Electrolytic polishing liquid and electrolytic polishing method suitable for nickel-titanium alloy stent

By using electrolytic polishing liquid of glacial acetic acid, perchloric acid, glycerol and ethylene glycol and specific electrolytic parameters, a viscous film is formed, which solves the problems of surface flatness and brightness after polishing of nickel-titanium alloy brackets, and significantly improves the product's pass rate .

CN115522254BActive Publication Date: 2024-11-08SINOMED NEUROVITA TECH INC
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202110713507.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-06-25
Publication Date
2024-11-08
Estimated Expiration
2041-06-25

AI Technical Summary

Technical Problem

The existing electrolytic polishing methods are not suitable for nickel-titanium alloy brackets, which makes it difficult to achieve flat surface and brightness after polishing, and have a low pass rate.

Method used

Provide an electrolytic polishing liquid including glacial acetic acid, perchloric acid, glycerin and ethylene glycol. Combined with specific electrolytic polishing parameters, such as temperature, voltage and time, an intermittent electrolytic polishing method is used to form a viscous film to balance the concave and concave areas of the surface. The resistance promotes metal dissolution and diffusion.

Benefits of technology

Effectively improve the surface flatness and brightness of nickel-titanium alloy brackets, and significantly improve the product's pass rate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115522254B_ABST
    Figure CN115522254B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of medical metal stents, and specifically relates to an electrolytic polishing liquid and an electrolytic polishing method suitable for nickel-titanium alloy stents. The electrolytic polishing liquid suitable for nickel-titanium alloy stents provided by the present invention comprises the following components in percentage by volume: 45%-90% glacial acetic acid; 5%-45% perchloric acid; 0.5%-15% glycerol; 1.5%-25% ethylene glycol. The present invention uses glacial acetic acid, perchloric acid, glycerol and ethylene glycol in a specific ratio to effectively control the dissolution rate of the metal anode (nickel-titanium alloy stent) and the diffusion rate from the anode surface to the electrolyte, and makes the dissolved product accumulate on the electrode surface and form a layer of sticky film, so that the thickness of the mucosa at the micro-convex part of the surface is balanced with the thickness of the concave part, oxygen is easily precipitated, which is beneficial to the dissolution and diffusion of the mucosa, accelerates the dissolution of the metal, and finally completes the polishing process of the nickel-titanium alloy stent, and improves the qualified rate of the product.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of medical metal stents, and particularly relates to an electrolytic polishing liquid and an electrolytic polishing method suitable for nickel-titanium alloy stents. Background Art

[0002] In recent years, stent implantation technology has been widely used, and commonly used materials include stainless steel, cobalt-chromium alloy, etc. Shape memory alloy is a special alloy material that can undergo plastic deformation at a certain temperature and can return to its original shape within a suitable temperature range. Among them, nickel-titanium alloy materials have been widely studied and concerned, and have been applied, due to their excellent biocompatibility, shape memory properties, superelasticity, and less thrombogenicity.

[0003] In order to ensure the long-term mechanical properties, durability and biocompatibility of the nickel-titanium alloy stent, the nickel-titanium alloy stent needs to be further polished and passivated. Electrochemical polishing and passivation treatment can effectively reduce the amount of nickel ions precipitated from the nickel-titanium alloy, form a stable titanium oxide layer, and improve the surface quality and biocompatibility of the nickel-titanium alloy. However, the nickel-titanium stent has corrosion resistance and is also an inactive metal. The methods and steps of conventional electrochemical polishing treatment have a great influence on the performance of the nickel-titanium alloy. The surface flatness and brightness of the nickel-titanium stent after polishing are difficult to achieve, and the qualified rate is low. The flatness of the stent appearance has a decisive influence on the endothelialization process. Therefore, it is necessary to develop a more effective nickel-titanium alloy electrochemical surface treatment process. Summary of the invention

[0004] Therefore, the technical problem to be solved by the present invention is to overcome the defects of the electrolytic polishing method in the prior art that is not suitable for nickel-titanium alloy stents, the surface flatness and brightness of the nickel-titanium stents after polishing are difficult to achieve, and the low pass rate, thereby providing an electrolytic polishing liquid and electrolytic polishing method suitable for nickel-titanium alloy stents.

