Moisture barrier laminated film

By setting a coating with low moisture permeability and high viscoelasticity between the inorganic barrier layer and the moisture trapping layer, the problem of reduced adhesion and barrier properties of moisture barrier laminates under high temperature and high humidity conditions is solved, achieving long-term and efficient moisture barrier effect, and making it suitable for sealing materials of high-performance electronic devices.

CN115551709BActive Publication Date: 2024-10-01TOYO SEIKAN GRP HLDG LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202180033581.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-05-12
Filing Date
2021-03-26
Publication Date
2024-10-01
Estimated Expiration
2041-03-26

AI Technical Summary

Technical Problem

Existing moisture-barrier laminated films exhibit significantly reduced interlayer adhesion and moisture barrier properties under high temperature and humidity conditions, failing to meet the requirements of high-performance electronic devices.

Method used

A viscoelastic coating with a permeability of less than 6.0×10⁴ g/m²/day and a storage modulus E' (@2πrad/s) of more than 30 MPa in a viscoelasticity test at 85°C is applied between the inorganic barrier layer and the moisture capture layer to inhibit alkali degradation and membrane peeling.

Benefits of technology

It maintains excellent moisture barrier properties over long periods under high temperature and high humidity conditions, and its performance can be quickly evaluated through degradation testing, making it suitable for sealing materials of electronic devices in high humidity environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115551709B_ABST
    Figure CN115551709B_ABST
Patent Text Reader

Abstract

A moisture barrier laminated film (10), characterized in that the moisture barrier laminated film comprises a plastic film (A) having an inorganic barrier layer (A1) and a moisture capture layer (B) containing an alkali component, a coating layer (C) is provided between the inorganic barrier layer (A1) and the moisture capture layer (B), and the moisture permeability of the coating layer (C) at 40°C and 90% RH is 6.0×10 4 g / m 2 / day or less, and the storage modulus E' (@2πrad / s) in the viscoelasticity measurement at 85°C is 30 MPa or more.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a moisture barrier laminate film having an inorganic barrier layer and a moisture capture layer, and in particular to a moisture barrier laminate film that exhibits high moisture barrier properties even in a high humidity atmosphere. Background Art

[0002] As a method for improving the properties of various plastic substrates, especially the gas barrier properties, it is known to form an inorganic thin film (inorganic barrier layer) composed of silicon oxide or the like on the surface of the plastic substrate by vapor deposition (Patent Document 1), and films having such inorganic thin films are widely used as barrier films.

[0003] In addition, various electronic devices developed and put into practical use in recent years, such as organic electroluminescence (organic EL), solar cells, touch panels, and electronic paper, also require high moisture barrier properties. In order to meet such requirements, the applicant has proposed a moisture barrier laminate having a structure with a moisture capture layer stacked thereon (Patent Document 2).

[0004] The moisture-capturing layer as described above is formed by coating a moisture-capturing layer-forming coating composition on an inorganic barrier layer formed on the surface of a plastic film by vapor deposition or the like, and curing the coating composition.

[0005] The moisture barrier laminate described in Patent Document 2 exhibits excellent moisture barrier properties and is used as a sealing material for electronic devices such as organic EL, for example.

[0006] Furthermore, recently, with the high performance of various electronic devices, the degree of moisture barrier properties required is increasing. Therefore, it is necessary to confirm whether the moisture barrier laminated film used as a sealing material has a high moisture barrier property that can meet such requirements. Such quality tests are carried out in a high temperature and high humidity atmosphere that is relatively high compared to the usual humidity atmosphere in which electronic devices are used to promote degradation.

[0007] However, conventionally known moisture barrier laminated films have a problem of significantly reduced interlayer adhesion and moisture barrier properties when their moisture barrier properties are measured in a high humidity environment, particularly in a high temperature and high humidity atmosphere such as an accelerated degradation test, and further improvements are needed.

[0008] Prior art literature

[0009] Patent Literature

[0010] Patent Document 1: Japanese Patent Application Publication No. 2000-255579

[0011] Patent Document 2: Japanese Patent Application Publication No. 2015-96320 Summary of the invention

[0012] Problem that the invention aims to solve

[0013] Therefore, an object of the present invention is to provide a moisture-barrier laminate film comprising a plastic film (A) having an inorganic barrier layer (A1) on the surface and a moisture-capturing layer (B), wherein the moisture-barrier laminate film can exhibit excellent moisture-barrier properties for a long period of time even in a high-temperature and high-humidity atmosphere.

[0014] Technical Solution

[0015] Regarding a moisture-barrier laminated film having excellent moisture-barrier properties in a high-temperature and high-humidity atmosphere, the applicant previously proposed a moisture-barrier laminated film in Japanese Patent Application No. 2020-183064 (Japanese Patent Application No. 2019-087677), characterized in that the moisture-barrier laminated film comprises a plastic film (A) of an inorganic barrier layer (A1) and a moisture-capturing layer (B) containing an alkali component, and is used in a degradation acceleration test in a high-temperature and high-humidity atmosphere at a temperature of 85°C or above and a relative humidity of 85% or above, in which a coating (C) is provided between the inorganic barrier layer (A1) and the moisture-capturing layer (B), and the coating (C) is composed of a plastic film (A) of 6.0×10 4 g / m 2 / day or less polymer formation.

[0016] That is, the moisture barrier laminate film has a moisture permeability of 6.0×10 4 g / m 2 / day or less, thereby fully utilizing the barrier properties of the moisture capture layer (B) and the inorganic barrier layer (A1), and showing excellent moisture barrier properties even in a high temperature and high humidity atmosphere above 85°C and a relative humidity above 85%.

[0017] The present inventors further advanced the technology of the above-mentioned prior applications (Japanese Patent Application No. 2019-087677; Japanese Patent Application No. 2020-183064), and discovered the following fact, thereby completing the present invention, that is, by providing a coating (C) between the moisture capture layer (B) containing an alkali component and the inorganic barrier layer (A1) with a certain storage modulus E', the deterioration of the moisture barrier property caused by the alkali component can be suppressed for a longer period of time.

[0018] According to the present invention, there is provided a moisture barrier laminate film, characterized in that the moisture barrier laminate film comprises a plastic film (A) having an inorganic barrier layer (A1) and a moisture capture layer (B) containing an alkali component,

[0019] A coating layer (C) is provided between the inorganic barrier layer (A1) and the moisture capture layer (B),

[0020] The moisture permeability of the coating (C) at 40°C and 90% RH is 6.0×10 4 g / m 2 / day or less, and the storage modulus E' (@2πrad / s) in the viscoelasticity measurement at 85°C is 30 MPa or more.

[0021] The moisture barrier laminated film of the present invention can preferably adopt the following aspects.

[0022] (1) The coating layer (C) is formed of a urethane (meth)acrylate polymer.

[0023] (2) The coating layer (C) contains a catalyst in a range of 0.02 to 1.0 mass %.

[0024] (3) The catalyst is a metal catalyst.

[0025] (4) The urethane (meth)acrylate polymer has a high glass transition point of 85° C. or higher.

[0026] (5) A protective layer (D) is provided between the inorganic barrier layer (A1) and the coating layer (C).

[0027] (6) The protective layer (D) contains, in addition to the water-soluble polymer (D1), at least one component (D2) selected from the group consisting of the following compounds:

[0028] Compounds of ingredient (D2):

[0029] Organoalkoxysilane or its hydrolyzate;

[0030] Metal alkoxides or their hydrolysates;

[0031] as well as

[0032] Phosphorus compounds.

[0033] (7) A coating layer (C) is also provided on the side of the moisture capture layer (B) opposite to the inorganic barrier layer (A1).

[0034] Such a moisture-barrier laminated film of the present invention is preferably used as a sealing material for electronic devices.

[0035] Effects of the Invention

[0036] The moisture barrier laminated film of the present invention has a basic structure in which a moisture capture layer (B) is provided on an inorganic barrier layer (A1) present in a plastic film (A), but has a remarkable feature in that a coating layer is provided between the inorganic barrier layer (A1) and the moisture capture layer (B), and the coating layer satisfies a moisture permeability of 6.0×10 4 g / m 2 / day or less, and a viscoelastic condition in which the storage modulus E' (@2πrad / s) in the viscoelasticity measurement at 85°C is 30 MPa or more.

[0037] That is, the inorganic barrier layer (A1) is formed by vapor deposition using plasma CVD or the like and is formed of oxides of Al and Si, but has the property of being reactive to alkali and having low alkali resistance.

[0038] On the other hand, as for the moisture capture layer (B), in order to ensure high moisture capture, an ionic polymer is used as a film-forming component, but such an ionic polymer contains an alkali component in any case of a cationic system and an anionic system. For example, a cationic polymer has a cationic group such as a quaternary ammonium group, and thus becomes a substance containing an amine component. In addition, anionic polymers contain alkali metal salts such as sodium salts and potassium salts, and generate alkalis such as NaOH and KOH through contact with water. Moreover, in the moisture capture layer (B), in order to seal the moisture after the above-mentioned ionic polymer absorbs moisture into the layer and prevent deformation such as swelling caused by moisture absorption, a hygroscopic agent is also provided. As such a hygroscopic agent, the most preferred is the sodium salt and potassium salt of cross-linked poly (meth) acrylic acid, which still generates alkali through contact with water.

[0039] Therefore, if the moisture capture layer (B) is directly formed on the inorganic barrier layer (A1), the inorganic barrier layer (A1) is alkaline-degraded because the moisture capture layer (B) contains an alkali component. In such a case, if the laminated film is maintained under the conditions of a high temperature and high humidity atmosphere, the moisture capture layer (B) in the film absorbs a large amount of moisture in a short time. As a result, the alkali degradation of the inorganic barrier layer (A1) is significantly promoted, and delamination occurs at the interface between the inorganic barrier layer (A1) and the moisture capture layer (B), or at the interface between the inorganic barrier layer (A1) and the plastic film (A), and moisture leaks from this part, and the moisture barrier property is greatly impaired. That is, even if it shows extremely high moisture barrier properties in a low humidity atmosphere, its moisture barrier properties are greatly reduced in a high temperature and high humidity atmosphere. In addition, even if the actual use environment is not a high temperature and high humidity atmosphere, there is a problem that it is impossible to perform a degradation promotion test and perform performance evaluation, resulting in poor quality control.

