A tungsten skeleton and its preparation method and use
The preparation of tungsten skeletons through three-stage hot pressing sintering method solves the problems of complex and low purity of existing tungsten copper alloys, achieves high purity and uniformity, is suitable for industrial production, and is also shown in the fields of aerospace and electronic communications Excellent thermal conductivity.
Patent Information
- Application Number
- CN202211166497.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-23
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2042-09-23
AI Technical Summary
The existing tungsten copper alloy process is complex, and the application of oxides affects thermal conductivity to varying degrees. The existing methods are not suitable for industrial production, making it difficult to achieve high purity and uniformity.
The tungsten skeleton is prepared by a three-stage hot pressing sintering method that controls the heating rate and pressure. The spherical tungsten powder is pressurized by the hot pressing equipment to obtain a tungsten skeleton with high purity, density and uniform pore distribution, and through copper seepage A good tungsten copper alloy is obtained.
The process flow is simplified, the purity and uniformity of tungsten copper alloys are improved, the process cost is reduced, the process is suitable for industrial production, and excellent thermal conductivity is shown in the fields of aerospace and electronic communications.
Smart Images

Figure CN115519123B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of powder metallurgy, and in particular relates to a tungsten skeleton and a preparation method and application thereof. Background Art
[0002] Tungsten copper alloy is an alloy composed of tungsten and copper. The copper content of the commonly used alloy is 10% to 50%, with good electrical and thermal conductivity, good high temperature strength and certain plasticity. At very high temperatures, such as above 3000℃, the copper in the alloy is liquefied and evaporated, absorbing a large amount of heat and reducing the surface temperature of the material. Therefore, this type of material is also called metal sweating material. Since the tungsten copper heat sink material is a pseudo alloy composed of tungsten and copper that do not dissolve each other, the material combines the low thermal expansion coefficient, high hardness, high thermal conductivity of tungsten and the electrical and thermal conductivity of copper. According to the working conditions of the material, the method of changing the copper content is usually used to achieve the target thermal conductivity and thermal expansion coefficient. Tungsten copper alloy is widely used in aerospace, electronic communications and other fields due to its excellent physical and chemical properties.
[0003] Tungsten copper alloy requires uniform microstructure and low impurity content due to its performance and actual needs of working conditions. The main preparation methods are copper-tungsten powder mixed injection molding method, copper oxide powder matrix method and tungsten skeleton infiltration method.
[0004] CN114160787A discloses a method for manufacturing a non-shrinking tungsten skeleton, which comprises adding tungsten oxide or molybdenum oxide metal oxide powder to tungsten powder, and adding paraffin or stearic acid as a forming agent, and pressing the powder into a block in a mold after the powder is evenly mixed; degumming in a furnace at 200-400°C, and then reducing in a hydrogen atmosphere at a reduction temperature between 700-900°C to form a non-shrinking tungsten skeleton; using tungsten oxide powder makes the purity of the tungsten skeleton and the tungsten-copper alloy low, which affects the electrical and thermal conductivity.
[0005] CN107498047A discloses a tungsten-copper composite material and a preparation method thereof, comprising a tungsten skeleton, a tungsten porous body and a copper filling phase, wherein the tungsten skeleton has a porous three-dimensional lattice structure, the pores of the tungsten skeleton are filled with a tungsten porous body, there are pores between the tungsten porous body and the tungsten skeleton, the copper filling phase is filled in the pores of the tungsten porous body and in the pores between the tungsten porous body and the tungsten skeleton, the composite structure formed by the tungsten porous body and the tungsten skeleton improves the strength of the tungsten-copper composite material, the copper filling phase is uniformly distributed in the pores of the tungsten porous body and in the pores between the tungsten porous body and the tungsten skeleton, and the ablation resistance of the tungsten-copper composite material is enhanced; a preparation method of a tungsten-copper composite material is also provided, wherein the tungsten skeleton is first prepared by a high-energy beam selective melting forming method, and then tungsten powder is filled into the tungsten skeleton by a cold isostatic pressing method and a high-temperature sintering method to form a tungsten porous body, and then the copper filling phase is prepared by combining with a copper infiltration method, the method has high precision, high efficiency and reliability, but the required environmental requirements and cost are too high, and it is not suitable for industrial production.
