently an alkyl group or an aromatic group; the alkyl group is preferably a C1-C18 straight-chain or branched alkyl group, and is particularly preferably a methyl group, ethyl group, n-propyl group, isopropyl group, n-butyl group, tert-butyl group, n-octyl group, n-dodecyl group, n-hexadecyl group, and n-octadecyl group; the aromatic group is a phenyl group, a naphthyl group, or a phenyl group substituted by a C1-C18 alkyl group.
[0107] In Formula XIII, R 1 , R 2 , R 3 , R 4 Each independently represents a hydrogen atom, a halogen atom, a cyano group, an alkyl group, or a halogen-substituted alkyl group; wherein the halogen atom refers to F, Cl, Br, I, etc.; the alkyl group is preferably a C1-C18 straight-chain or branched-chain alkyl group, more preferably a C1-C4 straight-chain or branched-chain alkyl group, including methyl, ethyl, propyl, isopropyl, butyl, isobutyl, sec-butyl, tert-butyl, and particularly preferably a methyl, ethyl, and tert-butyl group; the halogen-substituted alkyl group is preferably a halogen-substituted C1-C18 straight-chain or branched-chain alkyl group, more preferably a halogen-substituted C1-C4 straight-chain or branched-chain alkyl group, such as trifluoromethyl and pentafluoroethyl; R 5 is the structure shown in the figure; where R 6 It is an alkyl group, an aromatic group or a hydroxyl group; wherein the alkyl group is preferably a C1-C18 straight-chain or branched alkyl group, and is particularly preferably a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, a tert-butyl group, an n-octyl group, an n-dodecyl group, an n-hexadecyl group, or an n-octadecyl group; the aromatic group is a phenyl group, a naphthyl group or a phenyl group substituted by a C1-C18 alkyl group.
[0108] The organic fluorescent dye may be a benzoxazolyl pigment, a coumarin pigment, a styrene biphenyl pigment, a terphenyl pigment, an oxazole pigment, an indole pigment, a malachite green pigment, a rhodamine pigment, an oxazine pigment, an anthracene pigment, a pyrene pigment, a perylene pigment, etc. The organic fluorescent dye having a molecular weight of 200 g / mol or more is not particularly limited, and examples thereof include 2,5-bis(5-tert-butyl-2-benzoxazolyl)thiophene, 4,4'-bis(benzoxazolyl-2-yl)stilbene, 4,4'-bis(benzoxazolyl-2-yl)furan, 4,4-bis(benzoxazolyl-2-yl)naphthalene, 3-phenyl-7-aminocoumarin, 3-phenyl-7-(imino-1'3'5'-triazine-2'-diethylamino-4'- chloro) coumarin, 3-phenyl-7-(imino-1'3'5'-triazine-2'-diethylamino-4'-methoxy) coumarin, 3-phenyl-7-(2H-naphtho(1,2-d)-triazol-2-yl) coumarin, 4-methyl-7-hydroxycoumarin, 7-diethylamino-4-methylcoumarin, 4,4-bis(2-disulfonic acid styryl) biphenyl, 4,4-bis(2-methoxystyryl) biphenyl, etc.
[0109] The organic fluorescent dye is also preferably a compound represented by the following general formula XIV to XXI.
[0110]
[0111]
[0112]
[0113]
[0114]
[0115] In Formula XVIII, R 1 , R 2 R is independently a hydrogen atom, a hydroxyl group, an amino group, an alkoxy group, an alkyl-substituted amino group, the alkoxy group is preferably a C1-C18 straight-chain or branched alkoxy group, and is particularly preferably a methoxy group, an ethoxy group, a n-propoxy group, an isopropoxy group, an n-butoxy group, a tert-butoxy group, the alkyl-substituted amino group includes a monoalkyl-substituted amino group and a dialkyl-substituted amino group, the alkyl group is independently a C1-C18 straight-chain or branched alkane group, and is particularly preferably a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, a tert-butyl group, an n-octyl group, an n-dodecyl group, an n-hexadecyl group, and an n-octadecyl group; 3 is a hydrogen atom or an alkyl group, wherein the alkyl group is independently a C1-C18 straight-chain or branched alkane, and particularly preferably a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, a tert-butyl group, an n-octyl group, an n-dodecyl group, an n-hexadecyl group, or an n-octadecyl group.
[0116]
[0117] In Formula XIX, R 1 , R 2 , R 3 , R 4 , R 5 , R 6 Each is independently a hydrogen atom or an alkyl group, the alkyl group is preferably a C1-C18 straight chain or branched chain alkyl group, more preferably a C1-C4 straight chain or branched chain alkyl group, including methyl, ethyl, propyl, isopropyl, butyl, isobutyl, sec-butyl, tert-butyl, particularly preferably methyl or ethyl; R 7 , R 8 Each independently represents a hydrogen atom, a carboxyl group, an ester group, or a sulfonate group, wherein the ester group includes methyl formate, ethyl formate, propyl formate, and butyl formate, and methyl formate and ethyl formate are particularly preferred; X represents a halogen counter anion, wherein the halogen ion refers to a fluoride ion, a chloride ion, a bromide ion, or an iodide ion.
[0118]
[0119] In formula XX, R 1 , R 2 , X are each independently a hydrogen atom, a halogen, a nitro group, or an alkoxy group, wherein the halogen atom refers to F, Cl, Br, I, etc.; the alkoxy group is preferably a C1-C18 straight chain or branched alkoxy group, and particularly preferably a methoxy group, an ethoxy group, a n-propoxy group, an isopropoxy group, a n-butoxy group, or a tert-butoxy group.
[0120]
[0121] In Formula XXI, R 1 , R 2 , R 3 , R 4 , R 5 , R 6 , R 7 , R 8 , R 9 , R 10 , R 11 , R 12Each independently represents a hydrogen atom, an alkyl group, or an aromatic group. The alkyl group is preferably a C1-C18 straight-chain or branched alkyl group, more preferably a C1-C4 straight-chain or branched alkyl group, including methyl, ethyl, propyl, isopropyl, butyl, isobutyl, sec-butyl, tert-butyl, and particularly preferably methyl and ethyl. The aromatic group is a phenyl group or a substituted phenyl group. The substituted phenyl group is a phenyl group substituted by a halogen atom, methyl, ethyl, isopropyl, tert-butyl, methoxy, ethoxy, trifluoromethyl, or dimethylamino. The number and position of the substituents may be determined according to actual conditions, and preferably 2-fluorophenyl, 2-chlorophenyl, 2-bromophenyl, 3-fluorophenyl, 3-chlorophenyl, 3-bromophenyl, 4-fluorophenyl, 4-chlorophenyl, 4-bromophenyl, 2,3-dichlorophenyl, 2,4-dichlorophenyl, 2,5-dichlorophenyl, 2,6-dichlorophenyl, 3, 4-dichlorophenyl, 3,5-dichlorophenyl, 2-methylphenyl, 2-ethylphenyl, 2-isopropylphenyl, 2-tert-butylphenyl, 4-methylphenyl, 4-ethylphenyl, 4-isopropylphenyl, 4-tert-butylphenyl, 2,4-dimethylphenyl, 2,5-dimethylphenyl, 2,6-dimethylphenyl, 3,5-dimethylphenyl, 2-methyl-5-tert-butylphenyl, 2-methoxyphenyl, 3-methoxyphenyl, 4-methoxyphenyl, 2-dimethylaminophenyl, 4-dimethylaminophenyl, particularly preferably 2-methylphenyl, 3-methylphenyl, 4-methylphenyl, 2-methoxyphenyl, 3-methoxyphenyl, 4-methoxyphenyl; M is an acid that combines with the fluorescent molecule to form a salt, including hydrochloric acid, hydrobromic acid, and hydroiodic acid; X is a halogen counter anion, including fluoride ion, chloride ion, bromide ion, and iodide ion.
[0122] Specifically, the organic light conversion material (D) is preferably a rare earth complex or compound represented by the following general formulae XXII to XXXI.
[0123]
[0124]
[0125]
[0126]
[0127]
[0128]
[0129]
[0130]
[0131]
[0132]
[0133] The molecular weight of the organic light conversion material (D) is 200 or more, preferably 250 or more, and more preferably 300 or more. If the molecular weight of the organic light conversion material (D) is less than 200, the organic light conversion material (D) is easy to ooze out of the resin composition, which may lead to failure to maintain light conversion efficiency or deterioration of appearance. The molecular weight of the organic light conversion material (D) may be 1000 or less.
[0134] The organic light conversion material (D) preferably has at least one absorption peak in the range of 300 to 600 nm in the absorption spectrum for the absorption spectrum and the emission spectrum measured according to the method described in GB / T 9721-2006 and JY / T 0571-2020. Here, "absorption peak" refers to the spectral intensity reaching a maximum value at a specific wavelength. In addition, the organic light conversion material (D) preferably has at least one emission peak in the range of 400 to 800 nm in the emission spectrum, and more preferably has at least one emission peak in the range of 400 to 750 nm in the emission spectrum. Here, "emission peak" refers to the spectral intensity reaching a maximum value at a specific wavelength. By absorbing and emitting light in the above range by the organic light conversion material (D) and the resin composition, the photosynthetic rate of the plant can be increased.
[0135] The organic light conversion material (D) can be used alone or in combination of two or more. When two or more organic light conversion materials (D) are combined, the luminescence spectrum of one organic light conversion material (D) and the absorption spectrum of another organic light conversion material (D) can be partially overlapped; or the emission spectra of two or more organic light conversion materials (D) do not affect each other and are directly superimposed. In addition, an organic metal complex and an organic fluorescent dye can also be combined.
