Preparation method of silver powder for conductive paste

By using hydrophobic surfactant to form an emulsion as a surface treatment agent in the preparation of silver powder, the problem of wide particle size distribution of silver powder and precipitation of surface treatment agent is solved, the preparation of silver powder with uniform particle size and good dispersion is achieved, and the production efficiency is improved. and yield.

CN115519131BActive Publication Date: 2024-10-22SENJIA ZERO CARBON MATERIALS TECHNOLOGY (NANTONG) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210936906.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-08-05
Publication Date
2024-10-22
Estimated Expiration
2042-08-05

AI Technical Summary

Technical Problem

In the existing silver powder preparation method, the particle size distribution of the silver powder is wide, the average particle size is large, and the surface treatment agent is easy to precipitate, affecting the dispersion and particle size uniformity of the finished product.

Method used

Hydrophobic surfactants are mixed with solvents to form organic solvents. After heating and stirring, an emulsion is formed. As a surface treatment agent, it is added to the silver-containing solution to participate in the reaction of the silver powder. The surface treatment agent is used to protect the crystal nucleus during the growth process, forming Silver powder with uniform particle size and narrow distribution.

Benefits of technology

It achieves narrow particle size distribution and good uniformity of silver powder, improves the dispersion and yield of silver powder, simplifies the production process, and reduces operating errors and costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115519131B_ABST
    Figure CN115519131B_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing silver powder for conductive paste, wherein a hydrophobic surfactant and a solvent are mixed to form an organic solvent, and water is added to emulsify the mixture, and a surface treatment agent is prepared. The surface treatment agent is added to a silver-containing solution for dispersion treatment, and the obtained silver-containing mixture reacts with a reducing agent solution, and the generated wet silver powder is dried to obtain silver powder. The surface treatment agent adopts a hydrophobic surfactant and is emulsified to form an oil-in-water emulsion. The surface treatment agent is added during the reaction of the silver powder and participates in the reaction of the silver powder. The surface treatment agent plays a protective role during the growth of the crystal nucleus to prevent the particle size from increasing, so that the prepared silver powder particles have good dispersibility and no agglomeration, and can be dispersed again in a non-polar solvent. The silver powder particles have uniform particle size, narrow particle size distribution, small average particle size, high silver powder yield, and short production cycle.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing silver powder, in particular to a method for preparing silver powder for conductive paste. Background Art

[0002] A nanosilver and a synthesis method thereof (country: China, publication number: 109079154B, publication date: 2022-03-01), which discloses that wet silver powder with a hydrophilic surface treatment agent added thereto is placed in an oil bath and heated and stirred to form a nanosilver sol, and then a precipitant is added to make the surface of the silver powder present a hydrophobic structure.

[0003] A surface treatment liquid and addition method in the preparation process of silver powder (country: China, publication number: 112024906A, publication date: 2020-12-04), discloses mixing a lipophilic surfactant, a hydrophobic defoamer and an organic solvent to obtain a surface treatment liquid, and then adding the surface treatment liquid to the silver powder synthesis system, stirring and mixing, and then washing and drying. The surface treatment liquid overcomes the problem of poor dispersibility and easy agglomeration of silver powder in the prior art, and at the same time eliminates the tediousness of multiple heating of the surface treatment agent, improves operating efficiency, reduces operating errors, and saves time and effort. In the silver synthesis system, the hydrophobic defoamer will attract the hydrophobic end of the surfactant, making the hydrophobic defoamer hydrophilic, thereby reducing the concentration and tension of the surfactant in the bubble film in the silver synthesis system, thereby playing a defoaming role; the organic solvent can dissolve the lipophilic surfactant and the hydrophobic defoamer, thereby reducing the melting point of the two lipophilic surfactants and the hydrophobic defoamer.

[0004] However, the silver powder surface treatment agent in the above method is easy to precipitate and float on the surface, resulting in incomplete coating. The particle size distribution of the finished silver powder is wide and the average particle size is large. Summary of the invention

[0005] Purpose of the invention: The purpose of the present invention is to provide a method for preparing silver powder for conductive paste to obtain finished silver powder with narrow particle size distribution and uniform particle size.

