A method for increasing the nitriding speed of samarium iron nitride permanent magnet material
The nitriding catalyst is prepared by using active metal salts and carbon carriers to reduce the nitriding reaction temperature and activation energy, solve the problem of slow nitriding speed of samarium iron nitrogen permanent magnet materials, and achieve efficient magnetic performance improvement and industrial application.
Patent Information
- Application Number
- CN202211271780.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-18
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-10-18
AI Technical Summary
In the existing technology, the nitriding speed of the samarium iron nitrogen permanent magnet material is slow, resulting in the magnetic performance not reaching the expected level, and the existing method has high energy consumption and harsh conditions, making it difficult to apply industrially.
The active component solution is prepared by mixing active metal salts and initiators, combined with a carbon carrier to prepare a nitriding catalyst, and reacts with the samarium iron alloy to reduce the nitriding reaction temperature and activation energy, increase the nitriding rate, avoid material decomposition, and use solvent separation Obtain samarium iron nitrogen permanent magnet material.
It significantly increases the nitriding speed and improves the magnetic properties of the samarium iron nitrogen permanent magnet material. The maximum magnetic energy product reaches more than 2.61MGOe. It is simple to operate and suitable for industrial promotion.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of permanent magnetic material preparation, and in particular to a method for improving the nitriding speed of samarium iron nitride permanent magnetic material. Background Art
[0002] In recent years, due to the rare earth neodymium iron boron (chemical formula generally expressed as Nd2Fe 14 B) With the extensive use of permanent magnetic materials in air-conditioning compressors, new energy vehicles, wind power generation and other fields, the prices of rare earth Nd and Pr have risen rapidly. How to utilize relatively surplus rare earth resources such as cheap Sm and Ce has become a hot topic in the field of magnetic materials.
[0003] Samarium iron nitrogen permanent magnet material (chemical formula is generally expressed as Sm2Fe 17 N x ) has a saturation magnetization of 1.54 T, which is similar to that of Nd2Fe 14 The 1.6T of compound B is equivalent, and Sm2Fe 17 N x The Curie temperature of the compound is 470°C and the anisotropy field is 14T, both higher than that of Nd2Fe 14 B compound. Therefore, Sm2Fe 17 N x Compounds have broad prospects as a new generation of rare earth permanent magnet materials. 17 N x The process of preparing Sm2Fe 17 Alloy powder; (2) Sm2Fe 17 Alloy powder nitriding; (3) Final treatment of permanent magnet alloy. Among them, nitriding is a crucial step, which directly determines the Sm2Fe 17 N x The kinetics of the nitriding reaction during nitriding is poor, and the nitrogen-containing gas reacts very slowly with the magnetic powder under high temperature and high pressure. 17 N x The compound will decompose at a high temperature of 600°C, which makes it impossible to rely solely on increasing the temperature to increase the nitrogen activity to promote the reaction, which leads to low nitriding efficiency and poor nitriding effect in a medium containing nitrogen source. 17 N x The magnetic properties of the compound cannot reach the corresponding level.
[0004] CN113871124A discloses a method for preparing high-performance samarium iron nitrogen permanent magnet material with high nitriding efficiency. The method comprises the following steps: screening samarium iron alloy powder by classification, using a vacuum pump to evacuate a tower vacuum nitriding furnace to a low vacuum of 1×10 -3Pa, a high-speed high-purity nitrogen gas flow is continuously charged from the bottom of the tower vacuum nitriding furnace for nitriding treatment, and the SmFe alloy powder is flushed with nitrogen gas flow to improve the nitriding efficiency. However, this method requires the charging of a high-speed high-purity nitrogen gas flow, which not only consumes a lot of energy, but also has a very limited effect on the improvement of the nitriding rate.
