A polymer aggregate fiber spraying substrate and construction method thereof

Through the use of spray-bearing substrates with polymer agglomerated fibers, the stability and nutrient supply problems of substrates in the prior art during drought and rainy seasons have been solved, and better vegetation growth and ecological restoration effects have been achieved.

CN115568401BActive Publication Date: 2024-11-08BEIJING BAILINGTIANDI ENVIRONMENTAL PROTECTION TECH +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211205121.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-29
Publication Date
2024-11-08
Estimated Expiration
2042-09-29

AI Technical Summary

Technical Problem

The existing spray seeding technology is prone to cracking under drought conditions, serious soil erosion during the rainy season, and lacks long-term nutrient supply, resulting in vegetation degradation and ecological restoration failure.

Method used

The substrate is sprayed with polymer pellet fibers, and the reaction of polymer pellet agents with water forms a pellet structure, combining grass-soil mixed fibers and microbial agents to enhance the water-retaining, fertilizer-retaining and soil erosion resistance of the substrate, and passes through seaweed mud Improve the strength and water retention ability of the substrate.

Benefits of technology

It significantly improves the water, fertilizer and soil erosion resistance of the substrate, ensures the growth needs of vegetation in drought and rainy seasons, extends the service life of the substrate, and improves the restoration effect and safety of the slope.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003870773560000051
    Figure BDA0003870773560000051
  • Figure BDA0003870773560000061
    Figure BDA0003870773560000061
Patent Text Reader

Abstract

The present application relates to the technical field of slope repair, and specifically discloses a polymer aggregate fiber spraying substrate and a construction method thereof. A polymer aggregate fiber spraying substrate comprises the following raw materials: planting soil, grass-soil mixed fiber, organic fertilizer, polymer aggregate agent, compound fertilizer, microbial agent, water retaining agent and mixing water; the grass-soil mixed fiber is a mixture of grass fiber and seaweed mud. The polymer aggregate fiber spraying substrate of the present application has the advantages of strong water retention capacity, strong fertilizer retention capacity, strong resistance to soil and water loss, and high substrate strength through the combination of polymer aggregate agent, water retaining agent, grass-soil mixed fiber and microbial agent. It can prevent the cracking of the substrate in the dry season and prevent wind and rain erosion in the rainy season, and promote vegetation growth and effectively prevent soil and water loss, which can improve the safety of the slope.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of slope repair, and more specifically, to a polymer aggregate fiber spraying substrate and a construction method thereof. Background Art

[0002] In recent years, with the development of urban industry, mining areas, roads, hydropower projects and tourist attractions, the number of exposed abandoned sites and slopes has increased due to the continuous destruction of the ecological environment, and there is an urgent need for environmental governance and ecological restoration. Common ecological restoration methods include three-dimensional net grass planting technology and foreign soil spraying technology. Among them, foreign soil spraying technology refers to the use of a special sprayer to spray organic substrates such as grass seeds and water retaining agents onto the slope surface. The organic substrate is closely combined with the slope surface under the action of pressure to form a matrix layer for plant growth and development.

[0003] Compared with the three-dimensional net grass planting technology, soil spraying has a better restoration effect, so it is more suitable for rock and soil slopes and soil-rock slopes with a high degree of weathering. However, the existing spraying technology still has the following disadvantages: ① Poor water retention capacity: When the slope vegetation is in an area with a dry climate or low precipitation, if artificial water is not replenished in time, the slope vegetation will quickly wither, degenerate and die. ② Poor fertilizer retention capacity: The substrate does not have a long-term nutrient supply system. After the nutrients in the substrate are absorbed by the normal growth of the vegetation in the early stage, the slope vegetation will degenerate and die due to lack of nutrients in the later stage. ③ Poor resistance to soil and water erosion: The soil in the substrate does not have a granular structure and hydrophobic reaction. In the rainy season, as the precipitation continues, the rainwater runoff on the slope will become turbid, causing soil and water erosion of the substrate, which will lead to the gradual weakening of the site conditions of the vegetation in the later stage and the failure of the ecological restoration goal. ④Poor strength of substrate: The fixation of conventional spraying substrate mainly relies on the three-dimensional structure of wire mesh. Due to the limited soil-fixing ability of wire mesh, it will cause cracking and falling off during drought; after being saturated with water in the rainy season, the weight of the substrate increases, which will cause the substrate to slip. Summary of the invention

[0004] In order to solve the above technical problems, the present application provides a polymer aggregate fiber spraying substrate and a construction method thereof.