[0006] Technical solution: A method for preparing silver powder for conductive paste, comprising the following steps:

[0007] Step S10, preparing a surface treatment agent: mixing a hydrophobic surfactant and a solvent into an organic solvent, generating a solution under heating conditions, and then adding hot water and stirring to form an emulsion surface treatment agent;

[0008] Step S20, dispersion: adding a surface treatment agent to the silver-containing solution, performing a dispersion treatment, and obtaining a silver-containing mixture;

[0009] Step S30, preparing wet silver powder: reacting the silver-containing mixture with a reducing agent solution to generate a silver precipitate to form wet silver powder;

[0010] Step S40, drying the wet silver powder to obtain silver powder.

[0011] Furthermore, in step S20, the silver-containing solution is one of a silver ammonia solution, an Ag2O suspension or an Ag2CO3 suspension.

[0012] Furthermore, in step S30, the reducing agent solution is one of glucose, formaldehyde, hydrazine hydrate, ascorbic acid, sodium isoascorbate, and p-diphenol.

[0013] Furthermore, in step S10: the amount of the hydrophobic surfactant used is 0.0001 to 20% of the silver content of the silver-containing solution, in mass percentage; the hydrophobic surfactant and the solvent are mixed into an organic solvent in a mass ratio of 1:80 to 10:80; and the hot water and the hydrophobic surfactant are used in a mass ratio of 1:1 to 10:1.

[0014] Furthermore, in step S10, the hydrophobic surfactant is C6~C 22 Saturated fatty acids, C6~C 22 Unsaturated fatty acids, C6~C 22 Esters, C6~C 22 Amines, C6~C 22 Fatty amines, C6~C 22 One of the fatty amides or a mixture of at least two thereof; the solvent is one of ethanol, acetone, ethylene glycol, toluene or a mixture of at least two thereof.

[0015] Furthermore, in step S10, the heating condition is 30°C to 100°C, and the hot water temperature is 30°C to 100°C.

[0016] Furthermore, in step S10, stirring is performed using a homogenizer at a speed of 1000 to 30000 r / min for 1 to 3 minutes to form an emulsion, and the stirring speed is preferably such that an emulsion can be formed without splashing the liquid.

[0017] Beneficial effects: The advantages of the present invention are: the surface treatment agent used in the preparation of silver powder adopts a hydrophobic surfactant and is emulsified to form an oil-in-water emulsion. The surface treatment agent is added during the reaction of the silver powder and participates in the reaction of the silver powder. The surface treatment agent plays a protective role in the process of crystal nucleus growth to prevent the particle size from increasing, so that the prepared silver powder particles have good dispersibility and no agglomeration, and can be re-dispersed in a non-polar solvent. The silver powder particles have uniform particle size, narrow particle size distribution, small average particle size, high silver powder yield, and short production cycle. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 This is a microscope image of the silver powder obtained in Example 1;

[0019] Figure 2 This is a microscope image of the silver powder prepared in Comparative Example 8. DETAILED DESCRIPTION

[0020] The present invention is further explained below in conjunction with the accompanying drawings and specific embodiments.

[0021] The invention discloses a method for preparing silver powder for conductive paste. The method comprises the following steps: emulsifying an organic solvent prepared by mixing a hydrophobic surfactant and a solvent with water to prepare a surface treatment agent; mixing and dispersing the surface treatment agent with a silver-containing solution to obtain a silver-containing mixture; and then preparing wet silver powder by mixing with a reducing agent solution. The silver powder is then dried to obtain silver powder.

[0022] The silver-containing solution is one of silver ammonia solution, Ag2O suspension or Ag2CO3 suspension, and the reducing agent solution is one of glucose, formaldehyde, hydrazine hydrate, ascorbic acid, sodium isoascorbate, p-diphenol, etc. The hydrophobic surfactant is C6~C 22 Saturated fatty acids, C6~C 22 Unsaturated fatty acids, C6~C 22 Esters, C6~C 22 Amines, C6~C 22 Fatty amines, C6~C 22 One of the fatty amides or a mixture of at least two of them, specifically oleylamine, oleamide, erucamide, dodecylamine, octadecylamine, triethanolamine, stearic acid, glyceryl monostearate, sorbitan laurate, polyoxyethylene sorbitan monostearate, etc., and the solvent is one of ethanol, acetone, ethylene glycol, toluene or a mixture of at least two of them.