[0136] The content of the organic light conversion material (D) in the resin composition of the present invention is 0.01wt% or more, preferably 0.1% or more, and more preferably 1wt% or more. In addition, the content of the organic light conversion material (D) is less than 10wt%, preferably less than 9wt%, and more preferably less than 8wt%. If the content of the organic light conversion material (D) is more than 10wt%, it is easy to cause exudation, and the light conversion efficiency cannot be maintained for a long time, or the appearance deteriorates.
[0137] (Thermoplastic resin (E))
[0138] The resin composition of the present invention may include a thermoplastic resin (E) different from EVOH (C). If the resin composition of the present invention includes a thermoplastic resin (E), the reduction in gas barrier properties of the resin composition of the present invention due to moisture intrusion can be suppressed. On the other hand, by including a thermoplastic resin (E), the gas barrier properties are reduced. Therefore, under specific conditions such as using the multilayer structure of the present invention under a high humidity environment, it is preferred that the resin composition of the present invention includes a thermoplastic resin (E). In addition, in the case where the multilayer structure of the present invention described later does not provide an adhesive layer (Z) and directly stacks the layer (X) and the layer (Y), it is preferred that the resin composition of the present invention includes a thermoplastic resin (E) from the perspective of improving the peel strength of the layer (X) and the layer (Y). If the peel strength of the layer (X) and the layer (Y) is improved, the mechanical strength can be maintained for a long time. In addition, when layer (Y) contains a hydrophobic thermoplastic resin described later, the multilayer structure of the present invention can suppress the intrusion of moisture from the outside through layer (Y), thereby suppressing the reduction in the gas barrier properties of the resin composition of the present invention due to the intrusion of moisture. Therefore, by improving the peel strength between layer (X) and layer (Y), the gas barrier properties of the multilayer structure can be maintained for a long time, and as a result, the light conversion efficiency can be maintained for a long time.
[0139] The thermoplastic resin (E) may include an unmodified thermoplastic resin or an acid-modified thermoplastic resin. The resin composition of the present invention preferably includes an unmodified thermoplastic resin from the perspective of being able to maintain the light conversion efficiency for a long time by suppressing the reduction of gas barrier properties. In addition, from the perspective of the resin composition of the present invention further exerting gas barrier properties and the multilayer structure being able to maintain long-term light conversion efficiency, it is preferred to include an acid-modified thermoplastic resin. In addition, an unmodified thermoplastic resin and an acid-modified thermoplastic resin may be used in combination.
[0140] The unmodified thermoplastic resin is not particularly limited, but in order to prevent the gas barrier performance of the resin composition from being reduced due to moisture intrusion, a hydrophobic thermoplastic resin may be used, and a hydrophobic polyolefin resin is preferably used. Examples include polyethylene resins such as linear low-density polyethylene, low-density polyethylene, ultra-low-density polyethylene, ultra-low-density linear polyethylene, medium-density polyethylene, and high-density polyethylene, polyethylene resins such as ethylene-α-olefin copolymers, polypropylene, ethylene-propylene (block and random) copolymers, propylene-α-olefin (α-olefin with 4 to 20 carbon atoms) copolymers, polypropylene resins such as polybutene, polypentene, etc.; polyolefin resins such as grafted polyolefins obtained by grafting these polyolefins with unsaturated carboxylic acids or their esters, cyclic polyolefin resins, etc.; ionomers, ethylene-vinyl acetate copolymers, ethylene-acrylic acid copolymers, ethylene-acrylic acid ester copolymers, polyester resins, polyamide resins, polyvinyl chloride, polyvinylidene chloride, acrylic resins, polystyrene, vinyl ester resins, polyester elastomers, polyurethane elastomers, chlorinated polyethylene, chlorinated polypropylene, etc., halogenated polyolefins, aromatic or aliphatic polyketones, etc. Among them, polyolefin resins are preferred from the perspective of mechanical strength and molding processability, and polyethylene resins and polypropylene resins are more preferred.
[0141] The acid-modified group contained in the acid-modified thermoplastic resin is not particularly limited, and examples thereof include a carboxyl group or a derivative thereof, a phosphoric acid group or a derivative thereof, etc. Examples of the derivative of the carboxyl group include a carboxylic acid anhydride group (-CO-O-CO-), a carboxylic acid halide group (-COCl, -COBr, etc.), etc. Among them, a carboxyl group or a derivative thereof is preferred. It should be noted that the acidic group may exist in the form of a salt.
[0142] The acid-modified thermoplastic resin may be a modified thermoplastic resin containing a carboxyl group obtained by chemically bonding (e.g., by addition reaction, graft reaction, copolymerization, etc.) an ethylenically unsaturated carboxylic acid or its anhydride to a thermoplastic resin. The thermoplastic resin into which the acid-modified group is introduced may be the same as the unmodified thermoplastic resin described above. Specifically, the acid-modified thermoplastic resin is preferably an acid-modified polyolefin resin, preferably a carboxylic acid-modified polyolefin resin obtained by chemically bonding an ethylenically unsaturated carboxylic acid or its anhydride to a polyolefin resin.
[0143] Ethylenically unsaturated carboxylic acids or their anhydrides include ethylenically unsaturated monocarboxylic acids, esters thereof, ethylenically unsaturated dicarboxylic acids, mono- or diesters thereof, or anhydrides thereof, and ethylenically unsaturated dicarboxylic acid anhydrides are preferred. Specifically, maleic acid, fumaric acid, itaconic acid, maleic anhydride, itaconic anhydride, monomethyl maleate, monoethyl maleate, diethyl maleate, monomethyl fumarate, etc. are preferred, and maleic anhydride is preferred.
[0144] Examples of the acid-modified thermoplastic resin include maleic anhydride-modified polyethylene, maleic anhydride-modified polypropylene, maleic anhydride-modified ethylene-ethyl acrylate copolymer, maleic anhydride-graft-modified ethylene-vinyl acetate copolymer, etc. Among them, maleic anhydride-modified polyethylene or maleic anhydride-modified polypropylene is preferred, and maleic anhydride-modified polyethylene is more preferred from the perspective of mechanical strength and molding processability.
[0145] When the thermoplastic resin (E) contains an unmodified thermoplastic resin and an acid-modified thermoplastic resin, the mass ratio of the unmodified thermoplastic resin to the acid-modified thermoplastic resin (unmodified / acid-modified) is preferably 70:30 or less, more preferably 60:40 or less. On the other hand, the mass ratio (unmodified:acid-modified) is preferably 30:70 or more, more preferably 40:60 or more.
[0146] The proportion of at least one of the unmodified thermoplastic resin and the acid-modified thermoplastic resin in the thermoplastic resin (E) is preferably 50 wt % or more, more preferably 70 wt % or more, and further preferably 90 wt % or more. The resin composition (E) may also be composed of only at least one of the unmodified thermoplastic resin and the acid-modified thermoplastic resin.
[0147] When the resin composition of the present invention includes a thermoplastic resin (E), the content of the thermoplastic resin (E) in the resin composition of the present invention is preferably 10wt% or more, more preferably 20wt% or more. In addition, the content of the thermoplastic resin (E) is preferably 50wt% or less, more preferably 40wt% or less. When the resin composition of the present invention includes a thermoplastic resin (E) in the above range, the long-term light conversion efficiency can be maintained when the multilayer structure of the present invention is used under high humidity.
[0148] (Phosphoric acid compound (a1))
[0149] The resin composition of the present invention may include a phosphoric acid compound (a1). If the resin composition of the present invention includes a phosphoric acid compound (a1), coloring during melt molding can be suppressed. The phosphoric acid compound (a1) contained in the resin composition of the present invention is not particularly limited, and various acids such as phosphoric acid and phosphorous acid, and their salts, etc. can be used. Phosphate can be in any form of dihydrogen phosphate, monohydrogen phosphate, and phosphate, preferably dihydrogen phosphate. Its cation type is not particularly limited, and is preferably an alkali metal salt. Among them, sodium dihydrogen phosphate and potassium dihydrogen phosphate are preferably preferred. In the case where the resin composition of the present invention includes a phosphoric acid compound (a1), the content of the phosphoric acid compound (a1) is preferably 5ppm or more, more preferably 8ppm or more, and further preferably 10ppm or more in terms of phosphate conversion. In addition, the content of the phosphoric acid compound (a1) is preferably 200ppm or less, more preferably 100ppm or less, and further preferably 50ppm or less in terms of phosphate conversion.
[0150] (Alkali metal salt (a2))
[0151] The resin composition of the present invention may contain an alkali metal salt (a2). If the resin composition of the present invention contains an alkali metal salt (a2), the thermal stability during melt molding can be improved. The alkali metal constituting the alkali metal salt (a2) may include lithium, sodium, potassium, rubidium, cesium, etc., and sodium or potassium is preferred from the perspective of industrial acquisition.
[0152] Alkali metal salts (a2) include salts of organic acids such as aliphatic carboxylic acids, aromatic carboxylic acids, aliphatic dicarboxylic acids, aromatic dicarboxylic acids, tricarboxylic acids, tetracarboxylic acids, hydroxycarboxylic acids, ketodicarboxylic acids, and amino acids; and salts of inorganic acids such as nitric acid, sulfuric acid, sulfurous acid, carbonic acid, and phosphoric acid. Among them, aliphatic carboxylates or phosphates are preferred, and from the perspective of compatibility with EVOH, etc., aliphatic carboxylates or phosphates with a carbon number of 6 or less are more preferred. Fatty acids include saturated fatty acids such as formic acid, acetic acid, propionic acid, butyric acid, and caproic acid; and unsaturated fatty acids such as acrylic acid and methacrylic acid. Among them, from the perspective of compatibility with EVOH (A), etc., saturated fatty acids with a carbon number of 1 to 3 are preferred, and acetic acid is more preferred. Specifically, sodium acetate, potassium acetate, and sodium dihydrogen phosphate are preferred from the perspective of easy availability.
