A sustained-release nanoemulsion polycarboxylate water reducer and its preparation method and application

By introducing oily acrylates and bisacrylates into polycarboxylic acid water reducing agents, the problem of insufficient concrete slump and fluid retention ability in the prior art is solved, and the ultra-high-quality water reducing agents is achieved Improved stability and adaptability over a long period of time, suitable for super high-rise buildings and super long tunnel projects.

CN115536787BActive Publication Date: 2024-11-22CCCC SHEC DONGMENG ENG CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211285295.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-20
Publication Date
2024-11-22
Estimated Expiration
2042-10-20

AI Technical Summary

Technical Problem

The existing polycarboxylic acid water reducing agents have insufficient ability to maintain concrete slump and fluidity for a long time, especially in construction of ultra-long tunnels and super-high-rise buildings, and their stability and adaptability under thermal conditions are poor. .

Method used

The emulsion polymerization technology is used to introduce oily acrylate monomers and polymerizable bisacrylate crosslinking agents into the polycarboxylic acid water reducer to form a nanopolymer emulsion water reducer. Through gradient hydrolysis, the carboxylate roots are slowly released for a long time and nuclear formation. Shell-like nano-microsphere structure to maintain the flow and slump of concrete.

Benefits of technology

Maintain the flowability and slump of concrete within 4 to 7 hours, avoid the evaporation of mixed water caused by excessively long-distance transportation at high temperatures, and significantly improve the transportation and construction performance of concrete.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115536787B_ABST
    Figure CN115536787B_ABST
Patent Text Reader

Abstract

The invention discloses a sustained-release nanoemulsion polycarboxylate water-reducing agent and a preparation method and application thereof. Deionized water is sequentially added to a four-necked flask with a stirring and ventilation device, stirring is started and nitrogen is introduced, K12 and TX‑10 are dissolved successively, polyether macromonomers are continuously added successively to fully stir and dissolve and warm up to a certain temperature, acrylic acid and acrylate monomers are sequentially added while stirring, stirring and heating are continued to be fully emulsified; azobisisobutyronitrile aqueous solution is started to be added dropwise to the reaction vessel, and after the insulation reaction is continued, it is cooled to room temperature to obtain a sustained-release nanoemulsion polycarboxylate water-reducing agent. The present invention adopts emulsion polymerization technology to synthesize a cross-linked nano-microsphere dispersion, benzyl acrylate is a hydrophobic monomer, hydroxy acrylate is a sustained-release monomer, and diacrylic acid diol ester is a cross-linking monomer, and gradient hydrolysis is realized by utilizing the difference in the hydrolysis rates of the three types of monomers, and carboxyl groups are sequentially released, thereby realizing a long-term water reduction and collapse-preserving effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polycarboxylate water reducers, and in particular to a sustained-release nanoemulsion polycarboxylate water reducer and a preparation method and application thereof. Background Art

[0002] Polycarboxylate water reducer is a new type of high-efficiency concrete water reducer successfully developed in Japan in the mid-1980s. It has low dosage, high water reduction rate, is green and environmentally friendly, and can significantly improve the strength and dispersion performance of concrete. With the construction of special projects such as super-long tunnels, the engineering community has higher and higher requirements for the maintenance of concrete slump and fluidity. At present, due to the complex transportation routes in super-long tunnels, serious waterlogging and potholes on the road, extremely poor road conditions, and ultra-long-distance transportation of commercial concrete and ultra-high-rise concrete transportation, concrete must be required to have a slump retention ability of 4 to 6 hours or even longer, otherwise it will inevitably affect the smooth progress of construction and the quality of concrete engineering. Therefore, this field is in urgent need of an ultra-long slow-release polycarboxylate water reducer with good adaptability to meet the needs of large-scale engineering construction.

[0003] CN113121753A discloses an ultra-long slow-release polycarboxylate water-reducing agent and a preparation method and application thereof. The invention introduces triethyl citrate or trimethyl citrate into the polycarboxylate water-reducing agent molecule. Since the triethyl citrate or trimethyl citrate contains three ester groups, the hydrolysis rate is relatively slow, so that the carboxylate can be slowly released for a long time. At the same time, the hydrolysis releases citric acid, which also has a certain slow setting effect. The synergistic effect of the two makes the concrete collapse-preserving performance excellent. The PCE containing carboxylate is gradually hydrolyzed in the alkaline environment of cement slurry, thereby slowly releasing carboxylate ions to achieve the effect of maintaining fluidity. However, the strong slow setting effect of the citric acid ester also affects the working properties of the concrete such as initial and final setting, segregation, and water bleeding in the later stage, and the slow release adjustability is poor.

