A low temperature resistant hybrid vinyl ester resin and preparation method thereof
By combining the polyether type epoxy vinyl ester resin with the modified polyurethane acrylate resin to form a resin structure with ether bonds and unsaturated double bonds, the problem of poor mechanical properties of epoxy vinyl ester resin in low temperature environments is solved. , achieves high mechanical performance and flexibility effects, and simplifies the production process.
Patent Information
- Application Number
- CN202211125631.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-16
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-09-16
AI Technical Summary
Epoxy vinyl ester resin has poor mechanical properties in low temperature environments, and commonly used toughening methods will lead to a decrease in mechanical strength and heat resistance.
Using a preparation method of low-temperature hybrid vinyl ester resin, by combining the polyether type epoxy vinyl ester resin with a modified polyurethane acrylate resin and reacting with a crosslinked monomer to form an ether bond and a non-existent. The resin structure of saturated double bonds is to improve the flexibility and low temperature resistance of the resin.
It realizes the characteristics of high mechanical properties and good flexibility of resin in low temperature environments, and simplifies the preparation process, reduces production costs, and is suitable for large-scale production.
Smart Images

Figure CN115536784B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a low-temperature resistant hybrid epoxy vinyl ester resin and a preparation method thereof, and belongs to the field of carbon fiber composite materials. Background Art
[0002] Epoxy vinyl ester resin is prepared by reacting epoxy resin with unsaturated carboxylic acid and dissolving them in a cross-linking monomer. It retains the excellent mechanical properties, water resistance, corrosion resistance, heat resistance, electrical insulation properties, etc. of epoxy resin. At the same time, the introduction of unsaturated carbon-carbon double bonds can achieve free radical curing, which is easy to operate and has good curing performance. Therefore, it is widely used.
[0003] There are many rigid segments in the molecular structure of epoxy vinyl ester resin. At low temperatures, the molecular motion slows down, and the resin modulus increases, causing the resin to become brittle and easy to damage. Therefore, epoxy vinyl ester resin cannot be used in low temperature environments for a long time. The common toughening method for epoxy vinyl ester resin is liquid nitrile rubber toughening, which leads to a decrease in the mechanical strength and heat resistance of the resin. In addition, liquid nitrile rubber has a large molecular weight and high viscosity, and its dosage is limited. The molecular weight of the molecular structure containing liquid nitrile rubber is several to dozens of times that of the molecular structure without liquid nitrile rubber, resulting in a wide molecular weight distribution and affecting the uniformity of the material. Summary of the invention
[0004] The invention aims to solve the problem that epoxy vinyl ester resin has poor low temperature resistance, and further provides a method for preparing a low temperature resistant hybrid vinyl ester resin suitable for low temperature environment.
[0005] To achieve the above object, the present invention is achieved as follows:
[0006] The present invention provides a low-temperature resistant hybrid vinyl ester resin, characterized in that the resin is formed by curing raw materials including a vinyl ester resin prepolymer and a cross-linking monomer;
[0007] The vinyl ester resin prepolymer includes polyether epoxy vinyl ester resin and modified polyurethane acrylate resin;
[0008] In the polyether epoxy vinyl ester resin, the ether bond content is not less than 0.5 mol / 100g;
[0009] The modified polyurethane acrylate contains ether bonds and unsaturated double bonds.
[0010] Preferably, the polyether epoxy vinyl ester resin is produced by reacting raw materials including polyether epoxy resin and unsaturated carboxylic acid.
[0011] Preferably, the polyether epoxy vinyl ester resin prepolymer is as shown in formula (I):
[0012]
[0013] in,
[0014] x and y are independently selected from integers of 0-100 and x and y are not 0 at the same time;
[0015] R1 and R2 are independently selected from H and alkyl.
[0016] Preferably, the modified polyurethane acrylate resin is produced by the reaction of raw materials including polyether-modified isocyanate and hydroxy acrylate; and the polyether-modified isocyanate is produced by the reaction of raw materials including isocyanate and polyether polyol.
[0017] Preferably, the modified polyurethane acrylate resin is as shown in formula (II):
[0018]
[0019] in,
[0020] R3 is H, alkyl
[0021] R4 is selected from one of the following structures;
[0022]
[0023] R5 is selected from one of the following structures:
[0024]
[0025] R7, R10 are independently selected from H or alkyl;
[0026] R8, R9 are independently selected from H or alkyl;
[0027] m, n, i, j are independently selected from integers in the range of 0-100, and m and n are not 0 at the same time, and i and j are not 0 at the same time;
[0028] R6 is selected from Wherein, R11 is H or alkyl.
[0029] Preferably, the molar ratio of the epoxy vinyl ester resin prepolymer to the modified polyurethane acrylate resin for synthesizing the low-temperature resistant hybrid vinyl ester resin is 0.1:1-1:0.1.
[0030] Preferably, the crosslinking monomer is selected from one or more of styrene, vinyl toluene, methyl methacrylate, hydroxyethyl methacrylate, n-butyl methacrylate, lauryl methacrylate, hydroxypropyl methacrylate, trimethylolpropane diacrylate and pentaerythritol triacrylate.