[0005] CN1283142A discloses a Sm-Fe-N series alloy powder and a method for manufacturing the same, wherein the alloy powder and granular calcium are mixed, hydrogen at 1000°C is introduced for reduction diffusion reaction, the hydrogen is then extracted and nitrogen is introduced, and the mixture is heated for 5 hours at a pressure higher than atmospheric pressure to perform a nitriding reaction. The nitriding process provided by the method is carried out under high pressure, which not only has harsh reaction conditions, but also has a long nitriding time, and the nitriding speed and reaction efficiency are relatively low.
[0006] Therefore, it is of great significance to provide a method for increasing the nitriding speed of SmFeN permanent magnet materials. Summary of the invention
[0007] In view of the above problems, the purpose of the present invention is to provide a method for increasing the nitriding speed of samarium iron nitride permanent magnet materials. Compared with the prior art, the method provided by the present invention can greatly increase the nitriding rate, thereby improving the maximum magnetic energy product of the samarium iron nitride permanent magnet material, and is simple to operate and can be applied industrially.
[0008] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:
[0009] The present invention provides a method for increasing the nitriding speed of samarium iron nitrogen permanent magnet material, the method comprising the following steps:
[0010] (1) mixing an active metal salt and an initiator to obtain an active component solution;
[0011] (2) mixing the active component solution obtained in step (1) and the carbon support, and then sequentially allowing to stand, solidify and calcine to obtain a nitriding catalyst;
[0012] (3) mixing the nitriding catalyst and samarium-iron alloy obtained in step (2), and then sequentially heating and cooling in a nitrogen-containing atmosphere to obtain a solid mixture;
[0013] (4) immersing the solid mixture obtained in step (3) in a solvent, removing the solid floating matter in the upper layer, and then performing solid-liquid separation to obtain a solid precipitate in the lower layer, and then drying to obtain a samarium iron nitrogen permanent magnet material.
[0014] The method provided by the present invention first prepares an active component solution by an active metal salt and an initiator, and then prepares a nitriding catalyst by an active component solution and a carbon carrier, wherein the active metal element can reduce the activation energy required for the ion bond to break, thereby reducing the activation energy of the nitriding reaction, and achieving the purpose of improving the nitriding rate, wherein the initiator can accelerate the attachment of the metal salt on the carbon carrier, so that the metal salt in the solution is deposited on the carbon carrier. Further, the above-mentioned nitriding catalyst and samarium iron alloy are used for reaction, which can reduce the temperature of the nitriding reaction, increase the reaction rate, and can also avoid the decomposition of the samarium iron nitrogen permanent magnetic material. Finally, by immersing the solid mixture in a solvent, the nitriding catalyst is suspended in the upper layer of the solvent, and the solid precipitate of the lower layer is the samarium iron nitrogen permanent magnetic material, which can be completely separated by performing solid-liquid separation and drying. It can be seen from this that the method provided by the present invention can not only reduce the temperature of the nitriding reaction, making the reaction conditions more gentle, but also can improve the nitriding speed, and then improve the magnetic properties of the permanent magnetic material, but also has the advantages of simple separation, strong operability, and can be industrially promoted.
[0015] Preferably, the active metal element contained in the active metal salt in step (1) includes any one of nickel, cobalt, copper or zinc, or a combination of at least two of them, wherein typical but non-limiting combinations include a combination of nickel and cobalt, a combination of cobalt and copper or a combination of copper and zinc, preferably a combination of nickel and zinc.
[0016] The present invention preferably controls the active metal elements contained in the active metal salt to be nickel and zinc, which can further enhance the catalytic effect of the nitriding catalyst, thereby further enhancing the nitriding rate.
[0017] Preferably, the active metal salt comprises any one of nickel nitrate, cobalt nitrate, copper nitrate or zinc nitrate, or a combination of at least two thereof, wherein typical but non-limiting combinations include a combination of nickel nitrate and cobalt nitrate, a combination of cobalt nitrate and copper nitrate, a combination of copper nitrate and zinc nitrate, and preferably a combination of nickel nitrate and zinc nitrate.