[0023] The amount of the hydrophobic surfactant is 0.0001-20% of the silver content of the silver-containing solution, in mass percentage. The hydrophobic surfactant and the solvent are mixed into an organic solvent at a mass ratio of 1:80-10:80. Hot water and the hydrophobic surfactant are used at a mass ratio of 1:1-10:1.

[0024] The following examples are based on the above raw material selection.

[0025] Example 1

[0026] A method for preparing silver powder for conductive paste, specifically comprising the following steps:

[0027] Step S10, preparing a surface treatment agent: adding ethanol to octadecylamine, mixing and stirring at 80°C until completely dissolved to obtain an organic solvent, then adding 80°C hot water to the organic solvent, using a homogenizer to stir at a speed of 10,000 r / min for 3 minutes to form an emulsion surface treatment agent.

[0028] Step S20, dispersion: adding a surface treatment agent into the Ag2CO3 suspension, performing a dispersion treatment, and obtaining a silver-containing mixture.

[0029] Step S30, preparing wet silver powder: mixing the silver-containing mixture with a sufficient amount of formaldehyde solution to cause an oxidation-reduction reaction to generate silver precipitate to form wet silver powder.

[0030] Step S40, drying the wet silver powder to obtain silver powder.

[0031] The dosage of octadecylamine is 0.05% of the silver content of the Ag2CO3 suspension. Octadecylamine and ethanol are mixed into an organic solvent in a mass ratio of 8:80. Hot water and octadecylamine are used in a mass ratio of 1:1.

[0032] Example 2

[0033] A method for preparing silver powder for conductive paste, specifically comprising the following steps:

[0034] Step S10, preparing a surface treatment agent: adding ethanol to octadecylamine, mixing and stirring at 90°C until completely dissolved to obtain an organic solvent, then adding 90°C hot water to the organic solvent, using a homogenizer to stir at a speed of 10,000 r / min for 1 minute to form an emulsion surface treatment agent.

[0035] Step S20, dispersion: adding a surface treatment agent into the Ag2CO3 suspension, performing a dispersion treatment, and obtaining a silver-containing mixture.

[0036] Step S30, preparing wet silver powder: mixing the silver-containing mixture with a sufficient amount of formaldehyde solution to cause an oxidation-reduction reaction to generate silver precipitate to form wet silver powder.

[0037] Step S40, drying the wet silver powder to obtain silver powder.

[0038] The dosage of octadecylamine is 0.05% of the silver content of the Ag2CO3 suspension. Octadecylamine and ethanol are mixed into an organic solvent in a mass ratio of 8:80. Hot water and octadecylamine are used in a mass ratio of 4:1.

[0039] Example 3

[0040] A method for preparing silver powder for conductive paste, specifically comprising the following steps:

[0041] Step S10, preparing a surface treatment agent: adding ethanol to octadecylamine, mixing and stirring at 100°C until completely dissolved to obtain an organic solvent, then adding 100°C hot water to the organic solvent, using a homogenizer to stir at a speed of 10,000 r / min for 3 minutes to form an emulsion surface treatment agent.

[0042] Step S20, dispersion: adding a surface treatment agent into the Ag2CO3 suspension, performing a dispersion treatment, and obtaining a silver-containing mixture.

[0043] Step S30, preparing wet silver powder: mixing the silver-containing mixture with a sufficient amount of formaldehyde solution to cause an oxidation-reduction reaction to generate silver precipitate to form wet silver powder.

[0044] Step S40, drying the wet silver powder to obtain silver powder.

[0045] The dosage of octadecylamine is 0.05% of the silver content of the Ag2CO3 suspension. Octadecylamine and ethanol are mixed into an organic solvent at a mass ratio of 8:80. Hot water and octadecylamine are used at a mass ratio of 6:1.