[0031] The present invention also provides a method for preparing the low-temperature resistant hybrid vinyl ester resin, comprising the following steps:
[0032] reacting a vinyl ester resin prepolymer with a crosslinking monomer to obtain a low-temperature resistant hybrid vinyl ester resin;
[0033] The vinyl ester resin prepolymer includes polyether epoxy vinyl ester resin and modified polyurethane acrylate resin;
[0034] In polyether epoxy vinyl ester resin, the ether bond content is not less than 0.5 mol / 100g
[0035] The modified polyurethane acrylate contains ether bonds and unsaturated double bonds.
[0036] Preferably, the method further comprises the following steps:
[0037] (i) reacting bisphenol A polyether epoxy resin with unsaturated monocarboxylic acid to form the polyether epoxy vinyl ester resin prepolymer;
[0038] (ii) mixing a polyether polyol, a bisphenol A polyether and an isocyanate to react and generate a polyether-modified isocyanate having isocyanate groups at both ends;
[0039] (iii) reacting an acrylate containing a monohydroxyl group with the polyether-modified isocyanate to generate the modified polyurethane acrylate resin;
[0040] Preferably, one or more of the following conditions are included:
[0041] ① In step (i), the molar ratio of the bisphenol A polyether epoxy resin to the unsaturated monocarboxylic acid is 1:1.8-1:2.2;
[0042] ② In step (i), the reaction is carried out at a temperature of 90-110°C;
[0043] ③ In step (i), the unsaturated monocarboxylic acid includes methacrylic acid and acrylic acid;
[0044] ④ In step (i), it also includes a catalyst 1, which is selected from one or more of trimethylamine, pyridine, dimethyl sulfide, diethylene glycol dimethyl ether, triphenylphosphine, benzyltrimethylammonium chloride, benzyltriethylammonium chloride, benzyldimethylamine, imidazole, 1-methylimidazole, 2-ethyl-4-methylimidazole, 2-heptadecylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole and N-(3-aminopropyl)imidazole;
[0045] ⑤ In step (i), a polymerization inhibitor is also included, wherein the polymerization inhibitor is selected from one or more of tert-butyl hydroquinone, tert-butyl catechol, p-benzoquinone, hydroquinone and methyl hydroquinone;
[0046] ⑥ In step (ii), after mixing the polyether polyol and bisphenol A polyether, the temperature is raised to 110-115°C and kept at this temperature for 0.5-3h; the temperature is lowered to 60°C; after adding isocyanate, the mixture is reacted at a temperature of 60-80°C for 2-4h;
[0047] ⑦ In step (ii), the ratio of the sum of the moles of the polyether polyol and the bisphenol A polyether to the mole of the isocyanate is 1:2;
[0048] ⑧ In step (ii), the reaction formula further comprises a catalyst 2, and the catalyst 2 is selected from one or more of triethylenediamine, bis(dimethylaminoethyl) ether, N,N-dimethylcyclohexylamine, N-ethylmorpholine, N,N-dimethylbenzylamine, 2,4,6-(dimethylaminomethyl)phenol, dibutyltin dilaurate, stannous octoate and bismuth carboxylate;
[0049] ⑨ In step (iii), add monohydroxy acrylate and raise the temperature to 60-70°C;
[0050] ⑩ In step (iii), the molar ratio of the monohydroxy acrylate to the isocyanate is 1-1.5:1:1;
[0051] Preferably,
[0052] In step (i), the mass of catalyst 1 is 0.10%-0.30% of the sum of the mass of the bisphenol A polyether epoxy resin and the unsaturated monocarboxylic acid;
[0053] And / or, in step (i), the mass of the polymerization inhibitor is 0.02%-0.05% of the sum of the mass of the bisphenol A polyether epoxy resin and the unsaturated monocarboxylic acid;
[0054] and / or, in step (ii), the mass of catalyst 2 is 0.05%-0.50% of the sum of the mass of the polyether polyol, bisphenol A polyether and isocyanate;
[0055] Compared with the prior art, the technical solution of the present invention has at least the following advantages:
[0056] The low temperature resistant hybrid vinyl ester resin of the present invention has the characteristics of high mechanical properties, good flexibility and good low temperature resistance. The vinyl ester resin prepared by the present invention contains a mixed structure of polyether modified epoxy vinyl ester resin and modified polyurethane acrylate resin, wherein the polyether modified epoxy vinyl ester resin has an increased ether bond content and a carbon-carbon straight chain structure compared with the traditional epoxy vinyl ester resin, thereby improving flexibility. In addition, the modified polyurethane acrylate is a polyurethane modified flexible structure containing an ether bond and contains a carbon-carbon unsaturated double bond, which can be cross-linked and cured with the polyether modified epoxy vinyl ester resin through free radicals.
[0057] The epoxy vinyl ester preparation method of the invention has simple process, low production cost, no by-product generation, high yield, is suitable for large-scale quantitative production, and has extremely high promotion prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0058] Figure 1 Schematic diagram of the preparation process of low-temperature resistant hybrid vinyl ester resin in one embodiment of the present invention. DETAILED DESCRIPTION
[0059] The invention provides a method for preparing a low-temperature resistant hybrid vinyl ester resin suitable for low-temperature environments.