[0018] Preferably, the molar ratio of nickel to zinc in the active metal salt is (2-10):1, for example, 2:1, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1, 9:1 or 10:1, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0019] The present invention preferably controls the molar ratio of nickel to zinc in the active metal salt within a specific range, which can further enhance the catalytic effect and thus promote the nitriding reaction.
[0020] Preferably, the initiator comprises an acid solution.
[0021] Preferably, the acid solution comprises any one of sulfuric acid, nitric acid or hydrochloric acid or a combination of at least two of them, wherein typical but non-limiting combinations include a combination of sulfuric acid and nitric acid, a combination of nitric acid and hydrochloric acid or a combination of sulfuric acid and hydrochloric acid, preferably sulfuric acid.
[0022] Preferably, the molar concentration of the acid solution is 2-4%, for example, it can be 2%, 2.2%, 2.4%, 2.6%, 2.8%, 3%, 3.2%, 3.4%, 3.6%, 3.8% or 4%, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0023] Preferably, the added amount of the initiator accounts for 0.1-1.5% by volume of the active component solution, for example, it can be 0.1%, 0.2%, 0.4%, 0.6%, 0.8%, 1%, 1.2%, 1.4% or 1.5%, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0024] Preferably, the carbon carrier in step (2) comprises any one of mesoporous carbon, graphene or carbon nanotubes, or a combination of at least two of them, wherein typical but non-limiting combinations include a combination of mesoporous carbon and graphene, a combination of graphene and carbon nanotubes, or a combination of mesoporous carbon and carbon nanotubes, preferably mesoporous carbon.
[0025] The present invention has no special limitation on the mesoporous carbon, graphene or carbon nanotube, and the mesoporous carbon, graphene or carbon nanotube may be any mesoporous carbon, graphene or carbon nanotube commonly used in the art.
[0026] Preferably, the mass of the active metal element in the active component solution in step (2) accounts for 1-7% of the mass of the carbon carrier, for example, it can be 1%, 2%, 3%, 4%, 5%, 6% or 7%, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0027] Preferably, the standing time in step (2) is 12-48 h, for example, it can be 12 h, 14 h, 16 h, 18 h, 20 h, 22 h, 24 h, 26 h, 28 h, 30 h, 34 h, 36 h, 38 h, 40 h, 42 h, 46 h or 48 h, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0028] Preferably, the curing temperature is 200-500°C, for example, it can be 200°C, 220°C, 240°C, 260°C, 280°C, 300°C, 320°C, 340°C, 360°C, 380°C, 400°C, 420°C, 440°C, 460°C, 480°C or 500°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0029] Preferably, the curing time is 3-4 hours, for example, 3 hours, 3.2 hours, 3.4 hours, 3.6 hours, 3.8 hours or 4 hours, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0030] Preferably, the calcination temperature in step (2) is 600-850°C, for example, it can be 600°C, 620°C, 640°C, 680°C, 700°C, 720°C, 740°C, 760°C, 780°C, 800°C, 820°C, 840°C or 850°C, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0031] Preferably, the calcination time is 1.5-3 h, for example, 1.5 h, 1.6 h, 1.8 h, 2 h, 2.2 h, 2.4 h, 2.6 h, 2.8 h or 3 h, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0032] Preferably, the mass ratio of the nitriding catalyst and the samarium iron alloy in step (3) is (1-6):500, for example, it can be 1:500, 1.5:500, 2:500, 2.5:500, 3:500, 3.5:500, 4:500, 4.5:500, 5:500, 5.5:500 or 6:500, but is not limited to the listed values. Other values not listed within the numerical range are also applicable, preferably (2.5-6):500.
[0033] The present invention preferably controls the mass ratio of the nitriding catalyst and the samarium-iron alloy, which can further promote the nitriding reaction and thus improve the magnetic properties of the product.