[0006] CN114367664A discloses a wet process for preparing a non-shrinking tungsten skeleton, wherein the debonded and pre-burned tungsten compact is immersed in a solution containing tungsten and molybdenum salts, and is fished out and heated and dried after a certain period of time, and then heated in a hydrogen atmosphere. At this time, the precipitate of the tungsten and molybdenum salt solution undergoes a reduction reaction under the action of hydrogen and forms a sintering neck between the tungsten particles. Since the sintering neck is formed in the reduction stage and the temperature is relatively low, the tungsten skeleton does not shrink. The method can accurately control the amount of tungsten or molybdenum element added to the tungsten compact by controlling the concentration of the tungsten or molybdenum salt solution in the solution and the immersion time, and the precipitate is evenly distributed at the connection of the tungsten particles, ensuring that the strength of the tungsten skeleton is uniform everywhere. The present invention reduces the temperature of tungsten skeleton formation, has a simple process, and since the tungsten skeleton does not shrink, the subsequent infiltration metal content can be accurately controlled, greatly improving the chemical composition and performance consistency of the melt infiltration product; the reaction uses hydrogen high-temperature reaction, and has low safety.
[0007] In order to improve the purity and uniformity of tungsten-copper alloy, a safer, simpler and easier-to-operate method is needed to prepare tungsten-copper alloy. Summary of the invention
[0008] In view of the problems existing in the prior art such as complex process and the application of oxides affecting the thermal conductivity of tungsten-copper alloys to varying degrees, the present invention proposes a tungsten skeleton and a preparation method and use thereof, a hot pressing sintering step with three-stage control of heating rate, temperature and pressure, the density, purity and grain size of the product tungsten skeleton are controlled, and a tungsten-copper alloy with excellent performance is further obtained by copper infiltration.
[0009] To achieve this object, the present invention adopts the following technical solutions:
[0010] In a first aspect, the present invention provides a method for preparing a tungsten skeleton by hot pressing and sintering, the preparation method comprising the following steps:
[0011] The spherical tungsten powder is loaded into a mold, and the spherical tungsten powder carried by the mold is hot pressed and sintered to obtain a tungsten skeleton rough blank, and the tungsten skeleton rough blank is sequentially rough ground, cut and cleaned to obtain the tungsten skeleton.
[0012] The hot pressing and sintering preparation method of a tungsten skeleton provided by the present invention uses a hot pressing device to pressurize and sinter spherical tungsten powder, wherein hot pressing and sintering refers to a sintering method in which the powder is filled into a mold, and then the mold is pressurized from a uniaxial direction using a press device, and the molding and sintering are completed simultaneously while being pressurized and heated. The tungsten skeleton obtained by the hot pressing method has a high purity, and the pores are more evenly distributed and interconnected. There is no need to perform hydrogen reduction on the oxide, and there is no need to add additional strengthening metal, and the operation is simple.
[0013] Preferably, the particle size of the spherical tungsten powder is 3-20 μm, for example, 3 μm, 5 μm, 8 μm, 10 μm, 12 μm, 15 μm, 18 μm or 20 μm, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0014] Preferably, the material of the mold includes graphite.
[0015] Preferably, the mold flatness of the spherical tungsten powder after being loaded into the mold is less than 1 mm, for example, it can be 0.9 mm, 0.8 mm, 0.7 mm or 0.5 mm, etc., but it is not limited to the listed values, and other values not listed in the numerical range are also applicable.
[0016] Preferably, the three-stage hot pressing sintering comprises the following steps:
[0017] (1) Initial sintering stage: heating from the initial temperature to the first temperature at a heating rate, sintering at the first temperature and the first pressure for a first time, ensuring that the density of the tungsten skeleton reaches 25-35%, for example, 25%, 28%, 30%, 32% or 35%, but not limited to the listed values, and other values not listed within the numerical range are also applicable;
[0018] (2) Sintering mid-term: heating from the first temperature to the second temperature at a two-stage heating rate, sintering at the second temperature and the second pressure for a second time, ensuring that the density of the tungsten skeleton reaches 40-55%, for example, 40%, 45%, 50% or 55%, but not limited to the listed values, and other values not listed within the numerical range are also applicable;
[0019] (3) Late sintering: the temperature is raised from the second temperature to the third temperature at a three-stage heating rate, and sintered at the third temperature and the third pressure for a third time to ensure that the density of the tungsten skeleton reaches 60-80%, for example, it can be 60%, 65%, 70%, 75% or 80%, but it is not limited to the listed values. Other values not listed in the numerical range are also applicable. Cooling is performed to obtain a tungsten skeleton rough blank.
