Pole piece manufacturing method, pole piece and battery
By mechanically scribing the active material layer of the lithium-ion battery electrode sheet, the tortuosity and wrinkle problems caused by stress accumulation are solved, and the high energy density and power density characteristics of the electrode sheet are achieved, and the process controllability is achieved. Strong, suitable for mass production.
Patent Information
- Application Number
- CN202211236467.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-10
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2042-10-10
AI Technical Summary
When the existing lithium-ion battery electrodes meet the demand for high energy density, they are prone to increasing tortuosity and wrinkle problems due to stress accumulation, and it is difficult to take into account the characteristics of high power density.
The active material layer of the pole sheet is scribbed by a mechanical engraving knife to form grooves, release stress and absorb deformation, reduce tortuosity, and absorb powder through a negative pressure device to ensure the scoring accuracy and material performance.
It effectively reduces the tortuosity of the pole sheet, avoids wrinkles, takes into account the characteristics of high energy density and high power density, and has strong controllability in the process, suitable for large-scale production, and is not easily affected by heat or chemical reactions.
Smart Images

Figure CN115548268B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of battery technology, and in particular to a pole piece manufacturing method, a pole piece and a battery. Background Art
[0002] Lithium-ion batteries store and release energy by migrating lithium ions back and forth between the positive and negative electrodes, and the most important performance indicators are energy density and power density. To meet the demand for high energy density, the electrode process mainly uses technologies such as thick electrodes, high compaction, and high specific energy materials (such as silicon negative electrodes). However, the above technologies will increase the transmission distance and resistance of lithium ions, aggravate stress accumulation and lead to problems such as electrode wrinkles, making it difficult for the electrode to take into account high power density characteristics.
[0003] In view of this, this application is hereby filed. Summary of the invention
[0004] The purpose of this application is to provide a pole piece manufacturing method, a pole piece and a battery, which can reduce the tortuosity of the pole piece so that it can take into account both high energy density and high power density characteristics, and improve the problem that the existing pole piece is easily wrinkled due to stress accumulation, thereby improving battery performance.
[0005] This application is implemented as follows:
[0006] In a first aspect, the present application provides a method for manufacturing a pole piece, comprising:
[0007] Making an active material layer on the surface of the current collector to obtain a pole piece to be scribed;
[0008] A groove is carved on the active material layer of the electrode to be carved using a carving knife to obtain the electrode.
[0009] In an optional embodiment, the step of preparing an active material layer on the surface of the current collector to obtain a pole piece to be scribed includes:
[0010] applying a slurry comprising an active material and a binder to a current collector;
[0011] The current collector coated with the slurry is dried and baked to obtain the pole piece to be scribed.
[0012] In an optional embodiment, the binder is one or more of polyimide, polyacrylonitrile, and aramid.
[0013] In an optional embodiment, the baking temperature is 80-300°C.
[0014] In an optional embodiment, the step of preparing an active material layer on the surface of the current collector to obtain a pole piece to be scribed includes:
[0015] Using a dry process, a mixture containing active materials and a binder is laid on a current collector by means of film pressing and lamination to obtain a pole piece to be scribed.
[0016] In an alternative embodiment, the binder comprises a PTFE emulsion.
[0017] In an alternative embodiment, the mixture further comprises a conductive agent.
[0018] In an optional embodiment, the width of the groove is 100-1000 μm.
[0019] In an optional embodiment, the ratio of the depth of the groove to the thickness of the active material layer is 0.05-1.
[0020] In an optional embodiment, there are multiple grooves, and the multiple grooves are staggered to form a grid pattern.
[0021] In an optional embodiment, the pole piece manufacturing method further includes:
[0022] Negative pressure is created around the carving knife to absorb the powder generated during the carving process.
[0023] In an optional embodiment, the engraving knife is disposed in a dust hood, and the dust hood is connected to a negative pressure device, which is used to generate negative pressure in the dust hood. During the engraving process, the opening of the dust hood faces the active material layer, the end of the engraving knife extends from the opening of the dust hood to be inserted into the active material layer, and the dust hood moves with the engraving knife.
[0024] In a second aspect, the present application provides a pole piece, which is manufactured using the pole piece manufacturing method of any one of the aforementioned embodiments.
[0025] In a third aspect, the present application provides a battery, comprising the electrode of the aforementioned embodiment.