[0034] Preferably, the particle size of the samarium-iron alloy is 1-3 mm, for example, it can be 1 mm, 1.2 mm, 1.5 mm, 1.8 mm, 2 mm, 2.2 mm, 2.5 mm, 2.8 mm or 3 mm, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0035] Preferably, the nitrogen-containing atmosphere includes an ammonia atmosphere.
[0036] Preferably, the heating temperature in step (3) is 480-550°C, for example, it can be 480°C, 490°C, 500°C, 510°C, 520°C, 530°C, 540°C or 550°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0037] The present invention preferably controls the heating temperature, which can further promote the nitriding reaction, thereby improving the magnetic properties of the product.
[0038] Preferably, the heating time is 3-10 h, for example, 3 h, 4 h, 5 h, 6 h, 7 h, 8 h, 9 h or 10 h, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0039] The present invention preferably controls the heating time, which can further promote the nitriding reaction, thereby improving the magnetic properties of the product.
[0040] Preferably, the solvent in step (4) comprises anhydrous ethanol.
[0041] Preferably, the immersion time is 1-3 h, for example, it can be 1 h, 1.2 h, 1.5 h, 1.8 h, 2 h, 2.2 h, 2.5 h, 2.8 h or 3 h, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0042] Preferably, the drying temperature is 90-200°C, for example, it can be 90°C, 100°C, 110°C, 120°C, 130°C, 140°C, 150°C, 160°C, 170°C, 180°C, 190°C or 200°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0043] Preferably, the drying time is 1-3 h, for example, it can be 1 h, 1.2 h, 1.5 h, 1.8 h, 2 h, 2.2 h, 2.5 h, 2.8 h or 3 h, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0044] As a preferred technical solution of the present invention, the method comprises the following steps:
[0045] (1) mixing an active metal salt and an initiator to obtain an active component solution, wherein the amount of the initiator added is 0.1-1.5% by volume of the active component solution;
[0046] The active metal element contained in the active metal salt includes any one of nickel, cobalt, copper or zinc or a combination of at least two thereof; the active metal salt includes any one of nickel nitrate, cobalt nitrate, copper nitrate or zinc nitrate or a combination of at least two thereof; the initiator includes an acid solution; the acid solution includes any one of sulfuric acid, nitric acid or hydrochloric acid or a combination of at least two thereof; the molar concentration of the acid solution is 2-4%;
[0047] (2) mixing the active component solution obtained in step (1) with a carbon carrier, wherein the mass of the active metal element in the active component solution accounts for 1-7% of the mass of the carbon carrier, and then standing for 12-48 hours, and then curing at 200-500° C. for 3-4 hours, and then calcining at 600-850° C. for 1.5-3 hours to obtain a nitriding catalyst;
[0048] The carbon carrier includes any one of mesoporous carbon, graphene or carbon nanotubes or a combination of at least two thereof;
[0049] (3) mixing the nitriding catalyst obtained in step (2) and a samarium-iron alloy in a mass ratio of (1-6):500, wherein the particle size of the samarium-iron alloy is 1-3 mm, and then heating at 480-550° C. for 3-10 h in an ammonia atmosphere, and cooling to obtain a solid mixture;
[0050] (4) Immersing the solid mixture obtained in step (3) in anhydrous ethanol for 1-3 hours, removing the solid floating matter in the upper layer, and then performing solid-liquid separation to obtain a solid precipitate in the lower layer, and then drying at 90-200° C. for 1-3 hours to obtain a samarium iron nitrogen permanent magnet material.