[0020] Preferably, the pressure reached by the vacuuming in step (1) is less than 40Pa, for example, it can be 35Pa, 30Pa, 25Pa or 20Pa, etc., but it is not limited to the listed values, and other values not listed in the numerical range are also applicable.
[0021] Preferably, the initial temperature in step (1) is 20-30°C, for example, 20°C, 22°C, 25°C, 28°C or 30°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0022] Preferably, the heating rate in step (1) is 9.5-10.5°C / min, for example, 9.5°C / min, 9.8°C / min, 10°C / min, 10.2°C / min or 10.5°C / min, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0023] Preferably, the first temperature in step (1) is 980-1020°C, for example, 980°C, 990°C, 1000°C, 1010°C or 1020°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0024] Preferably, the first pressure in step (1) is 9-11 MPa, for example, 9 MPa, 9.5 MPa, 10 MPa, 10.5 MPa or 11 MPa, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0025] Preferably, in step (1), the first time is 30-60 min, for example, 30 min, 40 min, 50 min or 60 min, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0026] Preferably, the second-stage heating rate in step (2) is 4.5-5.5°C / min, for example, it can be 4.5°C / min, 4.8°C / min, 5°C / min, 5.2°C / min or 5.5°C / min, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0027] Preferably, the second temperature in step (2) is 1080-1220°C, for example, it can be 1080°C, 1100°C, 1120°C, 1150°C, 1180°C, 1200°C or 1220°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0028] Preferably, the second pressure in step (2) is 14-16 MPa, for example, 14 MPa, 14.5 MPa, 15 MPa, 15.5 MPa or 16 MPa, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0029] Preferably, in step (2), the second time is 50-70 min, for example, 50 min, 55 min, 60 min, 65 min or 70 min, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0030] Preferably, the three-stage heating rate in step (3) is <5°C / min, for example, it can be 4.5°C / min, 4°C / min, 3°C / min, 2°C / min or 1°C / min, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0031] Preferably, the third temperature in step (3) is 1400-1550°C, for example, it can be 1400°C, 1450°C, 1480°C, 1500°C, 1520°C or 1550°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0032] Preferably, the third pressure in step (3) is 19-21 MPa, for example, 19 MPa, 19.5 MPa, 20 MPa, 20.5 MPa or 21 MPa, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0033] Preferably, the third time in step (3) is 60-180 min, for example, 60 min, 70 min, 80 min, 100 min, 120 min, 150 min or 180 min, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0034] The present invention preferably adopts a three-stage heating method and a heating rate that decreases as the temperature increases. The advantages of the three-stage heating method are that the hot pressing process is simple to operate, the rough blank preparation is cost-effective, the production cycle is short, and the pore distribution of the obtained tungsten material meets the requirements. Considering the heating method of the furnace body, the heating rate decreases as the temperature increases. This is due to the characteristics of radiation heat transfer in the hot pressing process. It is necessary to ensure the temperature uniformity as much as possible in the medium and high temperature stages as the temperature increases, and the decreasing temperature in the later stage of sintering is beneficial to improving the uniformity of the pore distribution of the tungsten skeleton.
[0035] Preferably, the device used for the rough grinding comprises a grinder.
[0036] Preferably, the cutting device comprises a wire cutting machine.
[0037] Preferably, the cleaning comprises sequential steps of ultrasonic cleaning and drying.