[0040] However, in the present invention, a coating (C) satisfying the above-mentioned moisture permeability conditions and viscoelastic conditions is provided between the inorganic barrier layer (A1) and the moisture capture layer (B), thereby being able to effectively suppress the alkali degradation of the inorganic barrier layer (A1) caused by moisture absorbed by the moisture capture layer (B). For example, high moisture barrier properties can be exhibited even when a high temperature and high humidity atmosphere is maintained for a long time, and a degradation promotion test can be performed to evaluate the performance of the moisture barrier properties.

[0041] Here, the above-mentioned moisture permeability conditions and viscoelasticity conditions that the coating layer (C) should satisfy are briefly described.

[0042] First, the moisture permeability under the moisture permeability condition of 40°C and 90% RH is 6.0×10 4 g / m 2 / day means that the coating (C) is a film formed of a non-aqueous polymer, specifically a film formed of a solvent-based coating. The above conditions are also proposed in the prior application of the present inventors (Japanese Patent Application No. 2019-087677), and by providing a highly non-aqueous coating (C) between the inorganic barrier layer (A1) and the moisture capture layer (B), the transfer of alkaline water from the moisture capture layer (B) to the inorganic barrier layer (A1) is suppressed as much as possible, and the film peeling caused by alkali degradation of the inorganic barrier layer (A1) is effectively suppressed.

[0043] Next, regarding the storage modulus E' (@2πrad / s) in the viscoelastic measurement under viscoelastic conditions, i.e., at 85°C, it is 30MPa or more, which is the most important feature of the present invention. That is, the coating (C) showing the above storage modulus E' means that the coating (C) is a viscoelastic body, and when a certain stress is applied to the coating (C), strain (deformation) occurs with a certain time difference. In the present invention, the storage modulus E' (@2πrad / s) of the coating (C) formed by such a viscoelastic body at high temperature (85°C) shows a maximum value of 30MPa or more, and the relaxation of the coating film at high temperature is suppressed, and at high temperature, it is in a state that is not easily deformed relative to shear force (i.e., not easily peeled off).

[0044] Therefore, in the present invention, the coating (C) as described above is provided between the inorganic barrier layer (A1) and the moisture capture layer (B), so that even in a high temperature and high humidity atmosphere, the alkali degradation of the inorganic barrier layer (A1) is suppressed, and the coating (C) is in a state that is not easy to peel off even at high temperatures. As a result, even in a high temperature and high humidity atmosphere, the penetration of alkaline water into the inorganic barrier layer (A1) is suppressed, thereby exerting high moisture barrier properties for a long time.

[0045] For example, when the coating layer (C) satisfies the above-mentioned moisture permeability condition but does not satisfy the viscoelasticity condition, in an atmosphere of 85°C and 85% RH, the peel strength between the inorganic barrier layer (A1) and the substrate is high (for example, higher than 2N / 15mm), but the high moisture barrier property is exhibited for about 1 to 3 days. On the other hand, according to the present invention, when both the above-mentioned moisture permeability condition and the viscoelasticity condition are satisfied, the high peel strength can be ensured and the high moisture barrier property can be exhibited even after 10 days, and further after 20 days.

[0046] Therefore, the moisture-barrier laminated film of the present invention exhibits high moisture-barrier properties even when used in a high-temperature, high-humidity atmosphere, and its performance can be evaluated in a short time by an accelerated degradation test. BRIEF DESCRIPTION OF THE DRAWINGS

[0047] Figure 1 This is a diagram showing an example of the layer structure of the moisture-barrier laminated film of the present invention.

[0048] Figure 2 Yes means Figure 1 A diagram showing the structure of a moisture-capturing layer (B) in a moisture-barrier laminate film.

[0049] Figure 3 It is a figure which shows another example of the layer structure of the moisture-barrier laminated film of the present invention.

[0050] Figure 4 It is a figure which shows another example of the layer structure of the moisture-barrier laminated film of the present invention.

[0051] Figure 5 It is a figure which shows another example of the layer structure of the moisture-barrier laminated film of the present invention. DETAILED DESCRIPTION

[0052] exist Figure 1 In the figure, the moisture barrier laminated film of the present invention, which is represented as a whole by 10, has a plastic film (A) as a substrate, an inorganic barrier layer (A1) is formed on the surface of the plastic film (A), and a coating layer (C) is provided between the inorganic barrier layer (A1) and the moisture capture layer (B). That is, the coating layer (C) and the moisture capture layer (B) are sequentially formed on the inorganic barrier layer (A1) of the plastic film (A).

[0053] Furthermore, in the above-mentioned plastic film (A), if Figure 3 As shown in FIG. 1 , a protective layer (D) is sometimes provided on the inorganic barrier layer (A1). That is, the coating layer (C) may be directly laminated on the inorganic barrier layer (A1), or may be laminated on the inorganic barrier layer (A1). Figure 3 As shown, it is laminated on the protective layer (D) appropriately provided on the inorganic barrier layer (A1), and it only needs to be present between the inorganic barrier layer (A1) and the moisture capture layer (B).

[0054] <Plastic film (A)>

[0055] The film (A) becomes the base of the inorganic barrier layer (A1) and is usually formed from a thermoplastic or thermosetting resin by injection or co-injection molding, extrusion or co-extrusion molding, film or sheet molding, compression molding, cast polymerization, etc., depending on its form.

[0056] Generally, thermoplastic resins are preferred from the viewpoints of moldability, cost, and the like.

[0057] Examples of such thermoplastic resins are not limited thereto, and the following thermoplastic resins can be exemplified.

[0058] Polyolefins:

[0059] Low-density polyethylene; High-density polyethylene; Polypropylene;

[0060] Poly-1-butene; Poly-4-methyl-1-pentene;

[0061] Random or block copolymers of α-olefins such as ethylene, propylene, 1-butene, 4-methyl-1-pentene, etc.;

[0062] Cyclic olefin copolymers, etc.

[0063] Ethylene / vinyl copolymers:

[0064] Ethylene / vinyl acetate copolymer; Ethylene / vinyl alcohol copolymer; Ethylene / vinyl chloride copolymer, etc.;

[0065] Styrene resin:

[0066] Polystyrene; Acrylonitrile / Styrene Copolymer; ABS;

[0067] α-Methylstyrene / styrene copolymer, etc.;

[0068] Polyvinyl compounds:

[0069] Polyvinyl chloride; polyvinylidene chloride; vinyl chloride / vinylidene chloride copolymer; polymethyl acrylate; polymethyl methacrylate, etc.;

[0070] Polyamide:

[0071] Nylon 6; Nylon 6-6; Nylon 6-10; Nylon 11; Nylon 12, etc.;

[0072] Thermoplastic Polyester:

[0073] Polyethylene terephthalate (PET); Polybutylene terephthalate;

[0074] Polyethylene naphthalate (PEN), etc.

[0075] Polycarbonate:

[0076] Polyphenylene oxide:

[0077] Other resins:

[0078] Polyimide resin; Polyamide-imide resin; Polyetherimide resin;

[0079] Fluorine resin; Allyl resin; Polyurethane resin; Cellulose resin;

[0080] Polysulfone resin; Polyethersulfone resin; Ketone resin;

[0081] Amino resin; biodegradable resins such as polylactic acid, etc.;

[0082] Furthermore, a blend of the various resins exemplified above or a product obtained by appropriately copolymerizing these resins (for example, an acid-modified olefin resin) may be used.

[0083] The plastic film (A) is preferably formed of a gas barrier resin having excellent oxygen barrier properties such as ethylene / vinyl alcohol copolymer, and may have a multilayer structure including a layer formed of such a gas barrier resin.

[0084] In the present invention, from the perspective of ease of acquisition, cost, formability, or exhibiting a certain degree of barrier property against oxygen and being suitable as a base for the inorganic barrier layer (A1) described later, it is more preferred to use a polyester resin represented by polyethylene terephthalate (PET) or an olefin resin represented by polyethylene and polypropylene as the plastic film (A).

[0085] The thickness of such a plastic film (A) is not particularly limited as long as it has an appropriate thickness depending on the intended use.

[0086] <Inorganic barrier layer (A1)>

[0087] Furthermore, the inorganic barrier layer (A1) provided on the surface of the plastic film (A) may be a material known, for example, from Japanese Patent Application Laid-Open No. 2015-96320, and is preferably an inorganic vapor-deposited film formed by physical vapor deposition represented by sputtering, vacuum vapor deposition, ion plating, etc., or chemical vapor deposition represented by plasma CVD, etc., from the perspective of ensuring high oxygen barrier properties, such as a film formed of various metals or metal oxides. In particular, the plastic film (A) is preferably formed as a base by plasma CVD because it can be uniformly formed on a surface having uneven surfaces and has excellent barrier properties not only against oxygen but also against water.

[0088] It should be noted that the vapor-deposited film using plasma CVD is obtained in the following manner: a plastic film (A) serving as a base for an inorganic barrier layer (A1) is arranged in a plasma processing chamber maintained at a specified vacuum degree, and a gas (reaction gas) of a metal or a compound containing the metal to form the film and an oxidizing gas (usually a gas of oxygen or NOx) are appropriately supplied together with a carrier gas such as argon or helium to the plasma processing chamber shielded by a metal wall and depressurized to a specified vacuum degree using a gas supply pipe. In this state, a glow discharge is generated by a microwave electric field, a high-frequency electric field, or the like, and plasma is generated by using the electric energy, so that the decomposition reactants of the above-mentioned compounds are deposited on the surface of the plastic film A to form a film.

[0089] As the above-mentioned reaction gas, usually, from the viewpoint of being able to form a film having a soft area containing carbon components at the interface with the substrate film (A) and having an area with excellent barrier properties with a high degree of oxidation thereon, an organic metal compound, for example, a gas of an organic aluminum compound such as trialkylaluminum, an organic titanium compound, an organic zirconium compound, an organic silicon compound, etc., is used to form an inorganic barrier layer (A1) in the form of a metal oxide.