[0005] In a first aspect, the present application provides a polymer aggregate fiber spraying substrate, which adopts the following technical scheme: a polymer aggregate fiber spraying substrate, comprising the following raw materials in parts by weight: 200-300 parts of planting soil, 15-18 parts of grass-soil mixed fiber, 15-18 parts of organic fertilizer, 0.3-0.35 parts of polymer aggregate agent, 0.75-1.0 parts of compound fertilizer, 0.25-0.3 parts of microbial agent, 0.12-0.18 parts of water retaining agent and 420-450 parts of mixing water;

[0006] The grass-soil mixed fiber is a mixture of grass fiber and seaweed mud.

[0007] By adopting the above technical scheme, after the high molecular weight agglomerates react with water through a hydrophobic reaction and are mixed with the planting soil, agglomerates of different sizes and a pore structure can be formed. Through the coordinated use of the high molecular weight agglomerates and the water retaining agent, countless layers of polymer molecular membranes can be formed inside the substrate. While absorbing and storing water, the moisture inside the substrate can be effectively locked to reduce moisture evaporation, thereby maintaining the moisture demand for normal growth of slope vegetation for a longer period of time.

[0008] The use of microbial agents in the substrate of the present application can permanently decompose grass fibers, organic matter and fallen leaves of slope vegetation in the substrate to form humic acid, thereby fully supplying the nutrients required for the normal growth of vegetation on the slope in the later stage.

[0009] Grass fiber has strong toughness and strength, and has a certain pore structure. It can be used in the substrate to enhance the strength of the substrate. The main components of seaweed mud are diatomaceous earth, seaweed sedimentary minerals and colloids. Diatomaceous earth and seaweed sedimentary minerals have countless tiny pores on the surface and inside of the particles, which have good water absorption and permeability. The colloid in seaweed mud has strong water retention and moisturizing ability. The grass-soil fiber mixture formed by grass fiber and seaweed mud can not only enhance the strength of the substrate, but also improve the water retention and storage capacity of the substrate, thereby playing a better protective and repair role.

[0010] Optionally, the grass-soil mixed fiber is prepared by the following method:

[0011] ① Take dry grass fiber, add it to an acid anhydride solution, and after acidification and modification, wash and dry it to obtain modified grass fiber for standby use;

[0012] ② Mix corn cob powder, carboxymethyl cellulose, sodium lignosulfonate and water, heat and gelatinize, add acrylamide, stir and mix evenly to obtain an impregnation solution;

[0013] ③ Take the modified grass fiber, put it into the impregnation liquid, add the crosslinking agent and the initiator to react under the protection of nitrogen, wash the obtained product and drain the surface water, mix it with the seaweed mud and stir it evenly, and after drying, obtain the grass soil premix;

[0014] ④ Put the grass-soil premix into the impregnation liquid of step ②, after stirring and impregnating, filter the solid-liquid mixture to separate the solid precipitate, add seaweed mud to the solid precipitate, stir evenly, and dry to obtain a grass-soil mixture.

[0015] The traditional method of mixing the substrate raw materials is to react the polymer agglomerate with water to form a colloid, and then mix it with the planting soil and grass fiber. Because the planting soil and grass fiber are only physically mixed before mixing, when the two are mixed in the polymer colloid, the planting soil and grass fiber are easily separated from each other, and agglomeration between the grass fibers and the planting soil is likely to occur. In this case, in order to improve the uniformity of the raw material mixing, it is necessary to increase the mixing time or mixing speed. However, too long mixing time and mixing speed can easily damage the system structure and affect the repair stability of the substrate.

[0016] By adopting the above technical scheme, the surface of the hay fiber is modified by acid anhydride, so that the acid anhydride reacts with the hydroxyl groups on the surface of the hay fiber to obtain more hydrophilic groups, which is beneficial to the subsequent reaction; corn cob powder, carboxymethyl cellulose, sodium wood sulfonate, water and acrylamide are mixed to obtain an impregnation solution; the surface-treated grass fiber is put into the impregnation solution, and under the action of a cross-linking agent and an initiator, a water-retaining adhesive film with a more porous structure can be wrapped on the surface of the grass fiber. Subsequently, the porous and colloidal properties of seaweed mud can be used to combine with grass fibers wrapped with a water-retaining adhesive film to form a grass-soil premix; the grass-soil premix is ​​again put into the impregnation liquid to remove impurities, floating and sinking and other unbound substances on the surface of the grass-soil premix, and after the obtained solid precipitate is mixed with seaweed mud, the obtained grass-soil mixed fiber has a more stable structure; the grass-soil mixed fiber thus obtained has a more porous structure and a certain colloidal adhesive force, and when it is mixed with planting soil, it can improve the adhesion between it and the planting soil, and through low-speed, short-time stirring, it is also easier to mix with an aqueous solution of a polymer granulating agent, thereby forming a more stable three-dimensional network structure; and the treated grass-soil mixed fiber can increase the porosity of the substrate, so that it has higher water retention and moisture retention capabilities, thereby better reducing soil and water loss.

