A preparation method of magnetron sputtering copper target material and application of target material
Through continuous casting and large plastic deformation technology, combined with heat treatment, the problem of difficulty in preparing large-size, ultra-high-purity, ultra-fine crystal copper targets in the existing technology is solved, and the efficient preparation of large-sizes with uniform fine grains and consistent orientation is achieved. Copper targets meet the performance requirements of high-quality sputtering films of integrated circuit interconnects.
Patent Information
- Application Number
- CN202211044447.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-30
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2042-08-30
AI Technical Summary
The prior art is difficult to prepare large-size, ultra-high-purity, ultra-fine crystal high-purity copper targets, and the production efficiency is low, which cannot meet the performance requirements of high-quality sputtering films of nano-level process nodes of ultra-large-scale integrated circuit interconnection lines.
Continuous casting + large plastic deformation + heat treatment integrated technology is adopted to reduce impurities in the melt through bottom argon blowing and electromagnetic stirring treatment, and microstructure is refined by reducing diameter asynchronous stacking technology, and heat treatment ensures uniform grain size and consistent orientation. .
Large-size copper targets with uniform grain size and consistent orientation were prepared, which improved material purity and production efficiency, and were suitable for sputtering coatings of large-scale integrated circuit interconnects, reducing resistance and improving computing speed.
Smart Images

Figure CN115533447B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of sputtering coating of integrated circuit interconnects and magnetron sputtering target materials, and specifically relates to a method for preparing a magnetron sputtering copper target material and application of the target material in sputtering coating of integrated circuit interconnects. Background Art
[0002] In recent years, with the increasing integration of microelectronic devices, the size of materials is developing towards miniaturization, and coating devices are also developing rapidly. Sputtering is the main technical means to prepare high-quality thin film materials. The raw material of sputtering deposition thin film is the target material, which is a special electronic material with high added value.
[0003] At present, copper targets are one of the most widely used metal targets in the electronic information industry. Due to its excellent electromigration resistance, extremely high conductivity, low dielectric constant, good thermal conductivity, ductility and corrosion resistance, it has become one of the preferred key source products in the preparation of integrated circuit interconnects, magnetic heads in the information storage industry, and flat display thin-film transistors. Due to the obvious gap in scientific and technological levels with developed countries, ultra-high purity, ultra-fine grains, and large-size copper targets are still dependent on imports. Therefore, in order to break the international monopoly of related technologies and ensure the sustainable and healthy development of related industries in my country, it is urgent to independently develop key technologies for the preparation of high-purity copper targets to achieve full localization of this product.
[0004] Chinese patent CN113046705A discloses a method for preparing a copper target material for magnetron sputtering, which specifically includes: performing plastic deformation of upsetting and drawing of a high-purity copper target material ingot at high temperature, cooling the target material blank after multiple rounds of upsetting and drawing deformation; rolling and deforming the cooled high-purity copper target material blank into a high-purity copper target blank. The target blank is then heat treated to obtain a high-purity copper target material with a fine and uniform structure, and its average grain size is ≤50μm.
[0005] Chinese patent CN110578126A discloses a method for preparing high-purity copper targets of various specifications. The specific method includes heating the copper ingot, cooling it to room temperature after multiple hot rolling, leveling, cutting, rough machining, leveling, and fine machining to prepare copper targets of various specifications with an average grain size of ≤80μm.
[0006] Chinese patent CN104694888A discloses a copper target material and its preparation method and use. The specific method is to perform hot forging, first heat treatment, cold forging, second heat treatment, first static pressing, second static pressing and rolling on a copper ingot in sequence to prepare a copper target material with a grain size of ≤10μm.