[0046] Example 4

[0047] A method for preparing silver powder for conductive paste, specifically comprising the following steps:

[0048] Step S10, preparing a surface treatment agent: adding ethanol to erucamide, mixing and stirring at 90°C until all dissolved to obtain an organic solvent, then adding 90°C hot water to the organic solvent, using a homogenizer to stir at a speed of 10000r / min for 3 minutes to form an emulsion surface treatment agent.

[0049] Step S20, dispersion: adding a surface treatment agent into the Ag2CO3 suspension, performing a dispersion treatment, and obtaining a silver-containing mixture.

[0050] Step S30, preparing wet silver powder: mixing the silver-containing mixture with a sufficient amount of formaldehyde solution to cause an oxidation-reduction reaction to generate silver precipitate to form wet silver powder.

[0051] Step S40, drying the wet silver powder to obtain silver powder.

[0052] The dosage of erucic acid amide is 0.05% of the silver content of the Ag2CO3 suspension. Erucic acid amide and ethanol are mixed into an organic solvent in a mass ratio of 8:80. Hot water and erucic acid amide are used in a mass ratio of 8:1.

[0053] Example 5

[0054] A method for preparing silver powder for conductive paste, specifically comprising the following steps:

[0055] Step S10, preparing a surface treatment agent: adding ethylene glycol to dodecylamine, mixing and stirring at 80°C until completely dissolved to obtain an organic solvent, then adding 80°C hot water to the organic solvent, using a homogenizer to stir at a speed of 30,000 r / min for 3 minutes to form an emulsion surface treatment agent.

[0056] Step S20, dispersion: adding a surface treatment agent into the Ag2CO3 suspension, performing a dispersion treatment, and obtaining a silver-containing mixture.

[0057] Step S30, preparing wet silver powder: mixing the silver-containing mixture with a sufficient amount of formaldehyde solution to cause an oxidation-reduction reaction to generate silver precipitate to form wet silver powder.

[0058] Step S40, drying the wet silver powder to obtain silver powder.

[0059] The dosage of dodecylamine is 0.05% of the silver content of the Ag2CO3 suspension. Dodecylamine and ethylene glycol are mixed into an organic solvent at a mass ratio of 10:80. Hot water and dodecylamine are used at a mass ratio of 10:1.

[0060] Example 6

[0061] A method for preparing silver powder for conductive paste, specifically comprising the following steps:

[0062] Step S10, preparing a surface treatment agent: adding ethanol to triethanolamine, mixing and stirring at 90°C until completely dissolved to obtain an organic solvent, then adding 90°C hot water to the organic solvent, using a homogenizer to stir at a speed of 10,000 r / min for 3 minutes to form an emulsion surface treatment agent.

[0063] Step S20, dispersion: adding a surface treatment agent into the Ag2CO3 suspension, performing a dispersion treatment, and obtaining a silver-containing mixture.

[0064] Step S30, preparing wet silver powder: mixing the silver-containing mixture with a sufficient amount of formaldehyde solution to cause an oxidation-reduction reaction to generate silver precipitate to form wet silver powder.

[0065] Step S40, drying the wet silver powder to obtain silver powder.

[0066] The dosage of triethanolamine is 0.0001% of the silver content of the Ag2CO3 suspension. Triethanolamine and ethanol are mixed into an organic solvent in a mass ratio of 8:80. Hot water and triethanolamine are used in a mass ratio of 8:1.

[0067] Example 7

[0068] A method for preparing silver powder for conductive paste, specifically comprising the following steps:

[0069] Step S10, preparing a surface treatment agent: adding acetone to BYK-170, mixing and stirring at 90°C until all dissolved to obtain an organic solvent, then adding 90°C hot water to the organic solvent, stirring at a speed of 10000 r / min for 1 minute using a homogenizer to form an emulsion surface treatment agent.

[0070] Step S20, dispersion: adding a surface treatment agent into the Ag2CO3 suspension, performing dispersion treatment, and obtaining a silver-containing mixture.