[0090] Furthermore, the inorganic barrier layer (A1) may be formed on the plastic film (A) by coating, etc., instead of relying on vapor deposition, etc. That is, the inorganic barrier layer (A1) formed by coating has lower oxygen barrier properties, etc., compared with the one formed by vapor deposition, etc., but it may be formed by coating, depending on the degree of barrier properties to oxygen, etc. required.

[0091] The inorganic barrier layer (A1) formed by coating is typically composed of polysilazane, condensation-polymerizable silane compounds (such as alkoxysilane, etc.), and condensation-polymerizable aluminum oxide compounds (such as alkoxyaluminum, etc.) as film-forming components, and an organic solvent solution mixed with inorganic particles such as silica and aluminum oxide is appropriately used, applied to a specified surface, and heated to evaporate the organic solvent to form a film.

[0092] The thickness of the inorganic barrier layer (A1) varies depending on the purpose of the moisture barrier laminate film and the level of barrier properties required. Generally, the thickness is set to a value that does not impair the properties of the plastic film (A) or the like that serves as a base during vapor deposition and that ensures a water vapor permeability of 10 -1 g / m 2 ·Day / atom or less, especially 10 -2 g / m 2 The thickness is preferably less than 1000 nm / day / atom. Specifically, the thickness varies depending on the ratio of the high oxidation degree region, but is usually 4 to 500 nm, particularly 30 to 400 nm.

[0093] As such an inorganic barrier layer (A1), an inorganic barrier layer formed of aluminum oxide or silicon oxide particularly exhibits the highest barrier property against oxygen and is therefore most preferred in the present invention.

[0094] <Moisture Capturing Layer (B)>

[0095] The moisture-capturing layer (B) blocks the moisture flowing in the thickness direction relative to the moisture-barrier laminated film 10, and in particular, contains an ionic polymer as a film-forming component (i.e., a matrix) from the viewpoint of showing high moisture-capturing properties. In addition, it is most preferably a structure in which an ionic polymer is used as a matrix, and a hygroscopic agent having a lower humidity than that of the ionic polymer is dispersed in the matrix. Such a hygroscopic agent has the function of sealing the moisture captured by the ionic polymer, and by dispersing such a hygroscopic agent, deformation such as swelling caused by moisture absorption can be effectively avoided.

[0096] Ionic polymers;

[0097] The ionic polymer used in the present invention includes the following cationic polymers and anionic polymers.

[0098] Cationic polymers are polymers having cationic groups that can become positively charged in water, such as primary to tertiary amino groups, quaternary ammonium groups, pyridyl groups, imidazolyl groups, quaternary pyridinium groups, etc. In the case of such cationic polymers, since the nucleophilic effect of the cationic groups is strong and water is supplemented through hydrogen bonds, it can form a hygroscopic matrix.

[0099] The amount of cationic groups in the cationic polymer may be such that the water absorption of the resulting hygroscopic matrix (JIS K-7209-1984) is 5% or more, particularly 30% to 45%, at 80% RH and 30°C.

[0100] In addition, as cationic polymers, the following substances can be used: substances obtained by appropriately polymerizing or copolymerizing at least one of cationic monomers represented by amine monomers such as allylamine, ethyleneimine, vinylbenzyltrimethylamine, [4-(4-vinylphenyl)-methyl]-trimethylamine, vinylbenzyltriethylamine, etc.; nitrogen-containing heterocyclic monomers such as vinylpyridine and vinylimidazole; and their salts together with other copolymerizable monomers, and then partially neutralizing them by acid treatment as needed.

[0101] Such a cationic polymer is described in detail in JP-A-2015-96320 and the like, and the details thereof are omitted here, but generally speaking, polyallylamine is preferred from the viewpoint of film-forming properties and the like.

[0102] On the other hand, anionic polymers are polymers having anionic functional groups that can become negatively charged in water, such as carboxylic acid groups, sulfonic acid groups, phosphonic acid groups, or acid salt groups obtained by partial neutralization of these groups. Anionic polymers having such functional groups can form hygroscopic matrices because the functional groups can supplement water through hydrogen bonds.

[0103] The amount of anionic functional groups in the anionic polymer varies depending on the type of functional groups, but similarly to the above-mentioned cationic polymer, it can be an amount such that the water absorption rate (JIS K-7209-1984) of the formed hygroscopic matrix is ​​5% or more, particularly 30% to 45% in an atmosphere of 80% RH and 30°C.

[0104] As anionic polymers having functional groups as described above, for example, the following substances can be used: substances obtained by appropriately polymerizing or copolymerizing at least one of the anionic monomers represented by carboxylic acid monomers such as methacrylic acid, acrylic acid, and maleic anhydride; sulfonic acid monomers such as α-halogenated vinyl sulfonic acid, styrene sulfonic acid, and vinyl sulfonic acid; phosphonic acid monomers such as vinyl phosphoric acid; and salts of these monomers, together with other copolymerizable monomers, and then partially neutralizing them by alkali treatment as needed.

[0105] Such anionic polymers are described in detail in JP-A-2015-96320 and the like, and although the details are omitted, they are generally poly(meth)acrylic acid and partially neutralized products thereof (for example, a portion thereof is a sodium salt).

[0106] The structure of the moisture capture layer (B);

[0107] Reference Figure 2 In (a) or (b), it is preferred that the moisture-capturing layer (B) contains a hygroscopic agent having a lower ultimate humidity than that of the ionic polymer (cationic or anionic polymer) forming the matrix.

[0108] By dispersing the hygroscopic agent having a higher hygroscopicity than the matrix in this way, the moisture absorbed into the matrix formed by the above-mentioned ionic polymer is immediately captured by the hygroscopic agent, and the absorbed moisture is effectively sealed in the matrix. Not only can the hygroscopic capacity of moisture be effectively exerted in an extremely low humidity atmosphere, but the swelling of the moisture capture layer (B) caused by the absorption of moisture can also be effectively suppressed.

[0109] As the highly hygroscopic hygroscopic agent as described above, it is preferred to use a hygroscopic agent having a reaching humidity of 6% or less under environmental conditions of, for example, 80% RH and 30°C, with the reaching humidity being lower than that of the ionic polymer. That is, if the reaching humidity of the hygroscopic agent is higher than that of the ionic polymer, the water absorbed into the matrix is ​​not sufficiently sealed, and the water is easily released, etc., so a significant improvement in the water barrier property cannot be expected. In addition, even if the reaching humidity is lower than that of the ionic polymer, if the reaching humidity measured under the above conditions is higher than the above range, for example, the capture of water in a low humidity atmosphere becomes insufficient, and the water barrier property may not be fully exerted.

[0110] The above-mentioned moisture absorbent generally has a water absorption rate of 50% or more in an atmosphere of 80% RH and 30°C (JIS K-7209-1984), and there are inorganic and organic moisture absorbents.

[0111] Examples of the inorganic moisture absorbent include clay minerals such as zeolite, alumina, activated carbon, and montmorillonite; silica gel, calcium oxide, and magnesium sulfate.

[0112] As organic desiccant, crosslinked products of anionic polymers or partially neutralized products thereof can be cited. As the anionic polymer, the following substances can be cited: substances obtained by polymerizing at least one of anionic monomers represented by carboxylic acid monomers ((meth)acrylic acid, maleic anhydride, etc.), sulfonic acid monomers (halogenated vinyl sulfonic acid, styrene sulfonic acid, vinyl sulfonic acid, etc.), phosphonic acid monomers (vinyl phosphoric acid, etc.) and salts of these monomers, or copolymerizing them with other monomers. In particular, organic desiccant is effective in applications requiring transparency. For example, fine particles of crosslinked sodium poly(meth)acrylate or crosslinked potassium poly(meth)acrylate are representative organic desiccant.

[0113] In the present invention, from the viewpoint of increasing the specific surface area and showing high hygroscopicity, a hygroscopic agent with a small particle size (for example, an average primary particle size of 100 nm or less, especially 80 nm or less) is preferred, and in particular, a hygroscopic agent of an organic polymer with a small particle size is optimal.

[0114] That is, the organic polymer hygroscopic agent has extremely good dispersibility in the matrix of the ionic polymer, and not only can it be evenly dispersed, but also the polymerization method used to produce the hygroscopic agent, such as emulsion polymerization, suspension polymerization, etc., can make its particle shape become fine and uniform spherical. By mixing it to a certain degree or more, extremely high transparency can be ensured.

[0115] Furthermore, among the organic-based fine desiccant, not only can the above-mentioned reaching humidity be significantly lowered and high hygroscopicity be exhibited, but also the volume change caused by swelling due to cross-linking can be extremely small. Therefore, in terms of suppressing the volume change while reducing the humidity to the point where the ambient atmosphere becomes absolutely dry or close to absolutely dry, the organic-based fine desiccant is the best.

[0116] As such organic moisture absorbent microparticles, for example, cross-linked sodium polyacrylate microparticles (average particle size of about 70 nm) are commercially available from Toyobo Co., Ltd. under the trade name of Taftic HU-820E in the form of a colloidal dispersion (pH = 10.4).

[0117] In the present invention, particularly in applications requiring super moisture barrier properties, the moisture capture layer (B) is set to exhibit a water vapor permeability of 10 -5 g / m 2 The thickness of the film has a super barrier property of less than 1 μm / day (for example, 1 μm or more, particularly about 2 to 20 μm).

[0118] In addition, the amount of the hygroscopic agent is set according to the type of ionic polymer from the viewpoint of ensuring a higher moisture barrier than that shown by the inorganic barrier layer (A1) for a long time while giving full play to its characteristics, significantly improving the moisture barrier property, and effectively suppressing the dimensional change caused by swelling. For example, in the case where the matrix is ​​formed by a cationic polymer, the amount of the hygroscopic agent is preferably present in an amount of 50 parts by mass or more, especially 100 to 900 parts by mass, and more preferably 200 to 600 parts by mass, relative to 100 parts by mass of the ionic polymer in the moisture capture layer (B). In addition, in the case where the matrix is ​​formed by an anionic polymer, the amount of the hygroscopic agent is preferably present in an amount of 50 parts by mass or more, especially 100 to 1300 parts by mass, and more preferably 150 to 1200 parts by mass, relative to 100 parts by mass of the anionic polymer in the moisture capture layer (B).