[0153] The metal constituting the alkali metal salt (a2) may form a salt in the form of an anion corresponding to an alkali metal cation constituting the alkali metal salt (a2), or may form a salt in the form of an alkali metal EVOH alkoxide.
[0154] In the case where the resin composition of the present invention includes an alkali metal salt (a2), the content of the alkali metal ion (a2) in the resin composition of the present invention is preferably more than 10ppm, more preferably more than 20ppm, and more preferably more than 30ppm in terms of metal atom conversion. In addition, the content of the alkali metal salt (a2) in the resin composition of the present invention is preferably less than 400ppm, more preferably less than 350ppm, and more preferably less than 300ppm in terms of metal atom conversion. When the content of the alkali metal salt (a2) is within the above range, coloring during melt molding can be suppressed, while further improving thermal stability.
[0155] When the resin composition of the present invention contains the phosphoric acid compound (a1) and the alkali metal salt (a2), the phosphate-equivalent mass (W) of the phosphoric acid compound (a1) is a1 ) and the mass (W) of the alkali metal salt (a2) in terms of metal atoms a2 ) a1 / W a2 ) is preferably 0.01 or more, more preferably 0.05 or more, and further preferably 0.10 or more. a1 / W a2 ) is preferably 2 or less, more preferably 1.5 or less, and further preferably 1.0 or less. a1 / W a2 ) is within the aforementioned range, the coloring resistance and thermal stability during melt molding can be further improved.
[0156] (Other ingredients)
[0157] The resin composition of the present invention may contain other additives other than the organic photoconversion material (D), the phosphoric acid compound (a1) and the alkali metal salt (a2) as other components within a range that does not inhibit the effects of the present invention.
[0158] The aforementioned other additives include known additives such as carboxylic acids, boron compounds, alkaline earth metal salts, antioxidants, ultraviolet absorbers, plasticizers, antistatic agents, lubricants, colorants, fillers, antiblocking agents, desiccants, etc. However, the content of the aforementioned additives in the resin composition of the present invention is preferably 10 wt % or less, more preferably 5 wt % or less, and further preferably 1 wt % or less.
[0159] If the resin composition of the present invention contains carboxylic acid, the coloring resistance during melt molding can be improved. The carboxylic acid can be a carboxylic acid ion or a carboxylic acid derivative. In addition, the carboxylic acid can be a monocarboxylic acid, or a polycarboxylic acid compound having more than two carboxyl groups in the molecule, or a combination thereof. It should be noted that the polycarboxylic acid does not include a polymer. In addition, the polycarboxylic acid ion is a substance obtained by detaching at least one hydrogen ion from the carboxyl group of the polycarboxylic acid. The carboxyl group of the carboxylic acid can be an ester structure, and the carboxylic acid ion can form a salt with a metal.
[0160] The monocarboxylic acid is not particularly limited, and examples thereof include formic acid, acetic acid, propionic acid, butyric acid, caproic acid, capric acid, acrylic acid, methacrylic acid, benzoic acid, 2-naphthoic acid, etc. These carboxylic acids may have a hydroxyl group or a halogen atom. In addition, carboxylic acid ions include substances obtained by detaching the hydrogen ions of the carboxyl groups of the above-mentioned carboxylic acids. The pKa of the monocarboxylic acid (including monocarboxylic acids that give monocarboxylic acid ions) is preferably 3.5 or more, and more preferably 4 or more, from the perspective of the pH regulating ability and melt moldability of the composition. Such monocarboxylic acids include formic acid (pKa=3.68), acetic acid (pKa=4.74), propionic acid (pKa=4.85), butyric acid (pKa=4.80), etc., and acetic acid is preferred from the perspective of easy handling.
[0161] In addition, polycarboxylic acids are not particularly limited as long as they have two or more carboxyl groups in the molecule, and examples thereof include aliphatic dicarboxylic acids such as oxalic acid, malonic acid, succinic acid, maleic acid, fumaric acid, glutaric acid, adipic acid, and pimelic acid; aromatic dicarboxylic acids such as phthalic acid, isophthalic acid, and terephthalic acid; tricarboxylic acids such as aconitic acid; carboxylic acids having four or more carboxyl groups such as 1,2,3,4-butanetetracarboxylic acid and ethylenediaminetetraacetic acid; hydroxycarboxylic acids such as tartaric acid, citric acid, isocitric acid, malic acid, mucic acid, succinic acid, and citramalic acid; oxalatoacetic acid, dihydroxyoxalic acid, 2-ketomalonic acid, 3-ketomalonic acid, and other ketocarboxylic acids; amino acids such as glutamic acid, aspartic acid, and 2-aminoadipic acid. It should be noted that polycarboxylic acid ions include their anions. Among them, succinic acid, malic acid, tartaric acid, and citric acid are particularly preferred from the perspective of easy acquisition.
[0162] When the resin composition of the present invention contains carboxylic acid, from the perspective of coloration resistance during melt molding, the content thereof is preferably 0.01 μmol / g or more, more preferably 0.05 μmol / g or more, and further preferably 0.5 μmol / g or more in terms of carboxylate radical conversion. In addition, the content of carboxylic acid is preferably 20 μmol / g or less, more preferably 15 μmol / g or less, and further preferably 10 μmol / g or less in terms of carboxylate radical conversion.
[0163] If the resin composition of the present invention contains a boron compound, the thermal stability during melt molding can be improved. Boron compounds include, for example, boric acids, boric esters, borates, boron hydrides, etc. Specifically, boric acids include orthoboric acid (hereinafter also referred to as "boric acid"), metaboric acid, tetraboric acid, etc., boric esters include triethyl borate, trimethyl borate, etc., and borates include alkali metal salts, alkaline earth metal salts, borax, etc. of the aforementioned various boric acids. Among these compounds, orthoboric acid is preferred.
[0164] When the resin composition of the present invention includes a boron compound, its content is preferably 5 ppm or more, more preferably 10 ppm or more, and further preferably 50 ppm or more, calculated as boron element. In addition, the content of the boron compound is preferably 2000 ppm or less, more preferably 1000 ppm or less, further preferably 500 ppm or less, and particularly preferably 300 ppm or less, calculated as boron element.
[0165] If the resin composition of the present invention contains an alkaline earth metal salt, the thermal stability during melt molding can be improved. Alkaline earth metals constituting the alkaline earth metal salt include beryllium, magnesium, calcium, strontium, barium, etc., and magnesium or calcium is preferred from the perspective of easy industrial acquisition. Alkaline earth metal salts include salts of organic acids such as aliphatic carboxylic acids, aromatic carboxylic acids, aliphatic dicarboxylic acids, aromatic dicarboxylic acids, tricarboxylic acids, tetracarboxylic acids, hydroxycarboxylic acids, ketodicarboxylic acids, and amino acids; salts of inorganic acids such as sulfuric acid, sulfurous acid, carbonic acid, and phosphoric acid. Among them, from the perspective of compatibility with EVOH, etc., saturated fatty acids with 1 to 3 carbon atoms are preferred, and acetic acid is more preferred. In the case where the resin composition of the present invention contains an alkaline earth metal salt, its content is preferably 10 to 200 ppm in terms of metal atom conversion.
[0166] Examples of the antioxidant include 2,5-di-tert-butylhydroquinone, 2,6-di-tert-butyl-p-cresol, 4,4'-thiobis-(6-tert-butylphenol, 2,2'-methylene-bis(4-methyl-6-tert-butylphenol, tetrakis-[methylene-3-(3',5'-di-tert-butyl-4'-hydroxyphenyl)propionate]methane, octadecyl 3-(3',5-di-tert-butyl-4'-hydroxyphenyl)propionate, and 4,4'-thiobis-(6-tert-butylphenol).
[0167] Examples of the ultraviolet absorber include ethyl 2-cyano-3,3-diphenylacrylate, 2-(2'-hydroxy-5'-methylphenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-3'-tert-butyl-5'-methylphenyl)-5-chlorobenzotriazole, 2-hydroxy-4-methoxybenzophenone, 2,2'-dihydroxy-4-methoxybenzophenone, and 2-hydroxy-4-octyloxybenzophenone.
[0168] Examples of the plasticizer include dimethyl phthalate, diethyl phthalate, dioctyl phthalate, wax, liquid paraffin, and phosphoric acid ester.
[0169] Examples of the antistatic agent include pentaerythritol monostearate, sorbitan monopalmitate, sulfated oleic acid, polyethylene oxide, and carbowax.
[0170] Examples of the lubricant include ethylene bisstearylamide, butyl stearate, calcium stearate, zinc stearate and the like.
[0171] Examples of the colorant include carbon black, phthalocyanine, quinacridone, indoline, azo pigments, titanium oxide, and red iron.
[0172] Examples of fillers include glass fiber, mica, and wollastonite.
[0173] In addition, the resin composition of the present invention may contain various acids, various metal salts and other compounds from the perspective of thermal stability or viscosity adjustment. Examples of the aforementioned various acids include carboxylic acids, phosphoric acid compounds, boron compounds, etc., and examples of the aforementioned various metal salts include alkali metal salts or alkaline earth metal salts, etc. It should be noted that these compounds may be mixed with EVOH (C) in advance.
[0174] The resin constituting the resin composition of the present invention preferably contains EVOH (C) in a proportion of 50 wt % or more, more preferably 70 wt % or more, further preferably 90 wt % or more, further preferably 95 wt % or more. The resin constituting the resin composition of the present invention may also consist only of EVOH (C).
