Preparation method of silver-coated aluminum powder for electromagnetic shielding material conductive rubber

The surface of the aluminum powder is zinc-plated and then silver-plated through the chemical light finishing method to form a pre-plated thin zinc layer, which solves the problems of fluoride environmental pressure, nickel layer density and high temperature resistance in the existing technology, and improves the efficiency of silver-coated aluminum powder. Excellent electrical conductivity and shear and extrusion resistance, suitable for electromagnetic shielding materials.

CN115570133BActive Publication Date: 2024-10-11陈瑞春
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211325092.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-27
Publication Date
2024-10-11
Estimated Expiration
2042-10-27

AI Technical Summary

Technical Problem

In the existing silver-coated aluminum powder preparation method, fluoride has a great impact on the environment, the nickel layer has poor density, the silver layer is not resistant to high temperatures, and the polydopamine process is only suitable for low-concentration silver nitrate solutions, resulting in limited conductivity.

Method used

Using the chemical photofinishing method, the surface of the aluminum powder is first galvanized and then silver-plated to form a pre-plated thin zinc layer to improve the bonding force and density of the silver layer and the aluminum powder, and improve the conductivity through the replacement chemical silver plating process.

Benefits of technology

The prepared silver-coated aluminum powder has excellent binding force and conductive properties, is suitable for electromagnetic shielding materials, and exhibits good shear resistance, extrusion resistance and conductive properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115570133B_ABST
    Figure CN115570133B_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing silver-coated aluminum powder for conductive rubber of electromagnetic shielding material, characterized in that aluminum powder with a particle size of 10 to 100 μm is subjected to surface degreasing, surface finishing, zinc plating, silver plating, washing, suction filtration, and drying to obtain silver-coated aluminum powder, wherein the silver content is 15% to 30% and the aluminum content is 70% to 85%. The silver-coated aluminum powder prepared by the method steps of the invention has excellent bonding force and conductive performance due to the presence of a pre-plated thin zinc layer between the silver and aluminum interface. The silver-coated aluminum powder prepared by the invention has excellent shear resistance, extrusion resistance and excellent conductive performance when mixed with rubber.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of material technology, relates to electromagnetic shielding material technology, and particularly to a preparation technology of conductive functional powder material for electromagnetic shielding material. Background Art

[0002] Electronic communication plays an important role in modern life, but the electromagnetic radiation generated by electronic products also has obvious interference effects on the human body and the surrounding environment, causing certain hazards. Using electromagnetic shielding materials to shield electromagnetic waves is one of the main preventive measures. Conductive silicone rubber is a very important electromagnetic shielding material, which can fill the gaps of electronic equipment and instruments, and can be connected to EMI shielding windows, ventilation waveguides and other devices. The main raw materials for producing conductive rubber are highly conductive fillers such as conductive silver-coated copper powder, silver-coated aluminum powder, silver-coated nickel powder, silver-coated graphite powder, and pure silver powder. Aluminum powder has the advantages of being difficult to oxidize, low density, and low price, and has been widely used in electronics, aviation and other fields. However, since aluminum is an amphoteric metal, it cannot be used in complex environments; in addition, the poor conductivity of aluminum powder limits its application in the field of high conductivity. Silver-coated aluminum powder not only solves the defects of aluminum powder as an amphoteric metal, but also greatly improves its conductivity due to the presence of surface-coated silver, so it can be used as a highly conductive filler to prepare materials with good shielding effectiveness.

[0003] Patent CN 111531168A (application date 2020.08.14) provides a method for preparing silver-clad aluminum material for electromagnetic shielding. The method proposed by Su Xiaolei first pre-treats the aluminum powder, then puts the pre-treated aluminum powder into a constant temperature magnetic stirrer, adds an appropriate amount of copper nitrate solution dropwise, and adds fluoride at the same time, stirs evenly, and obtains copper-clad aluminum powder after the reaction is complete; then puts the copper-clad aluminum powder into a constant temperature magnetic stirrer, and adds an appropriate amount of silver nitrate solution dropwise, and adds a chelating agent at the same time, stirs evenly, and obtains silver-clad aluminum powder after the reaction is complete.

[0004] The journal article "Effects of Different Reducing Agents on the Microstructure and Properties of Silver-plated Aluminum Powder" by Su Xiaolei et al. ([J]. Journal of Xi'an Polytechnic University, 2022, 36(3): 106-114) proposed that nickel is first plated on the surface of aluminum powder, and then silver is plated using a double reduction system of tartaric acid + glucose. The silver deposition process consists of four steps: silver-nickel replacement → silver particle deposition → silver layer expansion → silver self-catalytic growth.