[0051] Compared with the prior art, the present invention has the following beneficial effects:
[0052] The method provided by the present invention can not only reduce the temperature of the nitriding reaction and make the reaction conditions milder, but also increase the nitriding speed, thereby improving the magnetic properties of the permanent magnet material. The maximum magnetic energy product can reach more than 2.61 MGOe. It also has the advantages of simple separation, strong operability, and industrial promotion. DETAILED DESCRIPTION
[0053] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0054] Example 1
[0055] This embodiment provides a method for increasing the nitriding speed of a samarium iron nitride permanent magnet material, the method comprising the following steps:
[0056] (1) mixing nickel nitrate, zinc nitrate and sulfuric acid to obtain an active component solution, wherein the amount of sulfuric acid added is 0.8% by volume of the active component solution;
[0057] The molar ratio of nickel to zinc in the active metal salt is 6:1, and the molar concentration of sulfuric acid is 3%;
[0058] (2) Mixing the active component solution obtained in step (1) and the mesoporous carbon (with a total pore volume of 0.9 cm 3 / g, with an average pore size of 5 nm), the mass of the active metal element in the active component solution accounts for 4% of the mass of the mesoporous carbon, and then standing for 24 hours, then curing at 350° C. for 3 hours, and then calcining at 720° C. for 2 hours to obtain a nitriding catalyst;
[0059] (3) Take samarium iron alloy (Sm2Fe 17 ) 50 kg, in a mass ratio of 3.5:500, the nitriding catalyst obtained in step (2) and the samarium-iron alloy, the particle size of the samarium-iron alloy is 2 mm, and then heated at 500 ° C for 6 h in an ammonia atmosphere, and cooled to obtain a solid mixture;
[0060] (4) Immersing the solid mixture obtained in step (3) in anhydrous ethanol for 2 hours, removing the solid floating matter in the upper layer, and then filtering to obtain a solid precipitate in the lower layer, and then drying at 120° C. for 2 hours to obtain a samarium iron nitrogen permanent magnet material.
[0061] Example 2
[0062] This embodiment provides a method for increasing the nitriding speed of a samarium iron nitride permanent magnet material, the method comprising the following steps:
[0063] (1) mixing nickel nitrate and sulfuric acid to obtain an active component solution, wherein the amount of sulfuric acid added is 1.5% by volume of the active component solution;
[0064] The molar concentration of the sulfuric acid is 2%;
[0065] (2) Mixing the active component solution obtained in step (1) and the mesoporous carbon (with a total pore volume of 0.9 cm 3 / g, with an average pore size of 5 nm), the mass of the active metal element in the active component solution accounts for 7% of the mass of the mesoporous carbon, and then standing for 12 hours, then curing at 500° C. for 3.5 hours, and then calcining at 600° C. for 1.5 hours to obtain a nitriding catalyst;
[0066] (3) Take samarium iron alloy (Sm2Fe 17 ) 50 kg, in a mass ratio of 2.5:500, the nitriding catalyst obtained in step (2) and the samarium-iron alloy, the particle size of the samarium-iron alloy is 3 mm, and then heated at 480 ° C for 10 h in an ammonia atmosphere, and cooled to obtain a solid mixture;
[0067] (4) Immersing the solid mixture obtained in step (3) in anhydrous ethanol for 3 hours, removing the solid floating matter in the upper layer, and then filtering to obtain a solid precipitate in the lower layer, and then drying at 90° C. for 3 hours to obtain a samarium iron nitrogen permanent magnet material.
[0068] Example 3
[0069] This embodiment provides a method for increasing the nitriding speed of a samarium iron nitride permanent magnet material, the method comprising the following steps:
[0070] (1) mixing copper nitrate and nitric acid to obtain an active component solution, wherein the amount of nitric acid added is 0.1% by volume of the active component solution;
[0071] The molar concentration of the nitric acid is 4%;
[0072] (2) mixing the active component solution obtained in step (1) and graphene, wherein the mass of the active metal element in the active component solution accounts for 1% of the mass of the graphene, and then standing for 48 hours, and then curing at 200° C. for 4 hours, and then calcining at 850° C. for 3 hours to obtain a nitriding catalyst;
[0073] (3) Take samarium iron alloy (Sm2Fe 17 ) 50 kg, in a mass ratio of 6:500, the nitriding catalyst obtained in step (2) and the samarium-iron alloy, the particle size of the samarium-iron alloy is 1 mm, and then heated at 550° C. for 3 h in an ammonia atmosphere, and cooled to obtain a solid mixture;
[0074] (4) Immersing the solid mixture obtained in step (3) in anhydrous ethanol for 1 hour, removing the solid floating matter in the upper layer, and then filtering to obtain the solid precipitate in the lower layer, and then drying at 200° C. for 1 hour to obtain the samarium iron nitrogen permanent magnet material.