[0071] Step S30, preparing wet silver powder: mixing the silver-containing mixture with a sufficient amount of formaldehyde solution to cause an oxidation-reduction reaction to generate silver precipitate to form wet silver powder.

[0072] Step S40, drying the wet silver powder to obtain silver powder.

[0073] The dosage of BYK-170 is 0.05% of the silver content of the Ag2CO3 suspension. BYK-170 and acetone are mixed in a mass ratio of 8:80 to form an organic solvent. Hot water and BYK-170 are used in a mass ratio of 4:1.

[0074] Example 8

[0075] A method for preparing silver powder for conductive paste, specifically comprising the following steps:

[0076] Step S10, preparing a surface treatment agent: adding ethanol to triethanolamine, mixing and stirring at 100°C until completely dissolved to obtain an organic solvent, then adding 100°C hot water to the organic solvent, using a homogenizer to stir at a speed of 10000 r / min for 3 minutes to form an emulsion surface treatment agent.

[0077] Step S20, dispersion: adding a surface treatment agent into the Ag2CO3 suspension, performing dispersion treatment, and obtaining a silver-containing mixture.

[0078] Step S30, preparing wet silver powder: mixing the silver-containing mixture with a sufficient amount of formaldehyde solution to cause an oxidation-reduction reaction to generate silver precipitate to form wet silver powder.

[0079] Step S40, drying the wet silver powder to obtain silver powder.

[0080] The dosage of triethanolamine is 20% of the silver content of the Ag2CO3 suspension. Triethanolamine and ethanol are mixed into an organic solvent in a mass ratio of 8:80. Hot water and triethanolamine are used in a mass ratio of 6:1.

[0081] Example 9

[0082] A method for preparing silver powder for conductive paste, specifically comprising the following steps:

[0083] Step S10, preparing a surface treatment agent: adding toluene to dodecylamine, mixing and stirring at 80°C until completely dissolved to obtain an organic solvent, then adding 80°C hot water to the organic solvent, using a homogenizer to stir at a speed of 30,000 r / min for 3 minutes to form an emulsion surface treatment agent.

[0084] Step S20, dispersion: adding a surface treatment agent into the Ag2CO3 suspension, performing a dispersion treatment, and obtaining a silver-containing mixture.

[0085] Step S30, preparing wet silver powder: mixing the silver-containing mixture with a sufficient amount of formaldehyde solution to cause an oxidation-reduction reaction to generate silver precipitate to form wet silver powder.

[0086] Step S40, drying the wet silver powder to obtain silver powder.

[0087] The dosage of dodecylamine is 0.05% of the silver content of the Ag2CO3 suspension. Dodecylamine and toluene are mixed in a mass ratio of 1:80 to form an organic solvent. Hot water and toluene are used in a mass ratio of 10:1.

[0088] Example 10

[0089] A method for preparing silver powder for conductive paste, specifically comprising the following steps:

[0090] Step S10, preparing a surface treatment agent: adding ethanol to erucamide, mixing and stirring at 90°C until all dissolved to obtain an organic solvent, then adding 90°C hot water to the organic solvent, using a homogenizer to stir at a speed of 10000r / min for 3 minutes to form an emulsion surface treatment agent.

[0091] Step S20, dispersion: adding a surface treatment agent into the Ag2CO3 suspension, performing a dispersion treatment, and obtaining a silver-containing mixture.

[0092] Step S30, preparing wet silver powder: mixing the silver-containing mixture with a sufficient amount of formaldehyde solution to cause an oxidation-reduction reaction to generate silver precipitate to form wet silver powder.

[0093] Step S40, drying the wet silver powder to obtain silver powder.

[0094] The dosage of erucic acid amide is 20% of the silver content of the Ag2CO3 suspension. Erucic acid amide and ethanol are mixed into an organic solvent in a mass ratio of 8:80. Hot water and erucic acid amide are used in a mass ratio of 8:1.