[0017] Optionally, in step ②, the weight ratio of corn cob powder, sodium lignosulfonate, carboxymethyl cellulose, polyacrylamide and water is 30:4-6:3-5:1-2:100.

[0018] Optionally, in step ③, the weight ratio of the modified grass fiber to the impregnation liquid is 1:5-10.

[0019] Optionally, in step ③, the weight ratio of modified grass fiber to seaweed mud is 10:1-2.

[0020] Optionally, in step ④, the weight ratio of the grass-soil premix to the impregnation liquid is 1:15-20.

[0021] Optionally, in step ④, the weight ratio of the grass soil premix to the seaweed mud is 10:1-3.

[0022] Optionally, the mixing water consists of immersion water and pure water in a weight ratio of 1:1-3;

[0023] The soaking water is the liquid obtained after filtering the solid-liquid mixture to separate the solid precipitate in step ④.

[0024] Optionally, the polymer aggregate fiber spray-seeding substrate is prepared by the following method: after evenly mixing planting soil, grass fiber, organic fertilizer, polymer aggregate agent, compound fertilizer, microbial agent and water-retaining agent, adding soaking water and stirring evenly to obtain a matrix material; adding the aggregate agent to pure water and stirring evenly to obtain a binder; mixing the binder and the matrix material and stirring evenly to obtain a polymer aggregate fiber spray-seeding substrate material.

[0025] In a second aspect, the present application provides a construction method for a polymer aggregate fiber spraying substrate, which adopts the following technical solution:

[0026] A construction method for a polymer aggregate fiber spraying substrate comprises the following steps:

[0027] S1. Slope finishing: remove debris and loose rocks from the working surface, and trim the corners and top edges of the slope into an arc shape;

[0028] S2. Hanging mesh and anchoring: After the slope surface is cleaned and leveled, lay the three-dimensional structure galvanized wire mesh and fix it into the rock with anchor nails;

[0029] S3, base material mixing: after the planting soil, grass fiber, organic fertilizer, high molecular weight granulating agent, compound fertilizer, microbial agent and water retaining agent are mixed evenly, a part of the mixing water is added, and the mixture is stirred evenly to obtain the base material; the granulating agent is added to the remaining mixing water, and the mixture is stirred evenly to obtain the binding material; after the binding material and the base material are mixed and stirred evenly, the high molecular weight granulating fiber spraying base material is obtained;

[0030] S4, spraying: Put the polymer aggregate fiber spraying base material into the spraying machine, and spray the base material on the slope after the net is hung;

[0031] S5. Maintenance management: After the spraying is completed, routine maintenance is required.

[0032] By adopting the above technical solution, the present application can form a stable bird's nest-like multi-dimensional physical protection structure through the cooperation of the substrate and the three-dimensional galvanized wire mesh. When the spraying thickness reaches 15-20cm, it still has excellent substrate strength.

[0033] Optionally, when the unit finishing area is ≥1000 square meters, drainage ditches need to be set up at the top, foot and platform of the slope before hanging the net and anchoring S2.

[0034] In summary, this application has the following beneficial effects:

[0035] 1. The polymer aggregate fiber spraying substrate of the present application has the advantages of strong water retention capacity, strong fertilizer retention capacity, strong water and soil resistance and high substrate strength through the combination of polymer aggregate agent, water retaining agent, grass-soil mixed fiber and microbial agent. It can prevent the substrate from cracking in the dry season and prevent wind and rain erosion in the rainy season, promote vegetation growth, effectively prevent soil erosion, and thus improve the safety of the slope.