[0060] The low temperature resistant hybrid vinyl ester resin provided by the present invention comprises epoxy vinyl ester prepolymers of chemical formula I and chemical formula II, modified polyurethane acrylate resin and diluent monomer;
[0061] [Chemical Formula I]
[0062]
[0063] Wherein, x, y are integers in the range of 0-100 and x, y are not 0 at the same time; R1, R2 are independently selected from H or alkyl;
[0064] [Chemical Formula II]
[0065]
[0066] In the formula, R3 is H or an alkyl group, and R4 is a polyether polyol or a bisphenol A polyether except for the structure of -OH, selected from one of the following structures:
[0067]
[0068] R5 is a structure other than isocyanate minus -NCO, selected from one of the following structures:
[0069]
[0070] R7, R10 are independently selected from H or alkyl;
[0071] R8, R9 are independently selected from H or alkyl;
[0072] m, n, i, and j are independently selected from integers in the range of 0-100, and m and n are not 0 at the same time, and i and j are not 0 at the same time;
[0073] R6 is selected from Wherein, R11 is H or alkyl.
[0074] The present invention provides an epoxy vinyl ester resin prepared by a method comprising the following steps:
[0075] Bisphenol A polyether epoxy resin reacts with unsaturated monocarboxylic acid to generate polyether epoxy vinyl ester resin prepolymer for standby use;
[0076] Put polyether polyol, bisphenol A polyether and isocyanate into a reaction kettle, heat and react to obtain polyether-modified isocyanate with isocyanate groups at both ends;
[0077] The acrylate containing monohydroxyl group is added to the polyether-modified isocyanate prepared in the second step to react, thereby obtaining a modified polyurethane acrylate resin containing carbon-carbon unsaturated double bonds.
[0078] The polyether epoxy vinyl ester resin prepolymer and the modified polyurethane acrylate resin are dissolved in a crosslinking monomer to obtain a low-temperature resistant hybrid vinyl ester resin.
[0079] Among them, the molar ratio of the bisphenol A polyether epoxy resin to the unsaturated monocarboxylic acid is 1:2; the ratio of the sum of the molar numbers of the polyether polyol and the bisphenol A polyether to the molar number of isocyanate is 1:2; the molar ratio of the polyether polyol to the bisphenol A polyether is 0.1-1:1; the molar ratio of the monohydroxy acrylate to the isocyanate is 1:1; the molar ratio of the polyether epoxy vinyl ester resin prepolymer to the modified polyurethane acrylate resin is 0.1:1-1:0.1; the mass of the cross-linking monomer is 50.0%-100.0% of the sum of the masses of the polyether epoxy vinyl ester resin prepolymer and the modified polyurethane acrylate resin.
[0080] Figure 1 Schematic diagram of the preparation process of epoxy vinyl ester resin in one embodiment of the present invention.
[0081] In the present invention, the bisphenol A polyether epoxy resin refers to an epoxy resin containing an ether bond structure in its molecular structure prepared by reacting bisphenol A polyether polyol with epichlorohydrin, and the epoxy value is 0.20-0.54eq / 100g.
[0082] In the present invention, the unsaturated monocarboxylic acid is one of methacrylic acid and acrylic acid.
[0083] In the present invention, the polyether polyol has a structure in which the molecular end groups contain two hydroxyl groups and the molecular chain segments are composed of ether chains (—R—O—R′—) and have a number average molecular weight of 100-400.
[0084] In the present invention, the bisphenol A polyether is obtained by reacting bisphenol A with propylene oxide or a mixture of ethylene oxide and propylene oxide. The generated molecular end groups contain two hydroxyl groups, the molecular chain segments are composed of ether chains (—R—O—R'—) and bisphenol A structures, and the molar ratio of propylene oxide or the mixture of ethylene oxide and propylene oxide to bisphenol A is 2:1 or 4:1.
[0085] In the present invention, the isocyanate is at least one of toluene diisocyanate, isophorone diisocyanate, diphenylmethane diisocyanate, dicyclohexylmethane diisocyanate, hexamethylene diisocyanate, lysine diisocyanate and xylylene diisocyanate.
[0086] In the present invention, the monohydroxy acrylate is at least one of hydroxyethyl acrylate, hydroxypropyl acrylate, hydroxyethyl methacrylate and hydroxypropyl methacrylate.
[0087] In the present invention, catalyst 1 is at least one of trimethylamine, pyridine, dimethyl sulfide, diethylene glycol dimethyl ether, triphenylphosphine, benzyltrimethylammonium chloride, benzyltriethylammonium chloride, benzyldimethylamine, imidazole, 1-methylimidazole, 2-ethyl-4-methylimidazole, 2-heptadecylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole and N-(3-aminopropyl)imidazole.
[0088] In the present invention, catalyst 2 is at least one of triethylenediamine, bis(dimethylaminoethyl) ether, N,N-dimethylcyclohexylamine, N-ethylmorpholine, N,N-dimethylbenzylamine, 2,4,6-(dimethylaminomethyl)phenol, dibutyltin dilaurate, stannous octoate and bismuth carboxylate.
[0089] In the present invention, the polymerization inhibitor is one or more of tert-butyl hydroquinone, tert-butyl catechol, p-benzoquinone, hydroquinone and methyl hydroquinone.
[0090] The present invention does not impose strict restrictions on the cross-linking monomer, as long as it can be cross-linked and cured with the resin base material. In some embodiments of the present invention, the cross-linking monomer can be at least one of styrene, vinyl toluene, methyl methacrylate, hydroxyethyl methacrylate, n-butyl methacrylate, lauryl methacrylate, hydroxypropyl methacrylate, trimethylolpropane diacrylate and pentaerythritol triacrylate.