[0005] To this end, the present invention provides the following technical solutions:

[0006] The present invention provides an electrolytic polishing solution suitable for a nickel-titanium alloy stent, comprising the following components in percentage by volume:

[0007] Glacial acetic acid 45%-90%;

[0008] Perchloric acid 4%-45%;

[0009] Glycerol 0.5%-15%;

[0010] Ethylene glycol 1.5%-25%.

[0011] Optionally, the electrolytic polishing solution of the nickel-titanium alloy stent comprises the following components in percentage by volume:

[0012] Glacial acetic acid 50%-85%;

[0013] Perchloric acid 10%-43%;

[0014] Glycerol 1%-13%;

[0015] Ethylene glycol 2%-23%.

[0016] The present invention also provides an electrolytic polishing method applicable to a nickel-titanium alloy stent, which adopts the electrolytic polishing liquid.

[0017] Optionally, the temperature of the electrolytic polishing is -5°C-40°C, the voltage of the electrolytic polishing is 3V-45V, and the time of the electrolytic polishing is 4min-12min.

[0018] Optionally, the temperature of the electrolytic polishing is -2°C-36°C, and the voltage of the electrolytic polishing is 5V-35V.

[0019] Optionally, the electrolytic polishing is intermittent electrolytic polishing.

[0020] Optionally, during the electrolytic polishing, the time of a single electrolytic polishing is 5s-35s, and the interval time is 2s-15s;

[0021] Preferably, after polishing half a round, turn around and continue polishing.

[0022] Optionally, during the electrolytic polishing, the time for a single electrolytic polishing is 7s-30s, and the interval time is 4-12s.

[0023] Optionally, the electrolytic polishing liquid is electrolytically polished in a circulating and / or stirring state.

[0024] Optionally, a cleaning step is further included before and / or after the electrolytic polishing step.

[0025] Regarding the mixing and preparation steps of the electrolytic polishing solution, the solution needs to be placed in a glass beaker, and the order of addition is: glycerol, ethylene glycol, glacial acetic acid, and perchloric acid. The stirring speed is controlled at 25-800r / min. Glycerol is an alcohol, and perchloric acid is a strong corrosive acid. When preparing the solution, in order to prevent the reaction between strong acid and alcohol, glacial acetic acid is placed in the middle of the order, and also for safety reasons to avoid splashing.

[0026] The technical solution of the present invention has the following advantages:

[0027] 1. The electrolytic polishing liquid of the nickel-titanium alloy stent provided by the present invention comprises the following components in percentage by volume: 45%-90% glacial acetic acid; 5%-45% perchloric acid; 0.5%-15% glycerol; 1.5%-25% ethylene glycol. The present invention uses glacial acetic acid, perchloric acid, glycerol and ethylene glycol in a specific ratio to effectively control the dissolution rate of the metal anode (nickel-titanium alloy stent) and the diffusion rate from the anode surface to the electrolyte, and makes the dissolved product accumulate on the electrode surface and form a sticky film, so that the thickness of the mucosa at the slightly convex part of the surface and the thickness of the concave part reach a balance, oxygen is easily precipitated, which is beneficial to the dissolution and diffusion of the mucosa and accelerates the dissolution of the metal. As the electrolytic polishing time increases, the convex part on the anode surface gradually flattens, making the entire stent surface smooth and bright, and finally completing the polishing process of the nickel-titanium alloy stent, improving the qualified rate of the product. The principle of electrolytic polishing is that under certain conditions, the dissolution rate of the metal anode is faster than the diffusion rate of the dissolved products from the anode surface to the electrolyte, so the dissolved products accumulate on the electrode surface and form a sticky film. The resistance of this mucous film is greater than the resistance of the electrolyte, and it can dissolve in the electrolyte. Its distribution along the anode surface is uneven, and the thickness of the mucous film at the micro-convex part of the surface is less than that at the concave part, which leads to a smaller resistance in the convex part, resulting in current concentration. Compared with the micro-concave part, the current density at the micro-convex part is larger, the potential is increased, and oxygen is easily precipitated, which is conducive to the dissolution and diffusion of the mucous film and accelerates the dissolution of the metal. As the electrolytic polishing time increases, the micro-convex part on the anode surface gradually flattens, making the entire stent surface smooth and bright.