[0036] 2. The grass-soil mixed fiber of the present application has a more stable structure. Since it has more porous structures and certain colloidal bonding force, when it is mixed with planting soil, the adhesion between it and the planting soil can be improved. Through low-speed and short-time stirring, it is also easier to mix with the aqueous solution of the polymer aggregate, thereby forming a more stable three-dimensional network structure; and the treated grass-soil mixed fiber can increase the porosity of the substrate, so that it has higher water retention and moisture retention capacity, thereby better reducing soil and water loss.

[0037] 3. The polymer aggregate fiber spraying substrate of the present application is suitable for stable hard rock slopes and steep rock slopes with a slope ratio of less than 1:0.25, concrete slopes and mortar-masonry slopes with a slope ratio of less than 1:0.25, soft mixed slopes and weathered rock slopes with a slope ratio of less than 1:0.5, including poor-quality slopes such as barren, acidic and alkaline slopes, as well as for ecological restoration of sites with damaged environments in factories, mining areas, and rivers, and has a wide range of uses. DETAILED DESCRIPTION

[0038] The present application is further described in detail below with reference to the embodiments.

[0039] Preparation Example

[0040] Unless otherwise specified, the raw materials in the preparation examples can be obtained from commercial sources, wherein the initiator is potassium persulfate and the cross-linking agent is N,N'-methylenebisacrylamide.

[0041] Preparation Example 1: Grass-soil mixed fiber is prepared by the following method:

[0042] ① Take dry grass fiber with a length of 3-5 cm, add 6% acetic anhydride solution with a mass fraction of twice its weight, and acidify and modify it at a temperature of 50°C for 2 hours; then take out the acidified grass fiber and wash it with clean water twice, and then dry it at a temperature of 60°C for 4 hours to obtain modified grass fiber for use;

[0043] ② Mix corncob powder with a fineness of 400 mesh, sodium lignin sulfonate, carboxymethyl cellulose and water, stir evenly, heat to 60°C, and gelatinize for 30 minutes; then add acrylamide, stir at a high speed of 2000r / min for 10 minutes to obtain an impregnation solution; wherein the weight ratio of corncob powder, sodium lignin sulfonate, carboxymethyl cellulose, acrylamide and water is 30:5:4:1.5:100;

[0044] ③ Take 20 kg of modified grass fiber, put it into 150 kg of impregnation liquid, add crosslinking agent and initiator under nitrogen protection, react for 4 hours, wash the obtained product with 50% ethanol solution by volume, drain the surface water, mix and stir evenly with 3 kg of seaweed mud, dry in the shade for 3 days, and obtain grass soil premix;

[0045] ④ Take 20kg of the grass-soil premix and put it into 350kg of the impregnation liquid in step ②, stir and impregnate for 30 minutes; then filter and separate the solid precipitate, and collect the remaining liquid (i.e., the impregnation water); add 4kg of seaweed mud to the solid precipitate, stir evenly, and dry in the shade for 5 days to obtain grass-soil mixed fiber.

[0046] Preparation Example 2

[0047] The grass-soil mixture in this preparation example is prepared by the following method: dry grass fiber and seaweed mud are mixed in a ratio of 5:1 and stirred evenly.

[0048] Preparation Example 3

[0049] The difference between this preparation example and preparation example 1 is that step ④ is not included, that is, the grass-soil premix in step ③ is the grass-soil mixed fiber.

[0050] Example

[0051] Unless otherwise specified, the raw materials in the examples can be obtained from commercial sources. The organic fertilizer is decomposed farmyard manure; the polymer granules are purchased from France Aisen; the compound fertilizer is nitrogen, phosphorus and potassium compound fertilizer; the microbial agent is purchased from Shandong Aofeng Biology; and the water retaining agent is polyacrylamide with a molecular weight of 10 million.

[0052] Examples 1-3

[0053] As shown in Table 1, the difference between Examples 1-3 is that the amount of raw materials used is different, and Example 1 is used as an example for description below.

[0054] The method for preparing the polymer aggregate fiber spraying substrate provided in Example 1 comprises the following steps:

[0055] (1) After the planting soil, grass soil mixed fiber, organic fertilizer, polymer granule, compound fertilizer, microbial agent and water retaining agent are evenly mixed, a portion of mixing water is added, and the mixture is stirred at a speed of 100 r / min for 10 minutes to obtain a matrix material;

[0056] (2) adding a granulating agent to the remaining mixing water and stirring at a speed of 30 r / min for 15 min to obtain a binder;

[0057] (3) Mix the binder and the matrix material and stir at a speed of 60 r / min for 15 minutes.