[0091] The low-temperature resistant hybrid vinyl ester resin as described above, wherein bisphenol A polyether epoxy resin reacts with unsaturated monocarboxylic acid to generate a polyether epoxy vinyl ester resin prepolymer. Bisphenol A polyether epoxy resin is prepared by reacting and cyclizing 1 mol of bisphenol A polyether with 2 mol of epichlorohydrin. 1 mol of bisphenol A polyether contains 2-4 ether bonds in its molecular structure. After reacting with 2 mol of epichlorohydrin, 2 ether bonds are added, so that 1 mol of bisphenol A polyether epoxy resin contains 4-6 ether bonds. Compared with bisphenol A epoxy resin prepared by the same method, the number of ether bonds is increased, giving the resin good flexibility. Including:
[0092] At 90-95° C., unsaturated monocarboxylic acid and polymerization inhibitor are added to bisphenol A polyether epoxy resin and mixed evenly, catalyst 1 is added, the temperature is raised to 105-110° C., the acid value is tested every 30 minutes, and the reaction is stopped when the acid value reaches 10-15 mg KOH / g to obtain the polyether epoxy vinyl ester resin prepolymer;
[0093] Wherein, the molar ratio of the bisphenol A polyether epoxy resin to the unsaturated monocarboxylic acid is 1:1.8-2.2.
[0094] The mass of the polymerization inhibitor is 0.02%-0.05% of the sum of the mass of the bisphenol A polyether epoxy resin and the unsaturated monocarboxylic acid.
[0095] The mass of the catalyst 1 is 0.10%-0.30% of the sum of the mass of the bisphenol A polyether epoxy resin and the unsaturated monocarboxylic acid.
[0096] The low-temperature resistant hybrid vinyl ester resin as described above, wherein polyether polyol, bisphenol A polyether, and isocyanate are put into a reactor, and the temperature is raised to react to obtain a polyether-modified isocyanate with isocyanate groups at both ends. 2 mol of isocyanate reacts with 1 mol of a mixture of polyether polyol and bisphenol A polyether, the isocyanate group at one end of the isocyanate is consumed, the molecular weight increases, and the ether bond and carbon-carbon straight chain in the polyether polyol or bisphenol A polyether increase the flexibility of the isocyanate, so that the obtained polyether-modified isocyanate with isocyanate groups at both ends has greatly improved flexibility compared with the original isocyanate. Including:
[0097] Put polyether polyol and bisphenol A polyether into a reaction kettle in sequence, heat to 110-115°C, keep warm for 0.5-3.0h, and remove moisture; cool to 60°C, add catalyst 2, gradually add isocyanate, control the reaction temperature at 60-80°C, start timing after the isocyanate is added, stop the reaction after 2.0-4.0h, and obtain a polyether-modified isocyanate with isocyanate groups at both ends;
[0098] The molar ratio of the sum of the polyether polyol and the bisphenol A polyether resin to the isocyanate is 1:2.
[0099] The mass of the catalyst 2# is 0.05%-0.50% of the sum of the mass of the polyether polyol, bisphenol A polyether and isocyanate.
[0100] The low-temperature resistant hybrid vinyl ester resin as described above, wherein the acrylate containing a monohydroxyl group is added to the polyether-modified isocyanate prepared in the second step for reaction, and the hydroxyl group in the monohydroxyl acrylate can react with the isocyanate group in the polyether-modified isocyanate, and at the same time, the carbon-carbon double bond in the monohydroxyl acrylate is introduced into the molecular structure to obtain a modified polyurethane acrylate resin containing a carbon-carbon unsaturated double bond. The hydroxyl group on the acrylate is used to end-cap the remaining isocyanate group of the isocyanate, and an unsaturated carbon-carbon double bond is introduced, which can be cross-linked and cured with the unsaturated double bond in the polyether-modified epoxy vinyl ester resin. At the same time, the obtained polyurethane acrylate structure has better flexibility than the polyether-modified epoxy vinyl ester resin, which can improve the low-temperature resistance of this hybrid vinyl ester resin. It includes:
[0101] Putting monohydroxy acrylate into a reaction kettle containing polyether-modified isocyanate, heating to 60-70°C, testing the isocyanate value, and stopping the reaction when the isocyanate value is 0 to obtain a modified polyurethane acrylate resin containing carbon-carbon unsaturated double bonds;
[0102] Wherein, the molar ratio of the monohydroxy acrylate to the isocyanate is 1-1.5:1.
[0103] The low temperature resistant hybrid vinyl ester resin as described above, wherein a polyether epoxy vinyl ester resin prepolymer and a modified polyurethane acrylate resin are dissolved in a cross-linking monomer to obtain the low temperature resistant hybrid vinyl ester resin, comprises:
[0104] Put the crosslinking monomer into a dilution kettle, add the above-mentioned inhibitor and stir evenly, gradually add the polyether epoxy vinyl ester resin prepolymer and the modified polyurethane acrylate resin into the reaction kettle containing the crosslinking monomer, stir for 2-4 hours, and obtain a low-temperature resistant hybrid vinyl ester resin;
[0105] Wherein, the molar ratio of the polyether epoxy vinyl ester resin prepolymer to the modified polyurethane acrylate resin is 0.1:1-1:0.1.
