Backing material, backing and preparation method thereof for air-coupled piezoelectric ultrasonic probe
By using open-pore structure backing material composed of E51 epoxy resin and sodium glutamate, the problem of bandwidth and sensitivity balance of air-coupled piezoelectric ultrasonic probe backing is solved, and the lower acoustic impedance and high acoustic attenuation are achieved, which suppresses the rest of the world Vibration, improving the bandwidth and sensitivity of the probe.
Patent Information
- Application Number
- CN202210918013.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-01
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2042-08-01
AI Technical Summary
The backing of the air-coupled piezoelectric ultrasonic probe is difficult to balance the relationship between bandwidth, resolution and sensitivity. The sensitivity of existing materials will decrease when increasing the bandwidth, and the residual vibration is longer, making it difficult to effectively suppress it.
The backing material consisting of E51 epoxy resin, curing agent and sodium glutamate is prepared by heating, vacuum defoaming, drying and grinding. The acoustic impedance is between 3.0 and 3.5MPa·s /m, the acoustic attenuation coefficient is 10-35dB/cm, which suppresses residual vibration and increases bandwidth.
It realizes lower acoustic impedance and high sensitivity, reduces the influence of reflected ultrasonic waves, increases bandwidth, reduces the size of the probe, effectively suppresses residual vibration, and improves the quality of narrow pulse signals.
Smart Images

Figure CN115508456B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of ultrasonic technology, and in particular to a backing material, a backing and a preparation method thereof applied to an air-coupled piezoelectric ultrasonic probe. Background Art
[0002] As a non-destructive testing technology, ultrasonic testing has a wide range of applications in the fields of medical treatment, food, and new energy. As one of the core components of ultrasonic testing technology, the piezoelectric ultrasonic probe can realize the mutual conversion between electrical signals and acoustic signals. The quality of its performance plays a decisive role in the ultrasonic testing results. Among them, the air-coupled ultrasonic probe, as a non-contact detection device, does not require a coupling agent compared to traditional ultrasonic probes, so it is easy to use and has good applicability and is widely concerned. The air-coupled piezoelectric ultrasonic probe consists of a matching layer, a piezoelectric element, and a backing. The piezoelectric element is the core component of the air-coupled ultrasonic probe, which affects the operating frequency, working efficiency, sensitivity, impedance characteristics, etc. of the probe.
[0003] The impedance of the matching layer and the backing needs to match the impedance of the piezoelectric element, which is conducive to the piezoelectric element receiving the ultrasonic signal and promoting the imaging quality of the probe. The backing needs to absorb the ultrasonic waves emitted backward by the piezoelectric element and increase the bandwidth of the transducer. The backing uses the damping effect to stop the vibration of the chip as soon as possible, and absorbs the ultrasonic waves generated by the piezoelectric element to the back, so that the ultrasonic waves are scattered and attenuated, reducing the influence of the reflected ultrasonic waves on the back on the ultrasonic signals emitted forward, and promoting the imaging of the probe. The backing also affects the bandwidth and sensitivity of the probe. Generally speaking, the closer the acoustic impedance of the backing material is to the acoustic impedance of the piezoelectric element, the higher the bandwidth can be obtained, but it will lead to reduced sensitivity. In order to balance the bandwidth and sensitivity, air-coupled piezoelectric ultrasonic probes generally use air backing. This method has a large sensitivity, but the residual vibration is long and the bandwidth is narrow. At present, it is difficult for the backing of air-coupled piezoelectric ultrasonic probes to balance the relationship between bandwidth, resolution and sensitivity. Summary of the invention
[0004] The purpose of the present invention is to provide an air-coupled piezoelectric ultrasonic probe backing material and a preparation method thereof in view of the deficiencies in the prior art, which has suitable acoustic impedance, high acoustic attenuation, suppresses the generation of residual vibration, increases the bandwidth of the probe and has good sensitivity.
[0005] A backing material used for an air-coupled piezoelectric ultrasonic probe consists of the following components in percentage by mass: 40-70 wt % of E51 epoxy resin, 10-20 wt % of a curing agent, and 20-40 wt % of sodium glutamate.
[0006] Furthermore, the backing material is composed of the following components in percentage by mass: 48 wt % of E51 epoxy resin, 16 wt % of curing agent, and 36 wt % of sodium glutamate.
[0007] A backing used for an air-coupled piezoelectric ultrasonic probe is formed from the backing material mentioned above.
[0008] Furthermore, under the test conditions of a temperature of 20° C. and a frequency of 400 kHz, the acoustic impedance of the backing material is 3.0 to 3.5 MPa·s / m, and the acoustic attenuation coefficient is 10 to 35 dB / cm.
