Multifunctional thermal insulation material and preparation method thereof
By combining rigid aerogel composite materials with flexible fiber materials and using perforated structure suture and fiber cloth to wrap, the existing insulation materials have been solved in aerospace vehicles with single insulation performance and poor assembly adaptability, and achieved the following: Efficient insulation performance and dynamic adjustment capabilities in large and complex spaces.
Patent Information
- Application Number
- CN202211204376.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-29
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2042-09-29
AI Technical Summary
The existing aerogel insulation materials have single thermal insulation performance in aerospace vehicles and poor assembly adaptability, so they cannot fully exert their thermal insulation performance, especially in large and complex spaces, which have poor thermal protection effects.
Using multi-functional thermal insulation material, the composite material formed can be improved on the basis of ensuring thermal insulation performance by combining rigid aerogel composite material with flexible fiber felt or fiber blanket. Assembly and dynamic adjustment.
It realizes a multifunctional thermal insulation material with excellent thermal insulation performance under 1200°C. It can be dynamically adjusted according to the gaps in the aircraft space structure, give full play to the thermal insulation performance, and is suitable for thermal insulation of large and complex aerospace vehicles.
Smart Images

Figure BDA0003873025870000161 
Figure BDA0003873025870000171
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of thermal insulation materials, and in particular to a multifunctional thermal insulation material and a preparation method thereof. Background Art
[0002] When an aerospace vehicle is flying in the atmosphere, due to intense aerodynamic heating, a large amount of heat is generated on its outer surface, which will be transferred into the cabin through the heat protection layer outside the vehicle, causing the temperature inside the cabin to rise, thereby threatening the safety of the cabin structure and equipment inside the cabin. Therefore, an insulation layer is generally required between the heat protection layer outside the aircraft and the cabin, between the cabin modules, and between the cabin and the equipment inside the cabin to prevent heat transfer.
[0003] Aerogel has great application prospects in the thermal protection system of aerospace vehicles due to its efficient thermal insulation performance. However, the commonly used aerogel thermal insulation materials have relatively single functions, poor assembly adaptability, and poor thermal insulation protection performance for large and complex spaces of aircraft. In view of this, it is necessary to study a new type of multifunctional thermal insulation material. Summary of the invention
[0004] The present invention provides a multifunctional thermal insulation material and a preparation method thereof. The thermal insulation material not only has good thermal insulation performance, but also has good compression performance, has good assembly adaptability to the thermal insulation space of an aircraft, and can be applied to thermal insulation protection of large and complex spaces.
[0005] In the first aspect, the present invention provides a multifunctional thermal insulation material, which includes a rigid thermal insulation material, a flexible thermal insulation material and a fiber cloth; the flexible thermal insulation material is located on the surface of the rigid thermal insulation material, and the fiber cloth is used to wrap the flexible thermal insulation material and the rigid thermal insulation material; the rigid thermal insulation material is provided with a perforated structure, and the fiber yarn is sewed and fixed together by the flexible thermal insulation material and the rigid thermal insulation material through the perforated structure.
[0006] Preferably, the rigid thermal insulation material is an aerogel composite material; the flexible thermal insulation material is a flexible fiber felt or a flexible fiber blanket; and the area of the flexible thermal insulation material is not less than the area of the rigid thermal insulation material.
[0007] More preferably, the flexible heat insulating material is at least one of cotton felt, needle felt or fiber blanket;
[0008] The density of the flexible thermal insulation material is 0.1 to 0.14 g / cm 3 .
[0009] Preferably, the rigid thermal insulation material is prepared by impregnating a fiber preform in a sol precursor, followed by aging, replacement and drying.
[0010] More preferably, the fiber preform is formed by needle punching; the density of the fiber preform is preferably 0.08-0.15 g / cm 3 .
[0011] More preferably, the fiber preform is formed from at least one of high silica fiber, quartz fiber, aluminum silicate fiber, alumina fiber or mullite fiber.
[0012] Preferably, the sol precursor comprises silica sol and a catalyst; the catalyst is at least one of hydrochloric acid, ammonia water or ammonium fluoride.
[0013] More preferably, the content of silicon dioxide in the silica sol is 5-40 wt %.
[0014] Preferably, the thickness of the rigid thermal insulation material is 5 to 25 mm; the thickness of the flexible thermal insulation material is 5 to 15 mm;
[0015] The surface density of the fiber cloth is 90-400 g / m 2 ; The thickness of the fiber cloth is 0.1 to 0.3 mm.
[0016] Preferably, the number of the perforated structures is not less than 4, and the perforated structures are evenly distributed on the rigid thermal insulation material.
[0017] More preferably, the perforated structures are distributed in equal proportions at edge positions of the rigid thermal insulation material.
[0018] More preferably, the aperture of the perforated structure is 1 to 2 mm.
[0019] More preferably, the flexible thermal insulation material is connected to at least one side of the rigid thermal insulation material.
[0020] The second aspect of the present invention provides a method for preparing the multifunctional thermal insulation material according to the first aspect, the method comprising the following steps:
[0021] (1) preparing a rigid thermal insulation material and a flexible thermal insulation material; and providing a perforated structure on the rigid thermal insulation material;
[0022] (2) sewing and fixing the flexible thermal insulation material and the rigid thermal insulation material together by passing the fiber yarn through the perforated structure to obtain a composite thermal insulation material;
[0023] (3) The composite thermal insulation material is wrapped with fiber cloth to obtain the multifunctional thermal insulation material.