[0038] Preferably, the ultrasonic cleaning time is 60-120 min, for example, 60 min, 70 min, 80 min, 90 min, 100 min, 110 min or 120 min, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0039] Preferably, the drying temperature is 65-75°C, for example, 65°C, 68°C, 70°C, 72°C or 75°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0040] Preferably, the drying time is 60-120 min, for example, 60 min, 80 min, 100 min or 120 min, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0041] As a preferred technical solution of the present invention, the preparation method comprises the following steps:
[0042] The spherical tungsten powder with a particle size of 3-20 μm is loaded into a graphite mold, and the spherical tungsten powder carried by the graphite mold is subjected to three-stage hot pressing sintering, and the three-stage hot pressing sintering includes the following steps:
[0043] (1) Initial sintering: The spherical tungsten powder carried by the mold enters the device and is evacuated to a vacuum of <40Pa. The temperature is raised from 20-30℃ to 980-1020℃ at a rate of 9.5-10.5℃ / min. The powder is sintered at 980-1020℃ and 9-11MPa for 30-60min to ensure that the density of the tungsten skeleton reaches 25-35%;
[0044] (2) Mid-sintering: heating from 980-1020°C to 1080-1220°C at a rate of 4.5-5.5°C / min, sintering at 1080-1220°C and 14-16MPa for 50-70min to ensure that the density of the tungsten skeleton reaches 40-55%;
[0045] (3) Sintering stage: heating from 1080-1220°C to 1400-1550°C at a rate of <5°C / min, sintering at 1400-1550°C and 19-21MPa for 60-180min to ensure that the density of the tungsten skeleton reaches 60-80%, and cooling to obtain a tungsten skeleton rough blank;
[0046] The rough tungsten skeleton blank is roughly ground by a grinder, and cut into a target size by a wire cutting machine, and then ultrasonically cleaned for 60-120 minutes, and dried at 65-75° C. for 60-120 minutes to obtain the tungsten skeleton.
[0047] In a second aspect, the present invention further provides a tungsten skeleton obtained by the preparation method of the tungsten skeleton by hot pressing and sintering as described in the first aspect.
[0048] The tungsten skeleton provided by the present invention has high purity, relatively uniform pore distribution and interconnection, controllable tungsten skeleton grain size, uniform internal pore distribution, and the regulation of grain size and internal pores is mainly carried out by adjusting the temperature and time in the later stage of sintering.
[0049] In a third aspect, the present invention further provides a tungsten skeleton as described in the second aspect, which is used in aerospace or electronic communications.
[0050] The tungsten skeleton provided by the present invention is subjected to copper infiltration to obtain a tungsten-copper alloy, which has excellent properties such as high thermal conductivity, low expansion coefficient, high strength, and high temperature resistance. It can be used to make high-voltage switches and electrical machining electrodes, and is widely used in the aerospace and electronic communication industries.
[0051] Compared with the prior art, the present invention has the following beneficial effects:
[0052] (1) The preparation method of the tungsten skeleton by hot pressing and sintering provided by the present invention uses spherical tungsten powder as a raw material for three-stage hot pressing and sintering, thereby ensuring the purity of the tungsten skeleton and improving the density and grain size of the tungsten skeleton. The method is simple, has low operation difficulty, and is suitable for promotion;
[0053] (2) The tungsten skeleton provided by the present invention has high purity, uniform and interconnected pore distribution, and the grain size of the tungsten skeleton can also be adjusted according to actual requirements;
[0054] (3) The tungsten skeleton provided by the present invention is a tungsten-copper alloy obtained by infiltrating copper on a tungsten skeleton with a relatively high pore distribution uniformity, which has excellent thermal conductivity and has broad prospects in the fields of aviation and communications. BRIEF DESCRIPTION OF THE DRAWINGS
[0055] Figure 1 This is a scanning electron microscope morphology image of the tungsten skeleton provided in Example 1 of the present invention.
[0056] Figure 2 This is a scanning electron microscope morphology image of the tungsten powder provided in Example 1 of the present invention. DETAILED DESCRIPTION
[0057] For the convenience of understanding the present invention, the present invention lists the following embodiments. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0058] It should be understood that, in the description of the present invention, the terms "center", "longitudinal", "lateral", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", etc., indicating the orientation or positional relationship are based on the orientation or positional relationship shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention. In addition, the terms "first", "second", etc. are only used for descriptive purposes, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first", "second", etc. may explicitly or implicitly include one or more of the features. In the description of the present invention, unless otherwise specified, "multiple" means two or more.