[0005] Zhang Zhenhua et al. (Study on the Process of Silver-coated Aluminum Powder [J]. Electroplating and Finishing, 2007, 26(1): 23-25) used alkaline washing to remove the surface oxide film, then copper-plated the aluminum powder surface, and then silver-plated the copper surface using the displacement method.

[0006] Zhang Ainv et al. (Study on Chemical Silver Plating Process of Aluminum Balls [J]. Electroplating and Environmental Protection, 2016, 36(1): 24-26) used polydopamine to pretreat the surface of aluminum balls. A layer of polydopamine was evenly coated on the surface of the aluminum powder matrix. Since its amino and catechol groups have weak reducing properties, highly active points can be formed on the surface of the aluminum balls. Then, Ag is converted into silver under the action of reducing agents such as glucose. + It is reduced to a silver-plated layer, and finally a uniform and dense silver layer is obtained.

[0007] Regarding the various methods of silver-coated aluminum powder mentioned above, fluoride has a great impact on the environment and brings great pressure to environmental protection; when nickel is replaced by plating on the surface of aluminum powder, the nickel layer is relatively loose, and the final surface silver layer is not very dense; when copper is replaced by plating on the middle layer, due to the presence of copper atoms or copper ions, the final silver-coated aluminum powder cannot withstand high temperatures; polydopamine is used to modify the surface of aluminum powder, and this process is only suitable for low-concentration silver nitrate solutions. Summary of the invention

[0008] In response to the problems raised by the above background technology, the present invention provides a method for preparing silver-coated aluminum powder with good bonding force between the silver plating layer and the aluminum powder interface and complete and dense coating. The silver-coated aluminum powder prepared by this method can be used in conductive rubber, conductive coatings, and conductive plastics of electromagnetic shielding materials.

[0009] In order to achieve the above technical objectives, the technical solution adopted by the present invention is as follows:

[0010] A method for preparing silver-coated aluminum powder for electromagnetic shielding material conductive rubber, wherein the surface of the aluminum powder is chemically finished, first chemically zinc-plated and then silver-plated, so as to improve the bonding force and compactness between the silver-plated layer and the substrate, and form a composite powder with a complete and compact coating structure;

[0011] The specific preparation process includes the following steps:

[0012] (1) Select aluminum powder of 10 to 100 μm and use alkaline solution at room temperature to remove oil and oxide film from the surface for 3 to 10 minutes, and then wash and filter it for later use;

[0013] (2) In order to reduce the specific surface area of ​​aluminum powder and increase the thickness and conductivity of the silver-plated layer, the aluminum powder after degreasing and oxide film removal is immersed in a strong alkaline solution for surface finishing at room temperature for 20 to 60 minutes, and then washed and filtered for standby use;

[0014] (3) Place the aluminum powder after surface finishing in a galvanizing solution at 15 to 25°C and stir for 30 to 60 seconds, then wash and filter for later use;

[0015] (4) The galvanized aluminum powder is stirred under acidic conditions of 30-50° C. and pH=2-3 to undergo chemical silver replacement plating until the silver floccules in the solution completely disappear, and then washed, filtered, and dried to obtain the finished product.

[0016] The aluminum powder in the above step 1 is spherical in shape and has a particle size of 10 to 100 um, wherein 10 to 20 um is a fine particle size, 20 to 60 um is a medium particle size, and 60 to 100 um is a coarse particle size.

[0017] In the above step 1, the alkali used in the alkaline solution for surface degreasing is NaOH or KOH, preferably NaOH, the prepared concentrated solution is 1% to 5%, and the optimal choice is 2%. The temperature used is room temperature, the optimal time is 5 minutes, and the cleaning solution used is deionized water, and the cleaning is performed until neutral.

[0018] The surface finishing modification in the above step 2 is to reduce the specific surface area of ​​the aluminum powder by etching the protrusions and the attached tiny aluminum particles on the surface of the aluminum powder particles, so as to increase the thickness of the silver-plated layer, thereby increasing the conductivity of the silver-coated aluminum powder. The strong alkaline solution used is a mixture of NaOH, sodium potassium tartrate and water, and the mass percentage is NaOH: sodium potassium tartrate: water = 6:3:91. The temperature used is 25°C, the optimal time used is 25 minutes, and the cleaning solution used is deionized water, and the cleaning is done until neutral.