[0058] Table 1 Raw material dosage table of Examples 1-3

[0059]

[0060]

[0061] Example 4

[0062] The difference between this embodiment and embodiment 1 is that the grass-soil mixed fiber is prepared by Preparation Example 2.

[0063] Example 5

[0064] The difference between this embodiment and embodiment 1 is that the grass-soil mixed fiber is prepared by Preparation Example 3.

[0065] Comparative Example

[0066] Comparative Example 1: This comparative example differs from Example 1 in that the grass-soil mixed fiber is replaced by an equal amount of grass fiber.

[0067] Performance test experiment

[0068] Referring to the method in CJJT292-2018 "Technical Standard for Slope Spray Seeding Greening Engineering", the maximum water holding capacity, cohesion and segregation of the spray seeding matrix were tested, and the test results are recorded in Table 2.

[0069] Table 2 Performance test table of the spraying substrate of Examples 1-5 and Comparative Example 1

[0070] project Maximum water holding capacity, % Cohesion, kPa Segregation, % Require >40 >25 ≤60 Example 1 62.7 38.9 2.6 Example 2 60.3 36.7 2.9 Example 3 60.1 36.0 3.2 Example 4 49.7 34.9 5.4 Example 5 57.2 35.8 3.5 Comparative Example 1 45.6 34.2 8.6

[0071] According to the data in Table 2, combined with Example 1 and Comparative Example 1, it can be seen that the addition of grass-soil mixed fibers in the spraying substrate has a significant effect on the performance of the substrate. The maximum water holding capacity and cohesion of the substrate of Example 1 are significantly greater than those of Comparative Example 1, and the degree of segregation of the substrate of Example 1 is significantly lower than that of Comparative Example 1, indicating that the use of grass-soil mixed fibers in this application can significantly improve the water retention and water storage capacity of the substrate. This is because traditional grass fibers only have fiber structures, and only physical mixtures are obtained when mixed with planting soil, and the raw materials in the physical mixture are bonded by the added polymer aggregates; and after the grass fibers are processed in this application, the colloidal properties and porous characteristics of seaweed mud are utilized, and the grass-soil mixed fibers obtained have strong cohesion, and then when mixed with planting soil, the cohesion between them and the planting soil can be improved, and because it has a large number of fine pores, the water retention and water storage capacity of the substrate can be improved, so that it can play a better role in water retention, fertilizer retention, and soil and water loss resistance.

[0072] Combining the data of Example 1, Example 4, Example 5 and Table 2, it can be seen that the maximum water holding capacity and cohesion of the substrate of Example 1 are significantly greater than those of Comparative Example 1, and the segregation degree of the substrate of Example 1 is significantly lower than that of Comparative Example 1, indicating that compared with directly mixing grass fiber and seaweed mud, when the method of the present application is used to treat grass fiber and seaweed mud, the obtained grass-soil mixed fiber can be used as a spraying substrate. The maximum water holding capacity and cohesion of the substrate can be significantly improved, and the segregation degree of the substrate can be significantly reduced, indicating that the grass-soil mixed fiber of the present application, when combined with other raw materials of the substrate, has better water retention, fertilizer retention and anti-soil and water loss effects.

[0073] Application Examples

[0074] Select the slope to be repaired, which is a basalt slope with a slope angle of 70°. Repair the slope in accordance with the following method:

[0075] S1. Slope finishing: remove debris and loose rocks from the working surface, and trim the corners and top edges of the slope into an arc shape;

[0076] S2. Hanging and anchoring: After the slope surface is cleaned and leveled, lay a three-dimensional galvanized wire mesh with a diameter of 2.0 mm and a mesh size of 50 mm*50 mm. The overlap of the wire mesh should be no less than 50 mm. Each overlap point should be 14 mm thick. # Lead wire is used for suturing and tying, and then φ12mm, L=350mm anchors are used to drive into the rock for fixing;

[0077] S3, base material mixing: using the polymer aggregate fiber spraying base material provided in Example 1, planting soil, grass fiber, organic fertilizer, polymer aggregate agent, compound fertilizer, microbial agent and water retaining agent are mixed evenly, and then soaking water is added and stirred evenly to obtain a base material; adding the aggregate agent to pure water and stirring evenly to obtain a binder; mixing the binder and the base material and stirring evenly to obtain a polymer aggregate fiber spraying base material;

[0078] S4, spraying: Mix the polymer aggregate fiber spraying base material and put it into the spraying machine, spray the base material on the slope after hanging the net, and the spraying thickness is 10cm;

[0079] S5. Maintenance and management: After the spraying is completed, spray the Robinia seeds, then cover the plant seed layer with non-woven fabric, and water the soil layer for maintenance.