[0075] Example 4
[0076] This embodiment provides a method for increasing the nitriding rate of samarium iron nitrogen permanent magnet materials. The only difference compared with embodiment 1 is that the molar ratio of nickel to zinc in the active metal salt is 2:1.
[0077] Example 5
[0078] This embodiment provides a method for increasing the nitriding rate of samarium iron nitrogen permanent magnet materials. The only difference compared with embodiment 1 is that the molar ratio of nickel to zinc in the active metal salt is 10:1.
[0079] Example 6
[0080] This embodiment provides a method for increasing the nitriding rate of samarium iron nitrogen permanent magnet materials. The only difference compared with embodiment 1 is that the molar ratio of nickel to zinc in the active metal salt is 1:1.
[0081] Example 7
[0082] This embodiment provides a method for increasing the nitriding rate of samarium iron nitrogen permanent magnet materials. The only difference compared with Example 1 is that the molar ratio of nickel to zinc in the active metal salt is 15:1.
[0083] Example 8
[0084] This embodiment provides a method for increasing the nitriding speed of samarium iron nitride permanent magnet materials. The only difference compared with embodiment 1 is that the mass ratio of the nitriding catalyst to the samarium iron alloy in step (3) is 1:500.
[0085] Example 9
[0086] This embodiment provides a method for increasing the nitriding speed of samarium iron nitride permanent magnet materials. The only difference compared with embodiment 1 is that the heating temperature in step (3) is 460°C.
[0087] Example 10
[0088] This embodiment provides a method for increasing the nitriding speed of samarium iron nitride permanent magnet materials. The only difference compared with embodiment 1 is that the heating time in step (3) is 2 hours.
[0089] Comparative Example 1
[0090] This comparative example provides a method for increasing the nitriding speed of samarium iron nitrogen permanent magnet material, which is different from Example 1 only in that no nitriding catalyst is prepared for nitriding. The method comprises the following steps:
[0091] Take samarium iron alloy (Sm2Fe 17 )50kg, with a particle size of 2mm, was heated at 500℃ for 6h in an ammonia atmosphere and cooled to obtain samarium iron nitrogen permanent magnet material.
[0092] The samarium iron nitrogen permanent magnet materials prepared in Examples 1-10 and Comparative Example 1 were crushed into samarium iron nitrogen powders with an average particle size of 2.5 μm under an ammonia atmosphere, and then the samarium iron nitrogen powders were mixed with polyphenylene sulfide resin containing 8% by weight of the samarium iron nitrogen powders, and mixed and granulated using a twin-screw extruder to obtain pellets. The pellets were injection molded in an injection molding machine to obtain samples to be tested.
[0093] The NIM-2000 permanent magnetic material precision measuring instrument is used to measure the maximum magnetic energy product BH of the sample to be tested. max The test was carried out and the results are shown in Table 1.
[0094] Table 1
[0095] <![CDATA[BH max / MGOe]]> Example 1 6.73 Example 2 6.38 Example 3 5.79 Example 4 5.33 Example 5 5.61 Example 6 4.52 Example 7 3.97 Example 8 2.61 Example 9 3.11 Example 10 2.85 Comparative Example 1 1.32
[0096] From Table 1, we can see the following points:
[0097] (1) From the data of Examples 1-10, it can be seen that the maximum magnetic energy product of the samples to be tested in Examples 1-10 can reach above 2.61 MGOe, indicating that the method provided by the present invention can promote nitriding and thus improve the magnetic properties of permanent magnet materials.