[0026] This application has the following beneficial effects:
[0027] The pole piece manufacturing method provided in the present application includes manufacturing an active material layer on the surface of a current collector to obtain a pole piece to be engraved; and using a carving knife to carve grooves on the active material layer of the pole piece to be engraved to obtain the pole piece. Carving grooves on the active material layer can release the stress in the active material layer of the pole piece, and when winding, the grooves can absorb a certain deformation, thereby improving the problem of wrinkles on the surface of the pole piece. The use of this manufacturing method can effectively reduce the tortuosity of the pole piece, so that it can take into account both high energy density and high power density characteristics. Moreover, the grooves are formed by mechanical carving with a carving knife, which has good controllability, uniformity, and reliability, and is conducive to mass production. In addition, the use of mechanical carving is not easy to have a negative impact on the material properties of the active material layer due to thermal effects or chemical reactions, thereby ensuring the performance of the pole piece.
[0028] The pole piece provided in the present application is made by the pole piece manufacturing method described above, has a low tortuosity, can take into account both high energy density and high power density characteristics, and is not easy to wrinkle. The battery provided in the present application includes the pole piece described above, and therefore also has corresponding beneficial effects. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.
[0030] Figure 1 This is a flow chart of a method for manufacturing a pole piece in one embodiment of the present application;
[0031] Figure 2 This is a flow chart of making a pole piece to be scribed in one embodiment of the present application;
[0032] Figure 3 A schematic diagram of a scribing process in one embodiment of the present application;
[0033] Figure 4 This is a schematic diagram of a pole piece in one embodiment of the present application;
[0034] Figure 5 A cross-sectional view of a pole piece in one embodiment of the present application;
[0035] Figure 6 This is a schematic diagram of active powder particles falling into a groove in one embodiment of the present application.
[0036] Explanation of the main component symbols: 110 - current collector; 120 - active material layer; 121 - groove; 200 - carving knife; 300 - dust cover; 310 - elastic sealing gasket. DETAILED DESCRIPTION
[0037] In lithium-ion batteries of related technologies, in order to meet the demand for high energy density, the pole piece manufacturing process mainly adopts technologies such as thick electrodes, high compaction, and high specific energy materials (such as silicon negative electrodes, etc.), but the above technologies will increase the transmission distance and resistance of lithium ions, aggravate stress accumulation and cause problems such as pole piece wrinkles, making it difficult for the pole piece to take into account high power density characteristics. The inventors found that by opening grooves on the active material layer on the surface of the pole piece, the pole piece tortuosity can be reduced and the above problems can be alleviated. However, the way of opening the grooves will affect the performance of the pole piece. For example, chemical etching is prone to produce inactive material residues that affect battery performance. At the same time, this method is complicated to operate and difficult to control accuracy; the use of laser etching will cause the physical properties of the active material layer to be destroyed due to thermal effects, and may also produce laser vapor residues, which is not conducive to battery performance. Other methods such as magnetic field induction, freeze drying, plant fiber templates, etc. are difficult to apply in industry.
[0038] Therefore, the embodiment of the present application provides a method for manufacturing a pole piece, which forms grooves on the active material layer of the pole piece by mechanically scratching, which can effectively reduce the tortuosity of the pole piece, avoid wrinkles on the surface of the pole piece, and is not easy to have a negative impact on the performance of the pole piece and even the battery. Moreover, the pole piece manufacturing method is highly controllable and easy to implement in industry. In addition, the present application also provides an electrode made by the above-mentioned pole piece manufacturing method and a battery containing the electrode.
[0039] In order to make the purpose, technical scheme and advantages of the embodiments of the present application clearer, the technical scheme in the embodiments of the present application will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to the conventional conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0040] Figure 1 This is a flow chart of a method for manufacturing a pole piece in one embodiment of the present application. The pole piece manufacturing method provided in the embodiment of the present application can be used to manufacture a positive pole piece, and can also be used to manufacture a negative pole piece. Figure 1 As shown, the pole piece manufacturing method includes:
[0041] Step S100, forming an active material layer on the surface of the current collector to obtain a pole piece to be scribed.
[0042] In the embodiment of the present application, the electrode to be scribed will be mechanically scribed later, so it is required to have certain mechanical properties, such as not being prone to cracking or collapse, and not being prone to producing excessive powder due to mechanical scribe.