[0028] The electrolytic polishing liquid of the nickel-titanium alloy stent provided by the present invention can further improve the electrolytic polishing effect of the nickel-titanium alloy stent and improve the qualified rate of the product by limiting the amount of each component of the electrolytic polishing.

[0029] 2. The electrolytic polishing method of the nickel-titanium alloy stent provided by the present invention uses the electrolytic polishing solution provided by the present invention. The electrolyte is specially designed for the nickel-titanium alloy stent and can effectively polish the surface of the stent, making it smooth and bright, and greatly improving the qualified rate.

[0030] The electrolytic polishing method of the nickel-titanium alloy stent provided by the present invention has the electrolytic polishing temperature of -5°C-40°C, the electrolytic polishing voltage of 3V-45V, and the electrolytic polishing time of 4min-12min. The present invention has the effect of making the stent surface bright and smooth by limiting the electrolytic polishing parameters. If the temperature is too high, over-corrosion will occur, and if the temperature is too low, the polishing will be incomplete; if the voltage is too low, the surface brightness and flatness cannot be achieved, and if the voltage is too high, the stent is prone to breakage. By limiting the electrolytic polishing parameters, the polishing effect and product qualification rate can be further improved.

[0031] The electrolytic polishing method of the nickel-titanium alloy stent provided by the present invention is intermittent electrolytic polishing. During electrolytic polishing, the time of a single electrolytic polishing is 5s-35s, the interval time is 2s-15s, and after polishing half a round, the polishing is turned around and continued. Such an arrangement can make the appearance and size of the stent after polishing uniform, and the qualified rate of the product is high.

[0032] In the electrolytic polishing method of the nickel-titanium alloy stent provided by the present invention, the electrolytic polishing liquid is electrolytically polished in a circulating and / or stirring state. Such a setting has the effect of making the solution uniform, and avoiding the problem that the stents polished with the same cup of polishing solution have significant differences in appearance and size due to different sequences. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0034] Figure 1 The electrolytic polishing device is used in Example 1 of the present invention;

[0035] Figure 2 This is a microscope image of the stent obtained in Example 1 of the present invention magnified 40 times;

[0036] Figure 3 This is a microscope image of the stent obtained in Example 2 of the present invention magnified 40 times;

[0037] Figure 4 This is a microscope image of the stent obtained in Example 3 of the present invention magnified 40 times;

[0038] Figure 5 This is a microscope image of the bracket obtained in Comparative Example 1 of the present invention magnified 40 times;

[0039] Figure 6 This is a microscope image of the stent obtained in Comparative Example 2 of the present invention magnified 25 times;

[0040] Figure 7 This is a microscope image of the stent obtained in Comparative Example 3 of the present invention magnified 30 times;

[0041] Reference numerals:

[0042] In the figure, a- represents the inner surface of the stent; b- represents the outer surface of the stent;

[0043] 1-solution tank; 2-anode; 3-cathode rod; 4-circulation pump; 5-circulation pipe; 6-mechanical arm; 7-stirrer; 8-control panel. DETAILED DESCRIPTION

[0044] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.

[0045] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.

[0046] Example 1

[0047] This embodiment provides an electrolytic polishing method applicable to a nickel-titanium alloy stent, and the specific steps are as follows:

[0048] (1) Use 10% diluted nitric acid and perform ultrasonic cleaning in an ultrasonic chamber for 10 minutes.

[0049] (2) Electrolytic polishing, using Figure 1 The electrolytic polishing device shown in the figure is operated. The composition of the electrolytic polishing liquid used is: 450 mL of glacial acetic acid, 50 mL of perchloric acid, 5 mL of glycerol, and 15 mL of ethylene glycol. The components of the electrolytic polishing liquid are measured in proportion, and glycerol, ethylene glycol, glacial acetic acid, and perchloric acid are added to a glass beaker in sequence, and stirred and mixed at 500 r / min to obtain the electrolytic polishing liquid.