[0007] Chinese patent CN112795876A discloses a copper target material and a preparation method thereof. The specific method is as follows: heating and annealing an oxygen-free copper plate to obtain a large-crystal domain copper plate; then removing the area outside the copper grain boundary in the large-crystal domain copper plate by stamping and cutting to obtain a grain-free copper layer; finally, overlapping and arranging multiple grain-free copper layers along the thickness direction of the target material, and then performing heating and rolling to prepare the copper target material. The copper target material prepared by this method does not mention key information such as grain size and distribution, and the grain-free copper layer is required to be a foil with a thickness of submicron level, and each cutting needs to be combined with characterization means; the overall process is numerous and the operation is complicated, which is not conducive to industrial production.
[0008] In summary, the current copper target material preparation is mainly controlled by forging, rolling, static pressing, and heat treatment to control its microstructure, but due to the limitation of die casting size, it is difficult to prepare large-size, ultra-high purity, ultra-fine-grained high-purity copper targets, and the production efficiency is low. Therefore, in order to meet the various performance requirements of high-quality sputtering films below the nano-scale process node of ultra-large-scale integrated circuit interconnects, it is imperative to independently develop large-size, ultra-fine-grained high-purity copper targets. Summary of the invention
[0009] The technical problem to be solved by the present invention is to overcome the shortcomings of the above-mentioned prior art and provide a method for preparing a magnetron sputtering copper target and an application of the target. On the basis of high-purity copper raw materials purchased from the market, a copper target with uniform and fine grain size, relatively consistent orientation and larger target size is prepared.
[0010] In order to solve the above technical problems, the present invention adopts continuous casting + large plastic deformation + heat treatment integrated technology to prepare copper targets with high density, uniform and fine grain size, relatively consistent orientation and larger target size specifications, which will provide a broader development space for the performance requirements of miniaturization of interconnect line size of ultra-large-scale integrated circuits, reduced resistance and increased computing speed.
[0011] The technical problems to be solved by the present invention include:
[0012] (1) The copper billet is prepared by continuous casting, and the bottom argon blowing and electromagnetic stirring are used to effectively reduce the gas impurity content in the melt; in addition, the electromagnetic braking of the crystallizer produces a "braking effect" and a "stirring effect", which causes the melt to produce strong convection to reduce the concentration gradient at the front of the solidification interface, thereby reducing the impurity content at the front of the solidification interface; ultimately achieving the effect of improving the quality and purity of the ingot. At the same time, the appropriate crystallizer outlet size and billet cutting length can be selected according to the final target product specifications, providing diversified options for subsequent target sizes, especially large sizes;
[0013] (2) Large plastic deformation method - Asymmetrical Accumulative Rolling Bonding (AARB). The deformation zone of this technology adds a rolling zone on the basis of the front sliding zone and the rear sliding zone of ordinary rolling, which causes the composite interface and the neutral layer to not coincide with each other. The pressure, shear force and friction force promote the welding of the interface. At the same time, under the condition of ensuring that the material thickness remains unchanged, the copper billet can be repeatedly and violently plastically deformed to cause the internal grains to be continuously broken, thereby achieving effective refinement of the microstructure and finally obtaining a copper target with ultrafine grains.
[0014] (3) The integrated technology of continuous casting + large plastic deformation + heat treatment can obviously meet the requirements of fine and uniform microstructure and relatively consistent orientation of high-purity copper target.
[0015] Specifically, a method for preparing a magnetron sputtering copper target comprises the following steps:
[0016] (1) Place copper raw materials with a purity of ≥4N into a high-speed continuous casting furnace and set the relevant parameters as follows: temperature 1200°C, vacuum degree 2.3×10 -2 Pa, inert gas protection is filled in, the working gas pressure is 0.01MPa, the cooling water is 25°C, the speed is 80-160mm / min, and continuous casting is performed to obtain copper billets; wherein, the crystallizer outlet length is 120mm-200mm, and the width is 3mm-10mm.