[0024] Preferably, in step (3), after wrapping the composite thermal insulation material with fiber cloth, the method further includes the step of sewing with fiber yarn.
[0025] Preferably, the fiber yarn is at least one of quartz fiber yarn, mullite fiber yarn or alumina fiber yarn.
[0026] More preferably, the linear density of the fiber yarn is 150-250 tex; in step (3), the suture spacing is 10-30 mm.
[0027] Compared with the prior art, the present invention has at least the following beneficial effects:
[0028] (1) The present invention fixes a flexible thermal insulation material on the surface of a rigid thermal insulation material. The rigid aerogel composite material has good thermal insulation performance and good strength, while the flexible thermal insulation material has poor thermal insulation performance, but its strength is low and has good compression performance. The present invention fixes the two together by perforating and sewing. The two can complement each other and give full play to their respective advantages, so that the thermal insulation material prepared in the present invention not only has excellent thermal insulation performance, but also can be dynamically adjusted according to the spatial gap of thermal protection, and can be applied to the thermal insulation of large and complex surfaces;
[0029] (2) The thermal insulation material of the present invention has a relatively strong aerogel material inside and a relatively compressible flexible fiber felt or fiber blanket outside. The present invention creatively combines the two materials, which not only ensures that the thermal insulation material has good thermal insulation performance, but also makes the thermal insulation material have better assembly performance during thermal protection, and can also be dynamically adjusted according to the gaps in the spatial structure of the profile.
[0030] (3) The preparation method of the present invention is simple and suitable for large-scale industrial production. The thermal insulation material is light in weight and has a density of only 0.15 to 0.35 g / cm 3 The temperature resistance is as high as 1200℃, and it has great application prospects especially in the complex surface activity space of aerospace. DETAILED DESCRIPTION
[0031] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0032] The present invention provides a multifunctional thermal insulation material, which includes a rigid thermal insulation material, a flexible thermal insulation material and a fiber cloth; the flexible thermal insulation material is located on the surface of the rigid thermal insulation material, and the fiber cloth is used to wrap the flexible thermal insulation material and the rigid thermal insulation material; the rigid thermal insulation material is provided with a perforated structure, and the fiber yarn is passed through the perforated structure to sew and fix the flexible thermal insulation material and the rigid thermal insulation material together.
[0033] At present, most of the research on thermal insulation materials generally focuses on the thermal insulation performance of thermal insulation materials. Although the thermal insulation performance of thermal insulation materials can be greatly improved, the inventors found that the functionality of thermal insulation materials in the prior art is relatively single. When it is applied to the internal space of an aerospace vehicle for thermal insulation, the thermal insulation materials cannot have both good and excellent assembly and dynamic adjustability, which ultimately leads to the thermal insulation materials being unable to fully exert their thermal insulation performance, thereby achieving a thermal protection effect; therefore, the inventors creatively fix the rigid thermal insulation materials and the flexible thermal insulation materials through a perforated structure. The rigid materials have good thermal insulation performance and are more convenient to assemble, but their adaptability when used for thermal insulation protection of large composite spaces is poor. Although the thermal insulation performance and strength of the flexible thermal insulation materials are relatively poor, the rigid thermal insulation materials and the flexible thermal insulation materials can be combined to complement each other, not only to make the composite thermal insulation materials have good assembly performance, but also to dynamically adjust the gap in the internal space of the aerospace vehicle, so that the thermal insulation materials can fully exert their thermal insulation performance and still have excellent thermal insulation performance under 1200°C conditions.
[0034] According to some preferred embodiments, the rigid thermal insulation material is an aerogel composite material; the flexible thermal insulation material is a flexible fiber felt or a flexible fiber blanket; the area of the flexible thermal insulation material is not less than the area of the rigid thermal insulation material; the present invention adopts an aerogel composite material as a rigid thermal insulation material, which has excellent thermal insulation performance and a certain strength, so that the thermal insulation material has a certain dimensionality, and when the thermal insulation space of an aerospace vehicle is insulated, the thermal insulation material can be better assembled, but its spatial adaptability is poor; in the prior art, in order to pursue higher thermal insulation performance of thermal insulation materials, materials with better thermal insulation performance are generally combined, although the thermal insulation performance of the thermal insulation material can be improved However, when it is applied to the space of aerospace vehicles for thermal insulation, its thermal insulation performance cannot be fully exerted. The inventors, through a lot of creative work, combine flexible thermal insulation materials with relatively poor thermal insulation performance with rigid thermal insulation materials with good thermal insulation performance. The flexible thermal insulation material in the present invention is preferably a flexible fiber felt or fiber blanket. The fiber felt or fiber blanket has low strength but good compression performance. By adjusting the parameters of the flexible thermal insulation material, the thermal conductivity of the flexible thermal insulation material is reduced as much as possible while ensuring that the flexible thermal insulation material has good compression performance, so that the final thermal insulation material has good assembly and dynamic adjustability, so that the thermal insulation performance of the thermal insulation material can be maximized.