[0004] CN104860572A discloses a polycarboxylic acid water reducer for wet spraying concrete with 6h collapse protection under hot conditions, which is composed of the following raw materials in weight percentage: 5-15% water-reducing polycarboxylic acid water reducer, 50-70% slow-release polycarboxylic acid water reducer, 0.02-0.1% water control agent, 8-15% new slow-setting collapse protection agent, 0.1-1% viscosity regulator, and the balance is 10-30% water. The water reducer prepared by the invention can significantly increase the effective amount of the slow-release polycarboxylic acid water reducer at one time, and does not cause concrete segregation and water bleeding, so that the amount of water reducer in the liquid phase of the concrete is continuously replenished and the working performance state of the concrete is controllable, and finally the collapse protection function of wet spraying concrete is realized for an ultra-long time (6h). This product has obvious effects on wet shotcrete, such as extending the slump retention time, improving volume stability, reducing temperature rise, and reducing viscosity. However, the stability is affected by the quality and source of components such as water-reducing polycarboxylic acid water-reducing agent and slow-release polycarboxylic acid water-reducing agent, which affects the controllability of its performance and the adaptability of cement.

[0005] Existing polycarboxylic acid water reducers have shortcomings such as sensitivity to soil, controlled slow release, and poor adaptability. Summary of the invention

[0006] In order to overcome the deficiencies of the above-mentioned prior art, the purpose of the present invention is to provide a slow-release nano-emulsion polycarboxylate water-reducing agent and a preparation method and application thereof. The purpose of the present application is to overcome the defect that the existing polycarboxylate water-reducing agent is used in concrete (especially machine-made sand concrete, etc.) in that the slump is not sufficiently maintained for 4 to 8 hours. The present invention uses emulsion polymerization technology to introduce oily acrylate monomers and polymerizable diacrylate crosslinking agents in the synthesis of polycarboxylate water-reducing agent to form a nano-polymer emulsion water-reducing agent. Since the polycarboxylate water-reducing agent prepared by emulsion polymerization must first undergo micelle dissociation and then undergo hydrolysis in a chemical process, three acrylates are used to achieve gradient hydrolysis, thereby achieving long-term slow release of carboxylate groups, and synergistic effects make the slump retention performance of the concrete excellent. The polycarboxylate water-reducing agent containing carboxylate groups is gradually hydrolyzed in an alkaline environment of cement slurry, thereby slowly releasing carboxylate ions, thereby achieving the effect of maintaining fluidity.

[0007] In order to achieve the above object, the technical solution adopted by the present invention is:

[0008] A sustained-release nanoemulsion polycarboxylate water reducer, using the following mass formula ratio:

[0009] Polyether macromonomer: 100 parts;

[0010] Acrylic acid: 200-240 parts

[0011] Hydroxyl acrylate: 110-140 parts

[0012] Benzyl acrylate: 80-110 parts

[0013] Diol diacrylate: 10-20 parts;

[0014] Emulsifier K12: 10-18 parts;

[0015] Emulsifier TX-10: 3.5-6 parts;

[0016] Azobisisobutyronitrile aqueous solution: 50-100 parts;

[0017] Thioglycolic acid: 0.5-1.0 parts

[0018] Deionized water: 750-900 parts.

[0019] The nano-emulsion polycarboxylic acid water-reducing agent utilizes the difference in hydrophobicity of each monomer, and forms a microsphere inner layer composed of water-reducing agent molecular segments mainly composed of highly hydrophobic benzyl acrylate during the emulsification process, and is sequentially composed of molecular segments mainly composed of diacrylic acid glycol ester and hydroxy acrylate outward, and the emulsified layer is composed of acrylic acid, reactive emulsifier and macromonomer, forming a core-shell nano-microsphere. In the alkaline environment of concrete, the nano-microsphere water-reducing agent can achieve gradient release and gradient hydrolysis, and gradually release carboxyl groups to play a role.

[0020] A method for preparing a sustained-release nanoemulsion polycarboxylate water-reducing agent, comprising the following steps:

[0021] (1) Deionized water was added sequentially into a reactor with stirring, and emulsifier K12, emulsifier TX-10, and polyether macromonomer were added sequentially while stirring to fully dissolve;

[0022] (2) After the temperature of the system (1) is raised to 50° C., acrylic acid is added while stirring, and then hydroxy acrylate, benzyl acrylate, diacrylic acid glycol ester, and 50% aqueous solution of thioglycolic acid are added in sequence, and the temperature is raised to 70±2° C. while stirring rapidly and maintaining the temperature for 10 minutes to fully emulsify the system;

[0023] (3) Finally, the aqueous solution of azobisisobutyronitrile was added dropwise to the reaction vessel of (2) within 0.5 to 1 hour, and the reaction was continued at 70±2° C. for 4 hours, and then cooled to room temperature under stirring to obtain a milky white emulsion, i.e., a sustained-release nanoemulsion polycarboxylate water-reducing agent.