[0095] Embodiment 11

[0096] A method for preparing silver powder for conductive paste, specifically comprising the following steps:

[0097] Step S10, preparing a surface treatment agent: adding ethanol to sorbitan laurate, mixing and stirring at 30°C until all dissolved to obtain an organic solvent, then adding 30°C hot water to the organic solvent, stirring at a speed of 10000r / min for 3 minutes using a homogenizer to form an emulsion surface treatment agent.

[0098] Step S20, dispersion: adding a surface treatment agent into the Ag2CO3 suspension, performing a dispersion treatment, and obtaining a silver-containing mixture.

[0099] Step S30, preparing wet silver powder: mixing the silver-containing mixture with a sufficient amount of formaldehyde solution to cause an oxidation-reduction reaction to generate silver precipitate to form wet silver powder.

[0100] Step S40, drying the wet silver powder to obtain silver powder.

[0101] The dosage of sorbitan laurate is 0.05% of the silver content of the Ag2CO3 suspension. Sorbitan laurate and ethanol are mixed in a mass ratio of 8:80 to form an organic solvent. Hot water and sorbitan laurate are used in a mass ratio of 1:1.

[0102] Example 12

[0103] A method for preparing silver powder for conductive paste, specifically comprising the following steps:

[0104] Step S10, preparing a surface treatment agent: adding ethanol to polyoxyethylene sorbitan monostearate, mixing and stirring at 70°C until completely dissolved to obtain an organic solvent, then adding 70°C hot water to the organic solvent, using a homogenizer to stir at a speed of 10000r / min for 3 minutes to form an emulsion surface treatment agent.

[0105] Step S20, dispersion: adding a surface treatment agent into the Ag2CO3 suspension, performing a dispersion treatment, and obtaining a silver-containing mixture.

[0106] Step S30, preparing wet silver powder: mixing the silver-containing mixture with a sufficient amount of formaldehyde solution to cause an oxidation-reduction reaction to generate silver precipitate to form wet silver powder.

[0107] Step S40, drying the wet silver powder to obtain silver powder.

[0108] The dosage of polyoxyethylene sorbitan monostearate is 0.05% of the silver content of the Ag2CO3 suspension. The polyoxyethylene sorbitan monostearate and ethanol are mixed in a mass ratio of 8:80 to form an organic solvent. Hot water and polyoxyethylene sorbitan monostearate are used in a mass ratio of 1:1.

[0109] Comparative Example 1

[0110] The difference from Example 1 is that the homogenizer is stirred at a speed of 400 r / min for 3 minutes.

[0111] Comparative Example 2

[0112] The difference from Example 1 is that the hydrophilic surfactant-polyvinyl alcohol is used to replace the hydrophobic surfactant-octadecylamine.

[0113] Comparative Example 3

[0114] The difference from Example 1 is that the hot water and octadecylamine are used in a mass ratio of 0.5:1.

[0115] Comparative Example 4

[0116] The difference from Example 5 is that the hot water and dodecylamine are used in a mass ratio of 11:1.

[0117] Comparative Example 5

[0118] The difference from Example 5 is that the homogenizer is stirred at a speed of 40000 r / min for 3 minutes.

[0119] Comparative Example 6

[0120] The difference from Example 5 is that the homogenizer is stirred at a speed of 30000 r / min for 0.5 minute.

[0121] Comparative Example 7

[0122] The difference from Example 4 is that the homogenizer is stirred at a speed of 10000 r / min for 5 minutes.

[0123] Comparative Example 8

[0124] The difference from Example 1 is that in step S10, ethanol is added to octadecylamine, and the mixture is mixed and stirred at 80° C. until the mixture is completely dissolved to obtain an organic solvent, which is used as a surface treatment agent. In this step, water is not heated for emulsification.

[0125] Comparative Example 9

[0126] The difference from Example 3 is that the heating condition is 25°C and the hot water temperature is 25°C.