[0019] The aluminum powder galvanizing in step 3 is prepared by mixing 5-12 g / L zinc oxide, 50-100 g / L sodium hydroxide, 10-30 g / L nickel sulfate, 9-14 g / L sodium citrate, and 20-120 g / L complexing agent into a mixed solution. Preferably, zinc oxide (Zn2O) is 8 g / L, sodium hydroxide (NaOH) is 65 g / L, and nickel sulfate (NiSO4) is 22 g / L. 2+ , can co-deposit with zinc, inhibit the growth of zinc, make the nucleus generation faster than the grain growth rate, reduce the size of zinc grains in the zinc immersion layer, make the zinc immersion layer thinner and finer, which is conducive to improving the bonding strength between the zinc immersion layer and the base, sodium citrate (C6H5Na3O7) is preferably 12g / L, and the complexing agent (EDTA) is preferably 86g / L. The temperature used is 21°C, the preferred time used is 35s, and the cleaning liquid used is deionized water, which is cleaned to neutrality.

[0020] The replacement chemical silver plating in the above step 4 is a reaction between solid-solid phases, which is to first add 10-30 g / L of sodium chloride (NaCl) to a 30-85 g / L silver nitrate (AgNO3) solution to form a silver chloride (AgCl) flocculent, adjust its pH to 2-3 with 10% dilute sulfuric acid, stir at 300-500 rpm, and replace the reaction temperature at 30-50°C, wherein the silver nitrate (AgNO3) is preferably 52 g / L, and is gradually and slowly added, the sodium chloride (NaCl) is preferably 18 g / L, the pH value is preferably 2, the stirring speed is preferably 450 rpm, and the reaction temperature is preferably 40°C;

[0021] The chemical reaction process of silver chloride (AgCl) floccules is:

[0022] AgNO3+NaCl=AgCl↓+NaNO3

[0023] Since the metal activity of Zn is much higher than that of Ag, and the activity of hydrogen (H) is higher than that of Ag, Zn will replace Ag in the AgCl suspension without releasing hydrogen (H2). The chemical reaction process is as follows:

[0024] 2AgCl↓+Zn=2Ag+ZnCl2

[0025] The beneficial effects of the present invention are as follows: the silver-coated aluminum powder prepared by the present invention has excellent bonding force and conductivity due to the presence of a pre-plated thin zinc layer between the silver and aluminum interfaces; the silver-coated aluminum powder prepared by the present invention has excellent shear resistance, extrusion resistance and excellent conductivity when mixed with rubber. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] The present invention can be further illustrated by the non-limiting examples given in the accompanying drawings;

[0027] Figure 1 The process flow chart of preparing silver-coated aluminum powder of the present invention;

[0028] Figure 2 This is an image of 20wt% of silver-coated aluminum powder with a medium particle size (40um) prepared by the present invention at a magnification of 100;

[0029] Figure 3 This is an image of 20 wt % of silver-coated aluminum powder with a medium particle size (40 um) prepared in the present invention at a magnification of 1000. DETAILED DESCRIPTION

[0030] In order to enable those skilled in the art to better understand the present invention, the technical solution of the present invention is further described below in conjunction with the accompanying drawings and embodiments.

[0031] Embodiment 1:

[0032] In this embodiment, spherical aluminum powder with a median particle size of 40 μm is selected, and the preparation method of silver-coated aluminum powder with 5 wt% zinc plating and 20 wt% silver plating is as follows:

[0033] (1) Take 50g aluminum powder, soak it in 100ml NaOH solution with a concentration of 2% at room temperature for 5min, and then wash it with deionized water until it is neutral;

[0034] (2) immersing the aluminum powder in 100 ml of an alkaline solution mixture prepared in a mass percentage ratio of NaOH: sodium potassium tartrate: water = 6:3:91, the immersion temperature is 25° C., the immersion time is 25 min, and after the light finishing etching is completed, the aluminum powder is cleaned to a neutral state for standby use;

[0035] (3) Add the above powder into 300 ml of zinc plating solution and slowly stir at 100 rpm for 35 seconds at 21°C, filter quickly and wash until neutral for standby use, wherein the ratio of the zinc plating solution is 8 g / L zinc oxide (ZnO), 65 g / L sodium hydroxide (NaOH), 22 g / L nickel sulfate (NiSO4), 12 g / L sodium citrate (C6H5Na3O7), and 86 g / L chelating agent (EDTA);

[0036] (4) The above powder was added to 250 ml of silver chloride (AgCl) suspension for solid phase replacement reaction, wherein sodium chloride (NaCl) 18 g / L, silver nitrate (AgNO3) 52 g / L, pH = 2-3, stirring speed 450 rpm, reaction temperature 40 ° C. After the floccules completely disappeared, the powder was washed, filtered and dried to obtain the silver-coated aluminum powder with a silver content of 20%. Its appearance is as follows: Figure 2 and 3 shown.