[0024] In the step (1), deionized water is 750-900 parts, emulsifier K12 is 10-18 parts, emulsifier TX-10 is 3.5-6 parts, and polyether macromonomer is 100 parts.

[0025] The polyether macromonomer in step (1) is one of methyl allyl polyoxyethylene ether (HPEG-2400), isopentanol polyoxyethylene ether (TPEG-2400) and vinyl butanediol polyoxyethylene ether (EPEG-3000).

[0026] In the step (2), 110 to 140 parts of hydroxy acrylate, 80 to 110 parts of benzyl acrylate, 10 to 20 parts of diacrylic acid glycol ester, and 0.5 to 1.0 parts of thioglycolic acid;

[0027] The hydroxy acrylate in step (2) is one of hydroxyethyl acrylate and hydroxypropyl acrylate.

[0028] 50 to 100 parts of the aqueous solution of azobisisobutyronitrile in step (3).

[0029] The azobisisobutyronitrile aqueous solution in step (3) is prepared by mixing azobisisobutyronitrile with water to form an aqueous solution with a mass fraction of 50%;

[0030] The diol diacrylate in step (2) is one of ethylene glycol diacrylate, diethylene glycol diacrylate and polyethylene glycol diacrylate.

[0031] The slow-release nano-emulsion polycarboxylate water-reducing agent is applied to the construction of super-high-rise buildings and ultra-long-distance transportation and delivery of concrete.

[0032] The significant beneficial effects of the present invention are:

[0033] The object of the present invention is to provide a slow-release nano-emulsion polycarboxylate water-reducing agent and a preparation method thereof, which can keep the fluidity of cement paste substantially constant within 4 to 7 hours, and substantially prevent concrete slump loss within 4 hours. The nano-polycarboxylate water-reducing agent using emulsion polymerization forms a special structure of nano-microspheres, and the characteristic of the nano-microsphere structure is that the hydrophobicity difference of each monomer is utilized. In the emulsification process, the inner layer of the microspheres is composed of hydrophobic benzyl acrylate and diacrylic acid glycol ester, and the outer layer is composed of multi-layer gradient microspheres composed of hydroxy acrylate, which can realize gradient release and gradient hydrolysis. When the nano-microsphere water reducer is added to the concrete system, the nano-microspheres will gradually dissociate from the outside to the inside after being adsorbed by cement particles, sand and gravel and other surfaces and demulsified. These ester monomers will gradually hydrolyze to release carboxyl groups, and later benzyl acrylate and diacrylic acid glycol ester will be released and hydrolyzed until they are completely dissociated and hydrolyzed to release all carboxyl groups and water reducer molecular segments. This gradient hydrolysis method allows the water reducer to gradually increase the fluidity of cement over time within 4 to 5 hours in the alkaline environment of cement paste, and still retain good fluidity after 6 to 7 hours. This feature can not only maintain a small slump loss of concrete after long-term transportation, avoid the evaporation of mixing water caused by ultra-long-distance transportation at high temperature, but also play an important role in the construction of super-high-rise buildings and ultra-long tunnel projects. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 This is a microscopic TEM image of a nanoemulsion polycarboxylate water reducer. DETAILED DESCRIPTION

[0035] The present invention is further described in detail below in conjunction with embodiments.

[0036] Example 1

[0037] 75 g of deionized water was added to a four-necked flask with a stirring device, and nitrogen was introduced while stirring. After 1 g of K12 and 0.35 g of TX-10 were dissolved, 10 g of polyether macromonomer TPEG-2400 was added in sequence to fully stir and dissolve, and the temperature was raised to 50° C., and then 20 g of acrylic acid was added while stirring, and 11 g of hydroxyethyl acrylate, 8 g of benzyl acrylate, 1 g of ethylene glycol diacrylate, and 0.05 g of thioglycolic acid were added in sequence. The temperature was raised to 70±2° C. while stirring rapidly, and the mixture was kept warm and stirred for 10 minutes to fully emulsify and disperse. Then, 5 g of azobisisobutyronitrile aqueous solution was added dropwise to the reaction container, and the addition was completed within 0.5 to 1 hour. The mixture was kept warm and reacted at 70±2° C. for 4 hours, and then cooled to room temperature under stirring to obtain a nanoemulsion polycarboxylic acid water reducer.