[0119] In addition, in the moisture-capturing layer (B) having the structure as described above, it is preferred to introduce a cross-linked structure into the ionic polymer. That is, when a cross-linked structure is introduced into the ionic polymer, when water is absorbed, the molecules of the cationic polymer are constrained to each other due to cross-linking, thereby suppressing the volume change caused by swelling (water absorption), resulting in an improvement in mechanical strength and dimensional stability.

[0120] Such a cross-linked structure can be introduced by pre-mixing a cross-linking agent in the coating composition for forming the moisture capture layer (B). In particular, in the case of anionic polymers, unlike cationic polymers, water is only replenished through hydrogen bonds, so by introducing a mesh structure (cross-linked structure) of spaces suitable for moisture absorption into the matrix, its hygroscopicity can be greatly improved.

[0121] The cross-linking agent for introducing such a cross-linked structure is slightly different between the case of introducing a cross-linked structure into a cationic polymer and the case of introducing a cross-linked structure into an anionic polymer.

[0122] As the crosslinking agent for the cationic polymer, a compound having a crosslinking functional group (e.g., epoxy group) that can react with a cationic group and a functional group (e.g., alkoxysilyl group) that can form a siloxane structure in the crosslinked structure through hydrolysis and dehydration condensation can be used. In particular, a silane compound represented by the following formula (1) is preferably used:

[0123] X-SiR 1 n (OR 2 ) 3-n (1)

[0124] In the formula, X is an organic group having an epoxy group at the terminal,

[0125] R 1 and R 2 are methyl, ethyl or isopropyl, respectively,

[0126] n is 0, 1 or 2.

[0127] Such silane compounds have epoxy and alkoxysilyl as functional groups, and the epoxy reacts with the functional groups (e.g., NH2) of the cationic polymer. On the other hand, the alkoxysilyl generates a silanol group (SiOH group) by hydrolysis, which forms a siloxane structure and grows through a condensation reaction, thereby eventually forming a cross-linked structure between cationic polymer chains. Thus, a cross-linked structure having a siloxane structure is introduced into the matrix of the cationic polymer.

[0128] Furthermore, the cationic polymer is alkaline, and as a result, when the coating composition containing the cationic polymer is applied to form the moisture-trapping layer B, the addition reaction between the cationic group and the epoxy group and the dehydration condensation between the silanol groups are also rapidly promoted, and a crosslinking structure can be easily introduced.

[0129] In the present invention, the organic group X having an epoxy group in the above formula (1) is typically a γ-glycidoxyalkyl group, and for example, γ-glycidoxypropyltrimethoxysilane and γ-glycidoxypropylmethyldimethoxysilane are preferably used as the crosslinking agent.

[0130] In addition, the epoxy group in the above formula (1) is an alicyclic epoxy group such as an epoxycyclohexyl group, which is also suitable as a crosslinking agent. For example, when a compound having an alicyclic epoxy group such as β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane is used as a crosslinking agent, the alicyclic structure is introduced into the crosslinking structure of the matrix together with the siloxane structure. The introduction of such an alicyclic structure can further effectively exert the function of the matrix forming a mesh structure of a space suitable for moisture absorption.

[0131] Furthermore, in order to introduce an alicyclic structure into the above cross-linked structure, a compound having a plurality of epoxy groups and alicyclic groups, such as diglycidyl ester represented by the following formula (2), can be used as a cross-linking agent:

[0132] GO(C=O)-A-(C=O)OG(2)

[0133] In the formula, G is a glycidyl group,

[0134] A is a divalent hydrocarbon group having an aliphatic ring, such as a cycloalkylene group. A representative substance of such a diglycidyl ester is represented by the following formula (2-1).

[0135] [Chemical formula 1]

[0136]

[0137] That is, although the diglycidyl ester of formula (2) does not have an alkoxysilyl group, it introduces an alicyclic structure into the cross-linked structure, and is therefore effective in forming a network structure of spaces suitable for moisture absorption in the matrix.

[0138] Preferably, the crosslinking agent is used in an amount of 5 to 60 parts by mass, particularly 15 to 50 parts by mass, based on 100 parts by mass of the cationic polymer. Preferably, at least 70% by mass, preferably 80% by mass or more of such a crosslinking agent is a silane compound of the above formula (1).

[0139] In addition, as a crosslinking agent for introducing a crosslinked structure into an anionic polymer, a compound having two or more crosslinkable functional groups (e.g., epoxy groups) that can react with the ionic groups possessed by the anionic polymer can be used, and preferably a diglycidyl ester represented by formula (2) also exemplified in the coating composition for a cationic substrate can be used:

[0140] GO(C=O)-A-(C=O)OG(2)

[0141] In the formula, G is a glycidyl group,

[0142] A is a divalent hydrocarbon group having an aliphatic ring, such as a cycloalkylene group.

[0143] That is, in the diglycidyl ester of the above formula (2), the epoxy group reacts with the anionic group to form a crosslinked structure in the matrix including an alicyclic structure based on the divalent group A. The crosslinked structure including such an alicyclic structure suppresses swelling.

[0144] Among the above-mentioned diglycidyl esters, preferred ones are those listed above, and in particular, the diglycidyl ester represented by the above-mentioned formula (2-1) is most preferred from the viewpoint of being able to form a network structure having spaces suitable for moisture absorption.

[0145] Such a cross-linking agent for anionic polymer is preferably used in an amount of 1 to 50 parts by mass, particularly 10 to 40 parts by mass, based on 100 parts by mass of the anionic polymer.

[0146] Formation of a moisture-capturing layer (B);

[0147] In addition, the moisture capture layer (B) is formed by using a coating composition in a resin serving as a matrix, wherein the coating composition is prepared by dissolving or dispersing a hygroscopic agent and, if necessary, a crosslinking agent in a predetermined solvent, applying the coating composition to a coating layer (C) formed on the inorganic barrier layer (A1) described later, and removing the solvent by heating and drying. The heating and drying is usually performed at a temperature of about 100 to 170° C. for less than 3 minutes, particularly for a short time of about 0.25 to 1 minute, thereby forming a moisture capture layer (B) firmly attached to the inorganic barrier layer (A1) via the coating layer (C).

[0148] In addition, in the coating composition used for forming the moisture capture layer (B) as described above, there are no particular restrictions on the solvent as long as it is a solvent that can be evaporated and removed by heating at a relatively low temperature. For example, alcohol solvents such as methanol, ethanol, propanol, and butanol; ketone solvents such as acetone and methyl ethyl ketone; or mixed solvents of these solvents and water; or aromatic hydrocarbon solvents such as benzene, toluene, and xylene can be used.

[0149] In addition, when a silane compound is used as a crosslinking agent, water or a mixed solvent containing water is preferably used to promote its hydrolysis. In addition, when a moisture capture layer (B) containing an anionic polymer is formed, it is preferred to adjust the pH to about 8 to 12 by adding an alkali (e.g., sodium hydroxide).

[0150] The solvent is used in an amount to give the coating composition a viscosity suitable for coating, but a nonionic polymer may be added in an appropriate amount to adjust the viscosity of the coating composition or adjust the water absorption of the formed hygroscopic matrix to an appropriate range.

[0151] Examples of such nonionic polymers include saturated aliphatic hydrocarbon polymers such as polyvinyl alcohol, ethylene-propylene copolymers, and polybutene; styrene polymers such as styrene-butadiene copolymers; chlorine polymers such as polyvinyl chloride; or various comonomers copolymerized with these polymers. It should be noted that representative comonomers include styrene monomers such as vinyltoluene, vinylxylene, chlorostyrene, chloromethylstyrene, α-methylstyrene, α-halogenated styrene, α, β, β'-trihalogenated styrene; monoolefins such as ethylene and butylene; and conjugated dienes such as butadiene and isoprene.

[0152] In the present invention, as the above-mentioned moisture capture layer (B), a substance containing a cationic polymer as a matrix (film-forming component) is particularly preferred. That is, a moisture capture layer having such a cationic polymer needs to be heated for a long time at a high temperature of 100°C or above in order to ensure particularly high adhesion, but in the present invention, by pre-arranging the coating layer (C) described below as a base, there is also an advantage that a moisture capture layer (B) that is firmly adhered and maintained can be formed without such high-temperature, long-term heating.

[0153] <Coating (C)>

[0154] As described above, in the present invention, the presence of the coating layer (C) between the inorganic barrier layer (A1) and the moisture capture layer (B) is essential.

[0155] The moisture capture layer (B) used to ensure high moisture barrier properties contains an alkali component. That is, when a cationic polymer is used as a film-forming component (matrix), a base such as an amine is included in the layer. The reason is that in cationic polymers, amine compounds are used to introduce cationic groups such as amino groups into polymers, so such amine compounds are included as inevitable components. In addition, anionic polymers contain alkali salt groups of carboxylic acids, and when moisture is captured, alkalis such as NaOH and KOH are generated. Moreover, when using cross-linked sodium polyacrylate, which is most suitable as a hygroscopic agent, alkalis such as NaOH and KOH are also generated due to the capture of moisture.

[0156] On the other hand, the inorganic barrier layer (A1) is reactive to alkali and therefore has extremely poor alkali resistance. If a moisture-capturing layer (B) is directly provided on the inorganic barrier layer (A1), the inorganic barrier layer (A1) reacts with the alkali contained in the moisture-capturing layer (B), resulting in delamination between the moisture-capturing layer (B) and the inorganic barrier layer (A1) or at the interface between the inorganic barrier layer (A1) and the plastic film (A). Therefore, when such a moisture-barrier laminated film is maintained in a high-temperature and high-humidity atmosphere at a temperature of 85° C. or higher and a relative humidity of 85% or higher and subjected to a degradation acceleration test, film peeling occurs in a short period of time, and the moisture barrier property is greatly reduced.

[0157] Therefore, in the present invention, the coating layer (C) is interposed between the inorganic barrier layer (A1) and the moisture capture layer (B).

[0158] In the present invention, as described above, such a coating (C) must satisfy a moisture permeability of 6.0×10 4 g / m 2 / day or less, and a viscoelastic condition in which the storage modulus E' (@2πrad / s) in the viscoelasticity measurement at 85°C is 30 MPa or more.