[0098] (2) A comprehensive comparison of the data of Example 1 and Examples 6-7 shows that the molar ratio of nickel to zinc in Example 1 is 6:1. Compared with the molar ratios of Examples 6-7 being 1:1 and 15:1 respectively, the maximum magnetic energy product in Example 1 is significantly higher than that in Examples 6-7. This indicates that the present invention preferably controls the molar ratio of nickel to zinc in the active metal salt, which can further improve the magnetic properties of the permanent magnet material.
[0099] (3) A comprehensive comparison of the data of Example 1 and Example 8 shows that the mass ratio of the nitriding catalyst to the samarium-iron alloy in Example 1 is 3.5:500, compared with 1:500 in Example 8. The maximum magnetic energy product in Example 1 is significantly higher than that in Example 8, which indicates that the present invention preferably controls the mass ratio of the nitriding catalyst to the samarium-iron alloy, which can further improve the magnetic properties of the permanent magnet material.
[0100] (4) A comprehensive comparison of the data of Example 1 and Example 9 shows that the heating temperature in Example 1 is 500°C, compared with 460°C in Example 9. The maximum magnetic energy product in Example 1 is significantly higher than that in Example 9, which indicates that the present invention preferably controls the heating temperature to further improve the magnetic properties of the permanent magnet material.
[0101] (5) A comprehensive comparison of the data of Example 1 and Example 10 shows that the heating time in Example 1 is 6 h, compared with 2 h in Example 10. The maximum magnetic energy product in Example 1 is significantly higher than that in Example 10, which indicates that the present invention preferably controls the heating time to further improve the magnetic properties of the permanent magnet material.
[0102] (6) A comprehensive comparison of the data of Example 1 and Comparative Example 1 shows that the only difference between Comparative Example 1 and Example 1 is that nitriding is performed without preparing a nitriding catalyst, and the maximum magnetic energy product in Example 1 is significantly higher than that in Comparative Example 1, which indicates that the method provided by the present invention can significantly improve the magnetic properties of permanent magnet materials.
[0103] In summary, the method provided by the present invention can not only reduce the temperature of the nitriding reaction and make the reaction conditions milder, but also increase the nitriding speed, thereby improving the magnetic properties of the permanent magnet material.
[0104] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.
Claims
1. A method for increasing the nitriding rate of samarium iron nitrogen permanent magnet material, characterized in that: The method comprises the following steps: (1) mixing an active metal salt and an initiator to obtain an active component solution; The active metal salt comprises any one of nickel nitrate, cobalt nitrate, copper nitrate or zinc nitrate or a combination of at least two thereof; the initiator comprises acid solution; (2) mixing the active component solution obtained in step (1) and the carbon support, and then sequentially allowing to stand, solidify and calcine to obtain a nitriding catalyst; (3) mixing the nitriding catalyst and samarium-iron alloy obtained in step (2), and then heating and cooling in a nitrogen-containing atmosphere to obtain a solid mixture; (4) Immersing the solid mixture obtained in step (3) in a solvent to remove the solid floating matter in the upper layer, and then performing solid-liquid separation to obtain a solid precipitate in the lower layer, which is then dried to obtain a samarium iron nitrogen permanent magnet material.
2. The method according to claim 1, characterized in that The active metal salt is a combination of nickel nitrate and zinc nitrate.
3. The method according to claim 2, characterized in that The molar ratio of nickel to zinc in the active metal salt is (2-10):
1.
4. The method according to claim 1, characterized in that: The acid solution includes any one of sulfuric acid, nitric acid or hydrochloric acid, or a combination of at least two of them.