[0038] Example 2

[0039] 90 g of deionized water was added to a four-necked flask with a stirring device, and nitrogen was introduced while stirring. After 1.8 g of K12 and 0.6 g of TX-10 were dissolved, 10 g of polyether macromonomer HPEG-2400 was added in sequence to fully stir and dissolve, and the temperature was raised to 50° C., and then 24 g of acrylic acid was added while stirring, and 14 g of hydroxypropyl acrylate, 11 g of benzyl acrylate, 1.6 g of diethylene glycol diacrylate, and 0.1 g of thioglycolic acid were added in sequence. The temperature was raised to 70±2° C. while stirring rapidly, and the mixture was kept warm and stirred for 10 minutes to fully emulsify and disperse. Then, 10 g of azobisisobutyronitrile aqueous solution was added dropwise to the reaction container, and the addition was completed within 0.5 to 1 hour. The reaction was continued at 70±2° C. for 4 hours, and then cooled to room temperature under stirring to obtain a nanoemulsion polycarboxylic acid water reducer.

[0040] Example 3

[0041] 80 g of deionized water was added to a four-necked flask with a stirring device, stirring was started and nitrogen was introduced. After 1.3 g of K12 and 0.5 g of TX-10 were dissolved, 10 g of polyether macromonomer EPEG-3000 was added in sequence to fully stir and dissolve, and the temperature was raised to 50° C., and then 22 g of acrylic acid was added while stirring, and 12 g of hydroxyethyl acrylate, 9 g of benzyl acrylate, 1.5 g of propylene glycol diacrylate, and 0.08 g of thioglycolic acid were added in sequence. The temperature was raised to 70±2° C. while stirring rapidly, and the mixture was kept warm and stirred for 10 minutes to fully emulsify and disperse. Then, 8 g of azobisisobutyronitrile aqueous solution was added dropwise to the reaction container, and the addition was completed within 0.5 to 1 hour. The reaction was continued at 70±2° C. for 4 hours, and then cooled to room temperature under stirring to obtain a nanoemulsion polycarboxylic acid water reducer.

[0042] Example 4

[0043] 80 g of deionized water was added to a four-necked flask with a stirring device, stirring was started and nitrogen was introduced. After 1.3 g of K12 and 0.5 g of TX-10 were dissolved, 10 g of polyether macromonomer EPEG-3000 was added in sequence to fully stir and dissolve, and the temperature was raised to 50° C., and then 18 g of acrylic acid was added while stirring, and 11 g of hydroxyethyl acrylate, 10 g of benzyl acrylate, 2.0 g of polyethylene glycol diacrylate, and 0.08 g of thioglycolic acid were added in sequence. The temperature was raised to 70±2° C. while stirring rapidly, and the mixture was kept warm and stirred for 10 minutes to fully emulsify and disperse. Then, 8 g of azobisisobutyronitrile aqueous solution was added dropwise to the reaction container, and the addition was completed within 0.5 to 1 hour. The reaction was continued at 70±2° C. for 4 hours, and then cooled to room temperature under stirring to obtain a nanoemulsion polycarboxylic acid water reducer.

[0044] Cement paste fluidity test:

[0045] According to GBT8077-2012 "Concrete admixture homogeneity test method", the cement paste fluidity is measured. The water-cement ratio is fixed at 0.29, and the PCE dosage (converted to solid) is 0.25% of the cement mass. The fluidity is measured every 1 hour, and the test is performed for a total of 7 hours. Table 1 shows the test results of the prepared nanoemulsion polycarboxylate water reducer on the cement dispersion effect.

[0046] Table 1 Changes of cement paste fluidity over time

[0047]

[0048] like Figure 1 a, 1b are microscopic morphology pictures of the nanoemulsion polycarboxylate water-reducing agent of the embodiment, respectively.

[0049] The above content is a further detailed description of the present invention. It cannot be determined that the specific implementation methods of the present invention are limited to these. For ordinary technicians in the technical field to which the present invention belongs, without departing from the concept of the present invention, they can also make several simple deductions or substitutions, which should be regarded as belonging to the protection scope of the present invention determined by the submitted claims.