[0037] Embodiment 2:

[0038] In this embodiment, spherical aluminum powder with a median particle size of 40 μm is selected, and the preparation method of silver-coated aluminum powder with 4 wt% zinc plating and 20 wt% silver plating is as follows:

[0039] The steps of Example 1 (1), (2) and (4) were followed, except that the ZnO concentration in (3) was changed to 6.4 g / L, and the rest remained unchanged.

[0040] Embodiment three:

[0041] In this embodiment, spherical aluminum powder with a median particle size of 40 μm is selected, and the preparation method of silver-coated aluminum powder with 5 wt% silver plating and 15 wt% silver plating is as follows:

[0042] The steps of Example 1 (1), (2) and (3) were followed, except that the concentration of silver nitrate in (4) was changed to 40 g / L, and the rest remained unchanged.

[0043] The performance indicators of the silver-coated aluminum powder under the above three embodiments are as follows:

[0044] Table 1 Performance index of silver-coated aluminum powder in the embodiment

[0045]

[0046]

[0047] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the technology may modify or change the above embodiments without violating the spirit and scope of the present invention. Therefore, all equivalent modifications or changes made by those with ordinary knowledge in the technical field without departing from the spirit and technical ideas disclosed by the present invention should still be covered by the claims of the present invention.

Claims

1. A method for preparing silver-coated aluminum powder for electromagnetic shielding material conductive rubber, characterized in that: The aluminum powder with a particle size of 10 to 100 μm is subjected to surface degreasing, surface finishing, galvanizing, silver plating, washing, filtering and drying to obtain silver-coated aluminum powder. The preparation process includes the following steps: (1) Select aluminum powder with a size of 10 to 100 μm, use an alkaline solution at room temperature to remove oil and oxide film from the surface for 3 to 10 minutes, and then wash and filter it for later use; (2) In order to reduce the specific surface area of ​​aluminum powder and increase the thickness and conductivity of the silver-plated layer, the aluminum powder after degreasing and oxide film removal is immersed in a strong alkaline solution, and the surface is polished for 20 to 60 minutes at room temperature, and then washed and filtered for standby use; (3) Place the aluminum powder after surface finishing in a galvanizing solution at 15-25°C and stir for 30-60 seconds, then wash and filter it for later use; (4) Stir the galvanized aluminum powder under acidic conditions of 30-50°C and pH=2-3 to perform chemical silver replacement until the silver flocs in the solution completely disappear, and then wash, filter and dry to obtain the finished product; During surface finishing, the strong alkaline solution used is a mixture of NaOH, sodium potassium tartrate and water, with a mass percentage of NaOH: sodium potassium tartrate: water = 6:3:

91. The cleaning solution used is deionized water, which is cleaned to neutrality. The surface finishing is performed by etching the protrusions on the surface of the aluminum powder particles and the accompanying tiny aluminum particles, thereby reducing the specific surface area of ​​the aluminum powder to increase the thickness of the silver-plated layer, thereby increasing the conductivity of the silver-coated aluminum powder. When aluminum powder is galvanized, the galvanizing solution is prepared by 5-12 g / L zinc oxide, 50-100 g / L sodium hydroxide, 10-30 g / L nickel sulfate, 9-14 g / L sodium citrate, and 20-120 g / L complexing agent. 2+ , can co-deposit with zinc, inhibit the growth of zinc, make the nucleus generation faster than the grain growth rate, reduce the size of zinc grains in the zinc immersion layer, make the zinc immersion layer thinner and more delicate, which is beneficial to improve the bonding strength between the zinc immersion layer and the base. The cleaning liquid used is deionized water, which is cleaned to neutrality; Silver plating refers to chemical silver plating by replacement. It uses a solid-solid phase reaction to first add 10-30 g / L of sodium chloride (NaCl) to a 30-85 g / L silver nitrate (AgNO3) solution to form a silver chloride (AgCl) flocculent. The pH is adjusted to 2-3 with 10% dilute sulfuric acid. The stirring speed is 300-500 rpm and the replacement reaction temperature is 30-50°C.

2. The method for preparing silver-coated aluminum powder for electromagnetic shielding material conductive rubber according to claim 1, characterized in that: The aluminum powder is spherical in shape and has a particle size of 10 to 100 um, wherein 10 to 20 um is a fine particle size, 20 to 60 um is a medium particle size, and 60 to 100 um is a coarse particle size.

3. The method for preparing silver-coated aluminum powder for electromagnetic shielding material conductive rubber according to claim 1, characterized in that: When degreasing the surface, the alkali used in the alkaline solution is NaOH or KOH, the concentration of the prepared alkaline solution is 2%, the temperature used is room temperature, the time is 5 minutes, the cleaning liquid used is deionized water, and the cleaning is carried out until neutral.