[0017] (2) Billet cutting: Cut the copper billet into equal blocks with lengths ranging from 200 to 600 mm;
[0018] (3) Different-diameter asynchronous stacking: After the two billets are stacked and aligned, one end is ground with a grinder or chamfered with an air hammer to facilitate the mill to bite in; different-diameter asynchronous stacking is carried out under the guidance of the guide groove; rolling speed: 20-30r / min; roller diameter ratio: (500mm-420mm) / 400mm; asynchronous ratio: 1.05-1.25, compression ratio: 50%; the width of the guide groove is 1-2mm wider than the billet; the billets are evenly cut after stacking; the upper and lower surfaces of the copper billet are polished with a belt machine or scrubbed with acid to remove the surface oxide layer until the billet reveals its original copper luster; repeat the above steps to complete 8-10 stacking passes, and perform stress relief annealing after every two stacking passes. Annealing temperature is 250℃-650℃, and heat treatment time is 0.5-2h.
[0019] (4) Same diameter synchronous rolling: rolling speed: 20-30r / min, roller diameter is 400mm, compression ratio: ≤5% / pass; according to the requirements of the final product, the billet after stack rolling is subjected to close-to-size finish rolling. If the size is close to the product size, this step can be omitted;
[0020] (5) Heat treatment: temperature 200℃-300℃, holding time 0.5-1h, vacuum furnace cooling.
[0021] After the above steps are completed, the copper target material prepared by the present invention needs to be leveled, machined, surface treated and cleaned in sequence.
[0022] The average grain size of the copper target material prepared by the invention is ≤1 μm and is evenly distributed, and can be applied to the sputtering coating of large-scale integrated circuit interconnection lines.
[0023] Compared with the prior art, the beneficial effects of the present invention are:
[0024] (1) The present invention adopts continuous casting technology to prepare copper billets. Compared with the existing die casting technology, it not only solves the problem of diversified sizes of high-purity copper targets, especially large sizes, but also improves the internal quality of the material (less inclusions, less component segregation), material purity (less impurities introduced, lower gas impurity content), material utilization rate and production efficiency, and is easy to realize industrial large-scale production;
[0025] (2) The present invention adopts the technology of asynchronous stacking with different diameters, which can significantly reduce the rolling pressure and rolling torque, improve the thickness accuracy and plate shape of the product, and improve the rolling efficiency. It can effectively refine the internal microstructure of the copper billet while ensuring that the material thickness remains unchanged; at the same time, it is not limited by the initial thickness of the ingot, ensuring that the ultrafine grain structure is obtained under the condition of thicker target size. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 : Process flow chart of the method for preparing the magnetron sputtering copper target of the present invention.
[0027] Figure 2 : SEM image of the microstructure of the target material prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0028] The present invention is further described below in conjunction with the accompanying drawings, but the present invention is not limited in any way. Any changes or improvements made based on the teachings of the present invention belong to the protection scope of the present invention.
[0029] The method for preparing a magnetron sputtering copper target of the present invention comprises the following steps:
[0030] (1) Preparation of copper billets by continuous casting: Copper raw materials with a purity of ≥4N are placed in a high-speed continuous casting furnace, and the relevant parameters are set as follows: temperature 1200°C, vacuum degree 2.3×10 -2Pa, inert gas protection is filled in, the working gas pressure is 0.01MPa, the cooling water is 25°C, the speed is 80-160mm / min, and continuous casting is performed to obtain copper billets; wherein, the crystallizer outlet length is 120mm-200mm, and the width is 3mm-10mm.
[0031] (2) Billet cutting: Cut the copper billet into equal blocks with lengths ranging from 200 to 600 mm;
[0032] (3) Different-diameter asynchronous stacking: After the two billets are stacked and aligned, one end is ground with a grinder or chamfered with an air hammer to facilitate the mill to bite in; different-diameter asynchronous stacking is carried out under the guidance of the guide groove: rolling speed: 20-30r / min, roller diameter ratio: (500mm-420mm) / 400mm; asynchronous ratio: 1.05-1.25, compression ratio: 50%; the width of the guide groove is 1-2mm wider than the billet; the billets are evenly cut after stacking; the upper and lower surfaces of the copper billet are polished with a belt machine or scrubbed with acid to remove the surface oxide layer until the billet reveals its original copper luster; repeat the above steps to complete 8-10 stacking passes, and perform stress relief annealing after every two stacking passes. Annealing temperature is 250℃-650℃, and heat treatment time is 0.5-2h.