[0106] The mass of the polymerization inhibitor is 0.01%-0.03% of the sum of the mass of the polyether epoxy vinyl ester resin prepolymer, the modified polyurethane acrylate resin and the cross-linking monomer.
[0107] The mass of the cross-linking monomer is 50.0%-100.0% of the sum of the mass of the polyether epoxy vinyl ester resin prepolymer and the modified polyurethane acrylate resin.
[0108] The mass of the polymerization inhibitor is 0.01%-0.03% of the sum of the mass of the polyether epoxy vinyl ester resin prepolymer, the modified polyurethane acrylate resin and the cross-linking monomer.
[0109] The low-temperature resistant hybrid vinyl ester resin of the present invention has the characteristics of high mechanical properties, good flexibility and good low-temperature resistance. The vinyl ester resin prepared by the present invention contains a mixed structure of polyether-modified epoxy vinyl ester resin and modified polyurethane acrylate resin. Among them, the polyether-modified epoxy vinyl ester resin is prepared by reacting a polyether-type epoxy resin with an unsaturated monocarboxylic acid. 1 mol of the polyether-type epoxy resin contains 4-10 mol of ether bonds, and a common epoxy resin of equivalent molecular weight contains 2-3 mol of ether bonds, and the ether bond content is increased by more than 100%; in addition, the modified polyurethane acrylate is a polyurethane-modified flexible structure containing ether bonds. 1 mol of the modified polyurethane acrylate contains 2 mol of carbon-carbon unsaturated double bonds. In the free radical-induced curing process, the carbon-carbon unsaturated double bonds become single bonds, which can be cross-linked and cured with the carbon-carbon unsaturated double bonds in the polyether-modified epoxy vinyl ester resin to form a cross-linked network.
[0110] The epoxy vinyl ester preparation method of the invention has simple process, low production cost, no by-product generation, high yield, is suitable for large-scale quantitative production, and has extremely high promotion prospects.
[0111] The following is a detailed description of the method for synthesizing the epoxy vinyl ester resin for carbon fiber of the present invention through specific examples. In the following examples, all raw materials can be purchased commercially.
[0112] Example 1
[0113] 464 g of bisphenol A polyether epoxy resin (1 mol of epoxy resin contains 4 ether bonds, and the epoxy equivalent is 0.43 eq / 100 g) is put into a reaction flask, the temperature is raised to 90-95° C., 172 g of methacrylic acid is added, 0.19 g of tert-butyl catechol is added, the mixture is stirred for 10 minutes, 1.27 g of triphenylphosphine is added, the temperature is raised to 105-110° C., the acid value is tested every 30 minutes, and the reaction is stopped when the acid value reaches 10-15 mg KOH / g to obtain a polyether epoxy vinyl ester resin prepolymer;
[0114] 200g of polyether polyol (PPG 400, molecular weight 400) and 236g of bisphenol A polyether (1mol of bisphenol A polyether contains 4 ether bonds, molecular weight 472) are sequentially added into another reaction flask, the temperature is raised to 110-115°C, the temperature is kept for 1h, and the water is removed; the temperature is lowered to 60°C, 1.9g of dibutyltin dilaurate is added, and 525g of diphenylmethane diisocyanate (NCO content 32%) is gradually added, and the reaction temperature is controlled at 60-80°C. The timing starts when the diphenylmethane diisocyanate is added, and the reaction is stopped after 3h to obtain a polyether-modified isocyanate with isocyanate groups at both ends; 232g of hydroxyethyl acrylate is added into the above reactor, the temperature is raised to 60-70°C, and the isocyanate value is tested every 30 minutes. When the isocyanate value is 0, the reaction is stopped to obtain a modified polyurethane acrylate resin containing carbon-carbon unsaturated double bonds;
[0115] 1465g of styrene was put into the dilution kettle in advance, and 0.33g of hydroquinone was added and stirred for 30 minutes; the polyether epoxy vinyl ester resin prepolymer and modified polyurethane acrylate resin prepared in the first two steps were added into the dilution kettle and stirred for 3h to obtain a low-temperature resistant hybrid vinyl ester resin.
[0116] Example 2
[0117] The raw materials used in Example 2 are the same as those in Example 1, except that the molar ratio of the polyether epoxy vinyl ester resin prepolymer to the modified polyurethane acrylate resin is changed from 1:1 to 2:1.
[0118] 464 g of bisphenol A polyether epoxy resin (1 mol of epoxy resin contains 4 ether bonds, and the epoxy equivalent is 0.43 eq / 100 g) is put into a reaction flask, the temperature is raised to 90-95° C., 172 g of methacrylic acid is added, 0.19 g of tert-butyl catechol is added, the mixture is stirred for 10 minutes, 1.27 g of triphenylphosphine is added, the temperature is raised to 105-110° C., the acid value is tested every 30 minutes, and the reaction is stopped when the acid value reaches 10-15 mgKOH / g to obtain a polyether epoxy vinyl ester resin prepolymer;
[0119] 100g of polyether polyol (PPG 400, molecular weight 400) and 118g of bisphenol A polyether (1 mol of bisphenol A polyether contains 4 ether bonds, molecular weight 472) are sequentially put into another reaction flask, the temperature is raised to 110-115°C, kept warm for 1h, and the water is removed; the temperature is lowered to 60°C, 0.95g of dibutyltin dilaurate is added, 262.5g of diphenylmethane diisocyanate (NCO content 32%) is gradually added, the reaction temperature is controlled at 60-80°C, the timing starts after the diphenylmethane diisocyanate is added, and the reaction is stopped after 3h to obtain a polyether-modified isocyanate with isocyanate groups at both ends; 116g of hydroxyethyl acrylate is put into the above reactor, the temperature is raised to 60-70°C, the isocyanate value is tested every 30 minutes, and the reaction is stopped when the isocyanate value is 0 to obtain a modified polyurethane acrylate resin containing carbon-carbon unsaturated double bonds;
[0120] 986 g of styrene was put into the dilution kettle in advance, and 0.22 g of hydroquinone was added and stirred for 30 minutes; the polyether epoxy vinyl ester resin prepolymer and modified polyurethane acrylate resin prepared in the first two steps were added into the dilution kettle and stirred for 3 hours to obtain a low-temperature resistant hybrid vinyl ester resin.