[0043] Figure 2 This is a flow chart of making a pole piece to be scribed in one embodiment of the present application. Figure 2 As shown, in an optional embodiment, a wet process may be used to obtain a pole piece to be scribed, and the specific method includes:
[0044] Step S101 : applying a slurry containing an active material and a binder to a current collector.
[0045] Furthermore, the binder is one or more of polyimide, polyacrylonitrile, and aramid. This type of binder has stronger viscosity than other conventional binders, and the active material layer 120 (see Figure 3-Figure 6 ) It is not easy to lose powder due to scratching.
[0046] Step S102, drying and baking the current collector coated with the slurry to obtain a pole piece to be scribed.
[0047] In this embodiment, the baking temperature may be 80-300° C., and further 120-250° C. After drying, high-temperature baking can complete pre-curing, greatly improving the bonding force of the active material layer 120 of the electrode, thereby further reducing the amount of powder falling during the scribing process.
[0048] In another optional embodiment, a dry process can also be used to obtain the electrode to be scribed. The specific method includes: using a dry process, a mixture containing active materials and a binder is laid on the current collector 110 by lamination and lamination (see Figure 3-Figure 6 Specifically, the mixture containing active materials and binders can be firstly squeezed into an electrode film (i.e., active material layer 120) by rollers, and then the electrode film is laminated on the current collector 110 by hot rollers or adhesive.
[0049] Since the active material layer 120 prepared by the dry process has strong self-supporting properties, it is suitable for preparing ultra-thick electrodes with a low risk of powder loss. Since the active material layer 120 prepared in this way is easy to scribe, the requirements for the scriber are low, and a simple scriber can be used to scribe the electrode to be scribed.
[0050] In the embodiment of adopting dry method to make the pole piece to be scribed, the adhesive may be selected as PTFE emulsion.
[0051] Furthermore, the mixture may further include a conductive agent, which may be a conventional conductive agent SP.
[0052] It should be understood that the material of the active material layer 120 should be reasonably selected according to whether the electrode to be manufactured is a positive electrode or a negative electrode.
[0053] When making the positive electrode, the active materials used include but are not limited to chemical formulas such as Li x Ni h Co y M z O 2-d Nd (where 0.95≤x≤1.2, h>0, y≥0, z≥0, and h+y+z=1, 0≤d≤1, M is selected from one or more combinations of Mn and Al, and N is selected from one or more combinations of F, P, and S). The active material suitable for the positive electrode sheet can also be LiCoO2, LiNiO2, LiVO2, LiCrO2, LiMn2O4, LiCoMnO4, Li2NiMn3O8, LiNi 0.5 Mn 1.5 O4, LiCoPO4, LiMnPO4, LiFePO4, LiNiPO4, LiCoFSO4, CuS2, FeS2, MoS2, NiS, TiS2, etc. The active material suitable for the positive electrode plate may also be modified by a modification method in the prior art, for example, the active material may be modified by coating, doping, etc. The additive materials used in the modification include but are not limited to a combination of one or more of Al, B, P, Zr, Si, Ti, Ge, Sn, Mg, Ce, W, etc.
[0054] When making negative electrode sheets, the active materials used include natural graphite, artificial graphite, mesophase microcarbon beads, hard carbon, soft carbon, silicon, silicon-carbon composites, Li-Sn alloys, Li-Sn-O alloys, Sn, SnO, SnO2, spinel-structured lithiated TiO2-Li4Ti5O 12 , Li-Al alloy, or one or more of the above materials, or modified products thereof.
[0055] Regardless of whether the electrode to be manufactured is a positive electrode or a negative electrode, the raw materials for manufacturing the active material layer 120 may contain a conductive agent.
[0056] Optionally, the active material layer 120 may completely cover or partially cover the current collector 110 ; the active material layer 120 may be disposed on both sides or one side of the current collector 110 .
[0057] Step S200 , using a carving knife to carve grooves on the active material layer 120 of the electrode to be carved, so as to obtain the electrode.
[0058] In the embodiment of the present application, grooves are carved on the active material layer 120 to alleviate the stress concentration problem of the active material layer 120, and can also allow the grooves to absorb a certain amount of deformation when the pole piece is wound to avoid wrinkles on the pole piece surface. The grooves are made by mechanical carving with a carving knife, which can well control the carving accuracy, and will not affect the chemical properties of the active material layer 120, and is not likely to have a negative impact on the performance of the pole piece.