[0080] Four months after the construction is completed, the survival rate of the plants is calculated according to the following formula:

[0081] Plant survival rate % = number of plants that emerged after 4 months / amount of original seeds used * 100%.

[0082] It is calculated that after the slope is repaired using the method of the application example, the plant survival rate can reach more than 90%, indicating that the construction method of the present application has a good repair effect on the slope.

[0083] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A polymer aggregate fiber spraying substrate, characterized in that: The raw materials include the following parts by weight: 200-300 parts of planting soil, 15-18 parts of grass-soil mixed fiber, 15-18 parts of organic fertilizer, 0.3-0.35 parts of polymer granules, 0.75-1.0 parts of compound fertilizer, 0.25-0.3 parts of microbial agent, 0.12-0.18 parts of water retaining agent and 420-450 parts of mixing water; The grass-soil mixed fiber is a mixture of grass fiber and seaweed mud; The grass-soil mixed fiber is prepared by the following method: ① Take dry grass fiber, add it to an acid anhydride solution, and after acidification and modification, wash and dry it to obtain modified grass fiber for standby use; ② Mix corn cob powder, carboxymethyl cellulose, sodium lignosulfonate and water, heat and gelatinize, add acrylamide, stir and mix evenly to obtain an impregnation solution; ③ Take the modified grass fiber, put it into the impregnation liquid, add the crosslinking agent and the initiator to react under the protection of nitrogen, wash the obtained product and drain the surface water, mix it with the seaweed mud and stir it evenly, and after drying, obtain the grass soil premix; ④ Put the grass-soil premix into the impregnation liquid of step ②, after stirring and impregnating, filter the solid-liquid mixture to separate the solid precipitate, add seaweed mud to the solid precipitate, stir evenly, and dry to obtain grass-soil mixed fiber; In the step ②, the weight ratio of corn cob powder, sodium lignosulfonate, carboxymethyl cellulose, polyacrylamide and water is 30:4-6:3-5:1-2:100; In the step ③, the weight ratio of the modified grass fiber to the impregnation liquid is 1:5-10; In the step ③, the weight ratio of the modified grass fiber to the seaweed mud is 10:1-2; In the step ④, the weight ratio of the grass-soil premix to the impregnation liquid is 1:15-20; In the step ④, the weight ratio of the grass soil premix to the seaweed mud is 10:1-3.

2. The polymer aggregate fiber spraying substrate according to claim 1, characterized in that: The mixing water is composed of immersion water and pure water in a weight ratio of 1:1-3; The soaking water is the liquid obtained after filtering the solid-liquid mixture to separate the solid precipitate in step ④.

3. The polymer aggregate fiber spraying substrate according to claim 2, characterized in that: The polymer aggregate fiber spraying substrate is prepared by the following method: planting soil, grass-soil mixed fiber, organic fertilizer, polymer aggregate agent, compound fertilizer, microbial agent and water retaining agent are mixed evenly, and then soaking water is added and stirred evenly to obtain a matrix material; the aggregate agent is added to pure water and stirred evenly to obtain a binder; the binder and the matrix material are mixed and stirred evenly to obtain a polymer aggregate fiber spraying substrate material.

4. The construction method of the polymer aggregate fiber spraying substrate according to claim 1, characterized in that: The steps include: S1. Slope finishing: remove debris and loose rocks from the working surface, and trim the corners and top edges of the slope into an arc shape; S2. Hanging mesh and anchoring: After the slope surface is cleaned and leveled, lay the three-dimensional structure galvanized wire mesh and fix it into the rock with anchor nails; S3, base material mixing: after the planting soil, grass soil mixed fiber, organic fertilizer, polymer granulating agent, compound fertilizer, microbial agent and water retaining agent are mixed evenly, a part of the mixing water is added, and the mixture is stirred evenly to obtain the base material; the granulating agent is added to the remaining mixing water, and the mixture is stirred evenly to obtain the binding material; after the binding material and the base material are mixed and stirred evenly, the polymer granulating fiber spraying base material is obtained; S4, spraying: Put the polymer aggregate fiber spraying base material into the spraying machine, and spray the base material on the slope after the net is hung; S5. Maintenance management: After the spraying is completed, routine maintenance is required.