[0175] When the resin composition of the present invention contains a thermoplastic resin (E), the proportion of EVOH (C) and the thermoplastic resin (E) constituting the resin composition of the present invention is preferably 50 wt% or more, more preferably 70 wt% or more, further preferably 90 wt% or more, and particularly preferably 95 wt% or more. The resin constituting the resin composition of the present invention may also consist only of EVOH (C) and the thermoplastic resin (E).
[0176] The proportion of EVOH (C) and the organic light conversion material (D) in the resin composition of the present invention is preferably 90 wt% or more, more preferably 97 wt% or more, and further preferably 99 wt% or more. The resin composition of the present invention may also consist only of EVOH (C) and the organic light conversion material (D).
[0177] When the resin composition of the present invention contains a thermoplastic resin (E), the proportion of EVOH (C), the organic light conversion material (D) and the thermoplastic resin (E) in the resin composition of the present invention is preferably 90 wt % or more, more preferably 97 wt % or more, and further preferably 99 wt % or more. The resin composition of the present invention may consist only of EVOH (C), the organic light conversion material (D) and the thermoplastic resin (E).
[0178] The resin composition of the present invention may have an oxygen permeability of 100 cc·20 μm / (m 2 ·day·atm) or less, more preferably 80cc·20μm / (m 2 ·day·atm) or less, more preferably 60cc·20μm / (m 2 ·day·atm) or less, more preferably 1.0cc·20μm / (m 2 ·day·atm) or less, particularly preferably 1.0cc·20μm / (m 2 ·day·atm) or less. The oxygen permeability of the resin composition of the present invention may be 0.005cc·20μm / (m 2 ·day·atm) or more.
[0179] The method for manufacturing the resin composition of the present invention is not particularly limited, and for example, it can be manufactured by mixing or kneading with an organic light conversion material (D) under the melting condition of EVOH (C). When manufacturing the resin composition of the present invention, in the method for manufacturing the multilayer structure described later, when the layer (X) is formed into a film, EVOH (C) and the organic light conversion material (D) can be mixed and manufactured, and after EVOH (C) and the organic light conversion material (D) are mixed, melt-kneaded, the resin composition pellets of the present invention can be manufactured in advance. From the perspective of making the organic light conversion material (D) in the resin composition of the present invention have good dispersibility, it is preferred to pre-manufacture the resin composition pellets of the present invention. In the case where the resin composition of the present invention contains a thermoplastic resin (E), it can be mixed with EVOH (C) and the organic light conversion material (D) at the same time. In addition, in the case where the resin composition of the present invention contains a phosphoric acid compound (a1), an alkali metal salt (a2) and other components, it can be mixed with EVOH (C) and the organic light conversion material (D) at the same time, or it can be pre-included in EVOH (C). The method of pre-including the phosphoric acid compound (a1), the alkali metal salt (a2) and other components in EVOH (C) includes a method of immersing EVOH (C) in a solution containing the phosphoric acid compound (a1), the alkali metal salt (a2) and other components, a method of adding the solution to EVOH (C), and a method of mixing various additives and melt-kneading. Mixing or kneading under molten conditions can be carried out using a known mixing device or kneading device such as a horizontal mixer, an extruder, a mixing roll, a Banbury mixer, etc. The temperature during melt kneading is usually 110 to 300°C.
[0180] (Multilayer structure)
[0181] The multilayer structure of the present invention comprises at least one layer (X) each composed of the resin composition of the present invention and a layer (Y) described below. The multilayer structure of the present invention can maintain long-term light conversion efficiency by comprising the layer (X).
[0182] The thickness of layer (X) is not particularly limited, but is preferably 5 to 50 μm, more preferably 10 to 40 μm, and further preferably 15 to 30 μm. When the thickness of layer (X) is within the above range, the multilayer structure can maintain a certain rigidity, can exert excellent gas barrier properties and maintain light conversion efficiency for a long time. The ratio of the thickness of layer (X) in the multilayer structure of the present invention is preferably 1 to 40%, more preferably 2 to 30%, and further preferably 3 to 20%.
[0183] [Layer(Y)]
[0184] The multilayer structure of the present invention preferably has a layer (Y) comprising a thermoplastic resin (B). The multilayer structure of the present invention improves mechanical strength by having a layer (Y). In addition, when the thermoplastic resin (B) is a hydrophobic thermoplastic resin, the layer (Y) suppresses water vapor permeation in the multilayer structure, and can suppress the reduction of gas barrier properties caused by water intrusion of the resin composition of the present invention, so that the light conversion efficiency can be maintained for a long time.
[0185] The thermoplastic resin (B) is not particularly limited, but a hydrophobic thermoplastic resin is preferably used in order to prevent the gas barrier properties of the resin composition of the present invention from being reduced due to moisture. For example, polyolefin resins include polyethylenes such as linear low-density polyethylene, low-density polyethylene, ultra-low-density polyethylene, ultra-low-density linear polyethylene, medium-density polyethylene, and high-density polyethylene, polyethylene resins such as ethylene-α-olefin copolymers, polypropylene, ethylene-propylene (block and random) copolymers, propylene-α-olefin (α-olefin with 4 to 20 carbon atoms) copolymers, polypropylene resins, polybutene, polypentene, etc.; grafted polyolefins obtained by grafting these polyolefins with unsaturated carboxylic acids or their esters, cyclic polyolefin resins; ionomers, ethylene-vinyl acetate copolymers, ethylene-acrylic acid copolymers, ethylene-acrylic acid ester copolymers, polyester resins, polyamide resins, polyvinyl chloride, polyvinylidene chloride, acrylic resins, polystyrene, vinyl ester resins, polyester elastomers, polyurethane elastomers, chlorinated polyethylene, chlorinated polypropylene, halogenated polyolefins, aromatic or aliphatic polyketones, etc. Among them, polyolefin resins are preferred in terms of mechanical strength and molding processability, and polyethylene and polypropylene are particularly preferred.
[0186] In addition, the thermoplastic resin (B) may include an acid-modified thermoplastic resin. When the thermoplastic resin (B) includes an acid-modified thermoplastic resin, in the multilayer structure of the present invention, the adhesion of the layer (X) directly stacked with the layer (Y) can be improved, the permeation of water vapor in the multilayer structure is suppressed, and the long-term light conversion efficiency can be maintained. Suitable forms of the acid-modified thermoplastic resin used as the thermoplastic resin (B) are the same as the acid-modified thermoplastic resin exemplified in the thermoplastic resin (E).
[0187] The layer (Y) may contain other components within a range that does not inhibit the effects of the present invention. As other components in the layer (Y), the same substances as exemplified as other components of the resin composition of the present invention can be used.
[0188] The ratio of the thermoplastic resin (B) to the layer (Y) is preferably 90 wt % or more, more preferably 97 wt % or more, and further preferably 99 wt % or more. The layer (Y) may consist only of the thermoplastic resin (B).
[0189] The thickness of layer (Y) is not particularly limited, and its thickness is preferably 10 to 200 μm, more preferably 20 to 100 μm, and further preferably 30 to 80 μm. In addition, the average thickness of layer (Y) is preferably 3 to 100 μm, more preferably 5 to 75 μm, and further preferably 10 to 50 μm. By setting the thickness of layer (Y) to the above range, the water vapor permeation in the multilayer structure is suppressed, and the reduction of gas barrier properties caused by moisture intrusion can be suppressed, so that the light conversion efficiency can be maintained for a long time. The thickness of layer (Y) is preferably 20 to 95% relative to the total thickness of the multilayer structure of the present invention, more preferably 25 to 85%, and further preferably 30 to 75%. In particular, in the case of two kinds of three-layer structures (layer (Y) / layer (X) / layer (Y)), the thickness of layer (Y) is preferably 45 to 85% relative to the total thickness of the multilayer structure, and is further preferably 75 to 85%. In addition, in the case of three types of five-layer structures (layer (Y) / layer (Z) / layer (X) / layer (Z) / layer (Y)), the ratio of the thickness of layer (Y) to the total thickness of the multilayer structure is preferably 50 to 90% or 60 to 80%, and is further preferably 30 to 50%.
[0190] [Adhesive layer (Z)]
[0191] The multilayer structure of the present invention can be laminated layer (Y) via a layer (Z) comprising an adhesive resin (F) on at least one surface of layer (X). The multilayer structure of the present invention has an adhesive layer (Z) comprising an adhesive resin (F), and by making layer (Z) be located between layer (X) and layer (Y), the peel strength of layer (X) and layer (Y) can be improved, and mechanical strength can be maintained for a long time. In addition, when thermoplastic resin (B) is a hydrophobic thermoplastic resin, layer (Y) can suppress water vapor permeation in the multilayer structure, therefore by improving the peel strength of layer (X) and layer (Y), the reduction of gas barrier caused by moisture intrusion of the resin composition of the present invention can be suppressed for a long time, so the light conversion efficiency can be maintained for a long time.
[0192] [Adhesive resin (F)]
[0193] The adhesive resin (F) is not particularly limited as long as it has adhesiveness between the layer (X) and the layer (Y), but it is preferable to use the same resins as exemplified as the acid-modified thermoplastic resin of the thermoplastic resin (E).
[0194] The acid value of the adhesive resin (F) is preferably more than 1.5 mgKOH / g, more preferably more than 2.0 mgKOH / g, and further preferably more than 2.5 mgKOH / g. By setting the acid value of the adhesive resin (F) to the above range, the peel strength of layer (X) and layer (Y) is improved, so that mechanical strength can be maintained for a long time. In addition, when the thermoplastic resin (B) is a hydrophobic thermoplastic resin, layer (Y) suppresses water vapor permeation in the multilayer structure, and therefore by improving the peel strength of layer (X) and layer (Y), the reduction of gas barrier properties caused by moisture intrusion of the resin composition of the present invention can be suppressed for a long time, so the light conversion efficiency can be maintained for a long time. The acid value of the adhesive resin (F) can be less than 50 mgKOH / g. It should be noted that the acid value in this specification can be measured by the method described in the examples.