[0033] (4) Same diameter synchronous rolling: rolling speed: 20-30r / min, roller diameter is 400mm, compression ratio ≤5% / pass; according to the requirements of the final product, the billet after stack rolling is subjected to close-to-size finish rolling. If the size is close to the product size, this step can be omitted;
[0034] (5) Heat treatment: temperature 200℃-300℃, holding time 0.5-1h, vacuum furnace cooling;
[0035] After the copper target material prepared by the present invention is processed through the above steps, it needs to be leveled, machined, surface treated and cleaned in sequence.
[0036] Example 1
[0037] The magnetron sputtering copper target is prepared by the following steps:
[0038] (1) Preparation of copper billets by continuous casting: Copper raw materials with a purity of ≥99.995 (wt.%) were placed in a high-speed continuous casting furnace, and the relevant parameters were set as follows: temperature 1200°C, vacuum degree 2.3×10 -2 Pa was then filled with nitrogen for protection, the working gas pressure was 0.01 MPa, the cooling water was 25°C, and the speed was 100 mm / min, and continuous casting was performed to obtain copper billets; wherein, the crystallizer outlet was 180 mm long and 8 mm wide.
[0039] (2) Copper billet cutting: Cut the copper billet into equal blocks with a length of 450 mm;
[0040] (3) Different-diameter asynchronous lamination: After the two billets are stacked and aligned, one end is ground with a grinder for chamfering; different-diameter asynchronous lamination is performed under the guidance of the guide groove; rolling speed: 25r / min, roller diameter ratio: 450mm / 400mm; asynchronous ratio: 1.12, compression ratio: 50%; guide groove width is 181mm; the billets are evenly cut after lamination; the upper and lower surfaces of the copper billets are ground with a belt machine until the billets reveal their original copper luster; repeat the above operation to complete 8 laminations, and perform stress relief annealing after every two laminations: stress relief annealing after 2 passes: 650℃, 1h; stress relief annealing after 4 passes: 500℃, 1h; stress relief annealing after 6 passes: 350℃, 0.5h; stress relief annealing after 8 passes: 300℃, 0.5h;
[0041] (4) Same diameter synchronous rolling: rolling speed: 25r / min, roller diameter is 400mm, compression ratio = 5% / pass; total compression ratio is 10%;
[0042] (5) Heat treatment: temperature 280°C, holding time 0.75h, vacuum furnace cooling;
[0043] After completing the above steps, the copper target material needs to be produced by leveling, machining, surface treatment and cleaning.
[0044] The SEM image of the copper target in this embodiment is as follows: Figure 2 shown.
[0045] Example 2
[0046] The difference from Example 1 is that (4) asynchronous rolling with different diameters: 9 passes of rolling are completed.
[0047] Example 3
[0048] The difference from Example 1 is that: (4) Different diameter asynchronous rolling: 10 passes of rolling are completed. Stress relief annealing after 10 passes: 280°C, 0.5h;
[0049] Example 4
[0050] The difference from Example 1 is that: (6) Secondary heat treatment: temperature 260°C.
[0051] Example 5
[0052] The difference from Example 1 is that: (6) Secondary heat treatment: temperature 300°C.
[0053] Example 6
[0054] The difference from Example 1 is that (5) the same-diameter synchronous rolling process is not performed.
[0055] Comparative Example 1
[0056] The difference from Example 1 is that (4) asynchronous rolling with different diameters: 4 passes of rolling are completed.
[0057] Comparative Example 2
[0058] The difference from Example 1 is that (4) asynchronous rolling with different diameters: 6 passes of rolling are completed.