[0009] The method for preparing the backing used for the air-coupled piezoelectric ultrasonic probe comprises the following steps:
[0010] (1) Mixing: Heat E51 epoxy resin to 60°C, add curing agent and sodium glutamate, and stir evenly to obtain a suspension;
[0011] (2) Degassing: Place the suspension in a vacuum drying oven at 0.08 MPa for 15 min to remove bubbles;
[0012] (3) Preparation of backing: The piezoelectric ceramic sheet is placed in a mold, and then the suspension after air bubbles are removed is poured into the mold, and the E51 epoxy resin is cured by drying at 80° C. for 3 h to obtain the backing of the piezoelectric ceramic sheet, and then the backing is polished;
[0013] (4) Open-hole preparation: The polished ceramic sheet composited with the backing is placed in warm water, and the sodium glutamate in the backing is dissolved, thereby obtaining a backing with an open-hole structure for use in an air-coupled piezoelectric ultrasonic probe.
[0014] Compared with the prior art, the effective effects of the present invention are:
[0015] 1. The backing with an open-pore structure prepared by the present invention has lower acoustic impedance and higher sensitivity.
[0016] 2. The backing with open-pore structure has large sound scattering and sound attenuation, which effectively reduces the influence of reflected ultrasound on the back side on the ultrasonic signal emitted forward. Large sound attenuation avoids the backing layer from being too thick, thus reducing the size of the ultrasonic probe.
[0017] 3. Compared with the air backing used in air-coupled ultrasonic probes, the backing with open-pore structure has an acoustic impedance closer to that of piezoelectric elements and a wider bandwidth.
[0018] 4. The backing with openings can effectively suppress the residual vibration of the piezoelectric element, increase the bandwidth, and obtain the required narrow pulse signal. The backing and the piezoelectric element are pressed against each other to reduce Q. m , further increasing the bandwidth of the air-coupled ultrasound probe.
[0019] 5. Use the self-sacrificial template method to prepare a backing with an open-pored structure, pour the suspension into the mold, and obtain the desired size after solidification, which reduces mechanical processing and facilitates the preparation and molding of the backing with an open-pored structure. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 is a physical picture of the backing prepared in Example 2 of the present invention;
[0021] Figure 2 is a graph of porosity and sound attenuation of a backing prepared by the present invention;
[0022] Figure 3 It is the time domain and frequency domain diagram of the air-backed transducer echo signal;
[0023] Figure 4 3 and 4 are time domain and frequency domain diagrams of the backing transducer echo signal prepared in Example 2 of the present invention. DETAILED DESCRIPTION
[0024] In order to further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples. However, it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, rather than limiting the claims of the present invention.
[0025] The reagents or instruments used in the present invention without indicating the manufacturer are all conventional products that can be purchased from the market.
[0026] Example 1
[0027] Step 1: Mixing
[0028] Weigh 40g of E51 epoxy resin, 20g of curing agent, and 40g of sodium glutamate, heat the E51 epoxy resin to 60°C to improve its fluidity, then add the curing agent and sodium glutamate in sequence, stir evenly, so that part of the sodium glutamate is on the edge of the resin and the sodium glutamate particles are in contact with each other, so that they are interconnected to form a suspension;
[0029] Step 2: Remove bubbles
[0030] The suspension was placed in a vacuum drying oven at room temperature and vacuumed for 15 min at a vacuum degree of 0.08 MPa to remove bubbles in the suspension;
[0031] Step 3: Backing Preparation
[0032] The defoamed suspension was poured into a mold with a piezoelectric ceramic sheet, and placed in a drying oven at 80°C for curing for 3 hours. The E51 epoxy resin was cured to obtain a backing of the piezoelectric ceramic sheet. The backing was polished to remove the resin layer on the surface, exposing the sodium glutamate to facilitate the subsequent dissolution of the sodium glutamate template.
[0033] Step 4: Opening preparation
[0034] The polished piezoelectric ceramic sheet composited with the backing was placed in 90° C. warm water and allowed to stand for 2 hours to allow the sodium glutamate to fully dissolve, thereby obtaining a backing with an open-pore structure for use in an air-coupled piezoelectric ultrasonic probe.
[0035] Under the test conditions of temperature 20°C and frequency 400 kHz, the acoustic impedance of the prepared backing was measured to be 3.0 MPa·s / m, and the acoustic attenuation coefficient was 35.0 dB / cm.
[0036] Example 2
[0037] The difference from Example 1 is that in the first step, 48 g of E51 epoxy resin, 16 g of curing agent, and 36 g of sodium glutamate are weighed.
[0038] Under the test conditions of temperature 20° C. and frequency 400 kHz, the acoustic impedance of the prepared backing was measured to be 3.2 MPa·s / m, and the acoustic attenuation coefficient was 25.0 dB / cm.
[0039] Example 3
[0040] The difference from Example 1 is that in the first step, 60 g of E51 epoxy resin, 10 g of curing agent, and 30 g of sodium glutamate are weighed.
[0041] Under the test conditions of temperature 20° C. and frequency 400 kHz, the acoustic impedance of the prepared backing was measured to be 3.3 MPa·s / m, and the acoustic attenuation coefficient was 18.0 dB / cm.