[0059] It should be noted that in the description of the present invention, unless otherwise clearly specified and limited, the terms "disposed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood by specific circumstances.
[0060] The technical solution of the present invention is further described below with reference to the accompanying drawings and through specific implementation methods.
[0061] In a specific embodiment, the present invention provides a method for preparing a tungsten skeleton by hot pressing and sintering, the preparation method comprising the following steps:
[0062] The spherical tungsten powder with a particle size of 3-20 μm is loaded into a graphite mold, and the spherical tungsten powder carried by the graphite mold is subjected to three-stage hot pressing sintering, and the three-stage hot pressing sintering includes the following steps:
[0063] (1) Initial sintering: The spherical tungsten powder carried by the mold enters the device and is evacuated to a vacuum of <40Pa. The temperature is raised from 20-30℃ to 980-1020℃ at a rate of 9.5-10.5℃ / min. The powder is sintered at 980-1020℃ and 9-11MPa for 30-60min to ensure that the density of the tungsten skeleton reaches 25-35%;
[0064] (2) Mid-sintering: heating from 980-1020°C to 1080-1220°C at a rate of 4.5-5.5°C / min, sintering at 1080-1220°C and 14-16MPa for 50-70min to ensure that the density of the tungsten skeleton reaches 40-55%;
[0065] (3) Sintering stage: heating from 1080-1220°C to 1400-1550°C at a rate of <5°C / min, sintering at 1400-1550°C and 19-21MPa for 60-180min to ensure that the density of the tungsten skeleton reaches 60-80%, and cooling to obtain a tungsten skeleton rough blank;
[0066] The rough tungsten skeleton blank is roughly ground by a grinder, and cut into a target size by a wire cutting machine, and then ultrasonically cleaned for 60-120 minutes, and dried at 65-75° C. for 60-120 minutes to obtain the tungsten skeleton.
[0067] In another specific embodiment, the present invention provides a tungsten skeleton obtained by the above-mentioned preparation method of tungsten skeleton by hot pressing and sintering.
[0068] It should be clear that the use of the process provided by the embodiment of the present invention or the replacement or change of conventional data all fall within the protection scope and disclosure scope of the present invention.
[0069] Example 1
[0070] This embodiment provides a method for preparing a tungsten skeleton. The method comprises the following steps:
[0071] The spherical tungsten powder with a particle size of 10 μm is loaded into a graphite mold, and the spherical tungsten powder carried by the graphite mold is subjected to three-stage hot pressing sintering, and the three-stage hot pressing sintering includes the following steps:
[0072] (1) Initial sintering stage: The spherical tungsten powder carried by the mold enters the device and is evacuated to a vacuum of <40 Pa. The spherical tungsten powder has a scanning electron microscope morphology as shown in the figure. Figure 2 As shown in the figure, the spherical tungsten powder has an uneven morphology and a large specific surface area, and the particle size is relatively uniform; the temperature is raised from 25°C to 1000°C at a rate of 10°C / min, and sintered at 1000°C and 10MPa for 45min to ensure that the density of the tungsten skeleton reaches 30%;
[0073] (2) Mid-sintering: heating from 1000°C to 1150°C at a rate of 5°C / min, sintering at 1150°C and 15 MPa for 60 min to ensure that the density of the tungsten skeleton reaches 50%;
[0074] (3) Sintering stage: heating from 1150°C to 1500°C at a rate of 2°C / min, sintering at 1500°C and 20MPa for 120min to ensure that the density of the tungsten skeleton reaches 70%, and cooling to obtain a tungsten skeleton rough blank;
[0075] The rough tungsten skeleton blank is roughly ground by a grinder, and cut into a target size by a wire cutting machine, and then ultrasonically cleaned for 90 minutes and dried at 70° C. for 90 minutes to obtain the tungsten skeleton.
[0076] This embodiment also provides a tungsten skeleton obtained by the preparation method of the tungsten skeleton. The scanning electron microscope morphology of the tungsten skeleton is as follows: Figure 1 As shown, it can be seen that there is a fine and regular grain structure distributed inside the tungsten skeleton shown in the figure, which proves that the tungsten skeleton product provided by the present invention has a uniform internal structure.