[0159] That is, by satisfying the above-mentioned moisture permeability conditions, the transfer of alkali-containing water contained in the moisture capture layer (B) to the inorganic barrier layer (A1) can be prevented, and the deterioration of the inorganic barrier layer (A1) caused by alkali can be avoided. In particular, in order to prevent the transfer of alkali-containing water to the inorganic barrier layer (A1), it is preferred that the above-mentioned moisture permeability is smaller, for example, the moisture permeability at 40°C and 90%RH is preferably 5.0×10 4 g / m 2 / day or less.

[0160] In addition, in the present invention, by satisfying the above-mentioned viscoelastic conditions, the relaxation of the molecules of the coating (C) at high temperatures is suppressed, thereby effectively preventing the coating (C) from being deformed by shear force, and more reliably suppressing the transfer of alkaline water to the inorganic barrier layer (A1) even at high temperatures.

[0161] As a result, the film peeling caused by alkali degradation of the inorganic barrier layer (A1) can be reliably prevented, and excellent moisture barrier properties can be exerted for a long time even in a high temperature and high humidity atmosphere. In particular, the higher the storage modulus E' (@2πrad / s), the higher the relaxation inhibition effect of the molecules of the coating (C), and the higher moisture barrier properties can be exerted for a longer time. For example, the storage modulus E' (@2πrad / s) at 85°C is preferably 20MPa or more, and more preferably 30MPa or more. In addition, if the storage modulus E' is too large, the film forming property may be impaired, so the storage modulus E' is preferably 1000MPa or less.

[0162] It should be noted that the storage modulus E' depends on the molecular weight Mc between crosslinks of the molecules of the cured polymer. For example, in a polymer having the storage modulus E' as described above, the molecular weight Mc between crosslinks is usually within a range of 5000 g / mol or less. Such molecular weight Mc between crosslinks is calculated using the rubber elasticity formula based on the value of the storage modulus E' calculated by viscoelasticity measurement at 85°C, as shown in the examples described below.

[0163] In the present invention, the coating layer (C) satisfying the above-mentioned moisture permeability and viscoelasticity conditions is formed of a non-aqueous polymer (specifically, an isocyanate polymer) having low moisture permeability and exhibiting viscoelasticity. For example, in order to achieve the above-mentioned moisture permeability, the thickness is preferably 0.1 μm or more, particularly preferably 0.2 μm or more, but if the thickness is too thick, when the moisture barrier property is improved by multi-layering, it will become excessively thick, so a moderately thin thickness is preferably, for example, preferably 7 μm or less, particularly preferably 5 μm or less.

[0164] In addition, the coating (C) preferably has a large water contact angle θ to a certain extent. That is, the larger the water contact angle θ is, the more hydrophobic the coating becomes, and the transfer of water after the moisture capture layer absorbs moisture can be reduced. On the other hand, if the value of the water contact angle is too large, the wettability when the moisture capture layer is applied to the coating (C) may deteriorate. Therefore, the value is more preferably in the range of 65 to 100°, especially in the range of 75 to 95°.

[0165] When achieving the above water contact angle, the solubility parameter (SP value) of the base resin reacting with the isocyanate as a component forming the coating layer (C) is more preferably in the range of 8.5 to 10.9, particularly 8.6 to 10.7°.

[0166] Furthermore, the coating layer (C) preferably has a high glass transition point Tg in order to further suppress moisture permeation in a high temperature environment such as the accelerated test environment.

[0167] That is, the higher the glass transition point Tg, the more the mobility of the polymer at high temperature is suppressed, and the transfer of water after the moisture capture layer absorbs moisture can be reduced. For example, the glass transition point of the coating (C) is preferably above 85°C. The moisture-barrier laminated film of the present invention provided with such a coating (C) shows excellent moisture barrier properties even in a degradation acceleration test maintained in a high-temperature and high-humidity atmosphere at a temperature of above 85°C and a relative humidity RH of above 85%. Its performance evaluation can be performed quickly and reliably.

[0168] In the present invention, the coating (C) having such characteristics is briefly described above, and the coating (C) is a substance formed by using an isocyanate-based polymer obtained by using an isocyanate as a reaction component, for example, a substance formed by curing an isocyanate-reactive resin (base resin) with a polyisocyanate (curing agent). For such a non-aqueous polymer, the isocyanate group present in the polymer not only shows reactivity to the MOH group (M is a metal atom such as Al, Si, etc.) present on the surface of the inorganic barrier layer (A1), but also shows reactivity to the ionic group in the ionic polymer in the moisture capture layer (B), and also shows high adhesion to the moisture barrier layer (B), so that the delamination of the moisture barrier layer (B) can be prevented for a long time, and the reduction of the moisture barrier property can be effectively prevented.

[0169] As such an isocyanate-reactive resin (base resin), examples include resins having functional groups capable of reacting with isocyanate, such as hydroxyl, carboxyl, amino, etc., especially hydroxyl or carboxyl groups. Specifically, ester resins, (meth)acrylic resins, polycarbonate resins, polyvinyl alcohol, etc. can be exemplified. Furthermore, polyurethane resins can also be used as isocyanate-reactive resins.

[0170] In the present invention, (meth)acrylic resin (poly(meth)acrylic acid, poly(meth)acrylate) is particularly preferred, and in particular, urethane (meth)acrylate obtained by reacting (meth)acrylic resin with isocyanate is more preferred due to the formation of coating (C). Furthermore, from the viewpoint of ensuring high adhesion with the moisture capture layer (B), it is preferred to use a (meth)acrylic resin introduced with a glycidyl group as a matrix resin, and it is particularly preferred that 0.5 to 97% by mass, and in particular 0.7 to 97% by mass of the (meth)acrylic resin is derived from a (meth)acrylate containing a glycidyl group. The glycidyl group introduced into the (meth)acrylic resin is used to ensure adhesion to the moisture capture layer, and by making the amount of the glycidyl group within the above range, a cured product that satisfies the viscoelastic condition can be formed without damaging the adhesion obtained by the glycidyl group. The glycidyl group-containing (meth)acrylate compound is, for example, represented by the following formula (3):

[0171] CH2=CH(R)-COO-(CH2)mG(3)

[0172] In the formula, R is a hydrogen atom or a methyl group,

[0173] G is glycidyl,

[0174] m is an integer of 0 or 1 or more.

[0175] A typical example of the glycidyl group-containing (meth)acrylate is glycidyl (meth)acrylate (where m=0 in the formula (3)).

[0176] Furthermore, it is preferred that the (meth) acrylic resin has a hydroxyl value (OHV) of 10 mgKOH or more, more preferably 10 to 150 mgKOH, in order to make the cured product satisfy the prescribed viscoelasticity conditions. That is, by appropriately containing a (meth) acrylic resin having a hydroxyl group, a viscoelastic body having a mesh structure satisfying the prescribed viscoelasticity conditions is formed by reacting with the isocyanate compound described later.

[0177] As a monomer used for forming a (meth)acrylic resin showing the above-mentioned hydroxyl value, a hydroxyl-containing (meth)acrylate is used. As such a hydroxyl-containing (meth)acrylate, the following can be exemplified.

[0178] 2-Hydroxymethyl (meth)acrylate;

[0179] 2-Hydroxypropyl (meth)acrylate;

[0180] 3-Hydroxypropyl (meth)acrylate;

[0181] 2,3-Dihydroxypropyl (meth)acrylate;

[0182] 2,4-Dihydroxypropyl (meth)acrylate;

[0183] 2-Hydroxymethyl-3-hydroxypropyl (meth)acrylate;

[0184] 2-Hydroxybutyl (meth)acrylate;

[0185] 4-Hydroxybutyl (meth)acrylate;

[0186] 5-Hydroxypentyl (meth)acrylate;

[0187] Diethylene glycol mono(meth)acrylate;

[0188] Triethylene glycol mono(meth)acrylate;

[0189] Tetraethylene glycol mono(meth)acrylate;

[0190] Pentaethylene glycol mono(meth)acrylate;

[0191] 2-Hydroxypropyl (meth)acrylate;

[0192] In addition, the following di(meth)acrylates can also be used.

[0193] Ethylene glycol di(meth)acrylate;

[0194] Triethylene glycol di(meth)acrylate;

[0195] Butanediol di(meth)acrylate;

[0196] Neopentyl glycol di(meth)acrylate;

[0197] Propylene glycol di(meth)acrylate;

[0198] 1,3-Butanediol di(meth)acrylate;

[0199] 1,4-Butanediol di(meth)acrylate;

[0200] 1,6-Hexanediol di(meth)acrylate;

[0201] Furthermore, in addition to the above-mentioned di(meth)acrylates, tri(meth)acrylates such as trimethylolpropane tri(meth)acrylate may be used.

[0202] As long as the above-mentioned glycidyl group content and hydroxyl value content are satisfied, the above-mentioned (meth)acrylic resin may include a polymer formed from the following substances, which are monomers used in the formation of conventional (meth)acrylic resins, such as methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, butyl (meth)acrylate, tert-butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, cyclohexyl (meth)acrylate, styrene, etc.

[0203] Furthermore, from the viewpoint of increasing the glass transition point Tg of the coating (C), the isocyanate-reactive resin, particularly the (meth)acrylic resin, preferably has a glass transition point Tg of 60° C. or higher, more preferably 65° C. or higher, and even more preferably 70° C. or higher. Furthermore, preferably, the weight average molecular weight (Mw) thereof is 10,000 or higher, more preferably 15,000 or higher, and even more preferably 20,000 or higher.

[0204] The isocyanate (i.e., curing agent) that reacts with the above-mentioned isocyanate-reactive resin is not limited thereto, and polyisocyanates having two or more isocyanate groups can be used, such as aromatic diisocyanates, aromatic aliphatic diisocyanates, alicyclic diisocyanates, aliphatic diisocyanates and other diisocyanates. These can be used alone or in combination of two or more, and trifunctional or higher polyisocyanates can also be used in combination.

[0205] As the aromatic diisocyanate, for example, the following compounds can be exemplified.

[0206] m- or p-phenylene diisocyanate or mixtures thereof;

[0207] 4,4'-diphenyl diisocyanate, 1,5-naphthalene diisocyanate (NDI), 4,4'-, 2,4'- or 2,2'-diphenylmethane diisocyanate or mixtures thereof (MDI);

[0208] 2,4- or 2,6-toluene diisocyanate or mixtures thereof (TDI);

[0209] 4,4'-Toluidine diisocyanate (TODI); 4,4'-Diphenyl ether diisocyanate.