Claims

1. A method for preparing a sustained-release nanoemulsion polycarboxylate water-reducing agent, characterized in that: 75 g of deionized water was added to a four-necked flask with a stirring device, stirring was started and nitrogen was introduced, 1 g of K12 and 0.35 g of TX-10 were added in sequence and dissolved, and then 10 g of polyether macromonomer TPEG-2400 was added in sequence to fully stir and dissolve, and the temperature was raised to 50°C, and then 20 g of acrylic acid was added while stirring, and 11 g of hydroxyethyl acrylate, 8 g of benzyl acrylate, 1 g of ethylene glycol diacrylate, and 0.05 g of thioglycolic acid were added in sequence, and the temperature was raised to 70±2°C while stirring rapidly, and the temperature was kept and stirred for 10 minutes to fully emulsify and disperse, and then 5 g of azobisisobutyronitrile aqueous solution was added dropwise to the reaction container, and the addition was completed within 0.5 to 1 hour, and the reaction was continued at 70±2°C for 4 hours, and then cooled to room temperature under stirring to obtain a nanoemulsion polycarboxylic acid water reducer.

2. A method for preparing a sustained-release nanoemulsion polycarboxylate water-reducing agent, characterized in that: 90 g of deionized water was added to a four-necked flask with a stirring device, stirring was started and nitrogen was introduced, 1.8 g of K12 and 0.6 g of TX-10 were added in sequence and dissolved, and then 10 g of polyether macromonomer HPEG-2400 was added in sequence to fully stir and dissolve, and the temperature was raised to 50°C, and then 24 g of acrylic acid was added while stirring, and 14 g of hydroxypropyl acrylate, 11 g of benzyl acrylate, 1.6 g of diethylene glycol diacrylate, and 0.1 g of thioglycolic acid were added in sequence, and the temperature was raised to 70±2°C while stirring rapidly, and the mixture was kept warm and stirred for 10 minutes to fully emulsify and disperse, and then 10 g of azobisisobutyronitrile aqueous solution was added dropwise to the reaction container, and the addition was completed within 0.5 to 1 hour, and the reaction was continued at 70±2°C for 4 hours, and then cooled to room temperature under stirring to obtain a nanoemulsion polycarboxylic acid water reducer.

3. A method for preparing a sustained-release nanoemulsion polycarboxylate water-reducing agent, characterized in that: 80 g of deionized water was added to a four-necked flask with a stirring device, stirring was started and nitrogen was introduced, 1.3 g of K12 and 0.5 g of TX-10 were added in sequence and dissolved, and then 10 g of polyether macromonomer EPEG-3000 was added in sequence to fully stir and dissolve and heated to 50°C, and then 22 g of acrylic acid was added while stirring, and 12 g of hydroxyethyl acrylate, 9 g of benzyl acrylate, 1.5 g of propylene glycol diacrylate, and 0.08 g of thioglycolic acid were added in sequence, and the temperature was raised to 70±2°C while stirring rapidly and kept warm and stirred for 10 minutes to fully emulsify and disperse, and then 8 g of azobisisobutyronitrile aqueous solution was added dropwise to the reaction container and added completely within 0.5 to 1 hour, and the reaction was continued at 70±2°C for 4 hours, and then cooled to room temperature under stirring to obtain a nanoemulsion polycarboxylate water reducer.

4. A method for preparing a sustained-release nanoemulsion polycarboxylate water-reducing agent, characterized in that: 80 g of deionized water was added to a four-necked flask with a stirring device, stirring was started and nitrogen was introduced, 1.3 g of K12 and 0.5 g of TX-10 were added in sequence and dissolved, and then 10 g of polyether macromonomer EPEG-3000 was added in sequence to fully stir and dissolve, and the temperature was raised to 50°C, and then 18 g of acrylic acid was added while stirring, and 11 g of hydroxyethyl acrylate, 10 g of benzyl acrylate, 2.0 g of polyethylene glycol diacrylate, and 0.08 g of thioglycolic acid were added in sequence, and the temperature was raised to 70±2°C while stirring rapidly, and the temperature was kept and stirred for 10 minutes to fully emulsify and disperse, and then 8 g of azobisisobutyronitrile aqueous solution was added dropwise to the reaction container, and the addition was completed within 0.5 to 1 hour, and the reaction was continued at 70±2°C for 4 hours, and then cooled to room temperature under stirring to obtain a nanoemulsion polycarboxylic acid water reducer.

5. A sustained-release nanoemulsion polycarboxylate water-reducing agent prepared by the method according to any one of claims 1 to 4, characterized in that: The slow-release nano-emulsion polycarboxylate water-reducing agent is applied to the construction of super-high-rise buildings and ultra-long-distance transportation and delivery of concrete.