[0121] Example 3
[0122] The raw materials used in Example 3 are the same as those in Example 1, except that the molar ratio of the polyether epoxy vinyl ester resin prepolymer to the modified polyurethane acrylate resin is changed from 1:1 to 1:2.
[0123] 464 g of bisphenol A polyether epoxy resin (1 mol of epoxy resin contains 4 ether bonds, and the epoxy equivalent is 0.43 eq / 100 g) is put into a reaction flask, the temperature is raised to 90-95° C., 172 g of methacrylic acid is added, 0.19 g of tert-butyl catechol is added, the mixture is stirred for 10 minutes, 1.27 g of triphenylphosphine is added, the temperature is raised to 105-110° C., the acid value is tested every 30 minutes, and the reaction is stopped when the acid value reaches 10-15 mg KOH / g to obtain a polyether epoxy vinyl ester resin prepolymer;
[0124] 400g of polyether polyol (PPG 400, molecular weight 400) and 472g of bisphenol A polyether (1 mol of bisphenol A polyether contains 4 ether bonds, molecular weight 472) are sequentially put into another reaction flask, the temperature is raised to 110-115°C, kept warm for 1h, and the water is removed; the temperature is lowered to 60°C, 3.8g of dibutyltin dilaurate is added, 1050g of diphenylmethane diisocyanate (NCO content 32%) is gradually added, the reaction temperature is controlled at 60-80°C, the timing starts after the diphenylmethane diisocyanate is added, and the reaction is stopped after 3h to obtain a polyether-modified isocyanate with isocyanate groups at both ends; 464g of hydroxyethyl acrylate is put into the above reactor, the temperature is raised to 60-70°C, the isocyanate value is tested every 30 minutes, and the reaction is stopped when the isocyanate value is 0 to obtain a modified polyurethane acrylate resin containing carbon-carbon unsaturated double bonds;
[0125] Put 2420g of styrene into the dilution kettle in advance, add 0.54g of hydroquinone, and stir for 30 minutes; add the polyether epoxy vinyl ester resin prepolymer and modified polyurethane acrylate resin prepared in the first two steps into the dilution kettle, stir for 3h, and obtain a low-temperature resistant hybrid vinyl ester resin.
[0126] Example 4
[0127] The molecular weight of the bisphenol A polyether epoxy resin used in Example 4 is different from that in Example 1, and other raw materials are the same. The selected bisphenol A polyether epoxy resin contains 6 ether bonds.
[0128] 584 g of bisphenol A polyether epoxy resin (1 mol of epoxy resin contains 6 ether bonds, and the epoxy equivalent is 0.34 eq / 100 g) is put into a reaction flask, the temperature is raised to 90-95° C., 172 g of methacrylic acid is added, 0.23 g of tert-butyl catechol is added, the mixture is stirred for 10 minutes, 1.51 g of triphenylphosphine is added, the temperature is raised to 105-110° C., the acid value is tested every 30 minutes, and the reaction is stopped when the acid value reaches 10-15 mg KOH / g to obtain a polyether epoxy vinyl ester resin prepolymer;
[0129] 200g of polyether polyol (PPG 400, molecular weight 400) and 236g of bisphenol A polyether (1mol of bisphenol A polyether contains 4 ether bonds, molecular weight 472) are sequentially added into another reaction flask, the temperature is raised to 110-115°C, the temperature is kept for 1h, and the water is removed; the temperature is lowered to 60°C, 1.9g of dibutyltin dilaurate is added, and 525g of diphenylmethane diisocyanate (NCO content 32%) is gradually added, and the reaction temperature is controlled at 60-80°C. The timing starts when the diphenylmethane diisocyanate is added, and the reaction is stopped after 3h to obtain a polyether-modified isocyanate with isocyanate groups at both ends; 232g of hydroxyethyl acrylate is added into the above reactor, the temperature is raised to 60-70°C, and the isocyanate value is tested every 30 minutes. When the isocyanate value is 0, the reaction is stopped to obtain a modified polyurethane acrylate resin containing carbon-carbon unsaturated double bonds;
[0130] 1560g of styrene was put into the dilution kettle in advance, and 0.35g of hydroquinone was added, and stirred for 30 minutes; the polyether epoxy vinyl ester resin prepolymer and modified polyurethane acrylate resin prepared in the first two steps were added into the dilution kettle, and stirred for 3h to obtain a low-temperature resistant hybrid vinyl ester resin.