[0059] Table 1 Microstructure of the copper target prepared in each embodiment
[0060]
[0061]
[0062] From the above results, it can be seen that when the number of lamination passes is ≥8, the average grain size of the copper target can be controlled at ≤1μm; and as the number of lamination passes increases, the grain refinement effect is more significant, the grain recrystallization temperature is lower, and after heat treatment under the same conditions, the grain structure is finer and more uniform, and the orientation distribution is more consistent. If the crystal plane texture coefficient TC value of a certain (hk1) plane is greater than the average value (25%), the crystal plane is preferentially oriented. The larger the TC value, the higher the degree of preferential orientation, that is, the grain orientation of a certain (hk1) plane is more consistent.
Claims
1. A method for preparing a magnetron sputtering copper target, characterized in that: The copper billet prepared by continuous casting is cut, asynchronously rolled with different diameters, synchronously rolled with the same diameter, and heat treated in sequence to obtain a high-purity copper target with an average grain size of ≤1μm, uniform grain size, and consistent orientation distribution; the specific steps include: Step 1: Place the copper raw material with a purity of ≥4N into a high-speed continuous casting furnace and set the relevant parameters as follows: temperature 1200°C, vacuum degree 2.3×10 -2 After the inert gas protection is filled in, the working gas pressure is 0.01MPa, the cooling water is 25℃, and the speed is 80-160mm / min, and the copper billet is obtained by continuous casting; wherein, the length of the crystallizer outlet is 120mm-200mm, and the width is 3mm-10mm; Step 2, billet cutting: cutting the copper billet into equal pieces; Step 3: Different diameter asynchronous stack rolling (1) After the two billets are stacked and aligned, one end is chamfered to facilitate the rolling mill to bite in; (2) Under the guidance of the guide groove, the different-diameter asynchronous stack rolling process is carried out, the rolling speed is: 20-30r / min, the roller diameter ratio is: (500mm-420mm) / 400mm; the asynchronous ratio is: 1.05-1.25, the compression ratio is: 50%; the width of the guide groove is 1-2mm larger than the width of the billet; (3) The billet is evenly cut after stacking and rolling; (4) Surface treatment of the blank to remove the surface oxide layer; Repeat (1) to (4) to complete 8-10 passes of rolling, and perform stress relief annealing after every two passes of rolling; the stress relief annealing: 250°C-650°C, 0.5-2h, vacuum furnace cooling; Step 4, synchronous rolling with the same diameter: according to the requirements of the final product, the billet after stack rolling is subjected to close-size finish rolling. If the size has reached the product size requirement, this step can be omitted; Step 5, heat treatment: temperature 200℃-300℃, holding time 0.5-1h, vacuum furnace cooling.
2. The preparation method according to claim 1, characterized in that: The dimensions of the crystallizer are: length 180 mm, width 8 mm.
3. The preparation method according to claim 1, characterized in that: In step 2: The copper billet is cut into equal blocks with a size of 200-600 mm.
4. The preparation method according to claim 1, characterized in that: In step 3: The chamfering treatment method is grinding with a grinding machine or forging with an air hammer.
5. The preparation method according to claim 1, characterized in that: In step 3: The copper blank is surface treated by grinding with a sanding machine or scrubbing the upper and lower surfaces of the copper blank with acid until the blank reveals its original copper luster.
6. The preparation method according to claim 1, characterized in that: In step 4: The same-diameter synchronous rolling process has the following characteristics: rolling speed: 20-30r / min, roller diameter is 400mm, and compression ratio is ≤5% / pass.
7. The preparation method according to any one of claims 1 to 6, characterized in that: After the copper target material blank is processed in step 5, it is further processed in sequence by leveling, machining, surface treatment and cleaning.
8. The magnetron sputtering copper target obtained by the method for preparing a magnetron sputtering copper target as described in any one of claims 1 to 7 is used for sputtering coating of large-scale integrated circuit interconnects.