[0077] Example 2
[0078] This embodiment provides a method for preparing a tungsten skeleton. The method comprises the following steps:
[0079] The spherical tungsten powder with a particle size of 3 μm is loaded into a graphite mold, and the spherical tungsten powder carried by the graphite mold is subjected to three-stage hot pressing sintering, and the three-stage hot pressing sintering includes the following steps:
[0080] (1) Initial sintering: The spherical tungsten powder carried by the mold enters the device and is evacuated to a vacuum of <40Pa. The temperature is raised from 30°C to 1020°C at a rate of 9.5°C / min. The sintering is performed at 1020°C and 9MPa for 30min to ensure that the density of the tungsten skeleton reaches 35%;
[0081] (2) Mid-sintering: heating from 1020°C to 1220°C at a rate of 4.5°C / min, sintering at 1220°C and 14 MPa for 50 min to ensure that the density of the tungsten skeleton reaches 55%;
[0082] (3) Sintering stage: heating from 1220°C to 1550°C at a rate of 2°C / min, sintering at 1550°C and 19 MPa for 60 min to ensure that the density of the tungsten skeleton reaches 80%, and cooling to obtain a tungsten skeleton rough blank;
[0083] The tungsten skeleton blank is roughly ground by a grinder, and cut into a target size by a wire cutting machine, and then ultrasonically cleaned for 120 minutes and dried at 75° C. for 120 minutes to obtain the tungsten skeleton.
[0084] This embodiment also provides a tungsten skeleton obtained by the preparation method of the above tungsten skeleton.
[0085] Example 3
[0086] This embodiment provides a method for preparing a tungsten skeleton. The method comprises the following steps:
[0087] The spherical tungsten powder with a particle size of 20 μm is loaded into a graphite mold, and the spherical tungsten powder carried by the graphite mold is subjected to three-stage hot pressing sintering, and the three-stage hot pressing sintering includes the following steps:
[0088] (1) Initial sintering: The spherical tungsten powder carried by the mold enters the device and is evacuated to a vacuum of <40 Pa. The temperature is raised from 20°C to 980°C at a rate of 10.5°C / min. The sintering is performed at 980°C and 11 MPa for 60 min to ensure that the density of the tungsten skeleton reaches 25%;
[0089] (2) Mid-sintering: heating from 980°C to 1080°C at a rate of 5.5°C / min, sintering at 1080°C and 16MPa for 70min to ensure that the density of the tungsten skeleton reaches 40%;
[0090] (3) Sintering stage: heating from 1080°C to 1400°C at a rate of 4.5°C / min, sintering at 1400°C and 21MPa for 180min to ensure that the density of the tungsten skeleton reaches 60%, and cooling to obtain a tungsten skeleton rough blank;
[0091] The tungsten skeleton blank is roughly ground by a grinder, and cut into a target size by a wire cutting machine, and then ultrasonically cleaned at 65° C. for 120 minutes and dried for 120 minutes to obtain the tungsten skeleton.
[0092] This embodiment also provides a tungsten skeleton obtained by the preparation method of the above tungsten skeleton.
[0093] Example 4
[0094] This embodiment provides a preparation method of a tungsten skeleton and a tungsten skeleton. The difference in the preparation method from Embodiment 1 is that the heating rate in the later stage of sintering is 5° C. / min.
[0095] Example 5
[0096] This embodiment provides a preparation method of a tungsten skeleton and a tungsten skeleton. The difference in the preparation method from Embodiment 1 is that the heating rates in the middle and late stages of sintering are both 10° C. / min.
[0097] Comparative Example 1
[0098] This comparative example provides a preparation method of a tungsten skeleton and a tungsten skeleton. The difference in the preparation method from Example 1 is: non-segmented hot pressing sintering: heating from 25°C to 1500°C at a rate of 10°C / min, and sintering at 1500°C and 20MPa for 225min.
[0099] Comparative Example 2
[0100] The present comparative example provides a method for preparing a tungsten skeleton, wherein the tungsten skeleton is prepared by the steps of Example 1 of CN110565033A, wherein the tungsten skeleton is prepared by laying alkali-washed tungsten-rhenium alloy fibers in a hot pressing mold or a hot isostatic pressing can, and then loading nearly round tungsten powder, and performing homogenization sintering by low-pressure hot pressing or hot isostatic pressing in a high vacuum environment to form a reinforced porous tungsten skeleton. Although the tungsten-rhenium alloy fibers introduce as few impurities as possible compared to the rhenium metal mesh, rhenium metal is still introduced, and the steps are relatively complicated, and the performance of the obtained porous tungsten material is also inferior to that of the tungsten skeleton provided by the present invention.