[0035] According to some preferred embodiments, the flexible thermal insulation material is at least one of cotton felt, needle felt or fiber blanket; it should be noted that the flexible thermal insulation material in the present invention is obtained by needle punching or wet forming of at least one of mullite fiber, quartz fiber, high silica fiber, aluminum silicate fiber or alumina fiber; preferably, the density of the flexible thermal insulation material mainly affects the thermal insulation performance and compression performance of the thermal insulation material, and the density of the flexible thermal insulation material in the present invention is 0.1-0.14 g / cm 3 (For example, it can be 0.1 g / cm 3 , 0.11g / cm 3 , 0.12g / cm 3 , 0.13g / cm 3 or 0.140.14g / cm 3); In the present invention, if the density of the flexible thermal insulation material is low, its structure is relatively loose, and the flexible thermal insulation material is prone to side heat leakage, resulting in poor thermal insulation performance. In addition, since the material is relatively soft when the density is low, it will have an adverse effect on the compression performance of the final thermal insulation material; if the density of the flexible thermal insulation material is high, the thermal insulation performance of the flexible thermal insulation material will also deteriorate. In addition, too high a density makes the material too dense, making it difficult to compress and the compression performance deteriorates. Too high or too low a density of the flexible thermal insulation material will affect the combination of the flexible material and the rigid material, which is not conducive to the full play of the two, and thus has an adverse effect on the comprehensive performance of the final thermal insulation material.
[0036] According to some preferred embodiments, the rigid thermal insulation material is prepared by impregnating a fiber preform in a sol precursor, and then aging, replacing and drying; in the present invention, the preparation of the rigid thermal insulation material can specifically adopt the following method, for example, first cutting the fiber preform to a target size and placing it in a molding mold, injecting the sol precursor into the mold by pressure injection, and impregnating the fiber preform for 5 to 20 minutes to obtain an impregnated body. In the present invention, it is preferred to impregnate the fiber preform by normal temperature pressure impregnation; then, the impregnated body is aged at room temperature (25 to 28°C) for 12 to 48 hours, and then placed in a solvent (for example, an ethanol solution with a mass concentration of 75%) for replacement 2 to 4 times, wherein the time for a single replacement is 5 to 10 days; after the replacement is completed, it is placed in a carbon dioxide medium for supercritical drying to finally obtain a rigid aerogel composite material.
[0037] According to some preferred embodiments, the fiber preform is formed by needle punching. In order to ensure the comprehensive performance of the rigid thermal insulation material, the density of the fiber preform in the present invention is preferably 0.08-0.15 g / cm 3 (For example, it can be 0.08 g / cm 3 , 0.09g / cm 3 , 0.10g / cm 3 , 0.11g / cm 3 , 0.12g / cm 3 , 0.13g / cm 3 , 0.14g / cm 3 or 0.15g / cm 3 ); when the density of the fiber preform is high, it will not only have an adverse effect on the thermal conductivity of the rigid thermal insulation material, but also be unfavorable for forming a lightweight thermal insulation material; when the density of the fiber preform is low, it will lead to poor mechanical properties of the rigid thermal insulation material. During the thermal protection process, the multifunctional thermal insulation material is prone to rupture, thereby affecting the thermal insulation performance.
[0038] According to some more preferred embodiments, the fiber preform in the present invention is formed from at least one of high-silica fiber, quartz fiber, aluminum silicate fiber, alumina fiber or mullite fiber. In the present invention, the fiber preform is preferably obtained by needle punching at least one of the above fibers, for example, it can be formed into a needle-punched felt or a fiber blanket.
[0039] According to some preferred embodiments, when preparing a rigid thermal insulation material, the sol precursor is firstly impregnated into the woven fiber preform by means of mold pressure injection to obtain an impregnated body; wherein the sol precursor preferably includes silica sol and a catalyst; wherein the mass ratio of silica sol to catalyst is 100:(2-10); the catalyst is at least one of hydrochloric acid, ammonia water or ammonium fluoride; using silica sol as the main component of the sol precursor can ensure that the prepared aerogel has a thick structure, good mechanical properties, and good temperature resistance; in the present invention, in order to ensure that the prepared aerogel thermal insulation material has good thermal insulation and mechanical properties, the content of silicon dioxide in the silica sol is preferably 5-40wt% (for example, it can be 5 wt%, 10wt%, 15wt%, 20wt%, 25wt%, 30wt%, 35wt% or 40wt%), more preferably, the content of silicon dioxide in the silica sol is 20-35wt%; it should be noted that the percentages in the present invention are all expressed in mass percentage; in the present invention, when the content of silicon dioxide in the silica sol is low, the thermal insulation performance and mechanical properties of the rigid thermal insulation material will be poor, but when the content of silicon dioxide in the silica sol exceeds a certain range, continuing to increase will also reduce the thermal insulation performance of the rigid thermal insulation material, and will cause the density of the rigid thermal insulation material to be larger, which is not conducive to obtaining a lightweight multifunctional thermal insulation material, and will cause the rigid thermal insulation material to be easily powdered when combined with the flexible material.