[0059] Optionally, during the scribing process, the electrode manufacturing method provided in the embodiment of the present application further includes: forming a negative pressure around the scribing knife to absorb the powder generated during the scribing process. By timely removing the powder generated during the scribing process from the electrode surface, it is possible to avoid the powder from clogging the groove and also to avoid the powder from scattering on the electrode surface, thereby ensuring the flatness of the electrode surface.
[0060] Optionally, this embodiment may use a specially designed scribing system to achieve scribing. Figure 3 FIG. 1 is a schematic diagram of a delineation process in one embodiment of the present application. Figure 3 As shown, the engraving system provided in the embodiment of the present application includes a controller (not shown in the figure), a driving mechanism (not shown in the figure), a dust hood 300, a carving knife 200 and a negative pressure device (not shown in the figure). The carving knife 200 is arranged in the dust hood 300, and the dust hood 300 is connected to the negative pressure device. The negative pressure device is used to generate negative pressure in the dust hood 300. During the engraving process, the opening of the dust hood 300 faces the active material layer 120, and the end of the carving knife 200 extends from the opening of the dust hood 300 to insert the active material layer 120, and the dust hood 300 moves with the carving knife 200. The driving mechanism is used to drive the carving knife 200 to move to achieve engraving. Further, the driving mechanism can drive the carving knife 200 to move in three-dimensional space under the control of the controller to control the carving knife 200 to engrave the required graphics and control the depth of the engraving.
[0061] Furthermore, in order to ensure a better carving and dust collection effect, the opening edge of the dust cover 300 is provided with an elastic sealing pad 310 for abutting the active material layer 120. By controlling the compression of the elastic sealing pad 310, the amount of the engraving knife 200 extending out of the opening of the dust cover 300 can be controlled, that is, the depth of the groove 121 can be controlled. Optionally, in actual use, the compression of the elastic sealing pad 310 can be characterized and fed back by pressure. For example, a pressure sensor is provided between the elastic sealing pad 310 and the dust cover 300. When the feedback downward pressure is large, it means that the elastic sealing pad 310 is compressed to a large extent, the engraving knife 200 extends to a large extent, and the groove 121 is deeper. Optionally, when the elastic sealing pad 310 is in an uncompressed state, the end of the engraving knife 200 does not extend out of the dust cover 300.
[0062] The groove 121 can be processed on the pole piece by using the above-mentioned scribing system, and no powder residue is left on the pole piece finally obtained.
[0063] Figure 4 Schematic diagram of a pole piece in one embodiment of the present application. Figure 4 As shown, the pole piece has a plurality of grooves 121 , and the plurality of grooves 121 are interlaced with each other to form a grid-like pattern. Figure 4In the figure, multiple grooves 121 in two extending directions intersect obliquely to form a diamond-shaped grid. In other optional embodiments, the pattern shape formed by the grooves 121 can be set as needed, such as rectangular, honeycomb, wavy, etc., and its depth, width, density, etc. can also be distinguished and matched according to the characteristics of different areas in the plane of the pole piece. By dividing the active material layer 120 of the entire pole piece into multiple small islands through the grooves 121, the stress that the pole piece (especially the pole piece of ultra-thick, high-density, and high-strain materials) must face can be released at the grooves 121 between the small islands, avoiding a large amount of stress accumulation, thereby avoiding wrinkles on the pole piece as a whole.
[0064] Figure 5 : is a cross-sectional view of a pole piece in one embodiment of the present application. Figure 5 As shown, since the width and depth of the groove 121 of the engraving will affect the performance of the pole piece, optionally, the width t of the groove 121 in the embodiment of the present application is 100-1000 μm. Further, the width of the groove 121 can be selected to be 150-500 μm, and this size range is between the sub-microscopic level between the microscopic and macroscopic levels, which can enhance its functional role. Optionally, the ratio of the depth h of the groove 121 to the thickness H of the active material layer 120 is 0.05-1, and the depths of different grooves 121 can be the same or different.