[0101] The density, strength and grain size of the tungsten skeletons of Examples 1-5 and Comparative Examples 1-2 are shown in Table 1.
[0102] Table 1
[0103] Thermal conductivity (W / M·K) Conductivity (Ω·M) Average tungsten grain size (μm) Example 1 77.8 <![CDATA[5.40×10 -8 ]]> <20 Example 2 75.6 <![CDATA[4.75×10 -8 ]]> <20 Example 3 74.2 <![CDATA[4.14×10 -8 ]]> <20 Example 4 76.9 <![CDATA[4.80×10 -8 ]]> <20 Example 5 75.6 <![CDATA[4.70×10 -8 ]]> <20 Comparative Example 1 75.6 <![CDATA[4.07×10 -8 ]]> <20 Comparative Example 2 76.4 <![CDATA[4.30×10 -8 ]]> <20
[0104] From the data in Table 1 we can see that:
[0105] (1) The tungsten skeleton obtained by the method of Examples 1-3 adopts three-stage hot pressing, and the heating rate decreases gradually, which ensures that the grain size inside the tungsten skeleton is fine and evenly distributed, and the average tungsten grain size is less than 20 μm, so that it has good thermal conductivity and electrical conductivity, with thermal conductivity ≥74.2 W / M·K and electrical conductivity ≥4.14×10 -8 Ω·M, simple steps and high production efficiency;
[0106] (2) Based on Example 1 and Examples 4-5, it can be seen that Example 4 adopts hot pressing with two-stage decreasing heating temperature, Example 5 adopts hot pressing with non-decreasing heating temperature, and Example 1 adopts hot pressing with three-stage decreasing heating temperature. The thermal conductivity of Examples 4 and 5 is only 76.9 W / M·K and 75.6 W / M·K respectively, and the electrical conductivity is only 4.80×10 -8 Ω·M and 4.70×10 -8Ω·M, while the thermal conductivity of Example 1 is 77.8W / M·K and the electrical conductivity is 5.40×10 -8 Ω·M, which shows that the use of a heating curve with decreasing temperature during hot pressing is conducive to improving the uniformity of its pore distribution, and can obtain a tungsten skeleton with a more uniform internal structure and higher thermal and electrical conductivity;
[0107] (3) It can be seen from the combination of Example 1 and Comparative Examples 1-2 that Comparative Example 1 adopts non-segmented hot pressing, Comparative Example 2 adopts tungsten-rhenium alloy fiber doped with tungsten powder to prepare the tungsten skeleton, and Example 1 adopts three-stage hot pressing. The thermal conductivity of Comparative Examples 1 and Comparative Examples 2 is only 75.6 W / M·K and 76.4 W / M·K respectively, and the electrical conductivity is only 4.07×10 -8 Ω·M and 4.30×10 -8 Ω·M, while the thermal conductivity of Example 1 is 77.8W / M·K and the electrical conductivity is 5.40×10 -8 Ω·M, which shows that the tungsten skeleton obtained by segmented hot pressing of the tungsten powder of the present application effectively reduces the impurity content, ensures uniformity, and improves thermal conductivity and electrical conductivity.
[0108] In summary, the present invention provides a tungsten skeleton and its preparation method and use, which adopts a segmented hot pressing sintering method and controls the heating rate at the same time to prepare a tungsten skeleton with uniform structure, interconnected pores and different densities. The method is simple, low-cost and suitable for industrial promotion and use.
[0109] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.