[0040] According to some preferred embodiments, the rigid thermal insulation material described in the present invention is obtained by mold forming or by mold forming followed by mechanical processing. More preferably, the thickness of the rigid thermal insulation material is 5 to 25 mm (for example, it can be 5 mm, 10 mm, 15 mm, 20 mm or 25 mm); the thickness of the flexible thermal insulation material is 5 to 15 mm (for example, it can be 5 mm, 6 mm, 7 mm, 8 mm, 9 mm, 10 mm, 12 mm, 13 mm or 15 mm); in the present invention, by further limiting the thickness of the rigid thermal insulation material and the flexible thermal insulation material, it can be ensured that the prepared multifunctional thermal insulation material has a lower thermal conductivity and has excellent assembly and dynamic adjustability; if the thickness of the rigid thermal insulation material and the flexible thermal insulation material is lower or higher than the range in the present invention, not only will the rigid thermal insulation material and the flexible thermal insulation material be unable to better play a synergistic role, but the comprehensive performance of the thermal insulation material finally prepared will also deteriorate. , and it will also increase the difficulty of combining the two; it should be noted that, in the present invention, the thickness ratio of the rigid thermal insulation material and the flexible thermal insulation material is preferably (5-25): (5-15). In actual application, the thickness ratio of the rigid thermal insulation material and the flexible thermal insulation material can be selected and adjusted according to the needs of use. For example, when the aircraft space structure is relatively complex and the compressibility of the thermal insulation material is required to be high, the thickness ratio of the rigid thermal insulation material and the flexible thermal insulation material is preferably (5-15): (10-15). Under this ratio, the thermal insulation material can dynamically adjust the gap between the aircraft components, so that it can give full play to its thermal insulation performance; for example, when the aircraft space structure is relatively simple and the thermal insulation performance of the thermal insulation material is required to be high, the thickness ratio of the rigid material and the flexible material is preferably (15-25): (5-10). Under this ratio, the thermal insulation material can be more easily assembled, the gap between the aircraft components can be fine-tuned, and it is not easy to have the risk of heat leakage, and the thermal insulation performance is better.
[0041] According to some preferred embodiments, the surface density of the fiber cloth is 90 to 400 g / m 2 (For example, it can be 90g / m 2 , 100g / m 2 , 150g / m 2 , 200g / m 2 , 250g / m 2 , 300g / m 2 , 350g / m 2 or 400g / m 2); the thickness of the fiber cloth is 0.1-0.3 mm (for example, it can be 0.1 mm, 0.15 mm, 0.2 mm, 0.25 mm or 0.3 mm); after the rigid thermal insulation material and the flexible thermal insulation material are fixed, in order to further improve the firmness of the two, so that the two are not easily separated during use and the thermal insulation material is not worn, the present invention also uses a fiber cloth with certain parameters to wrap the rigid thermal insulation material and the flexible thermal insulation material. The fiber cloth not only has certain thermal insulation performance and mechanical strength, but is also relatively soft, and can better fix the rigid thermal insulation material and the flexible thermal insulation material together to prevent the composite material from being dislocated or powdering during use; it should be noted that in the present invention, The linear density of the fiber yarn used to prepare the fiber cloth is 30-50 tex (for example, it can be 30, 35, 40, 45 or 50 tex), and the twist of the fiber yarn is 50-80 tex / m (for example, it can be 50, 55, 60, 65, 70, 75 or 80 tex / m); when preparing the fiber cloth, the greater the linear density of the fiber yarn used, the thicker the prepared fiber cloth is. At the same time, within a certain range, the greater the twist of the fiber yarn, the greater the yarn strength, and the better the mechanical strength of the prepared fiber cloth. However, when it exceeds a certain range, the softness of the fiber cloth will be reduced. In the present invention, the linear density and / or twist of the fiber yarn can be adjusted to prepare fiber cloths with different thicknesses, surface densities and strengths within the above range.
[0042] According to some preferred embodiments, in order to ensure that the thermal insulation material has good thermal insulation performance and to fix the rigid thermal insulation material and the flexible thermal insulation material together, the number of the perforated structures in the present invention is not less than 4 (for example, it can be 4, 5 or 6), and the perforated structures are evenly distributed on the rigid thermal insulation material, and then the rigid thermal insulation material and the flexible thermal insulation material are sewn together with fiber yarn; it should be noted that the distribution of the perforated structures in the present invention on the rigid thermal insulation material must be able to meet the fixation requirements of the rigid thermal insulation material. Since the perforated structure will increase the risk of heat leakage of the rigid thermal insulation material to a certain extent, the number of perforated structures in the present invention is preferably 4; more preferably, when the perforated structure is set at the edge of the rigid thermal insulation material, the adverse effect of the perforated structure on the thermal insulation performance of the rigid thermal insulation material can be avoided to the greatest extent. Therefore, in the present invention, it is preferred to set the perforated structure at the edge of the rigid thermal insulation material, and at the same time in order to meet the better fixation requirements. According to the requirements, the perforated structure is preferably distributed in equal proportion at the edge of the rigid thermal insulation material, and the distance between the perforated structure and the edge is not less than 1 cm; for example, when the rigid thermal insulation material is square or rectangular, holes can be punched at the four corners of the rigid thermal insulation material; when the rigid thermal insulation material is circular, holes can be evenly punched at the edge of the rigid thermal insulation material to fix the rigid thermal insulation material and the flexible thermal insulation material; at the same time, in the present invention, according to some preferred embodiments, the aperture of the perforated structure is 1 to 2 mm (for example, it can be 1 mm, 1.2 mm, 1.5 mm, 1.8 mm or 2 mm). If the aperture of the perforated structure is too large, it will not only have an adverse effect on the thermal insulation performance of the rigid thermal insulation material, but also cause the fixing effect between the rigid thermal insulation material and the flexible thermal insulation material to deteriorate. If the aperture of the perforated structure is too small, it will be not conducive to the perforation and suturing of the fiber yarn, resulting in poor operability. It should be noted that the perforated structure in the present invention can be specifically obtained by processing using a CNC machine tool.