[0042] Example 4
[0043] The difference from Example 1 is that in the first step, 70 g of E51 epoxy resin, 10 g of curing agent, and 20 g of sodium glutamate are weighed.
[0044] Under the test conditions of temperature 20° C. and frequency 400 kHz, the acoustic impedance of the prepared backing was measured to be 3.5 MPa·s / m, and the acoustic attenuation coefficient was 10.0 dB / cm.
[0045] Figure 1 : It can be seen that the prepared porous backing surface has a large number of interconnected open pores, which can achieve lower acoustic impedance and higher acoustic attenuation.
[0046] Figure 2: The porosity of backings with different contents of sodium glutamate in four groups of embodiments was studied, among which the porosity of the backing was nearly linearly related to the amount of sodium glutamate added. The amounts of sodium glutamate added to the four components were 20 wt%, 30 wt%, 36 wt%, and 40 wt%, respectively. The relationship between the porosity of the porous backing and sound attenuation was determined. With the increase of porosity, the sound attenuation gradually increased, but after the porosity reached a certain level, the increase in sound attenuation slowed down.
[0047] Figure 3 , Figure 4 They are respectively the echo time domain and frequency domain signal diagrams of the air backing probe and the echo time domain and frequency domain signal diagrams of the porous backing probe of the present invention. From the time domain signal, it can be seen that although the addition of the porous backing reduces the amplitude of the signal received by the probe and reduces the sensitivity, the reduction in vibration time effectively suppresses the residual vibration of the piezoelectric element and improves the efficiency of the probe. From the frequency domain signal, it can be seen that the addition of the porous backing increases the bandwidth of the probe from 20% to 29%. The porous backing effectively increases the bandwidth of the probe. The bandwidth calculation formula is as follows:
[0048]
[0049] f C Probe operating frequency, f L The low frequency point corresponding to the highest peak value in the frequency domain dropping by 6dB, f H The high frequency domain point corresponding to a 6dB rise in the highest peak value in the frequency domain.
[0050]
[0051] BW -6dB Relative bandwidth of ultrasonic transducers.
[0052] It can be seen that the porous backing structure of the present invention has lower acoustic impedance and higher sensitivity.
[0053] The open-pore structure backing has large sound scattering and sound attenuation, which effectively reduces the impact of reflected ultrasound on the forward-transmitted ultrasonic signal. Large sound attenuation prevents the backing layer from being too thick, thus reducing the size of the ultrasonic probe.
[0054] Compared with the air backing used in air-coupled ultrasound probes, the backing with an open-pore structure has an acoustic impedance closer to that of piezoelectric elements and a wider bandwidth.
[0055] The backing with holes can effectively suppress the residual vibration of the piezoelectric element, increase the bandwidth, and obtain the required narrow pulse signal. The backing and the piezoelectric element are pressed against each other to reduce the Q m , further increasing the bandwidth of the air-coupled ultrasound probe.
[0056] According to the explanation of the above description, those skilled in the art to which the present invention belongs may also make appropriate changes and modifications to the above embodiments. Therefore, the present invention is not limited to the specific embodiments disclosed and described above, and some modifications and changes to the present invention should also fall within the scope of protection of the claims of the present invention. In addition, although some specific terms are used in this specification, these terms are only for the convenience of description and do not constitute any limitation to the present invention.
Claims
1. A backing material for an air-coupled piezoelectric ultrasonic probe, characterized in that: The invention is composed of the following components in percentage by mass: 48 wt % of E51 epoxy resin, 16 wt % of curing agent and 36 wt % of sodium glutamate.
2. A backing for an air-coupled piezoelectric ultrasonic probe, characterized in that: The backing is formed of the backing material of claim 1 .
3. The backing for an air-coupled piezoelectric ultrasonic probe according to claim 2, characterized in that: Under the test conditions of a temperature of 20° C. and a frequency of 400 kHz, the acoustic impedance of the backing material is 3.0 to 3.5 MPa•s / m, and the acoustic attenuation coefficient is 10 to 35 dB / cm.
4. A method for preparing a backing for an air-coupled piezoelectric ultrasonic probe according to claim 2 or 3, characterized in that: The steps include: (1) Mixing: Heat E51 epoxy resin to 60°C, add curing agent and sodium glutamate, stir evenly to obtain a suspension; (2) Degassing: Place the suspension in a vacuum drying oven at 0.08 MPa for 15 min to remove bubbles; (3) Preparation of backing: Place the piezoelectric ceramic sheet into a mold, then pour the suspension after removing bubbles into the mold, dry it at 80°C for 3 hours to solidify the E51 epoxy resin, obtain the backing of the piezoelectric ceramic sheet, and then polish the backing; (4) Open-pore preparation: The polished ceramic sheet composited with the backing is placed in warm water, and the sodium glutamate in the backing is dissolved to obtain a backing with an open-pore structure for use in an air-coupled piezoelectric ultrasonic probe.