Claims
1. A method for preparing a tungsten framework, characterized in that: The preparation method comprises the following steps: The spherical tungsten powder is loaded into a mold, and the spherical tungsten powder carried by the mold is hot pressed and sintered to obtain a tungsten skeleton rough blank; the tungsten skeleton rough blank is sequentially rough ground, cut and cleaned to obtain the tungsten skeleton; The hot pressing sintering comprises the following steps: (1) Initial sintering stage: The spherical tungsten powder carried by the mold enters the hot pressing sintering device and is vacuumed. The temperature is raised from the initial temperature to 980-1020°C at a heating rate of 9.5-10.5°C / min. The powder is sintered at 980-1020°C and 9-11MPa for the first time to ensure that the density of the tungsten skeleton reaches 25-35%; (2) Mid-sintering: heating from 980-1020℃ to 1080-1220℃ at a heating rate of 4.5-5.5℃ / min, sintering for the second time at 1080-1220℃ and 14-16MPa to ensure that the density of the tungsten skeleton reaches 40-55%; (3) Late sintering: Heat up from 1080-1220°C to 1400-1550°C at a rate of ≤5°C / min, sinter for a third time at 1400-1550°C and 19-21MPa to ensure that the density of the tungsten skeleton reaches 60-80%, and cool to obtain a tungsten skeleton rough blank.
2. The preparation method according to claim 1, characterized in that: The particle size of the quasi-spherical tungsten powder is 3-20 μm.
3. The preparation method according to claim 1, characterized in that: The material of the mold includes graphite.
4. The preparation method according to claim 1, characterized in that: The mold flatness of the spherical tungsten powder after being loaded into the mold is less than 1mm.
5. The preparation method according to claim 1, characterized in that: The pressure reached by the vacuuming in step (1) is less than 40 Pa.
6. The preparation method according to claim 1, characterized in that: The initial temperature of step (1) is 20-30°C.
7. The preparation method according to claim 1, characterized in that: The first time in step (1) is 30-60 minutes.
8. The preparation method according to claim 1, characterized in that: In step (2), the second time is 50-70 minutes.
9. The preparation method according to claim 1, characterized in that: The third time in step (3) is 60-180 minutes.
10. The preparation method according to claim 1, characterized in that: The device used for the rough grinding includes a grinding machine.
11. The preparation method according to claim 1, characterized in that: The device used for cutting includes a wire cutting machine.
12. The preparation method according to claim 1, characterized in that: The cleaning comprises ultrasonic cleaning and drying steps performed sequentially.
13. The preparation method according to claim 12, characterized in that: The ultrasonic cleaning time is 60-120 minutes.
14. The preparation method according to claim 12, characterized in that: The drying temperature is 65-75°C.
15. The preparation method according to claim 12, characterized in that: The drying time is 60-120 minutes.
16. The preparation method according to claim 1, characterized in that: The preparation method comprises the following steps: The spherical tungsten powder with a particle size of 3-20 μm is loaded into a graphite mold, and the spherical tungsten powder carried by the graphite mold is subjected to three-stage hot pressing sintering, and the three-stage hot pressing sintering includes the following steps: (1) Initial sintering stage: the spherical tungsten powder carried by the mold enters the device and is evacuated to a temperature of <40Pa. The temperature is raised from 20-30℃ to 980-1020℃ at a rate of 9.5-10.5℃ / min. The powder is sintered at 980-1020℃ and 9-11MPa for 30-60min to ensure that the density of the tungsten skeleton reaches 25-35%; (2) Mid-sintering: Heat from 980-1020℃ to 1080-1220℃ at a rate of 4.5-5.5℃ / min, and sinter at 1080-1220℃ and 14-16MPa for 50-70min to ensure that the density of the tungsten skeleton reaches 40-55%; (3) Later stage of sintering: the temperature is raised from 1080-1220°C to 1400-1550°C at a rate of ≤5°C / min, and sintered at 1400-1550°C and 19-21MPa for 60-180min to ensure that the density of the tungsten skeleton reaches 60-80%, and then cooled to obtain a rough tungsten skeleton; The rough tungsten skeleton blank is roughly ground by a grinder, and cut into a target size by a wire cutting machine, and then ultrasonically cleaned at 65-75° C. for 60-120 minutes and dried for 60-120 minutes to obtain the tungsten skeleton.
17. A tungsten skeleton obtained by the preparation method of the tungsten skeleton by hot pressing and sintering as claimed in any one of claims 1 to 16.
18. Use of the tungsten framework as claimed in claim 17, characterized in that: The tungsten skeleton is used in aerospace or electronic communications.