[0043] According to some more preferred embodiments, the flexible thermal insulation material is connected to at least one side of the rigid thermal insulation material. For example, the flexible thermal insulation material can be placed on one side of the rigid thermal insulation material, and the rigid thermal insulation material and the flexible thermal insulation material can be fixed together by perforating and sewing with fiber yarns. For example, two flexible thermal insulation materials can be placed on the upper and lower sides of the rigid thermal insulation material respectively, and perforated and sewn with fiber yarns for fixation. For another example, a flexible thermal insulation material with a larger area can be used to wrap the rigid thermal insulation material, and then the fiber yarns are sewn and fixed. At this time, the area of the flexible thermal insulation material is slightly larger than twice the area of the rigid thermal insulation material. In the present invention, the placement method of the flexible thermal insulation material can be selected according to the actual demand for the comprehensive performance of the multifunctional thermal insulation material during use.
[0044] The present invention also provides a method for preparing the multifunctional thermal insulation material according to the first aspect, the method comprising the following steps:
[0045] (1) preparing a rigid thermal insulation material and a flexible thermal insulation material; providing a perforated structure on the rigid thermal insulation material; for example, a CNC machine tool may be used to punch holes on the rigid thermal insulation material;
[0046] (2) using fiber yarn to sew and fix the flexible thermal insulation material and the rigid thermal insulation material together through the perforated structure to obtain a composite thermal insulation material;
[0047] (3) The composite thermal insulation material is wrapped with fiber cloth to obtain the multifunctional thermal insulation material.
[0048] According to some preferred embodiments, in step (3), in order to further improve the fixing effect between the composite materials and prevent the composite thermal insulation material from powdering, the present invention further includes the step of sewing with fiber yarn after wrapping the composite thermal insulation material with fiber cloth; in the present invention, the fiber yarn used when the rigid thermal insulation material and the flexible thermal insulation material are fixed and when the fiber cloth is sewn is at least one of quartz fiber yarn, mullite fiber yarn or alumina fiber yarn; according to some preferred embodiments, the linear density of the fiber yarn is 150-250tex (for example, it can be 150tex, 160tex, 180tex, 200tex, 220tex or 250tex); at the same time, when the composite thermal insulation material is wrapped and sewn with fiber cloth, the sewing spacing is preferably 10-30mm (for example, it can be 10mm, 15mm, 20mm, 25mm or 30mm). The sewing spacing within the scope of the present invention can ensure that the material after sewing and fixing has overall mechanical properties and strain adaptability.
[0049] The multifunctional thermal insulation material prepared in the present invention has a low density of only 0.15 to 0.35 g / cm 3 The thermal conductivity at room temperature is 0.024-0.029 W / m·K, with good compression performance. The compressive strength is 0.005-0.2 MPa at 10% compression. It can withstand a maximum temperature of 1200°C. When used for space insulation of large and complex aerospace vehicles, it not only has good assembly properties, but also can dynamically adjust the space gaps of aircraft components, thereby maximizing the thermal insulation performance of the multifunctional thermal insulation material.
[0050] In order to more clearly illustrate the technical solution and advantages of the present invention, a multifunctional thermal insulation material and a preparation method thereof are described in detail below through several embodiments.
[0051] Embodiment 1:
[0052] (1) Preparation of rigid thermal insulation materials;
[0053] The fiber preform (mullite fiber felt) is prepared by needle punching mullite fiber, wherein the density of the fiber preform is 0.10 g / cm 3 The fiber preform is cut into a size of 350*350*23mm, placed in a mold of 380*380*20mm, and the sol precursor is placed in the mold by pressure injection to impregnate the fiber preform for 20 minutes; the sol precursor includes silica sol and catalyst (hydrochloric acid) (mass ratio is 100:5), and the content of silicon dioxide in the silica sol is 25wt% (mass percentage), and then the aerogel composite material is prepared after aging, replacement and drying in sequence; the aerogel composite material is processed to have a thickness of 15mm;
[0054] Using a CNC machine tool, four holes were punched at the four edge positions of the aerogel composite material to obtain four perforated structures; wherein the aperture of the perforated structure was 1.5 mm;
[0055] Preparation of flexible thermal insulation material; forming quartz needle felt by needle punching quartz fiber, the density of which is 0.1 g / cm 3 , thickness is 5mm;
[0056] (2) placing a flexible thermal insulation material on the upper surface of a rigid thermal insulation material, and fixing the rigid thermal insulation material and the flexible thermal insulation material by perforating and sewing using quartz fiber yarn with a linear density of 190 tex to obtain a composite thermal insulation material;
[0057] (3) The composite thermal insulation material is wrapped with a quartz fiber cloth having a thickness of 0.1 mm and sewed with a quartz fiber yarn having a linear density of 190 tex, with a sew interval of 20 mm, to obtain a multifunctional thermal insulation material.