[0210] Examples of aromatic aliphatic diisocyanates include:

[0211] 1,3- or 1,4-xylylene diisocyanate or mixtures thereof (XDI);

[0212] 1,3- or 1,4-tetramethylxylylene diisocyanate or mixtures thereof (TMXDI);

[0213] ω,ω'-Diisocyanate-1,4-diethylbenzene.

[0214] Examples of alicyclic diisocyanates include:

[0215] 1,3-Cyclopentene diisocyanate;

[0216] 1,4-cyclohexane diisocyanate;

[0217] 1,3-cyclohexane diisocyanate;

[0218] 3-isocyanatomethyl-3,5,5-trimethylcyclohexyl isocyanate (isophorone diisocyanate; IPDI);

[0219] 4,4'-, 2,4'- or 2,2'-dicyclohexylmethane diisocyanate or mixtures thereof (hydrogenated MDI);

[0220] Methyl-2,4-cyclohexane diisocyanate;

[0221] Methyl-2,6-cyclohexane diisocyanate;

[0222] 1,3- or 1,4-bis(isocyanatemethyl)cyclohexane or mixtures thereof (hydrogenated XDI).

[0223] Examples of aliphatic diisocyanates include:

[0224] Trimethylene diisocyanate;

[0225] Tetramethylene diisocyanate;

[0226] Hexamethylene diisocyanate (HDI);

[0227] Pentamethylene diisocyanate;

[0228] 1,2-Propylene diisocyanate;

[0229] 1,2-, 2,3- or 1,3-butylene diisocyanate;

[0230] 2,4,4- or 2,2,4-trimethylhexamethylene diisocyanate;

[0231] Methyl 2,6-diisocyanate hexanoate.

[0232] In the present invention, among the above-mentioned isocyanate compounds, preferred are diphenylmethane diisocyanate (MDI), toluene diisocyanate (TDI), hexamethylene diisocyanate (HDI), meta-xylylene diisocyanate, tetramethylene diisocyanate, pentamethylene diisocyanate, lysine isocyanate, isophorone diisocyanate (IPDI) and the multi-core condensation products of these isocyanates, etc. In addition, when more than 1% by mass of the total amount of the isocyanate compounds is a polyisocyanate having a weight average molecular weight in the range of 400 to 1200, it is advantageous to form a cured product having an average molecular weight between crosslinking points in a prescribed range.

[0233] Formation of coating (C);

[0234] The coating layer (C) can be formed by applying a coating composition in which the isocyanate-reactive resin and the isocyanate compound (curing agent) are dissolved or dispersed in a solvent onto the inorganic barrier layer (A1), and heating the composition to a temperature of 100° C. or higher for baking.

[0235] As the solvent used in forming the coating composition, an organic solvent that does not become excessively high in temperature due to heating for solvent volatilization is used, for example, an alcohol organic solvent, a dialkyl glycol ether solvent, an ethylene glycol ether solvent, a propylene glycol ether solvent, an ester solvent, a ketone solvent, an ether solvent, a hydrocarbon solvent, etc. are used.

[0236] These solvents are used in such an amount that the coating composition has a viscosity suitable for coating.

[0237] It should be noted that, as described above, the polymer forming the coating layer (C) must be non-aqueous in order to satisfy certain moisture permeability conditions, and therefore, water or a mixed solvent of water and an organic solvent cannot be used to prepare the coating composition. The reason is that if dispersed in an aqueous solvent, the moisture permeability in a high temperature and high humidity atmosphere becomes high, and alkaline water is supplied to the inorganic barrier layer (A1) through the coating layer (C), causing alkali degradation of the inorganic barrier layer (A1), and the moisture barrier property and adhesion are greatly reduced due to the occurrence of delamination.

[0238] In addition, in the above-mentioned coating composition, the isocyanate-reactive resin and the isocyanate compound used are used in combination according to the type and number of their functional groups in a manner to form a cured body that satisfies the above-mentioned moisture permeability conditions and viscoelasticity conditions. For example, from the viewpoint of satisfying the moisture permeability conditions and viscoelasticity conditions, it is preferred to use a (meth) acrylic resin having a hydroxyl value of at least 10 mgKOH / g or more relative to the isocyanate-reactive resin in an amount of 1% by mass or more, and in addition, 0.5 to 97% by mass of the isocyanate-reactive resin is preferably the above-mentioned glycidyl group-containing (meth) acrylic compound.

[0239] Furthermore, when the weight of isocyanate required to react with the amount of isocyanate-reactive functional groups of the isocyanate-reactive resin is set to 1 equivalent, the isocyanate is preferably contained in an amount of at least 0.4 equivalents, particularly 0.6 equivalents or more. When the amount is less than 0.4, the number of reaction points with the ionic groups in the MOH (M is a metal atom such as Al or Si) present on the surface of the inorganic barrier layer (A1) and the ionic polymer in the moisture capture layer (B) decreases, resulting in reduced adhesion.

[0240] Furthermore, the coating composition may contain a catalyst from the viewpoint of promoting the curing reaction. Representative examples of the catalyst include amine catalysts and metal catalysts.

[0241] Examples of the amine catalyst include the following catalysts.

[0242] 1,4-diazabicyclo(2,2,2)octane;

[0243] PMDETA;

[0244] N,N-dimethylcyclohexylamine;

[0245] N-Methyldicyclohexylamine;

[0246] N,N,N,N-Tetramethylpropylenediamine;

[0247] N,N,N,N-Tetramethylhexamethylenediamine;

[0248] N-ethylmorpholine;

[0249] N-methylmorpholine;

[0250] N,N-dimethylethanolamine;

[0251] N,N-diethylethanolamine;

[0252] Examples of the metal catalyst include organic tin compounds such as dibutyltin laurate and organic zinc compounds.

[0253] These catalysts may be used alone or in combination of two or more. In addition, metal catalysts are particularly preferred.

[0254] These catalysts are blended in an amount of 0.02 to 1.0 parts by mass relative to 100 parts by mass of the total amount of the isocyanate-reactive resin and the isocyanate compound. That is, the coating layer (C) contains the catalyst in a ratio corresponding to the amount.

[0255] By containing the above catalyst, not only the reaction between the isocyanate-reactive resin in the coating (C) and the isocyanate compound can be promoted, but also the reaction between the OH group present in the layer of the base (e.g., the inorganic barrier layer) and the isocyanate compound can be promoted, and a material with a stronger adhesion between the layer of the base and the coating (C) can be produced. For example, as in actual production, even when the production speed is high and a high heat load is not applied to the formation of the coating (C), the adhesion between the layer of the base and the coating (C) can be stably maintained.

[0256] Furthermore, various compounding agents may be added to the above-mentioned coating composition as long as the adhesion between the formed coating layer (C) and the moisture-capturing layer (B) or the inorganic barrier layer (A1) is not impaired.

[0257] As such compounding agents, for example, there can be listed: layered inorganic compounds, stabilizers (antioxidants, heat stabilizers, ultraviolet absorbers, etc.), plasticizers, antistatic agents, lubricants, antiblocking agents, colorants, fillers, crystal nucleating agents, etc. Of course, as long as the above-mentioned adhesion is not impaired, a small amount of resin that is not reactive with isocyanate, such as olefin resins, etc., can also be compounded.

[0258] It should be noted that, from the viewpoint of storage stability, the ends of the polyisocyanate in the above-mentioned coating composition can be blocked with a blocking agent. Representative examples of such blocking agents include: alcohols such as methanol, ethanol, and lactic acid esters; compounds containing phenolic hydroxyl groups such as phenol and salicylic acid esters; amides such as ε-caprolactam and 2-pyrrolidone; oximes such as acetone oxime and methyl ethyl ketone oxime; active methylene compounds such as methyl acetoacetate, ethyl acetoacetate, acetylacetone, dimethyl malonate, and diethyl malonate, etc. These blocking agents can be used alone or in combination of two or more.

[0259] As described above, the coating layer (C) formed on the inorganic barrier layer (A1) is generally an adhesion-promoting coating layer of the moisture-capturing layer (B), and the moisture-capturing layer (B) is formed thereon with the coating layer (C) serving as a base.

[0260] In addition, if Figure 4 , Figure 5 As shown, the coating layer (C) can also be provided on the side of the moisture capture layer (B) opposite to the inorganic barrier layer (A1). By adopting such a layer structure, it is possible to suppress not only the migration of the alkali component to the inorganic barrier layer (A1) but also the migration of the alkali component to the opposite side.

[0261] For example, when other substrates are bonded to the moisture capture layer (B) via an adhesive layer by dry lamination, the transfer of the alkali component to the adhesive layer side can be suppressed by providing a coating layer (C) between the moisture capture layer (B) and the adhesive layer. As a result, the adhesion of the entire laminate can be stably maintained.

[0262] <Protective layer (D)>

[0263] It should be noted that in the present invention, the coating layer (C) only needs to be present between the inorganic barrier layer (A1) and the moisture capture layer (B). Figure 3 As shown, a protective layer (D) may be provided on the inorganic barrier layer (A1), and the above-mentioned coating layer (C) may be provided on the protective layer (D).

[0264] The protective layer (D) is used to prevent the inorganic barrier layer (A1) from peeling, damage, breakage, etc. after film formation. It is not particularly limited as long as it is a layer that does not reduce the barrier properties of the barrier film under a test environment (85°C-85% RH environment). Generally speaking, it is formed by combining two or more compounds of the components (D1) and (D2) shown below.

[0265] Component (D1) is a water-soluble polymer, and examples thereof include polyvinyl alcohol, polyvinyl pyrrolidone, starch, methyl cellulose, carboxymethyl cellulose, sodium alginate, etc. Polyvinyl alcohol is particularly preferred.

[0266] Component (D2) is at least one compound selected from the group consisting of organoalkoxysilane or hydrolyzate thereof, metal alkoxide or hydrolyzate thereof, and phosphorus-based compounds.