[0065] Furthermore, the active material layer 120 of the current electrode is generally composed of microscopic active powder particles with a size between 2 and 50 μm. Under the influence of the volume effect during the charge and discharge process, the powder particles will continuously shrink, expand, and slip, that is, the particle distribution will continue to rearrange. Figure 6 FIG. 1 is a schematic diagram of active powder particles falling into the groove 121 in one embodiment of the present application. Figure 6 As shown, during use, it is inevitable that a single particle (particle size d) will be peeled off from the edge of the groove 121 (width t) into the groove 121, and the apparent average volume expansion rate of the currently practical pole piece is generally between 0% and 80% (that is, the average particle size maximum of the larger single particle during the charge and discharge process will be between 30 and 70 μm). In the embodiment of the present application, the width of the groove 121 reaches hundreds of microns. On the one hand, the groove 121 can effectively achieve the above-mentioned avoidance of a large amount of stress accumulation. On the other hand, due to the large ratio of the width of the groove 121 to the particle size of the single particle (t / d value), it can avoid the groove 121 of the pole piece after a short period of charge and discharge. It is quickly blocked and damaged by sporadic particles, resulting in a weakened effect of reducing the tortuosity of the pole piece, affecting the energy density and power density.
[0066] When the pole piece is applied to the battery, the active material layer 120 needs to withstand the pressure from the isolation membrane and the pole piece on the other side of the isolation membrane. Since the width of the groove 121 is limited to hundreds of microns in this embodiment, the pole piece is still continuous in macroscopic terms, and the isolation membrane and the pole piece on the other side of the isolation membrane can still be effectively supported in the vicinity of the groove 121, avoiding the problem that the isolation membrane is excessively sunken toward the bottom of the groove 121 due to the unequal support force of the pole pieces on both sides of the isolation membrane caused by the groove 121 being too wide.
[0067] The battery provided in the embodiment of the present application (not shown in the figure) includes a housing, a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte. The positive electrode sheet and the negative electrode sheet are separated by a separator, and the stacked structure of the three is wound into a core and stored in the housing, and the housing is filled with an electrolyte. The battery provided in the embodiment of the present application can be a lithium-ion battery, in which one or both of the positive electrode sheet and the negative electrode sheet are made by the electrode sheet manufacturing method provided in the above embodiment of the present application.
[0068] The material of the isolation membrane can be selected from one or a combination of polyethylene, polypropylene, polyvinylidene fluoride, aramid, polyethylene terephthalate, polytetrafluoroethylene, polyacrylonitrile, polyimide, polyamide, polyester and natural fiber.
[0069] In the case where the battery is a lithium-ion battery, the electrolyte includes an organic solvent, an electrolyte lithium salt and an additive. Among them, the electrolyte lithium salt can be LiPF6 and / or LiBOB used in high-temperature electrolytes; it can also be at least one of LiBF4, LiBOB, and LiPF6 used in low-temperature electrolytes; it can also be at least one of LiBF4, LiBOB, LiPF6, and LiTFSI used in anti-overcharge electrolytes; it can also be at least one of LiClO4, LiAsF6, LiCF3SO3, and LiN(CF3SO2)2. The organic solvent can be a cyclic carbonate, including PC and EC; it can also be a chain carbonate, including DFC, DMC, or EMC; it can also be a carboxylic acid ester, including MF, MA, EA, MP, etc. The additives include but are not limited to at least one of film-forming additives, conductive agents, flame retardant additives, anti-overcharge additives, additives for controlling the content of H2O and HF in the electrolyte, additives for improving low-temperature performance, and multifunctional additives.
[0070] The characteristics and performance of the battery provided in the embodiments of the present application are further described in detail below in conjunction with the embodiments.
[0071] Example 1
[0072] Make the battery using the following steps:
[0073] 1) Preparation of positive electrode sheet: positive electrode active material (NCM), conductive agent (SP), binder (PVDF) etc. are mixed according to proportion, solvent (NMP) is added, and the mixture is stirred and mixed evenly under the action of a vacuum mixer to obtain positive electrode slurry; the positive electrode slurry is evenly coated on the positive electrode collector (aluminum foil), and the positive electrode sheet is obtained after drying and baking.