[0058] Embodiment 2:
[0059] (1) Preparation of rigid thermal insulation materials;
[0060] The fiber preform (mullite fiber felt) is prepared by needle punching mullite fiber, wherein the density of the fiber preform is 0.10 g / cm 3The fiber preform is cut into a size of 350*350*23mm, placed in a mold of 380*380*20mm, and the sol precursor is placed in the mold by pressure injection to impregnate the fiber preform for 20 minutes; the sol precursor includes silica sol and catalyst (ammonium fluoride) (mass ratio is 100:5), and the content of silicon dioxide in the silica sol is 20wt% (mass percentage), and then the aerogel composite material is prepared after aging, replacement and drying in sequence; the aerogel composite material is processed to have a thickness of 15mm;
[0061] A CNC machine tool was used to punch holes at four edge positions of the aerogel composite material to obtain four perforated structures, wherein the aperture of the perforated structure was 1 mm;
[0062] Prepare flexible thermal insulation material; needle-punch the mullite fiber into a mullite fiber needle-punched felt, the density of the mullite fiber needle-punched felt is 0.1g / cm 3 , thickness is 5mm;
[0063] (2) placing a flexible thermal insulation material on the upper surface of a rigid thermal insulation material, and fixing the rigid thermal insulation material and the flexible thermal insulation material by perforating and sewing using quartz fiber yarn with a linear density of 230 tex to obtain a composite thermal insulation material;
[0064] (3) The composite thermal insulation material is wrapped with a quartz fiber cloth having a thickness of 0.2 mm and sewed with a quartz fiber yarn having a linear density of 230 tex, with a sew interval of 15 mm, to obtain a multifunctional thermal insulation material.
[0065] Embodiment 3:
[0066] (1) Preparation of rigid thermal insulation materials;
[0067] The fiber preform (mullite fiber felt) is prepared by needle punching mullite fiber, wherein the density of the fiber preform is 0.11 g / cm 3 The fiber preform is cut into a size of 350*350*23mm, placed in a mold of 380*380*20mm, and the sol precursor is placed in the mold by pressure injection to impregnate the fiber preform for 20 minutes; the sol precursor includes silica sol and catalyst (hydrochloric acid) (mass ratio is 100:5), and the content of silicon dioxide in the silica sol is 30wt% (mass percentage), and then the aerogel composite material is prepared after aging, replacement and drying in sequence; the aerogel composite material is processed to have a thickness of 15mm;
[0068] A CNC machine tool was used to punch holes at four edge positions of the aerogel composite material to obtain four perforated structures; the aperture of the perforated structure was 1.6 mm;
[0069] Prepare flexible thermal insulation material; needle-punch high-silica fiber into high-silica fiber needle-punched felt, the density of which is 0.12 g / cm 3 , thickness is 5mm;
[0070] (2) placing a flexible thermal insulation material on the upper surface of a rigid thermal insulation material, and fixing the rigid thermal insulation material and the flexible thermal insulation material by perforating and sewing using a mullite fiber yarn with a linear density of 250 tex to obtain a composite thermal insulation material;
[0071] (3) The composite thermal insulation material is wrapped with a quartz fiber cloth with a thickness of 0.2 mm, and is sewed with a mullite fiber yarn with a linear density of 250 tex, with a sew interval of 20 mm, to obtain a multifunctional thermal insulation material.
[0072] Embodiment 4:
[0073] (1) Preparation of rigid thermal insulation materials;
[0074] The fiber preform (mullite fiber felt) is prepared by needle punching of mullite fiber, wherein the density of the fiber preform is 0.13 g / cm 3 The fiber preform is cut into a size of 350*350*22mm, placed in a mold of 380*380*20mm, and the sol precursor is placed in the mold by pressure injection to impregnate the fiber preform for 20 minutes; the sol precursor includes silica sol and catalyst (hydrochloric acid) (mass ratio is 100:5), and the content of silicon dioxide in the silica sol is 35wt% (mass percentage), and then the aerogel composite material is prepared after aging, replacement and drying; the aerogel composite material is processed to have a thickness of 10mm; a CNC machine tool is used to punch holes at four edge positions of the aerogel composite material to obtain 4 perforated structures; wherein the aperture of the perforated structure is 1mm;
[0075] Preparation of flexible thermal insulation material; forming quartz fiber needle-punched felt by needle-punching quartz fiber, wherein the density of the quartz fiber needle-punched felt is 0.14 g / cm 3 , thickness is 10mm;
[0076] (2) placing a flexible thermal insulation material on the upper surface of a rigid thermal insulation material, and fixing the rigid thermal insulation material and the flexible thermal insulation material by perforating and sewing using alumina fiber yarn with a linear density of 180 tex to obtain a composite thermal insulation material;
[0077] (3) The composite thermal insulation material is wrapped with a quartz fiber cloth with a thickness of 0.15 mm and sewed with a mullite fiber yarn with a linear density of 180 tex, with a sew interval of 30 mm, to obtain a multifunctional thermal insulation material.
[0078] Embodiment 5:
[0079] (1) Preparation of rigid thermal insulation materials;
[0080] The fiber preform (mullite fiber felt) is prepared by needle punching mullite fiber, wherein the density of the fiber preform is 0.11 g / cm 3 The fiber preform is cut into a size of 350*350*6mm, placed in a mold of 380*380*5mm, and the sol precursor is placed in the mold by pressure injection to impregnate the fiber preform for 20 minutes; the sol precursor includes silica sol and catalyst (hydrochloric acid) (mass ratio is 100:5), the content of silicon dioxide in the silica sol is 25wt% (mass percentage), and then the aerogel composite material is prepared after aging, replacement and drying; the thickness of the aerogel composite material is 5mm; a CNC machine tool is used to punch holes at four edge positions of the aerogel composite material to obtain 4 perforated structures; wherein the aperture of the perforated structure is 1.2mm;
[0081] Prepare flexible thermal insulation material; needle-punch quartz fiber into quartz fiber needle-punched felt, the density of quartz fiber needle-punched felt is 0.15g / cm 3 , thickness is 15mm;
[0082] (2) placing a flexible thermal insulation material on the upper surface of a rigid thermal insulation material, and fixing the rigid thermal insulation material and the flexible thermal insulation material by perforating and sewing using a mullite fiber yarn with a linear density of 150 tex to obtain a composite thermal insulation material;
[0083] (3) The composite thermal insulation material is wrapped with a quartz fiber cloth with a thickness of 0.3 mm, and is sewed with a mullite fiber yarn with a linear density of 150 tex, with a sew interval of 25 mm, to obtain a multifunctional thermal insulation material.