[0050] After adding electrolytic polishing liquid to the solution tank 1 to the specified scale, turn on the circulation pump 4 and the agitator 7. During the electrolytic polishing process, the electrolyte circulates through the circulation pipe 5 to ensure uniform concentration in the solution tank. The temperature is set to -5°C and the speed is set to 50r / min. The single power-on time is set to 10s, the interval is 6s, and the voltage is 15V through the control box. Fix the cathode rod 3 (stainless steel) in the solution tank 1, fix the nickel-titanium alloy bracket to the anode 2, click Start, the automatic lifting robot arm 6 descends, and the bracket is completely immersed in the middle of the solution. The power is turned on and the voltage and current are displayed on the control screen 8. After 9 single polishings, turn around and continue single polishing 1. After polishing is completed, the robot arm 6 automatically rises.

[0051] (3) The electropolished nickel-titanium alloy stent is ultrasonically cleaned with purified water for 1 to 5 minutes.

[0052] Example 2

[0053] This embodiment provides an electrolytic polishing method applicable to a nickel-titanium alloy stent, and the specific steps are as follows:

[0054] (1) Use 0.5% diluted nitric acid and perform ultrasonic cleaning in an ultrasonic chamber for 1 min.

[0055] (2) Electrolytic polishing, using Figure 1 The electrolytic polishing device shown in the figure is operated. The composition of the electrolytic polishing liquid used is: 90 mL of glacial acetic acid, 45 mL of perchloric acid, 15 mL of glycerol, and 25 mL of ethylene glycol. The components of the electrolytic polishing liquid are measured in proportion, and glycerol, ethylene glycol, glacial acetic acid, and perchloric acid are added to a glass beaker in sequence, and stirred and mixed at 500 r / min to obtain the electrolytic polishing liquid.

[0056] After adding electrolytic polishing liquid to the solution tank to the specified scale, turn on the circulation pump and agitator, set the temperature to 10℃, and the speed to 100r / min. Set the single power-on time to 20s, the interval to 10s, and the voltage to 25V through the control box. Fix the cathode rod (stainless steel) in the solution tank, fix the nickel-titanium alloy bracket to the anode, click start, the automatic mechanical lifting arm descends, the bracket is completely immersed in the middle of the solution, and the power is turned on. The voltage and current are displayed on the control screen. After 4 single polishings, turn around and continue single polishing 5 times. After polishing is completed, the mechanical arm automatically rises.

[0057] (3) The electropolished nickel-titanium alloy stent is ultrasonically cleaned with purified water for 5 minutes.

[0058] Example 3

[0059] This embodiment provides an electrolytic polishing method applicable to a nickel-titanium alloy stent, and the specific steps are as follows:

[0060] (1) Use 5% diluted nitric acid and perform ultrasonic cleaning in an ultrasonic chamber for 5 minutes.

[0061] (2) Electrolytic polishing, using Figure 1 The electrolytic polishing device shown in the figure is operated. The composition of the electrolytic polishing liquid used is: 600 mL of glacial acetic acid, 400 mL of perchloric acid, 60 mL of glycerol, and 60 mL of ethylene glycol. The components of the electrolytic polishing liquid are measured in proportion, and glycerol, ethylene glycol, glacial acetic acid, and perchloric acid are added to a glass beaker in sequence, and stirred and mixed evenly at 500 r / min to obtain the electrolytic polishing liquid.

[0062] After adding electrolytic polishing liquid to the solution tank to the specified scale, turn on the circulation pump and agitator, set the temperature to -2℃, and the speed to 50r / min. Set the single power-on time to 10s, the interval to 10s, and the voltage to 15V through the control box. Fix the cathode rod (stainless steel) in the solution tank, fix the nickel-titanium alloy bracket to the anode, click start, the automatic mechanical lifting arm descends, the bracket is completely immersed in the middle of the solution, and the power is turned on. The voltage and current are displayed on the control screen. After 6 single polishings, turn around and continue single polishing 5 times. After polishing is completed, the mechanical arm automatically rises.

[0063] (3) The electropolished nickel-titanium alloy stent is ultrasonically cleaned with purified water for 1 min.