[0267] The above-mentioned organoalkoxysilane is represented by, for example, the following formula (4):

[0268] R 1 -Si(OR 2 )3(4)

[0269] In the formula, R 1 is an organic group,

[0270] R 2 It is an alkyl group.

[0271] As the organic group R 1 , and examples thereof include an alkyl group and groups having various functional groups (for example, a (meth)acryloyl group, a vinyl group, an amino group, an epoxy group, an isocyanate group, etc.).

[0272] In addition, as R 2 The alkyl group represented is not particularly limited, but is usually a lower alkyl group having 4 or less carbon atoms (for example, methyl, ethyl, propyl, and butyl).

[0273] Examples of such organoalkoxysilane include the following silane compounds.

[0274] Ethyltrimethoxysilane;

[0275] (Meth)acryloxypropyltrimethoxysilane;

[0276] Vinyltrimethoxysilane;

[0277] Glycidoxytrimethoxysilane;

[0278] Glycidoxypropyltrimethoxysilane;

[0279] Epoxycyclohexylethyltrimethoxysilane;

[0280] Isocyanatepropyltrimethoxysilane;

[0281] The hydrolysis condensation product of the above silane compound;

[0282] These silane compounds (and their hydrolysis condensates) can be used alone or in combination of two or more. Among them, epoxy-containing glycidoxytrimethoxysilane, epoxycyclohexylethyltrimethoxysilane, and isocyanate-containing isocyanatepropyltrimethoxysilane are particularly preferred. These organosilanes are not limited to monomers, and compounds such as dimers and trimers can also be used according to the structure.

[0283] In addition, the above metal alkoxide is a compound represented by the following formula (5):

[0284] M(OR 2 )n(5)

[0285] In the formula, M is a metal atom,

[0286] R 2 As with the above formula (4), it is an alkyl group,

[0287] n is an integer representing the valence of the metal atom M.

[0288] Examples of such metal alkoxides include tetraethoxysilane and tripropoxyaluminum. These metal alkoxides may be used alone or in combination of two or more.

[0289] Furthermore, the above-mentioned organoalkoxysilane and metal alkoxide may be used as the component (D2) in the form of hydrolyzates.

[0290] Such a hydrolyzate can be obtained by a known method using an acid or an alkali, and a reaction catalyst such as a tin compound may be used during the hydrolysis as necessary.

[0291] Furthermore, phosphoric acid or its salts can be cited as phosphorus compounds. Specifically, orthophosphoric acid, pyrophosphoric acid, metaphosphoric acid or their alkali metal salts, ammonium salts; condensed phosphoric acids such as trimetaphosphoric acid, tetrametaphosphoric acid, hexametaphosphoric acid, and supermetaphosphoric acid or their alkali metal salts, ammonium salts, etc. can be cited. In addition, phosphoric acid esters such as triphenyl phosphate can also be used.

[0292] These phosphorus compounds may be used alone or in combination of two or more.

[0293] The above-mentioned components (D1) and (D2) are melt-mixed at a mass ratio of (D1) / (D2) = 99 / 1 to 70 / 30, and the melt-mixed mixture is applied to the surface of the inorganic barrier layer (A1) to form a protective layer (D).

[0294] The thickness of the protective layer (D) formed in this way is usually preferably in the range of 0.01 to 50 μm, particularly preferably 0.1 to 2 μm.

[0295] In the present invention, Figure 1 and Figure 3 In the example, the inorganic barrier layer (A1) is provided only on one surface of the plastic film (A). Of course, the inorganic barrier layer (A1) may be formed on both surfaces of the film (A). Furthermore, a moisture capture layer (B) may be formed on each of the inorganic barrier layers (A1) formed on both surfaces in such a manner as to sandwich the coating layer (C).

[0296] The moisture-barrier laminated film 10 of the present invention having the above-mentioned layer structure forms a moisture-capturing layer (B) in the above-mentioned order, releases moisture from the moisture-capturing layer (B), and then adheres a dry film to the surface of the moisture-capturing layer (B) and stores it in a protected state, and peels off the dry film when used.

[0297] As described above, the moisture-capturing layer (B) may be laminated on another barrier film or provided on another barrier film, for example, by dry lamination to form a coating layer (C).

[0298] The moisture barrier laminated film does not delaminate during the degradation acceleration test in a high temperature and high humidity atmosphere at a temperature of 85°C or higher and a relative humidity of 85% or higher, and can exhibit excellent moisture barrier properties, so its quality can be confirmed in a short time, which is extremely advantageous in industry. Of course, it can also be used as a sealing material for electronic devices used in such a high temperature and high humidity environment.

[0299] Such a moisture-barrier laminated film of the present invention is particularly preferably used as a film for sealing electronic circuits such as organic EL elements, solar cells, and electronic paper.

[0300] Example

[0301] <Method for measuring molecular weight>

[0302] 3 mL of solvent was added to about 10 mg of isocyanate-reactive resin and sample, and the mixture was slowly stirred at room temperature. After visually confirming that the mixture had dissolved, the mixture was filtered with a 0.45 μm filter, and the filtrate was subjected to GPC measurement (polystyrene conversion) to measure the weight average molecular weight (Mw). Polystyrene was used as the standard.

[0303] Device: HLC-8120 manufactured by Tosoh Co., Ltd.

[0304] Detector: RI differential refractive index detector.

[0305] Chromatographic column: TSKgel SuperHM-H×2

[0306] (TSKguard column as a guard column

[0307] SuperH-H).

[0308] Solvent: Chloroform.

[0309] Flow rate: 0.5 mL / min.

[0310] Column temperature: 40°C.

[0311] <Measurement method of moisture permeability>

[0312] The water vapor permeability of each coating layer (C) was measured at 40° C. and 90% RH by forming a film of each resin layer alone using PERMATRAN (manufactured by MOCON).

[0313] <Measurement Method of Glass Transition Point Tg and Storage Modulus E'>

[0314] A coating film of each coating layer (C) was prepared, and the value obtained when the dynamic viscoelasticity was measured under the following conditions was described.

[0315] Device: DMS-6100 manufactured by Hitachi High-Tech Science Co., Ltd.

[0316] Test piece: size 10 mm × 20 mm, thickness 60 μm.

[0317] Measurement temperature: 30~130℃.

[0318] <Calculation method of molecular weight Mc between crosslinking points>

[0319] The molecular weight Mc between crosslinking points was calculated using the following formula.

[0320] Mc=3ρRT / Emin

[0321] Mc: molecular weight between crosslinks (g / mol).

[0322] ρ: Density of the sample coating (g / cm 3 ).

[0323] R: gas constant (8.314 J / K / mol).

[0324] T: Absolute temperature (K) when the storage modulus is Emin.

[0325] Emin: Minimum value of storage modulus (MPa).

[0326] <Method for measuring water contact angle θ>

[0327] Under the conditions of 23° C. and 50% RH, 3 μL of pure water was placed on the coating (C) using a solid-liquid interface analysis system DropMaster 700 (manufactured by Kyowa Interface Science Co., Ltd.) to measure the water contact angle.

[0328] <Evaluation Method of Barrier Layer Degradation>

[0329] A 100 μm thick PET film was dry-laminated on the produced moisture barrier laminate film using an adhesive, and aged at 50° C. for 3 days to cure the adhesive layer, thereby producing a sample for a T-type peel test.

[0330] In an atmosphere of 23°C and 50% RH, the lamination strength (unit: N / 15mm) between the moisture-barrier laminate film and PET of the laminate was measured by a T-type peel test using a test piece with a width of 15mm and a length of 200mm (including a non-adhesive portion of 50mm) at a peeling speed of 300mm / min (n=4).

[0331] The value at this time was set as the initial value, and the degree of degradation (initial region) was evaluated.

[0332] In addition, the T-type peel test samples prepared in the same manner were stored at 85°C and 85% RH for 5, 10 and 20 days, and then subjected to the same measurement to measure the lamination strength after moisture absorption (5 day section, 10 day section, 20 day section).

[0333] In addition, the evaluation criteria are as follows.

[0334] ×: When the strength is 1 N / 15 mm or less.

[0335] Δ: When the strength exceeds 1 N / 15 mm and is 2 N / 15 mm or less.

[0336] ○: When the strength exceeds 2N / 15mm and is 3N / 15mm or less.

[0337] ◎: Exceeds 3N / 15mm.

[0338] <Preparation of Moisture Capture Layer Coating Liquid (B1) Using Cationic Polymer>

[0339] Polyallylamine (PAA-15C, manufactured by NITTOBO MEDICAL, aqueous solution, solid content 15%) as a cationic polymer was diluted with water so that the solid content was 5% by mass to obtain a polymer solution.

[0340] On the other hand, γ-glycidoxypropyltrimethoxysilane was used as a crosslinking agent and dissolved in water so as to become 5 mass % to prepare a crosslinking agent solution.

[0341] Next, the polymer solution and the crosslinking agent solution were mixed in an amount of 20 parts by mass of γ-glycidoxypropyltrimethoxysilane relative to 100 parts by mass of polyallylamine, and a crosslinked product of sodium polyacrylate (TAFTIC HU-820E manufactured by Toyobo Co., Ltd., water dispersion, solid content 13%) was added as a moisture absorbent to the mixed solution in an amount of 420 parts by mass relative to the polyallylamine. The mixture was adjusted with water to a solid content of 5%, and then stirred thoroughly to prepare a coating solution (B1) for a moisture capture layer.

[0342] <Preparation of Moisture Capture Layer Coating Liquid (B2) Using Anionic Polymer>

[0343] As an anionic polymer, polyacrylic acid (AC-10LP, manufactured by Nippon Junyaku Co., Ltd.) was used and dissolved in a water / acetone mixed solvent (80 / 20 by weight) so that the solid content was 5% by mass. Sodium hydroxide was added so that the neutralization rate of the polyacrylic acid was 80% to obtain a polymer solution.

[0344] In the polymer solution, 1,2-cyclohexanedicarboxylic acid diglycidyl ester as a crosslinking agent was added in an amount of 20 parts by mass relative to the partially neutralized polyacrylic acid. Next, β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane as a bonding agent was added in an amount of 3 parts by mass relative to the partially neutralized polyacrylic acid. In the bonding agent mixture, a granular moisture absorbent (Toyobo, TAFTIC HU-820E, water dispersion, solid content 13%) was added in an amount of 431 parts by mass relative to the partially neutralized polyacrylic acid. Finally, a water / acetone mixed solvent (80 / 20 by weight) was used to adjust the total solid content to 5% by mass, and the mixture was stirred thoroughly to prepare a coating liquid (B2) for a moisture capture layer.