[0127] The silver powders obtained in each embodiment and each comparative example were tested and compared in the following table:

[0128] Serial number Average particle size μm <![CDATA[Specific surface area m 2 / g]]> <![CDATA[Tap density g / cm 3 > Example 1 0.5 1.6 6.2 Example 2 0.7 1.0 6.0 Example 3 0.7 1.2 6.1 Example 4 1.5 0.5 5.8 Example 5 2 0.4 5.5 Example 6 1.6 0.6 5.6 Example 7 0.7 1.3 6.2 Example 8 0.9 1.1 6.1 Example 9 1.9 0.5 5.7 Example 10 1.2 0.7 6.1 Embodiment 11 0.6 1.5 6.3 Example 12 0.6 1.5 6.2 Comparative Example 1 2.2 0.3 5.2 Comparative Example 2 2.5 0.2 5.1 Comparative Example 3 2.1 0.3 5.5 Comparative Example 4 2.8 0.2 5.1 Comparative Example 5 2.3 0.3 5.2 Comparative Example 6 2.4 0.4 5.5 Comparative Example 7 1.5 0.4 5.0 Comparative Example 8 3.0 0.2 5.0 Comparative Example 9 2.9 0.2 5.4

[0129] The silver powder prepared in the present application can be used to prepare a low-temperature curing conductive paste, which is used in HJT batteries, membrane switches, medical PVC tubes, touch screens, and mobile phone antennas. It can also be used to prepare a high-temperature sintering conductive paste, which is used in TOPcon batteries, PERC batteries, piezoelectric ceramics, chip resistors, chip capacitors, chip inductors, automotive glass, and 5G antennas.

[0130] The working principle of the silver powder preparation method of the present application is as follows: the surface treatment agent is prepared by using a hydrophobic surfactant, and a small amount of hot water is added during the preparation process, and a homogenizer is used for high-speed stirring to form an emulsion phase to form an oil-in-water emulsion. The lipophilic surfactant is lipophilic, and the silver synthesis system is hydrophilic. During the reaction of the silver powder, after the emulsified lipophilic surfactant is added, the surface treatment agent plays a protective role in the growth of the silver powder crystal nucleus to prevent the particle size from increasing. After the reaction is completed, the silver powder particles have a small particle size, uniform distribution, good dispersibility, and no agglomeration, and can be redispersed in a non-polar solvent.

[0131] The data analysis of the embodiments of the present application is as follows:

[0132] 1. From the comparison of the various embodiments, it can be seen that when preparing the surface treatment agent, the mass ratio of the amount of emulsified hot water to the amount of hydrophobic surfactant increases, the particle size of the obtained silver powder increases, and the amount of solvent mixed with the hydrophobic surfactant to form an organic solvent increases, and the particle size of the obtained silver powder decreases. The silver powder prepared by the preparation method of the present application has a particle size range that can be controlled within 0.5 to 2 μm, and the silver powder particles have a narrow particle size distribution and a small average particle size. The smaller the particle size, the larger the specific surface area and the greater the tap density. The specific surface area range can reach 0.3 to 1.5 m 2 / g, the tap density can reach 5.5~6.5g / cm 3 , reflecting the good dispersion of particles.

[0133] 2. Comparison between Example 1 and Comparative Example 1, and between Example 5 and Comparative Example 5 shows that when preparing the surface treatment agent, the emulsification stirring speed is lower than 1000 r / min or higher than 30000 r / min, and the quality of the obtained silver powder is significantly reduced. Figure 1 , 2 They are microscope pictures of the silver powder prepared in Example 1 and Comparative Example 8, both with a magnification of 10,000 times. By comparing the two, it can be seen that the silver powder prepared in Example 1 has uniform particle size, narrow particle size distribution, small average particle size and good dispersibility.

[0134] 3. From the comparison between Example 1 and Comparative Example 2, it can be seen that when the surface treatment agent is prepared, the active agent used is a hydrophilic surfactant, and the quality of the obtained silver powder is significantly reduced.

[0135] 4. By comparing Example 1 with Comparative Example 3, and Example 5 with Comparative Example 4, it can be seen that when preparing the surface treatment agent, the mass ratio of the amount of emulsified hot water to the amount of hydrophobic surfactant is lower than 1:1 or higher than 10:1, and the quality of the obtained silver powder is significantly reduced.