[0074] 2) Preparation of negative electrode sheet: Using the electrode sheet manufacturing method (dry process) provided in the embodiment of the present application, the negative electrode active material (graphite), conductive agent (SP), binder (PTFE emulsion) and the like are mixed in a dry process according to a proportion, and the mixture is laid on the negative electrode current collector by lamination and lamination to obtain a negative electrode sheet to be scribed; the negative electrode sheet to be scribed is scribed with a scriber to form a negative electrode sheet with a groove structure. The groove width t is 220 μm, and the ratio of the groove depth h to the thickness H of the active material layer is 0.53.
[0075] 3) Forming the positive electrode sheet, the negative electrode sheet and the separator into a winding core;
[0076] 4) The core is then packaged, dried, injected, and formed into a battery.
[0077] Example 2
[0078] Make the battery using the following steps:
[0079] 1) Preparation of positive electrode sheet: positive electrode active material (NCM), conductive agent (SP), binder (PVDF) etc. are mixed according to proportion, solvent (NMP) is added, and the mixture is stirred and mixed evenly under the action of a vacuum mixer to obtain positive electrode slurry; the positive electrode slurry is evenly coated on the positive electrode collector (aluminum foil), and the positive electrode sheet is obtained after drying and baking.
[0080] 2) Preparation of negative electrode sheet: Using the electrode sheet manufacturing method (wet process) provided in the embodiment of the present application, the negative electrode active material (graphite), conductive agent (SP), binder (polyimide, polyacrylonitrile or aramid) and the like are prepared into slurry in proportion; the prepared slurry is wet coated on the corresponding negative electrode current collector foil, and after drying and high-temperature baking, a negative electrode sheet to be scribed is formed; the negative electrode sheet to be scribed is scribed with a scriber to form a negative electrode sheet with a groove structure. The groove width t is 210 μm, and the ratio of the groove depth h to the thickness H of the active material layer is 0.75.
[0081] 3) The positive electrode sheet, negative electrode sheet and separator are made into a winding core.
[0082] 4) The core is then packaged, dried, injected, and formed into a battery.
[0083] Example 3
[0084] Make the battery using the following steps:
[0085] 1) Preparation of positive electrode sheet: positive electrode active material (NCM), conductive agent (SP), binder (PVDF) etc. are mixed according to proportion, solvent (NMP) is added, and the mixture is stirred and mixed evenly under the action of a vacuum mixer to obtain positive electrode slurry; the positive electrode slurry is evenly coated on the positive electrode collector (aluminum foil), and the positive electrode sheet is obtained after drying and baking.
[0086] 2) Preparation of negative electrode sheet: Using the electrode sheet manufacturing method (wet process) provided in the embodiment of the present application, the negative electrode active material (graphite), conductive agent (SP), binder (polyimide, polyacrylonitrile or aramid) and the like are prepared into slurry in proportion; the prepared slurry is wet coated on the corresponding negative electrode current collector foil, and after drying and high-temperature baking, a negative electrode sheet to be scribed is formed; the negative electrode sheet to be scribed is scribed with a scriber to form a negative electrode sheet with a groove structure. Among them, the groove width t is 350 μm, and the ratio of the groove depth h to the thickness H of the active material layer is 0.52.
[0087] 3) The positive electrode sheet, negative electrode sheet and separator are made into a winding core.
[0088] 4) The core is then packaged, dried, injected, and formed into a battery.
[0089] Comparative Example 1
[0090] Make the battery using the following steps:
[0091] 1) Preparation of positive electrode sheet: positive electrode active material (NCM), conductive agent (SP), binder (PVDF) etc. are mixed according to proportion, solvent (NMP) is added, and the mixture is stirred and mixed evenly under the action of a vacuum mixer to obtain positive electrode slurry; the positive electrode slurry is evenly coated on the positive electrode collector (aluminum foil), and the positive electrode sheet is obtained after drying and baking.
[0092] 2) Preparation of negative electrode sheet: The negative electrode active material (graphite), conductive agent (SP), binder (PTFE emulsion) and the like are mixed in proportion by a dry process, and the mixture is laid on the negative electrode collector by pressing and laminating to obtain the negative electrode sheet.
[0093] 3) The positive electrode sheet, negative electrode sheet and separator are made into a winding core.
[0094] 4) The core is then packaged, dried, injected, and formed into a battery.
[0095] Since the negative electrode plate component designs of the above-mentioned embodiments 1-3 and comparative example 1 are substantially consistent and their absolute capacities are similar, their energy density and power density can be compared and evaluated by the high-rate energy discharge retention rate, and the results are shown in the following table.