[0195] The adhesive layer (Z) may contain the same resin as exemplified for the unmodified thermoplastic resin of the thermoplastic resin (E). When the adhesive layer (Z) contains the adhesive resin (F) and the unmodified thermoplastic resin, the mass ratio of the adhesive resin (F) to the unmodified thermoplastic resin (F / unmodified) is preferably 10:90 or more, more preferably 20:80 or more. The mass ratio (F / unmodified) may be 95:5 or less.
[0196] The acid value of the adhesive layer (Z) is preferably 0.4 mgKOH / g or more, more preferably 0.5 mgKOH / g or more. If the acid value of the adhesive layer (Z) is 0.5 mgKOH / g or more, by increasing the peel strength between the layer (X) and the layer (Y), the reduction in gas barrier properties of the resin composition of the present invention due to water intrusion can be suppressed for a long time, so that the light conversion efficiency can be maintained for a long time. The acid value of the adhesive layer (Z) may be 20 mgKOH / g or less.
[0197] The adhesive layer (Z) may contain other components within a range that does not inhibit the effects of the present invention. As other components in the layer (Z), the same substances as exemplified as other components of the resin composition of the present invention can be used.
[0198] The proportion of the adhesive resin (F) in the layer (Z) is preferably 90 wt % or more, and preferably 97 wt % or more and 99 wt % or more. The layer (Z) may consist only of the adhesive resin (F).
[0199] When layer (Z) contains an unmodified polyolefin resin, the proportion of the adhesive resin (F) and the unmodified polyolefin in layer (Z) is preferably 90 wt % or more, more preferably 97 wt % or more, and further preferably 99 wt % or more. Layer (Z) may also consist only of the adhesive resin (F) and the unmodified polyolefin resin.
[0200] The thickness of layer (Z) is not particularly limited, and its thickness is preferably 10 to 60 μm, more preferably 20 to 50 μm, and further preferably 25 to 45 μm. In addition, the average thickness of layer (Z) is preferably 3 to 50 μm, and is also preferably 5 to 40 μm, 10 to 30 μm, and is also preferably 30 to 50 μm. By setting the thickness of layer (Z) within the above range, water vapor permeation in the multilayer structure can be suppressed, and the reduction in gas barrier properties caused by moisture intrusion can be suppressed, so that the light conversion efficiency can be maintained for a long time. The ratio of the thickness of layer (Z) to the total thickness of the multilayer structure of the present invention is preferably 1 to 40%, and is also preferably 2 to 30% or 3 to 20%, and is also preferably 30 to 50%.
[0201] [Configuration of Multilayer Structure]
[0202] The multilayer structure of the present invention must have layer (X) and layer (Y), then there is no particular limitation, with layer (X) and layer (Y) directly stacked or layer (X) and layer (Y) stacked via adhesive layer (Z), it is possible to maintain the mechanical properties and gas barrier properties of the multilayer structure for a long time, so it is preferred. In addition, when the thermoplastic resin (B) constituting layer (Y) is a hydrophobic thermoplastic resin, from the perspective of being able to suppress the reduction of the gas barrier properties caused by moisture intrusion of the resin composition of the present invention, it is preferred to have a structure with layer (Y) on both sides of layer (X), and more preferably, layer (Y) is stacked via adhesive layer (Z) on both sides of layer (X). The specific example of the structure of the multilayer structure of the present invention is shown below. In addition, the following specific examples can be stacked or multilayers can be combined. It should be noted that layer (X) and layer (Y) can each be continuously stacked multilayer.
[0203] 2 layers: Layer(Y) / Layer(X)
[0204] 3 layers: layer (Y) / layer (X) / layer (Y), layer (Y) / adhesive layer (Z) / layer (X)
[0205] 4 layers: layer (Y) / adhesive layer (Z) / layer (X) / adhesive layer (Z), adhesive layer (Z) / layer (Y) / adhesive layer (Z) / layer (X)
[0206] 5 layers: layer (Y) / adhesive layer (Z) / layer (X) / adhesive layer (Z) / layer (Y), layer (X) / adhesive layer (Z) / layer (Y) / adhesive layer (Z) / layer (X), layer (Y) / adhesive layer (Z) / layer (X) / adhesive layer (Z) / layer (X), adhesive layer (Z) / layer (Y) / adhesive layer (Z) / layer (X) / adhesive layer (Z)
[0207] 6 layers: layer (Y) / adhesive layer (Z) / layer (X) / adhesive layer (Z) / layer (Y) / adhesive layer (Z)
[0208] 7 layers: layer (Y) / adhesive layer (Z) / layer (X) / adhesive layer (Z) / layer (X) / adhesive layer (Z) / layer (Y)
[0209] Among the above layer structures, the layer structures having layer (Y) / layer (X) / layer (Y) and layer (Y) / adhesive layer (Z) / layer (X) / adhesive layer (Z) / layer (Y) are preferred, because they can maintain the light conversion efficiency for a long period of time.
[0210] The number of layers constituting the multilayer structure of the present invention is preferably 2 or more layers, more preferably 3 or more layers. In addition, the multilayer structure of the present invention may be 11 or less layers, preferably 9 or less layers, more preferably 7 or less layers, and further preferably 5 layers. By setting the number of layers of the multilayer structure within the above range, water vapor permeation in the multilayer structure can be suppressed, and the reduction in gas barrier properties due to water intrusion can be suppressed, so that the light conversion efficiency can be maintained for a long time.
[0211] The thickness of the multilayer structure of the present invention is generally 5 to 200 μm, preferably 10 to 150 μm, and more preferably 20 to 100 μm in total thickness.
[0212] The peel strength between layer (X) and the layer adjacent to layer (X) is preferably 400 g / 15 mm or more, more preferably 800 g / 15 mm or more, and further preferably 1200 g / 15 mm or more. By setting the peel strength between layer (X) and the layer adjacent to layer (X) to be within the above range, the multilayer structure of the present invention can maintain the light conversion efficiency for a long time. The peel strength may be 5000 g / 15 mm or less.
[0213] The oxygen permeability of the multilayer structure of the present invention measured at a temperature of 20° C. and a humidity of 65% RH according to the method described in ISO14663-2 is 100 cc·20 μm / (m 2 ·day·atm) or less, more preferably 80cc·20μm / (m 2 ·day·atm) or less, more preferably 60cc·20μm / (m 2 ·day·atm) or less, more preferably 5.0cc·20μm / (m 2 ·day·atm) or less, particularly preferably 1.0cc·20μm / (m 2 By setting the oxygen permeability within the above range, the multilayer structure of the present invention can maintain the light conversion efficiency for a long time. The above oxygen permeability can be 0.005cc·20μm / (m 2 ·day·atm) or more.
[0214] The water vapor transmission rate of the multilayer structure of the present invention measured at a temperature of 40° C. and a humidity of 90% RH is preferably less than 20 g / (m 2 ·day), more preferably less than 15g / (m 2 ·day), and more preferably less than 10g / (m 2 ·day). By setting the water vapor transmission rate within the above range, the multilayer structure of the present invention can maintain the light conversion efficiency for a long time. The water vapor transmission rate can be 0.1 g / (m 2 ·day) or above.
[0215] The method for obtaining the multilayer structure of the present invention includes, for example, extrusion lamination, dry lamination, co-injection molding, co-extrusion molding, etc. Co-extrusion molding includes, for example, co-extrusion lamination, co-extrusion sheet molding, co-extrusion film molding, co-extrusion tube molding, co-extrusion hose molding, co-extrusion blown film molding, co-extrusion blow molding, etc.
[0216] The sheets, films, preforms, etc. of the aforementioned multilayer structure obtained in this way can be reheated at a temperature below the melting point of the polymer contained therein, and uniaxially or biaxially stretched by thermoforming methods such as stretching molding, roll stretching, butterfly stretching, inflation stretching, blow molding, etc., to obtain stretched molded products.
[0217] The multilayer structure of the present invention can maintain the light conversion efficiency for a long time, so it can be effectively used as a light conversion film. The light conversion film refers to a functional film that absorbs light of a specific wavelength and emits light of a wavelength different from the absorption wavelength, mainly a film that converts short-wavelength light into long-wavelength light. The light conversion film of the present invention can maintain the light conversion efficiency for a long time, so it can also be used as an agricultural film used under conditions such as outdoor. In the case of using the multilayer structure of the present invention as an agricultural film, an organic light conversion material (D) that can absorb light in a specific wavelength range in sunlight and emit light in a specific wavelength range effective for plant growth is used, thereby forming an agricultural film that can effectively promote plant growth. Agricultural films include roofing materials for facility agriculture such as greenhouses, curtains set inside facility agriculture such as greenhouses, and other components for facility agriculture such as greenhouses; tunnel materials, etc. In addition, the agricultural film of the present invention can be attached to a glass surface, etc. When the agricultural film of the present invention is used as a roofing material comprising a two-layer greenhouse, it can be used as a greenhouse indoor film on the plant side, or as an outdoor film on the outside of the greenhouse. The agricultural film of the present invention may be in any shape as long as it can be used in greenhouse horticulture. The film may be cut into small pieces and woven into a net or woven fabric. Example
[0218] Hereinafter, the present invention will be described in more detail with reference to Examples, but the present invention is not limited to these Examples.