[0345] <Example 1>

[0346] A polymer solution (solid content 50%) containing acrylic resin A (Mw=70000, glass transition point=100°C, OHV (hydroxyl value)=30, glycidyl group content (G content)=0 mass %) as a matrix resin was prepared.

[0347] The polymer solution was mixed with 30 parts by mass of polyisocyanate (Mw=700) as a curing agent based on 100 parts by mass of the solid content of the polymer solution, and diluted with methyl ethyl ketone to prepare a coating solution having a solid content of 20%.

[0348] A commercially available barrier film (Relief printing, GX, substrate: PET (12 μm)) having a protective layer (D) on an aluminum oxide layer (inorganic barrier layer) was prepared.

[0349] The coating solution was applied onto the protective layer (D) of the barrier film using a bar coater, and heat treated in an electric oven at a peak temperature of 100° C. and a peak temperature retention time of 1 minute to obtain a coating layer (C) of 1.0 μm.

[0350] On the coating layer (C), a moisture-capturing layer coating liquid (B1) using the above-mentioned cationic polymer is applied using a rod coater, and heat-treated under the conditions of a peak temperature of 100°C and a peak temperature holding time of 1 minute to form a moisture-capturing layer (B) with a thickness of 3 μm, thereby obtaining a moisture-barrier laminate film.

[0351] <Example 2>

[0352] A polymer solution (solid content 50%) containing acrylic resin A (Mw = 70,000, glass transition point = 100°C, OHV = 30, epoxypropylene content = 0 mass %) and acrylic resin B (Mw = 3,000, glass transition point = 70°C, OHV = 100, epoxypropylene content = 30 mass %) with a solid content ratio of 95 / 5 as a matrix resin is prepared.

[0353] A moisture-barrier laminated film was obtained in the same manner as in Example 1 except that this polymer solution was used.

[0354] <Example 3>

[0355] A polymer solution (solid content 50%) containing an acrylic resin C (Mw=45000, glass transition point=95° C., OHV=45, glycidyl group content=5% by mass) as a matrix resin was prepared.

[0356] A moisture-barrier laminated film was obtained in the same manner as in Example 1 except that this polymer solution was used.

[0357] <Example 4>

[0358] A moisture-barrier laminated film was obtained in the same manner as in Example 3 except that 0.2 parts by mass (corresponding to 0.15% by mass with respect to the coating layer) of an amine compound was added as a catalyst based on 100 parts by mass of the acrylic resin.

[0359] <Example 5>

[0360] A moisture-barrier laminated film was obtained in the same manner as in Example 3 except that 0.2 parts by mass (corresponding to 0.15% by mass with respect to the coating layer) of an organic tin compound was added as a catalyst based on 100 parts by mass of the acrylic resin.

[0361] <Example 6>

[0362] A moisture-barrier laminate film was obtained in the same manner as in Example 3 except that 0.2 parts by mass (corresponding to 0.15% by mass with respect to the coating layer) of an organic zinc compound was added as a catalyst based on 100 parts by mass of the acrylic resin.

[0363] <Example 7>

[0364] A moisture-barrier laminated film was obtained in the same manner as in Example 6 except that the amount of the catalyst was changed to 0.03 parts by mass (corresponding to 0.02% by mass with respect to the coating layer) based on 100 parts by mass of the acrylic resin.

[0365] <Example 8>

[0366] A moisture-barrier laminated film was obtained by the same method as in Example 6 except that the thickness of the coating layer (C) was 0.3 μm.

[0367] <Example 9>

[0368] A moisture-barrier laminated film was obtained by the same method as in Example 6 except that the thickness of the coating layer (C) was 0.15 μm.

[0369] <Example 10>

[0370] A moisture-barrier laminate film was obtained by the same method as in Example 6 except that the amount of the curing agent was changed to 15 parts by mass based on 100 parts by mass of the acrylic resin.

[0371] <Example 11>

[0372] A moisture barrier laminate film was obtained in the same manner as in Example 6 except that a commercially available barrier film (barrialox 1011HG manufactured by Toray Film, substrate: PET 12 μm) having alumina as the inorganic barrier layer and not provided with the protective layer (D) was used.

[0373] <Example 12>

[0374] A moisture barrier laminate film was obtained in the same manner as in Example 6 except that the inorganic barrier layer was changed to a commercially available barrier film (letterpress printing, GL-RD, substrate: PET 12 μm) having silicon oxide as the inorganic barrier layer and having a protective layer (D).

[0375] <Example 13>

[0376] A moisture barrier laminate film was obtained in the same manner as in Example 6 except that the inorganic barrier layer was changed to a commercially available barrier film (Mitsubishi Chemical, Techbarrier LX, substrate: PET 12 μm) having silicon oxide as the inorganic barrier layer and not provided with the protective layer (D).

[0377] <Example 14>

[0378] A moisture-barrier laminated film was obtained by the same method as in Example 6 except that the moisture-capturing layer coating liquid (B2) using an anionic polymer was used.

[0379] <Example 15>

[0380] In Example 6, a moisture-barrier laminated film was obtained by the same method as in Example 6 except that a coating layer (C) of 1.0 μm was further formed on the moisture-capturing layer (B).

[0381] <Comparative Example 1>

[0382] A moisture-barrier laminated film was obtained in the same manner as in Example 1 except that a moisture-capturing layer coating liquid (B1) containing a cationic polymer was applied on the protective layer (D) of the barrier film to form a moisture-capturing layer (B) having a thickness of 3 μm without forming the coating layer (C).

[0383] <Comparative Example 2>

[0384] A polymer solution (solid content: 30%) containing a water-dispersible polyurethane resin (Mw=1,000,000, glass transition point=68° C., OHV=25, glycidyl group content=0% by mass) as a matrix resin was prepared.

[0385] The polymer solution was mixed with blocked isocyanate (Mw=2500) as a curing agent so that the solid content of the curing agent was 10 parts by mass relative to 100 parts by mass of the solid content of the polymer solution, and diluted with a mixed solvent of water and 2-propanol to prepare a coating solution with a solid content of 20%.

[0386] A moisture-barrier laminated film was obtained in the same manner as in Example 1 except that this coating solution was used.

[0387] <Comparative Example 3>

[0388] A polymer solution (solid content 40%) containing an acrylic resin D (Mw=69000, glass transition point=70° C., OHV=80, glycidyl group content=0 mass %) was prepared as a matrix resin.

[0389] A moisture-barrier laminated film was obtained in the same manner as in Example 1 except that this polymer solution was used.

[0390] Tables 1 and 2 show the materials used to form each layer and the presence or absence of a protective layer in the above-mentioned Examples and Comparative Examples.

[0391] It should be noted that the meanings of the abbreviations used in Tables 1 and 2 are as follows.

[0392] AlO: Aluminum oxide.

[0393] SiO: Silicon oxide.

[0394] Am: amine catalyst.

[0395] Sn: organic tin catalyst.

[0396] Zn: organic zinc catalyst.

[0397] M polymer: matrix polymer.

[0398] In addition, in the table, the amount of curing agent is expressed in parts by mass relative to 100 parts by mass of the base resin.

[0399] <Evaluation Test>

[0400] Regarding the moisture barrier laminated films of the above-produced examples and comparative examples, in addition to the thickness of the coating layer, the glass transition point Tg, moisture permeability, storage modulus E', water contact angle θ of the coating layer and degradation evaluation of the barrier layer were measured by the above-mentioned method. The results are shown in Tables 3 and 4.

[0401] [Table 1]

[0402]

[0403] [Table 2]

[0404]

[0405]

[0406] [Table 3]

[0407]

[0408] [Table 4]

[0409]

[0410] Description of Reference Numerals

[0411] (A) Plastic film

[0412] (A1): Inorganic barrier layer

[0413] (B): Moisture capture layer

[0414] (C): Coating

[0415] (D): Protective layer

[0416] 10: Moisture barrier laminate film

Claims

1. A moisture barrier laminate film, It is characterized in that The moisture barrier laminate film comprises a plastic film (A) having an inorganic barrier layer (A1) and a moisture capture layer (B) containing an alkali component, A coating layer (C) is provided between the inorganic barrier layer (A1) and the moisture capture layer (B), wherein the coating layer (C) is formed of a urethane (meth)acrylate polymer obtained by reaction of a (meth)acrylic resin and an isocyanate and having a high glass transition point of 85° C. or higher, and has a moisture permeability of 6.0×10 4 g / m 2 / day or less, and the storage modulus E' at 2πrad / s in the viscoelasticity measurement at 85°C is 30 MPa or more.

2. The moisture barrier laminate film according to claim 1, in, The coating layer (C) contains a catalyst in an amount within a range of 0.02 to 1.0 mass %.

3. The moisture barrier laminate film according to claim 2, in, The catalyst is a metal catalyst.

4. The moisture barrier laminate film according to claim 1, in, A protective layer (D) is provided between the inorganic barrier layer (A1) and the coating layer (C).

5. The moisture barrier laminate film according to claim 4, in, The protective layer (D) contains, in addition to the water-soluble polymer (D1), at least one component (D2) selected from the group consisting of the following compounds: Compounds of ingredient (D2): Organoalkoxysilane or its hydrolyzate; Metal alkoxides or hydrolysates thereof; and Phosphorus compounds.

6. The moisture barrier laminate film according to claim 1, in, A coating layer (C) is also provided on the side of the moisture capture layer (B) opposite to the inorganic barrier layer (A1). 7 . A sealing material for an electronic device, comprising the moisture-barrier laminated film according to claim 1 .

Citation Information

Patent Citations

  • Plastic container and manufacture thereof

    JP2000255579A

  • Gas barrier laminate good in moisture barrier properties

    JP2015096320A

  • Gas barrier multilayer film

    CN106660352A

  • Laminate film having moisture-barrier properties

    JP2019084747A

  • Urethane (METH) acrylate, active energy ray-curable composition containing the same, and cured product thereof

    JP2020041101A