[0131] Example 5
[0132] The isocyanate type used in Example 5 is different from that in Example 1, and the other raw materials are the same. The selected isocyanate is xylylene diisocyanate, and the isocyanate group is not directly connected to the benzene ring to prevent the resonance of the isocyanate group and the benzene ring, and the yellowing resistance is good.
[0133] 464 g of bisphenol A polyether epoxy resin (1 mol of epoxy resin contains 4 ether bonds, and the epoxy equivalent is 0.43 eq / 100 g) is put into a reaction flask, the temperature is raised to 90-95° C., 172 g of methacrylic acid is added, 0.19 g of tert-butyl catechol is added, the mixture is stirred for 10 minutes, 1.27 g of triphenylphosphine is added, the temperature is raised to 105-110° C., the acid value is tested every 30 minutes, and the reaction is stopped when the acid value reaches 10-15 mg KOH / g to obtain a polyether epoxy vinyl ester resin prepolymer;
[0134] 200g of polyether polyol (PPG 400, molecular weight 400) and 236g of bisphenol A polyether (1mol of bisphenol A polyether contains 4 ether bonds, molecular weight 472) are sequentially added into another reaction flask, the temperature is raised to 110-115°C, the temperature is kept for 1h, and the water is removed; the temperature is lowered to 60°C, 1.6g of dibutyltin dilaurate is added, and 377.5g of xylylene diisocyanate (NCO content 44.5%) is gradually added, the reaction temperature is controlled at 60-80°C, the timing starts after the xylylene diisocyanate is added, and the reaction is stopped after 3h to obtain a polyether-modified isocyanate with isocyanate groups at both ends; 232g of hydroxyethyl acrylate is added into the above reactor, the temperature is raised to 60-70°C, the isocyanate value is tested every 30 minutes, and the reaction is stopped when the isocyanate value is 0 to obtain a modified polyurethane acrylate resin containing carbon-carbon unsaturated double bonds;
[0135] 1345g of styrene was put into the dilution kettle in advance, and 0.30g of hydroquinone was added and stirred for 30 minutes; the polyether epoxy vinyl ester resin prepolymer and modified polyurethane acrylate resin prepared in the first two steps were added into the dilution kettle and stirred for 3h to obtain a low-temperature resistant hybrid vinyl ester resin.
[0136] Comparative Example 1
[0137] Comparative Example 1: A bisphenol A epoxy resin having an epoxy equivalent equivalent to that of Example 1 is selected and reacted with methacrylic acid to obtain an epoxy vinyl ester resin, which does not contain a polyurethane acrylate structure.
[0138] 454.5 g of bisphenol A epoxy resin (1 mol of epoxy resin contains 2 ether bonds, E44 epoxy resin, epoxy equivalent 0.44 eq / 100 g) was put into a reaction flask, the temperature was raised to 90-95° C., 172 g of methacrylic acid was added, 0.18 g of tert-butyl catechol was added, the mixture was stirred for 10 minutes, 1.26 g of triphenylphosphine was added, the temperature was raised to 105-110° C., the acid value was tested every 30 minutes, and the reaction was stopped when the acid value reached 10-15 mg KOH / g to obtain an epoxy vinyl ester resin prepolymer;
[0139] 501 g of styrene was put into the dilution kettle in advance, and 0.11 g of hydroquinone was added and stirred for 30 minutes; the above epoxy vinyl ester resin prepolymer was added into the dilution kettle and stirred for 3 hours to obtain ordinary epoxy vinyl ester resin.
[0140] Test example
[0141] The vinyl ester resins obtained in the above Examples 1-5 and Comparative Example 1 were tested for the retention rate of cast bodies at low temperatures. The test results are shown in Table 1.
[0142] Table 1 Test results of strength retention rate of cast-in-place at low temperature
[0143] category Example 1 Example 2 Example 3 Example 4 Example 5 Comparative Example 1 -80℃ casting tensile strength retention rate, % 53.6 44.8 63.4 56.9 49.7 25.2 -80℃ casting bending strength retention rate, % 55.1 51.2 66.5 59.3 51.5 27.9
[0144] From Table 1, we can see that:
[0145] 1. The strength retention rate of the cast body of Examples 1-5 at -80°C is increased by more than 75% compared with that of Comparative Example 1;
[0146] 2. Example 3 has the best effect, and the retention rates of tensile and bending strength of the cast body at -80°C are both above 60%.
[0147] 3. The requirements of the technical solution of the present invention are achieved through Examples 1-5, and the low-temperature resistance of the obtained hybrid vinyl ester resin is greatly improved.