[0064] Comparative Example 1

[0065] This comparative example provides an electrolytic polishing method suitable for a nickel-titanium alloy stent, and the specific steps are as follows:

[0066] (1) Use 5% diluted nitric acid and perform ultrasonic cleaning in an ultrasonic chamber for 5 minutes.

[0067] (2) Electrolytic polishing, using Figure 1 The electrolytic polishing device shown in the figure is operated. The electrolytic polishing liquid used is composed of: 600 mL of glacial acetic acid, 400 mL of perchloric acid, 60 mL of ethanol, and 60 mL of ethylene glycol. The components of the electrolytic polishing liquid are measured in proportion, and glycerol, ethylene glycol, glacial acetic acid, and perchloric acid are added to a glass beaker in sequence, and stirred and mixed at 200 to 500 r / min to obtain the electrolytic polishing liquid.

[0068] After adding electrolytic polishing liquid to the solution tank 1 to the specified scale, turn on the circulation pump 4 and the agitator 7. During the electrolytic polishing process, the electrolyte circulates through the circulation pipe 5 to ensure uniform concentration in the solution tank. The temperature is set to -2°C and the speed is 50-100r / min. The control box sets the single power-on time to 10-20s, the interval to 6-10s, and the voltage to 15-25V. Fix the cathode rod 3 (stainless steel) in the solution tank 1, fix the nickel-titanium alloy bracket to the anode 2, click to start, the automatic lifting robot arm 6 descends, the bracket is completely immersed in the middle of the solution, and the power is turned on. The voltage and current are displayed on the control screen 8. After 6 single polishings, turn around and continue single polishing 5 times. After polishing is completed, the robot arm 6 automatically rises.

[0069] (3) The electropolished nickel-titanium alloy stent is ultrasonically cleaned with purified water for 1 to 5 minutes.

[0070] Comparative Example 2

[0071] This comparative example provides an electrolytic polishing method suitable for a nickel-titanium alloy stent, and the specific steps are as follows:

[0072] (1) Use 5% diluted nitric acid and perform ultrasonic cleaning in an ultrasonic chamber for 5 minutes.

[0073] (2) Electrolytic polishing, using Figure 1 The electrolytic polishing device shown in the figure is operated. The electrolytic polishing liquid used is composed of: 600 mL of glacial acetic acid, 400 mL of nitric acid, 60 mL of ethanol, and 60 mL of ethylene glycol. The components of the electrolytic polishing liquid are measured in proportion, and glycerol, ethylene glycol, glacial acetic acid, and perchloric acid are added to a glass beaker in sequence, and stirred and mixed at 350 r / min to obtain the electrolytic polishing liquid.

[0074] After adding electrolytic polishing liquid to the solution tank to the specified scale, turn on the circulation pump and agitator, set the temperature to 10℃, and the speed to 100r / min. Set the single power-on time to 20s, the interval to 10s, and the voltage to 25V through the control box. Fix the cathode rod (stainless steel) in the solution tank, fix the nickel-titanium alloy bracket to the anode, click start, the automatic mechanical lifting arm descends, the bracket is completely immersed in the middle of the solution, and the power is turned on. The voltage and current are displayed on the control screen. After 6 single polishings, turn around and continue single polishing 5 times. After polishing is completed, the mechanical arm automatically rises.

[0075] (3) The electropolished nickel-titanium alloy stent is ultrasonically cleaned with purified water for 5 minutes.

[0076] Comparative Example 3

[0077] This comparative example provides an electrolytic polishing method suitable for a nickel-titanium alloy stent, and the specific steps are as follows:

[0078] (1) Use 5% diluted nitric acid and perform ultrasonic cleaning in an ultrasonic chamber for 5 minutes.

[0079] (2) Electrolytic polishing, using Figure 1 The electrolytic polishing device shown in the figure is operated. The electrolytic polishing liquid used is composed of: 600 mL of glacial acetic acid, 400 mL of perchloric acid, 60 mL of glycerol, and 60 mL of ethylene glycol. The components of the electrolytic polishing liquid are measured in proportion, and glycerol, ethylene glycol, glacial acetic acid, and perchloric acid are added to a glass beaker in sequence, and stirred and mixed at 200 to 500 r / min to obtain the electrolytic polishing liquid.