[0219] [Evaluation method]
[0220] (1) Acid value of acid-modified polyolefin
[0221] 400 mg of the acid-modified polyolefin used as a material was dissolved in 80 ml of xylene, and titrated with an ethanol solution of potassium hydroxide using phenolphthalein as an indicator according to the method described in JIS K0070: 1992 to determine the acid value. The concentration of the ethanol solution of potassium hydroxide was appropriately adjusted in the range of 0.005 to 0.5 mol / L according to the acid value.
[0222] (2) Quantification of phosphate ions and alkali metal ions
[0223] 0.5 g of the EVOH pellets obtained in the synthesis example or the resin composition pellets obtained in the examples and comparative examples are added to a Teflon (registered trademark) pressure-resistant container of ACTAC, and 5 mL of nitric acid for precision analysis of Wako Pure Chemical Industries, Ltd. is added. After standing for 30 minutes, a cover containing a bursting disc is added to the container, and the decomposition treatment is carried out using ACTAC's microgrid high-speed decomposition system "SpeedWave MWS-2" at 150°C for 10 minutes, followed by 180°C for 10 minutes. In the case of insufficient decomposition of the EVOH pellets, the treatment conditions are appropriately adjusted. Dilute with 10 mL of ion exchange water, transfer all the liquid to a 50 mL volumetric flask, and make up to volume with deionized water to obtain a decomposition solution. The above-mentioned decomposition solution is measured using the ICP atomic emission spectrometer "Optima 4300 DV" of Perkin Elmer Japan to quantify the phosphate ions and alkali metal ions.
[0224] (3) Quantification of carboxylic acid
[0225] 20 g of the EVOH pellets obtained in the synthesis example and the resin composition pellets obtained in the examples and comparative examples were put into 100 ml of deionized water and heated and extracted at 95°C for 6 hours. The extract was acid-base titrated with a 0.02 mol / L NaOH standard solution using phenolphthalein as an indicator to obtain the acid concentration. The value obtained by subtracting the above-quantified phosphate ion amount from the acid concentration obtained by titration was recorded as the carboxylic acid amount.
[0226] (4) Thermal stability and hue
[0227] The multilayer structures produced in Examples and Comparative Examples were continuously produced, and after being baked for 100 hours, their thermal stability and color were evaluated according to the following criteria.
[0228] (Thermal stability evaluation)
[0229] A: No streaks were observed in the multilayer structure.
[0230] B: Fine streaks are observed in the multilayer structure.
[0231] C: Streaks are observed in the multilayer structure.
[0232] (Hue Evaluation)
[0233] A: Colorless and transparent.
[0234] B: Slightly yellowish coloration.
[0235] C: Yellow coloration.
[0236] (5) Oxygen Transmission Rate (OTR)
[0237] The multilayer structures obtained in the examples and comparative examples were measured using an oxygen permeability measuring apparatus "OX-TRAN 2 / 20" (detection limit critical value 0.01 cc / (m 2 The oxygen transmission rate (OTR) was measured at 20°C and 65%RH according to the method described in ISO14663-2.
[0238] (6) Water vapor transmission rate
[0239] The water vapor transmission rates of the multilayer structures obtained in Examples and Comparative Examples were measured using a water vapor transmission rate measuring apparatus "PERMATRAN W3 / 33" manufactured by MOCON INC. at a temperature of 40° C. and a humidity of 90% RH in accordance with the method described in ISO 15106-1:2003.
[0240] (7) Peel strength
[0241] The multilayer structures obtained in the examples and comparative examples were humidified at 23°C and 50% RH, cut into pieces with a length of 150 mm in the longitudinal direction and 15 mm in the lateral direction, and the peel strength between the resin composition layer and its adjacent layer was measured in a T-type peeling mode using a tester "DCS-50M" produced by Shimadzu Corporation. The evaluation criteria were as follows.
[0242] A: Peel strength 1200 g / 15 mm or more
[0243] B: Peel strength 800 g / 15 mm or more and less than 1200 g / 15 mm
[0244] C: Peel strength 400 g / 15 mm or more and less than 800 g / 15 mm
[0245] D: Peel strength is less than 400 g / 15 mm.
[0246] (8) Exudation test
[0247] The multilayer structures obtained in Examples and Comparative Examples were stored under the conditions of 40° C. / 100% RH for 6 months. Thereafter, bleeding from the edges was confirmed visually and by touch, and the evaluation criteria were as follows.
[0248] A: No exudation occurred.
[0249] B: Slight bleeding was observed.
[0250] C: Significant bleeding was observed.
[0251] (9) Determination of absorption and emission spectra
[0252] For the multilayer structures obtained in the embodiments and comparative examples, the transmittance of the multilayer structures was measured using the integrating sphere module of a PerkinElmer Lambda750 UV-visible absorption spectrometer, and the test wavelength range was 700-200 nm. The absorption range of the photoconversion material was determined by comparing it with the transmittance spectrum of a blank film without any photoconversion material, and its absorption peak wavelength was recorded. The transient and steady-state fluorescence spectrometer FLS1000 of Edinburgh Steady State was used to measure the emission spectrum of the multilayer structure with the maximum absorption wave as the excitation wavelength, and the wavelength at the emission peak was recorded.
[0253] (10) Determination of light conversion efficiency (luminous intensity)
[0254] The luminous intensity of a film sample is equal to the product of the number of absorbed photons and the photoluminescence quantum efficiency; considering that the light source intensity of different devices or even the same device in different time periods will vary greatly, it will also cause changes in the luminous intensity of the film sample (device-induced errors), so using luminous intensity to examine the light conversion capacity of the film has a certain deviation. Therefore, the light conversion efficiency is defined as a measure of the light conversion capacity of the film instead of the luminous intensity.
[0255] Light conversion efficiency at the measured wavelength = light absorption rate of the film sample at that wavelength × photoluminescence quantum efficiency
[0256] For the multilayer structures obtained in the embodiments and comparative examples, the light transmittance of the multilayer structures was measured using the integrating sphere module of the PerkinElmer Lambda750 UV-visible absorption spectrometer; the light absorptivity of the film sample at this wavelength was defined as the difference between the baseline light transmittance of the multilayer structure (such as the light transmittance at 700nm) and the light transmittance at the measured wavelength; the steady-state and transient fluorescence spectrometer FLS1000 of Edinburgh Steady State was used to test the photoluminescence quantum efficiency of the film sample under excitation at this wavelength through the quantum yield test module. According to the above formula, the product of the two is the light conversion efficiency of the film sample at a certain wavelength.
[0257] (11) UV accelerated aging evaluation
[0258] The multilayer structures obtained in the examples and comparative examples were irradiated with UVA340 ultraviolet lamp at a temperature of 50°C using a light irradiation device ultraviolet aging instrument produced by Shanghai Guangpin Testing Equipment Manufacturing Co., Ltd., with an irradiation intensity of 0.68 W / m 2 / nm@340nm, the time it takes for the light conversion efficiency to decay by 50% after accelerated aging is the half-life. If the initial light conversion efficiency is maintained at more than 50% for more than 80 hours, it is expressed as a half-life of >80 h. The light conversion efficiency decay rate is calculated using the following formula.
[0259] Light conversion efficiency decay rate (%) = (initial light conversion efficiency - light conversion efficiency after any time) / (initial light conversion efficiency) × 100.
[0260] (12) Growth of vegetables
[0261] Multiple greenhouses were set up for comparative tests. Adjacent plots of the same base were selected. The size of the test field was 60*80 m (length*width). Three plots were selected in each greenhouse for the test using the equidistant sampling method. Each plot contained three rows of plants. The planting varieties were consistent, the spacing was consistent, and the management methods such as fertilization and irrigation were consistent.
[0262] Green peppers were planted using the multilayer structures obtained in Example 1 and Comparative Examples 1, 2, and 4, and the ratio of the yield per unit area was calculated based on the actual yield in Example 1. The results are shown in Table 3.
[0263] [Materials used in Examples and Comparative Examples]
[0264] Thermoplastic resin (E)
[0265] UF943: "Novatec (trademark) UF943" (LLDPE, manufactured by Japan Polyethylene Co., Ltd.)
[0266] Organic photoconversion materials (D)
[0267] D1: Agrilumino B2 (as shown in Formula XXIX, organic fluorescent dye, molecular weight 518, Suzhou Ruiersi Technology Co., Ltd.)
[0268] D2: Agrilumino R7 (as shown in Formula XXIV, an organometallic complex, molecular weight 812, produced by Suzhou Ruiers Technology Co., Ltd.)
[0269] D'1: 4-Hydroxycoumarin (organic fluorescent dye, molecular weight 162, manufactured by Tokyo Chemical Industry Co., Ltd.)
[0270] Adhesive resin (F)
[0271] NF617: "Admer (trademark) NF617" (carboxylic acid-modified LLDPE, acid value 3.8 mgKOH / g, manufactured by Mitsui Chemicals, Inc.)
[0272] The acid value of the carboxylic acid-modified LLDPE (acid-modified polyolefin) was measured by the method described in the above-mentioned evaluation method (1).
[0273] [Synthesis of EVOH Pellets (EVOH(C))]
[0274] <Synthesis example 1>
[0275] Hydrous EVOH pellets having an ethylene unit content of 32 mol%, a saponification degree of 99.9 mol%, and a water content of 50% were added to an aqueous solution containing phosphoric acid, acetic acid, and sodium acetate, and immersed while stirring at 25°C for 6 hours, and then dehydrated, dried at 80°C for 4 hours using a hot air dryer ("DN6101" manufactured by Yamato Scientific Co., Ltd.), and then dried at 120°C for 40 hours to obtain EVOH pellets EVOH (C1) having a water content of 0.25%. It should be noted that the concentrations of the aqueous solution of phosphoric acid, acetic acid, and sodium acetate can be appropriately adjusted so that the contents of phosphate ions and alkali metal ions in the final EVOH (C1) pellets reach the contents described in Synthesis Example 1 in Table 1, and the acetic acid content reaches 100 ppm. For the obtained EVOH (C1), the phosphate ions and alkali metal ions were quantitatively determined according to the method described in the above evaluation method (2), and the results were 110 ppm and 200 ppm, respectively; the carboxylic acid content was quantitatively determined according to the method described in the above evaluation method (3), and the result was 100 ppm.