[0084] Embodiment 6:
[0085] Example 6 is basically the same as Example 1, except that: in step (1), a fiber preform (quartz fiber felt) is prepared by needle punching quartz fiber, wherein the density of the fiber preform is 0.10 g / cm 3 .
[0086] Embodiment 7:
[0087] Example 7 is basically the same as Example 1, except that in step (3), 0.1 mm mullite fiber cloth is used to wrap the composite thermal insulation material.
[0088] Embodiment 8:
[0089] Example 8 is basically the same as Example 1, except that in step (1), the perforated structures are evenly distributed on the entire surface of the aerogel composite material, the interval between adjacent perforated structures is 20 mm, and the pore diameter is 1.5 mm.
[0090] Embodiment 9:
[0091] Example 9 is basically the same as Example 1, except that: in step (1), the perforated structures are randomly distributed on the aerogel composite material (non-edge area), and the number of perforated structures is 4.
[0092] Embodiment 10:
[0093] Example 10 is substantially the same as Example 1, except that in step (1), in the sol precursor, the content of silicon dioxide in the silica sol is 50 wt %.
[0094] Embodiment 11:
[0095] Example 11 is basically the same as Example 1, except that in step (1), the thickness of the rigid insulation material is 35 mm, and the thickness of the flexible insulation material is 3 mm.
[0096] Comparative Example 1:
[0097] (1) Preparation of rigid thermal insulation materials;
[0098] The fiber preform (mullite fiber felt) is prepared by needle punching mullite fiber, wherein the density of the fiber preform is 0.10 g / cm 3 The fiber preform is cut into a size of 350*350*23mm, placed in a mold of 380*380*20mm, and the sol precursor is placed in the mold to impregnate the fiber preform by pressure injection; the sol precursor includes silica sol and catalyst (hydrochloric acid) (mass ratio is 100:5), the content of silicon dioxide in the silica sol is 20wt% (mass percentage), and then the aerogel composite material is prepared after aging, replacement and drying in sequence; the thickness of the aerogel composite material is 20mm;
[0099] (2) The rigid thermal insulation material is wrapped with a quartz fiber cloth having a thickness of 0.1 mm and sewed with a quartz fiber yarn having a linear density of 190 tex at a sew interval of 20 mm to obtain a thermal insulation material.
[0100] Comparative Example 2:
[0101] Comparative Example 2 is substantially the same as Comparative Example 1, except that in step (1), a fiber preform (quartz fiber felt) is prepared by needle punching quartz fiber.
[0102] Comparative Example 3:
[0103] (1) Preparing a flexible thermal insulation material; needle-punching quartz fibers into quartz needle-punched felt, wherein the density of the quartz needle-punched felt is 0.1 g / cm 3 , thickness is 20mm;
[0104] (2) The flexible thermal insulation material is wrapped with a quartz fiber cloth having a thickness of 0.1 mm, and is sewed with a quartz fiber yarn having a linear density of 190 tex, with a sew interval of 20 mm, to obtain a thermal insulation material.
[0105] Comparative Example 4:
[0106] Comparative Example 4 is substantially the same as Comparative Example 3, except that in step (1), mullite fiber is needle-punched to form mullite fiber felt.
[0107] Comparative Example 5:
[0108] Comparative Example 5 is substantially the same as Comparative Example 3, except that in step (1), high-silica fiber is needle-punched to form high-silica fiber felt.
[0109] Comparative Example 6:
[0110] Comparative Example 6 is basically the same as Example 1, except that: in step (1), the quartz needle felt in step (1) is replaced by a fiber fabric woven from quartz fibers, the thickness of the fiber fabric is 5 mm, and the density is 1.3 g / cm 3 .
[0111] Comparative Example 7:
[0112] (1) Preparation of flexible aerogel composite material: A fiber preform (mullite fiber felt) was prepared by needle punching mullite fiber, wherein the density of the fiber preform was 0.10 g / cm 3 The fiber preform is cut into a size of 350*350*17mm, placed in a mold of 380*380*15mm, and the sol precursor is placed in the mold to impregnate the fiber preform by pressure injection; the sol precursor is tetraethyl orthosilicate, and then the aerogel composite material is prepared after aging, replacement and drying in sequence; the thickness of the aerogel composite material is 15mm;
[0113] Preparation of flexible thermal insulation material; forming quartz needle felt by needle punching quartz fiber, the density of which is 0.1 g / cm 3 , thickness is 5mm;
[0114] (2) placing a flexible thermal insulation material on the upper surface of the aerogel composite material, and fixing the aerogel composite material and the flexible thermal insulation material by perforating and sewing using quartz fiber yarn with a linear density of 190 tex to obtain a composite thermal insulation material;
[0115] (3) The composite thermal insulation material is wrapped with a quartz fiber cloth having a thickness of 0.1 mm, and is sewed with a quartz fiber yarn having a linear density of 190 tex, with a sew interval of 20 mm, to obtain a thermal insulation material.