[0136] 5. By comparing Example 5 with Comparative Example 6, it can be seen that when preparing the surface treatment agent, the emulsification stirring time is less than 1 min, and the quality of the obtained silver powder is significantly reduced; by comparing Example 4 with Comparative Example 7, it can be seen that when preparing the surface treatment agent, the emulsification stirring time is more than 3 min, and the quality of the obtained silver powder is equivalent and has not been improved, but the electricity cost and time cost are increased.

[0137] 6. From the comparison between Example 1 and Comparative Example 8, it can be seen that when preparing the surface treatment agent, heated water was not added for emulsification, and the quality of the obtained silver powder was significantly reduced.

[0138] 7. By comparing Example 3 and Comparative Example 9, it can be seen that the dispersibility of the obtained silver powder is closely related to the heating conditions and hot water temperature in the process of preparing the surface treatment agent. Among them, when the heating conditions and hot water temperature are in the range of 80°C to 100°C, the emulsification effect of the surface treatment agent is good and the dispersibility of the silver powder is high; when the heating conditions and hot water temperature are in the range of 30°C to 80°C, the temperature contributes more to the emulsification effect of the surface treatment agent. Generally speaking, when the temperature rises, the smaller the liquid droplets wrapped in the surface treatment agent material system, the better the solubilization effect in the silver powder system, and the better the dispersibility of the obtained silver powder. That is to say, when the temperature is lower than 30°C, the particle size of the liquid droplets formed in the emulsification process is larger, and emulsification may not be achieved.

[0139] 8. For the heating conditions of 30°C to 100°C and hot water temperature of 30°C to 100°C in the step of preparing the surface treatment agent in the technical solution of the present application, preferably under the heating conditions of 80°C to 100°C and hot water temperature of 80°C to 100°C, and using a hydrophobic surfactant with a hydrophile-lipophile balance (HLB) value of 0 to 10, silver powder with good dispersibility and narrow particle size distribution can be prepared; and under the heating conditions of 30°C to 80°C and hot water temperature of 30°C to 80°C, and using a hydrophobic surfactant with a hydrophile-lipophile balance (HLB) value of 8 to 10 (for example, Example 11 and Example 12), silver powder with good dispersibility and narrow particle size distribution can be prepared.

Claims

1. A method for preparing silver powder for conductive paste, characterized in that The following steps are involved: Step S10, preparing a surface treatment agent: mixing a hydrophobic surfactant and a solvent into an organic solvent, generating a solution under heating conditions, and then adding hot water and stirring to form an emulsion surface treatment agent; The hydrophobic surfactant and the solvent are mixed in a mass ratio of 1:80 to 10:80 to form an organic solvent; hot water and the hydrophobic surfactant are used in a mass ratio of 1:1 to 10:1; the hydrophobic surfactant is C6 to C 22 Saturated fatty acids, C6~C 22 Unsaturated fatty acids, C6~C 22 Esters, C6~C 22 Amines, C6~C 22 Fatty amines, C6~C 22 One of the fatty amides or a mixture of at least two of them; the solvent is one of ethanol, acetone, ethylene glycol, toluene or a mixture of at least two of them; the heating condition is 70°C to 100°C, and the hot water temperature is 70°C to 100°C; The amount of the hydrophobic surfactant used is 0.05-20% of the silver content of the silver-containing solution, by mass percentage; the mixture is stirred with a homogenizer at a speed of 10000-30000 r / min for 1-3 minutes to form an emulsion; Step S20, dispersion: adding a surface treatment agent to the silver-containing solution, performing a dispersion treatment, and obtaining a silver-containing mixture; Step S30, preparing wet silver powder: reacting the silver-containing mixture with a reducing agent solution to generate a silver precipitate to form wet silver powder; Step S40, drying the wet silver powder to obtain silver powder.

2. The method for preparing silver powder for conductive paste according to claim 1, characterized in that: In step S20, the silver-containing solution is one of a silver ammonia solution, an Ag2O suspension or an Ag2CO3 suspension.

3. The method for preparing silver powder for conductive paste according to claim 1, characterized in that: In step S30, the reducing agent solution is one of glucose, formaldehyde, hydrazine hydrate, ascorbic acid, sodium isoascorbate, and p-diphenol.