[0148] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A low temperature resistant hybrid vinyl ester resin, characterized in that: The resin is formed by curing raw materials including vinyl ester resin prepolymer and cross-linking monomer; The vinyl ester resin prepolymer includes a polyether epoxy vinyl ester resin prepolymer and a modified polyurethane acrylate resin; in the polyether epoxy vinyl ester resin prepolymer, the ether bond content is not less than 0.5 mol / 100g; Modified polyurethane acrylate contains ether bonds and unsaturated double bonds; The preparation method of modified polyurethane acrylate comprises: putting polyether polyol, bisphenol A polyether and isocyanate into a reaction kettle, heating the reaction to obtain polyether modified isocyanate with isocyanate groups at both ends; putting monohydroxy acrylate into the reaction kettle containing the polyether modified isocyanate, heating the temperature to 60-70°C, testing the isocyanate value, and stopping the reaction when the isocyanate value is 0 to obtain a modified polyurethane acrylate resin containing carbon-carbon unsaturated double bonds; Bisphenol A polyether epoxy resin reacts with unsaturated monocarboxylic acid to generate polyether epoxy vinyl ester resin prepolymer; The polyether epoxy vinyl ester resin prepolymer is shown in formula (I): in, x and y are independently selected from integers of 0-100 and x and y are not 0 at the same time; R1, R2 are independently selected from H or alkyl; The modified polyurethane acrylate resin is shown in formula (II): in, R3 is H, alkyl; R4 is selected from one of the following structures; R5 is selected from one of the following structures: R7 and R10 are independently selected from H or alkyl; R8 and R9 are independently selected from H or alkyl; m, n, i, and j are independently selected from integers in the range of 0-100, and m and n are not 0 at the same time, and i and j are not 0 at the same time; R6 is selected from Wherein, R11 is H or alkyl; The molar ratio of the polyether epoxy vinyl ester resin prepolymer to the modified polyurethane acrylate resin is 0.1:1-1:0.
1.
2. The low temperature resistant hybrid vinyl ester resin according to claim 1, characterized in that: The crosslinking monomer is selected from one or more of styrene, vinyl toluene, methyl methacrylate, hydroxyethyl methacrylate, n-butyl methacrylate, lauryl methacrylate, hydroxypropyl methacrylate, trimethylolpropane diacrylate and pentaerythritol triacrylate.
3. A method for preparing the low-temperature resistant hybrid vinyl ester resin according to any one of claims 1 to 2, characterized in that: The following steps are involved: reacting a vinyl ester resin prepolymer with a crosslinking monomer to obtain a low-temperature resistant hybrid vinyl ester resin; The vinyl ester resin prepolymer includes a polyether epoxy vinyl ester resin prepolymer and a modified polyurethane acrylate resin; in the polyether epoxy vinyl ester resin prepolymer, the ether bond content is not less than 0.5 mol / 100g; The modified polyurethane acrylate contains ether bonds and unsaturated double bonds.
4. The method according to claim 3, characterized in that The following steps are involved: (i) reacting bisphenol A polyether epoxy resin with unsaturated monocarboxylic acid to form the polyether epoxy vinyl ester resin prepolymer; (ii) mixing a polyether polyol, a bisphenol A polyether and an isocyanate to react and generate a polyether-modified isocyanate having isocyanate groups at both ends; (iii) reacting a monohydroxyl-containing acrylate with the polyether-modified isocyanate to generate the modified polyurethane acrylate resin.
5. The method according to claim 4, characterized in that Includes one or more of the following conditions: ① In step (i), the molar ratio of the bisphenol A polyether epoxy resin to the unsaturated monocarboxylic acid is 1:2-1:2.2; ② In step (i), the reaction is carried out at a temperature of 90-110°C; ③ In step (i), the unsaturated monocarboxylic acid comprises methacrylic acid and / or acrylic acid; ④ In step (i), it also includes a catalyst 1, which is selected from one or more of trimethylamine, pyridine, dimethyl sulfide, diethylene glycol dimethyl ether, triphenylphosphine, benzyltrimethylammonium chloride, benzyltriethylammonium chloride, benzyldimethylamine, imidazole, 1-methylimidazole, 2-ethyl-4-methylimidazole, 2-heptadecylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole and N-(3-aminopropyl)imidazole; ⑤ In step (i), a polymerization inhibitor is also included, wherein the polymerization inhibitor is selected from one or more of tert-butyl hydroquinone, tert-butyl catechol, p-benzoquinone, hydroquinone and methyl hydroquinone; ⑥ In step (ii), after mixing the polyether polyol and bisphenol A polyether, the temperature is raised to 110-115°C and kept at this temperature for 0.5-3h; the temperature is lowered to 60°C; after adding isocyanate, the mixture is reacted at a temperature of 60-80°C for 2-4h; ⑦ In step (ii), the ratio of the sum of the molar numbers of the polyether polyol and the bisphenol A polyether to the molar number of the isocyanate is 1:2; ⑧ In step (ii), the reaction further comprises a catalyst 2, wherein the catalyst 2 is selected from one or more of triethylenediamine, bis(dimethylaminoethyl) ether, N,N-dimethylcyclohexylamine, N-ethylmorpholine, N,N-dimethylbenzylamine, 2,4,6-(dimethylaminomethyl)phenol, dibutyltin dilaurate or stannous octoate and bismuth carboxylate; ⑨ In step (iii), add monohydroxy acrylate and raise the temperature to 60-70°C; ⑩ In step (iii), the molar ratio of the monohydroxy acrylate to the polyether-modified isocyanate is 1:1-1.5:
1.
6. The method according to claim 5, characterized in that When the method includes condition ④, in step (i), the mass of catalyst 1 is 0.10%-0.30% of the sum of the mass of the bisphenol A polyether epoxy resin and the unsaturated monocarboxylic acid; And / or, when the method includes condition ⑤, in step (i), the mass of the inhibitor is 0.02%-0.05% of the sum of the mass of the bisphenol A polyether epoxy resin and the unsaturated monocarboxylic acid; And / or, when the method includes condition ⑧, in step (ii), the mass of catalyst 2 is 0.05%-0.50% of the sum of the masses of the polyether polyol, bisphenol A polyether and isocyanate.