[0096]
[0097] It can be seen from the above table that the rate discharge retention ratios in Examples 1 to 3 are significantly better than those in Comparative Example 1, which indicates that the electrode sheets provided with grooves have lower tortuosity and the batteries assembled therefrom have better performance.
[0098] In summary, the pole piece manufacturing method provided in the present application includes manufacturing an active material layer on the surface of a current collector to obtain a pole piece to be engraved; and using a carving knife to carve grooves on the active material layer of the pole piece to be engraved to obtain the pole piece. Carving grooves on the active material layer can release the stress in the active material layer of the pole piece, and when winding, the grooves can absorb certain deformations, thereby improving the problem of wrinkles on the surface of the pole piece. The use of this manufacturing method can effectively reduce the tortuosity of the pole piece, so that it can take into account both high energy density and high power density characteristics. Moreover, the grooves are formed by mechanical carving with a carving knife, which has good controllability, uniformity, and reliability, and is conducive to mass production. In addition, the use of mechanical carving is not easy to have a negative impact on the material properties of the active material layer due to thermal effects or chemical reactions, thereby ensuring the performance of the pole piece.
[0099] The pole piece provided in the present application is made by the pole piece manufacturing method described above, has a low tortuosity, can take into account both high energy density and high power density characteristics, and is not easy to wrinkle. The battery provided in the present application includes the pole piece described above, and therefore also has corresponding beneficial effects.
[0100] The above are only preferred embodiments of the present application and are not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.
Claims
1. A method for manufacturing a pole piece, It is characterized in that include: Making an active material layer on the surface of the current collector to obtain a pole piece to be scribed; Using a carving knife to carve grooves on the active material layer of the electrode to be carved, so as to obtain the electrode; The active material layer is composed of microscopic active powder particles with a size between 2 and 50 μm, and the width of the groove is 150 to 500 μm; The electrode manufacturing method further includes: forming negative pressure around the carving knife to absorb powder generated during the carving process; The engraving knife is arranged in a dust hood, and the dust hood is connected to a negative pressure device, and the negative pressure device is used to generate negative pressure in the dust hood. During the engraving process, the opening of the dust hood faces the active material layer, and the end of the engraving knife extends from the opening of the dust hood to be inserted into the active material layer, and the dust hood moves with the engraving knife; an elastic sealing pad for abutting the active material layer is provided at the opening edge of the dust hood, and a pressure sensor is provided between the elastic sealing pad and the dust hood, and the pressure sensor is used to feedback the downward pressure of the dust hood; the depth of the groove is controlled according to the downward pressure.
2. The method for manufacturing a pole piece according to claim 1, It is characterized in that The steps of forming an active material layer on the surface of the current collector to obtain a pole piece to be scribed include: applying a slurry comprising an active material and a binder to the current collector; The current collector coated with the slurry is dried and baked to obtain the pole piece to be scribed.
3. The method for manufacturing a pole piece according to claim 2, It is characterized in that The binder is one or more of polyimide, polyacrylonitrile and aramid.
4. The method for manufacturing a pole piece according to claim 2, It is characterized in that The baking temperature is 80-300°C.
5. The method for manufacturing a pole piece according to claim 1, It is characterized in that The steps of forming an active material layer on the surface of the current collector to obtain a pole piece to be scribed include: By using a dry process, a mixture containing active materials and a binder is laid on the current collector by means of film pressing and lamination to obtain the electrode to be scribed.
6. The method for manufacturing a pole piece according to claim 5, It is characterized in that The binder includes PTFE emulsion.
7. The method for manufacturing a pole piece according to claim 5, It is characterized in that The mixture also includes a conductive agent.
8. The method for manufacturing a pole piece according to claim 1, It is characterized in that The ratio of the depth of the groove to the thickness of the active material layer is 0.05-1.
9. The method for manufacturing a pole piece according to claim 1, It is characterized in that There are multiple grooves, and the multiple grooves are interlaced to form a grid pattern.
10. A pole piece, It is characterized in that The pole piece is manufactured by the pole piece manufacturing method described in any one of claims 1 to 9.
11. A battery, It is characterized in that Including the pole piece as claimed in claim 10.