[0276] <Synthesis Examples 2~6>
[0277] The concentration of the aqueous solution containing phosphoric acid and sodium acetate was appropriately adjusted so that the contents of phosphate ions and alkali metal ions contained in the obtained EVOH pellets reached the requirements described in Table 1. EVOH pellets (EVOH (C2) to EVOH (C6)) were prepared and evaluated by the same method as in Synthesis Example 1. The results are shown in Table 1. It should be noted that the amount of carboxylic acid (acetic acid) was 100 ppm.
[0278] <Synthesis Example 7>
[0279] EVOH pellets (EVOH (C7)) were prepared and evaluated by the same method as in Synthesis Example 1 except that potassium acetate was used instead of sodium acetate and the concentration of the aqueous solution containing phosphoric acid and potassium acetate was appropriately adjusted so that the contents of phosphate ions and alkali metal ions contained in the obtained EVOH pellets met the requirements described in Table 1. The results are shown in Table 1. It should be noted that the amount of carboxylic acid (acetic acid) was 100 ppm.
[0280] Table 1
[0281] .
[0282] [Example]
[0283] <Example 1>
[0284] 99 parts by mass of EVOH pellets (EVOH (C1)) and 1 part by mass of an organic light conversion material (D1) were mixed and melt-kneaded under the conditions of the extruder shown below to obtain resin composition A1 pellets. For the obtained resin composition A1 pellets, phosphate ions and alkali metal ions were quantified according to the method described in the above evaluation method (2), and carboxylic acids were quantified according to the method described in the above evaluation method (3). The results are shown in Table 2.
[0285] (Extruder conditions)
[0286] Extruder: Toyo Seiki Co., Ltd. twin-screw extruder "LABOPLASTOMIL"
[0287] Screw diameter: 25
[0288] Screw speed: 100 rpm
[0289] Feeder speed: 80 rpm.
[0290] Barrel and die temperature settings: C1 / C2 / C3 / C4 / C5 / die=180℃ / 210℃ / 220℃ / 220℃ / 220℃ / 220℃
[0291] A material (Ad) obtained by mixing resin composition A1 pellets, linear low-density polyethylene "Novatec (trademark) UF943" (LLDPE), carboxylic acid-modified LLDPE "Admer (trademark) NF617" and linear low-density polyethylene "Novatec (trademark) UF943" in a ratio of 25 / 75 parts by mass was formed into films under the following film-forming conditions to obtain three types of five-layer multilayer structures (layer (Y) / adhesive layer (Z) / layer (X) / adhesive layer (Z) / layer (Y) = LLDPE / Ad / A1 / Ad / LLDPE = 20 μm / 20 μm / 20 μm / 20 μm / 20 μm). It should be noted that the film-forming equipment has a temperature-controllable traction roller behind an extruder having a film-forming die, and the obtained multilayer structure is wound up by a winder to obtain the multilayer structure of Example 1.
[0292] (Film Forming Conditions)
[0293] Extruder for resin composition (A1): Single screw extruder (Testing machine ME type CO-EXT, manufactured by Toyo Seiki Seisaku-sho)
[0294] Caliber 20 , L / D=20, full thread screw
[0295] Supply section / compression section / metering section / die head = 175 / 210 / 220 / 220℃
[0296] Extruder for LLDPE: Single screw extruder (GT-32-A, manufactured by Research Laboratory of Plastics Technology Co., Ltd.)
[0297] Caliber 32 , L / D=28, full thread screw
[0298] Supply section / compression section / metering section / die head = 150 / 200 / 210 / 220℃
[0299] Extruder for Ad: Single screw extruder (SZW20GT-20MG-STD, TECHNOVEL CORPORATION)
[0300] Caliber 20 , L / D=20, full thread screw
[0301] Supply section / compression section / metering section / die head = 150 / 200 / 220 / 220 ℃
[0302] Die: 300 mm hanger die (Research Laboratory of Plastics Technology Co., Ltd.)
[0303] Pulling roller temperature: 80°C.
[0304] The obtained multilayer structure was tested and evaluated for thermal stability and hue, oxygen permeability, water vapor permeability, peel strength, exudation test, absorption spectrum and emission spectrum, light conversion efficiency, and ultraviolet aging performance according to the methods described in the above evaluation methods (4) to (11). The results are shown in Tables 2 and 3.
[0305] <Examples 2 to 11, Comparative Examples 1 to 5>
[0306] Resin composition pellets A2 to A11, AC1 to AC5 and multilayer structures were prepared by the same method as in Example 1. The type and content of EVOH (C), the content of thermoplastic resin (E), and the type and content of organic light conversion material (D) in the resin composition pellets A2 to A11 and AC1 to AC5 are shown in Table 2. For the obtained resin composition pellets A2 to A11 and AC1 to AC5, phosphate ions and alkali metal ions were quantified according to the method described in the above evaluation method (2), and carboxylic acid was quantified according to the method described in the above evaluation method (3). The results are shown in Table 2. For the obtained multilayer structure, thermal stability and hue, oxygen permeability, water vapor permeability, peel strength, exudation test, absorption spectrum and emission spectrum wavelength, luminescence conversion efficiency, and ultraviolet aging performance were evaluated according to the methods described in the above evaluation methods (4) to (11).
[0307] In Examples 1 and 11 and Comparative Examples 1 and 2, evaluations related to the degree of growth of vegetables were performed according to the method described in the above-mentioned evaluation method (12). The results are shown in Table 3.
[0308]
[0309]
[0310] <Example 12>
[0311] A multilayer structure was prepared by a method similar to that of Example 1. The thicknesses of layer (X) and layer (Z) were changed as shown in Table 4. The obtained multilayer structure was tested and evaluated for thermal stability and hue, oxygen permeability, water vapor permeability, peel strength, bleed test, light conversion efficiency, and ultraviolet aging performance according to the methods described in the above evaluation methods (4) to (11). The results are shown in Table 4.
[0312] <Example 13>
[0313] The film-making conditions of Example 1 (stopping the extruder for Ad) were such that a material obtained by mixing carboxylic acid-modified LLDPE "Admer (trademark) NF617" and linear low-density polyethylene "Novatec (trademark) UF943" in a ratio of 25:75 parts by mass formed layer (Y), and two kinds of three-layer multilayer structures (layer (Y) / A1 / layer (Y) = 40 μm / 20 μm / 40 μm) were prepared by the same method as in Example 1 and evaluated. The obtained multilayer structures were tested and evaluated for thermal stability and hue, oxygen permeability, water vapor permeability, peel strength, seepage test, light conversion efficiency, and ultraviolet aging performance according to the methods described in the above-mentioned evaluation methods (4) to (11). The results are shown in Table 4.
[0314] <Example 14>
[0315] EVOH pellets (EVOH (C1)) 75 parts by mass, carboxylic acid-modified LLDPE "Admer (trademark) NF617" 24 parts by mass, and organic fluorescent dye D1 1 part by mass as an organic light conversion material (D) were mixed and melt-kneaded under the same conditions as in Example 1 to obtain resin composition A12 pellets. The phosphate ions and alkali metal ions of the obtained resin composition A12 pellets were quantified according to the method described in the above evaluation method (2), and the phosphate ions were 83 ppm and the alkali metal ions were 150 ppm. The carboxylic acid content was quantified according to the method described in the above (3), and the carboxylic acid content was 35 ppm.
[0316] Instead of the pellets of the resin composition A1, the pellets of the resin composition A12 were used, and the linear low-density polyethylene "Novatec (trademark) UF943" was used as the layer (Y) to prepare a 3-layer multilayer structure similar to that of Example 12 (layer (Y) / A11 / layer (Y) = 40 μm / 20 μm / 40 μm). The multilayer structure was prepared and evaluated by the same method as in Example 12. The results are shown in Table 4.
[0317] <Example 15>
[0318] Using the resin composition A1 pellets (A1), a single-layer film having a thickness of 20 μm of layer (X) was prepared under the film-forming conditions shown below. The obtained single-layer film was tested and evaluated for thermal stability and hue, oxygen permeability, water vapor permeability, peel strength, bleed test, light conversion efficiency, and ultraviolet aging performance according to the methods described in the above evaluation methods (4) to (11). The results are shown in Table 4.
[0319] (Film Forming Conditions)
[0320] Single screw extruder: (D2020, Toyo Seiki Co., Ltd.)
[0321] Caliber 20 , L / D=20, full thread screw
[0322] C1 / C2 / C3 / die head=180 / 220 / 220 / 220℃
[0323] Die head: 300 mm hanger type die head
[0324] Pulling roller temperature: 80°C.
[0325]
[0326] <Example 16>
[0327] 99 parts by mass of EVOH pellets (EVOH (C1)) and 0.5 parts by mass of organic fluorescent dye D1 and 0.5 parts by mass of D2 as organic light conversion materials (D) were mixed and melt-kneaded under the same conditions as in Example 1 to obtain resin composition A13 pellets. The phosphate ion and alkali metal ion content of the obtained resin composition A13 pellets were quantified according to the method described in the above evaluation method (2), and the phosphate ion content was measured to be 109 ppm and the alkali metal ion content was measured to be 196 ppm. The carboxylic acid content was quantified according to the method described in the above (3), and the carboxylic acid content was measured to be 48 ppm.