[0080] After adding electrolytic polishing liquid to the solution tank to the specified scale, turn on the circulation pump and agitator, set the temperature to -2℃, and the speed to 50r / min. Set the single power-on time to 10s, the interval to 6-10s, and the voltage to 50V through the control box. Fix the cathode rod (stainless steel) in the solution tank, fix the nickel-titanium alloy bracket to the anode, click start, the automatic mechanical lifting arm descends, the bracket is completely immersed in the middle of the solution, power on, the voltage and current are displayed on the control screen, after 6 single polishings, turn around, and continue single polishing 5 times. After polishing is completed, the mechanical arm automatically rises.

[0081] (3) The electropolished nickel-titanium alloy stent is ultrasonically cleaned with purified water for 1 min.

[0082] Experimental example

[0083] The inner and outer surfaces of the stents of Examples 1-3 and Comparative Examples 1-3 of the present invention were observed and inspected using a stereo microscope to check the brightness and flatness of the stents after polishing. The specific observation results are as follows: Figure 2-7 shown.

[0084] It can be seen from the table that the brightness and flatness of the samples in Examples 1 to 3 are within the acceptable range, and the product qualification rate is about 96%, while the brightness and flatness of the samples in Comparative Examples 1 to 3 are unacceptable, and qualified products cannot be obtained at all. Specifically, in Comparative Example 1, ethanol replaces glycerol, which affects the flatness of the sample. In Comparative Example 2, nitric acid replaces perchloric acid, and the chemical corrosion is higher than the electrochemical corrosion, which affects the flatness. In Comparative Example 3, the voltage is higher than 45V and the same number of polishing circles, the surface brightness is worse than that of the voltage higher than 45V.

[0085] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the scope of protection of the invention.

Claims

1. An electrolytic polishing solution suitable for nickel-titanium alloy stents, It is characterized in that The composition is as follows in terms of volume percentage: Glacial acetic acid 45%-90%; Perchloric acid 10%-45%; Glycerin 0.5%-15%; Ethylene glycol 1.5%-25%.

2. The electrolytic polishing liquid of the nickel-titanium alloy stent according to claim 1, It is characterized in that The composition is as follows in terms of volume percentage: Glacial acetic acid 50%-85%; Perchloric acid 10%-43%; Glycerin 1%-13%; Ethylene glycol 2%-23%.

3. An electrolytic polishing method suitable for nickel-titanium alloy stents, It is characterized in that The electrolytic polishing liquid according to claim 1 or 2 is used, and the voltage of electrolytic polishing is 3V-45V.

4. The electrolytic polishing method of the nickel-titanium alloy stent according to claim 3, It is characterized in that The temperature of the electrolytic polishing is -5°C-40°C, and the time of the electrolytic polishing is 4min-12min.

5. The electrolytic polishing method of the nickel-titanium alloy stent according to claim 4, It is characterized in that The temperature of the electrolytic polishing is -2°C-36°C, and the voltage of the electrolytic polishing is 5V-35V.

6. The electrolytic polishing method of the nickel-titanium alloy stent according to any one of claims 3 to 5, It is characterized in that The electrolytic polishing is intermittent electrolytic polishing.

7. The electrolytic polishing method of the nickel-titanium alloy stent according to claim 6, It is characterized in that During the electrolytic polishing, the time of a single electrolytic polishing is 5s-35s, and the interval time is 2s-15s; After polishing half a round, turn around and continue polishing.

8. The electrolytic polishing method of the nickel-titanium alloy stent according to claim 7, It is characterized in that During the electrolytic polishing, the time of a single electrolytic polishing is 7s-30s, and the interval time is 4-12s.

9. The electrolytic polishing method of the nickel-titanium alloy stent according to any one of claims 3-5 or 7-8, It is characterized in that The electrolytic polishing liquid is electrolytically polished in a circulating and / or stirring state.

10. The electrolytic polishing method of the nickel-titanium alloy stent according to any one of claims 3-5 or 7-8, It is characterized in that A cleaning step is also included before and / or after the electrolytic polishing step.

Citation Information

Patent Citations

  • Electrochemical polishing solution as well as preparation method and application thereof

    CN112267145A

  • Matting treatment of titanium alloy

    JP1991120400A