5. The method according to claim 4, characterized in that The acid solution is sulfuric acid.
6. The method according to claim 1, characterized in that The molar concentration of the acid solution is 2-4%.
7. The method according to claim 1, characterized in that The added amount of the initiator accounts for 0.1-1.5% by volume of the active component solution.
8. The method according to claim 1, characterized in that The carbon carrier in step (2) includes any one of mesoporous carbon, graphene or carbon nanotubes, or a combination of at least two of them.
9. The method according to claim 8, characterized in that The carbon carrier in step (2) is mesoporous carbon.
10. The method according to claim 1, characterized in that The mass of the active metal element in the active component solution in step (2) accounts for 1-7% of the mass of the carbon carrier.
11. The method according to claim 1, characterized in that: The standing time in step (2) is 12-48 hours.
12. The method according to claim 1, characterized in that The curing temperature is 200-500°C.
13. The method according to claim 1, characterized in that The curing time is 3-4h.
14. The method according to claim 1, characterized in that The calcination temperature in step (2) is 600-850°C.
15. The method according to claim 1, characterized in that The calcination time is 1.5-3h.
16. The method according to claim 1, characterized in that The mass ratio of the nitriding catalyst to the samarium-iron alloy in step (3) is (1-6):
500.
17. The method according to claim 16, characterized in that The mass ratio of the nitriding catalyst to the samarium-iron alloy in step (3) is (2.5-6):
500.
18. The method according to claim 1, characterized in that The particle size of the samarium-iron alloy is 1-3 mm.
19. The method according to claim 1, characterized in that The nitrogen-containing atmosphere includes an ammonia atmosphere.
20. The method according to claim 1, characterized in that The heating temperature in step (3) is 480-550°C.
21. The method according to claim 1, characterized in that The heating time is 3-10h.
22. The method according to claim 1, characterized in that The solvent in step (4) includes anhydrous ethanol.
23. The method according to claim 1, characterized in that The immersion time in step (4) is 1-3 hours.
24. The method according to claim 1, characterized in that The drying temperature in step (4) is 90-200°C.
25. The method according to claim 1, characterized in that The drying time in step (4) is 1-3 hours.
26. The method according to claim 1, characterized in that The method comprises the following steps: (1) mixing an active metal salt and an initiator to obtain an active component solution, wherein the amount of the initiator added is 0.1-1.5% by volume of the active component solution; The active metal salt includes any one of nickel nitrate, cobalt nitrate, copper nitrate or zinc nitrate or a combination of at least two thereof; the initiator includes an acid solution, and the acid solution includes any one of sulfuric acid, nitric acid or hydrochloric acid or a combination of at least two thereof; the molar concentration of the acid solution is 2-4%; (2) mixing the active component solution obtained in step (1) with a carbon carrier, wherein the mass of the active metal element in the active component solution accounts for 1-7% of the mass of the carbon carrier, and then standing for 12-48 hours, and then curing at 200-500° C. for 3-4 hours, and then calcining at 600-850° C. for 1.5-3 hours to obtain a nitriding catalyst; The carbon carrier includes any one of mesoporous carbon, graphene or carbon nanotubes or a combination of at least two thereof; (3) mixing the nitriding catalyst obtained in step (2) and a samarium-iron alloy in a mass ratio of (1-6):500, wherein the particle size of the samarium-iron alloy is 1-3 mm, and then heating at 480-550° C. for 3-10 h in an ammonia atmosphere, and cooling to obtain a solid mixture; (4) Immersing the solid mixture obtained in step (3) in anhydrous ethanol for 1-3 hours, removing the solid floating matter in the upper layer, and then performing solid-liquid separation to obtain a solid precipitate in the lower layer, and then drying at 90-200° C. for 1-3 hours to obtain a samarium iron nitrogen permanent magnet material.
Citation Information
Patent Citations
Method for preparing anisotropic sintering SmFeN permanent magnet
CN108766755A
Method for preparing high-performance samarium-iron-nitrogen permanent magnet material with high nitriding efficiency
CN113871124A