[0328] A multilayer structure was prepared and evaluated by using the resin composition A13 pellets instead of the resin composition A1 pellets in the same manner as in Example 1. The results are shown in Table 4.
Claims
1. A resin composition comprising an ethylene-vinyl alcohol copolymer (C) and an organic light conversion material (D) having a molecular weight of 200 or more, The content of the ethylene-vinyl alcohol copolymer (C) is 50 wt% or more and 99.99 wt% or less, The content of the organic light conversion material (D) is 0.01 wt % or more and 1 wt % or less, The proportion of the ethylene-vinyl alcohol copolymer (C) and the organic light conversion material (D) in the resin composition is more than 90 wt %, and the total content of each component is 100 wt %. The ethylene-vinyl alcohol copolymer (C) has an ethylene unit content of 20 mol% or more and 60 mol% or less, a saponification degree of 90 mol% or more, The absorption spectrum and luminescence spectrum of the organic light conversion material (D) measured according to the method described in GB / T 9721-2006 and JY / T 0571-2020 have at least one absorption peak wavelength of the absorption spectrum in the range of 300nm-600nm, and at least one emission peak wavelength of the luminescence spectrum in the range of 400-800nm, The resin composition comprises 5 ppm or more and 200 ppm or less of a phosphoric acid compound (a1) in terms of phosphate radical, and 10 ppm or more and 400 ppm or less of an alkali metal salt (a2) in terms of metal atom, The phosphate-converted mass W of the phosphate compound (a1) a1 The mass W converted to metal atoms of the alkali metal salt (a2) a2 The mass ratio W a1 / W a2 It is 0.01 or more and 2 or less.
2. A resin composition comprising an ethylene-vinyl alcohol copolymer (C), an organic light conversion material (D) having a molecular weight of 200 or more, and a thermoplastic resin (E), The content of the ethylene-vinyl alcohol copolymer (C) is 50 wt% or more and 99.99 wt% or less, The content of the organic light conversion material (D) is 0.01 wt % or more and 1 wt % or less, The thermoplastic resin (E) is a thermoplastic resin different from the ethylene-vinyl alcohol copolymer (C), and its content is 1 wt% or more and 49.99 wt% or less, The total content of each component is 100wt%, The ethylene-vinyl alcohol copolymer (C) has an ethylene unit content of 20 mol% or more and 60 mol% or less, a saponification degree of 90 mol% or more, The absorption spectrum and luminescence spectrum of the organic light conversion material (D) measured according to the method described in GB / T 9721-2006 and JY / T 0571-2020 have at least one absorption peak wavelength of the absorption spectrum in the range of 300nm-600nm, and at least one emission peak wavelength of the luminescence spectrum in the range of 400-800nm, The resin composition comprises 5 ppm or more and 200 ppm or less of a phosphoric acid compound (a1) in terms of phosphate radical, and 10 ppm or more and 400 ppm or less of an alkali metal salt (a2) in terms of metal atom, The phosphate-converted mass W of the phosphate compound (a1) a1 The mass W converted to metal atoms of the alkali metal salt (a2) a2 The mass ratio W a1 / W a2 It is 0.01 or more and 2 or less.
3. The resin composition according to claim 1 or 2, wherein The ethylene unit content of the ethylene-vinyl alcohol copolymer (C) is 22 mol% or more and 55 mol% or less, and the saponification degree is 95 mol% or more.
4. The resin composition according to claim 1 or 2, comprising 8 ppm or more and 100 ppm or less of the phosphoric acid compound (a1) in terms of phosphate radical conversion, and 20 ppm or more and 350 ppm or less of the alkali metal salt (a2) in terms of metal atom conversion, wherein the phosphate radical conversion mass W of the phosphoric acid compound (a1) is a1 The mass W converted to metal atoms of the alkali metal salt (a2) a2 The mass ratio W a1 / W a2 It is 0.05 or more and 1.5 or less.
5. The resin composition according to claim 2, wherein The resin composition contains 10 to 49.99 wt% of a thermoplastic resin (E) different from the ethylene-vinyl alcohol copolymer (C).
6. The resin composition according to claim 1 or 2, wherein The organic light conversion material (D) includes at least one selected from the group consisting of an organic metal complex and an organic fluorescent dye.
7. The resin composition according to claim 6, wherein The aforementioned organometallic complex contains a rare earth element.
8. The resin composition according to claim 7, wherein The rare earth element is europium or terbium.
9. The resin composition according to claim 7, wherein The aforementioned organometallic complex is A m Ln(La) x (Lb) y B n or A m Ln(Lc) z B n In the metal complex shown, A is a positive monovalent counter cation, B is a negative monovalent counter anion, La is an anionic bidentate ligand, Lb is a neutral ligand, Lc is a tridentate ligand, and Ln is a positive trivalent rare earth metal ion; wherein x=any one of 0 to 4, y=any one of 0 to 4, and x+y=4 or 5; z=any one of 1 to 3; m=any one of 0 to 3, and n=any one of 0 to 3.
10. The resin composition according to claim 9, wherein The aforementioned organometallic complex is Ln(La)3(Lb) y The organometallic complex shown, y = 1 or 2, La is at least one selected from the following general formulas I to II, Lb is at least one selected from the following general formulas VII to XI, In formula I, R1, R2, R3, R4 and R5 are respectively a hydrogen atom, a halogen atom, a cyano group, an alkyl group or a haloalkyl group; in formula II, R1 and R2 are respectively an aromatic group, an alkyl group or a haloalkyl group; in formula VII, formula VIII, formula IX and formula XI, R1, R2, R3, R4 and R5 are respectively an alkyl group or an aromatic group.
11. The resin composition according to claim 9, wherein The aforementioned organometallic complex is an organometallic complex represented by ALn(La)4, A is an alkali metal ion or an organic amine ion, and La is at least one selected from the following general formulas I to II, In formula I, R1, R2, R3, R4 and R5 are respectively a hydrogen atom, a halogen atom, a cyano group, an alkyl group or a halogenated alkyl group; in formula II, R1 and R2 are respectively an aromatic group, an alkyl group or a halogenated alkyl group.
12. The resin composition according to claim 9, wherein The aforementioned organometallic complex is an organometallic complex represented by Ln(Lc)3, Lc is at least one selected from the following general formula XII or XIII, In Formula XII, R1, R2, and R3 are each independently a structure shown in the figure, and R4 and R5 are each independently an alkyl group or an aromatic group; In formula XIII, R1, R2, R3, and R4 are each independently a hydrogen atom, a halogen atom, a cyano group, an alkyl group, or a halogen-substituted alkyl group; R5 is the structure shown in the figure; and R6 is an alkyl group, an aromatic group, or a hydroxyl group.
13. The resin composition according to claim 6, wherein The aforementioned organic fluorescent dye is a compound represented by the following general formula XIV to XXI, In Formula XVIII, R1 and R2 are each a hydrogen atom, a hydroxyl group, an amino group, an alkoxy group or an alkyl-substituted amino group, and R3 is a hydrogen atom or an alkyl group; In Formula XIX, R1, R2, R3, R4, R5 and R6 are each a hydrogen atom or an alkyl group, R7 and R8 are each independently a hydrogen atom, a carboxyl group, an ester group or a sulfonate group, and X is a halogen counter anion, and the halogen counter anion refers to a fluoride ion, a chloride ion, a bromide ion or an iodide ion; In formula XX, R1, R2 and X are hydrogen atom, halogen, nitro or alkoxy respectively; In Formula XXI, R1, R2, R3, R4, R5, R6, R7, R8, R9, R 10 , R 11 and R 12 are respectively a hydrogen atom, an alkyl group or an aromatic group, M is hydrochloric acid, hydrobromic acid or hydroiodic acid; and X is a halogen counter anion, including fluoride ion, chloride ion, bromide ion or iodide ion.
14. The resin composition according to claim 1 or 2, wherein The aforementioned organic light conversion material (D) is an organic metal complex or compound represented by the following general formula XXII to XXXI, 15 . A multilayer structure comprising at least one layer (X) composed of the resin composition according to claim 1 , and a layer (Y) comprising a thermoplastic resin (B). 16 . The multilayer structure according to claim 15 , which has a structure in which the layer (Y) is laminated on at least one surface of the layer (X) via an adhesive layer (Z) containing an adhesive resin (F).
17. The multilayer structure according to claim 16, wherein The adhesive resin (F) is an acid-modified polyolefin resin, and the acid value of the acid-modified polyolefin resin is 1.5 mgKOH / g or more. 18 . The multilayer structure according to claim 15 , which has a structure in which the layer (X) and the layer (Y) are directly laminated.
19. The multilayer structure according to any one of claims 15 to 18, wherein The aforementioned layer (Y) contains an unmodified polyolefin resin.
20. The multilayer structure according to any one of claims 15 to 18, wherein The aforementioned layer (Y) contains an acid-modified polyolefin resin.
21. The multilayer structure according to any one of claims 15 to 18, wherein The peel strength between the layer (X) and the layer adjacent to the layer (X) is 400 g / 15 mm or more.
22. The multilayer structure according to any one of claims 15 to 18, wherein The oxygen permeability measured according to the method described in ISO14663-2 under the conditions of temperature 20°C and humidity 65% RH is 100cc / (m 2 ·day·atm) or less.
23. The multilayer structure according to any one of claims 15 to 18, wherein The water vapor transmission rate measured by the method described in ISO 15106-1:2003 at a temperature of 40°C and a humidity of 90% RH is less than 20 g / (m 2 ·day). 24 . A light conversion film comprising the multilayer structure according to claim 15 .
25. An agricultural film comprising the multilayer structure according to any one of claims 15 to 23.