[0116] Comparative Example 8:
[0117] (1) Preparation of rigid thermal insulation materials;
[0118] The fiber preform (mullite fiber felt) is prepared by needle punching mullite fiber, wherein the density of the fiber preform is 0.10 g / cm 3 The fiber preform is cut into a size of 350*350*23mm, placed in a mold of 380*380*20mm, and the sol precursor is placed in the mold to impregnate the fiber preform by pressure injection; the sol precursor includes silica sol and catalyst (hydrochloric acid) (mass ratio is 100:5), the content of silicon dioxide in the silica sol is 25wt% (mass percentage), and then the aerogel composite material is prepared after aging, replacement and drying; the aerogel composite material is processed to have a thickness of 15mm; a CNC machine tool is used to punch holes at four edge positions of the aerogel composite material to obtain four perforated structures; wherein the aperture of the perforated structure is 1.5mm;
[0119] Preparation of flexible aerogel composite materials: A fiber preform (mullite fiber felt) was prepared by needle punching mullite fiber, wherein the density of the fiber preform was 0.10 g / cm 3 The fiber preform is cut into a size of 350*350*6mm, placed in a mold of 380*380*5mm, and the sol precursor is placed in the mold to impregnate the fiber preform by pressure injection; the sol precursor is ethyl orthosilicate, and then an aerogel composite material is prepared after aging, replacement and drying in sequence; the thickness of the aerogel composite material is 5mm;
[0120] (2) placing the aerogel composite material on the upper surface of the rigid thermal insulation material, and fixing the aerogel composite material and the flexible thermal insulation material by perforating and sewing with quartz fiber yarn with a linear density of 190 tex to obtain a composite thermal insulation material;
[0121] (3) The composite thermal insulation material is wrapped with a quartz fiber cloth having a thickness of 0.1 mm and sewed with a quartz fiber yarn having a linear density of 190 tex, with a sew interval of 20 mm, to obtain a multifunctional thermal insulation material.
[0122] Comparative Example 9:
[0123] Comparative Example 9 is substantially the same as Example 1, except that in step (1), quartz needle felt is used instead of the aerogel composite material, that is, the composite thermal insulation material is composed of two layers of flexible thermal insulation materials.
[0124] Comparative Example 10:
[0125] Comparative Example 10 is substantially the same as Example 1, except that in step (1), an aerogel composite material is used instead of the quartz fiber felt, that is, the composite thermal insulation material is composed of two layers of rigid thermal insulation materials.
[0126] The thermal insulation materials prepared in Examples 1 to 11 and Comparative Examples 1 to 10 were subjected to performance tests. The specific test methods are as follows. The test results are shown in Table 1:
[0127] Density test: refer to GB / T 6343-2009 "Determination of apparent density of foam plastics and rubber";
[0128] 10% compression strength test: The compression performance test of the thermal insulation materials in the embodiments and comparative examples was carried out using a Xinsansi microcomputer-controlled electronic universal testing machine;
[0129] Thermal conductivity test at room temperature: refer to GB / T 10295-2008 "Determination of steady-state thermal resistance and related properties of insulation materials-Heat flow meter method".
[0130] Table 1
[0131]
[0132]
[0133] As can be seen from Table 1, the thermal insulation material prepared in the present invention is a multifunctional composite material, which has a low thermal conductivity and good thermal insulation performance. Moreover, after being compressed by 10%, it still has good compression strength. Therefore, when the multifunctional thermal insulation material in the present invention is used to insulate the space of aerospace vehicles, since the rigid thermal insulation material can provide a certain strength, the thermal insulation material has good assembly adaptability. At the same time, the flexible thermal insulation material gives the multifunctional thermal insulation material good compression performance, so that the thermal insulation material can dynamically adjust the gap when insulating a complex space, thereby ensuring that the thermal insulation material fully exerts its thermal insulation performance.
[0134] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A multifunctional thermal insulation material, characterized in that: It comprises a rigid thermal insulation material, a flexible thermal insulation material and a fiber cloth; the flexible thermal insulation material is located on the surface of the rigid thermal insulation material, and the fiber cloth is used to wrap the flexible thermal insulation material and the rigid thermal insulation material; a perforated structure is provided on the rigid thermal insulation material, and fiber yarns sew and fix the flexible thermal insulation material and the rigid thermal insulation material together through the perforated structure; the rigid thermal insulation material is an aerogel composite material; The rigid thermal insulation material is prepared by impregnating a fiber preform in a sol precursor, and then aging, replacing and drying the sol precursor; the sol precursor includes silica sol and a catalyst; the content of silicon dioxide in the silica sol is 5-40wt%; The thickness of the rigid thermal insulation material is 5~25mm; the thickness of the flexible thermal insulation material is 5~15mm; the number of the perforated structures is not less than 4, and the perforated structures are evenly distributed on the rigid thermal insulation material; the perforated structures are distributed in equal proportions at the edge positions of the rigid thermal insulation material; the aperture of the perforated structure is 1~2mm.
2. The multifunctional thermal insulation material according to claim 1, characterized in that: The flexible thermal insulation material is a flexible fiber felt or a flexible fiber blanket; the area of the flexible thermal insulation material is not less than the area of the rigid thermal insulation material.
3. The multifunctional thermal insulation material according to claim 2, characterized in that: The flexible thermal insulation material is at least one of cotton felt, needle felt or fiber blanket; the density of the flexible thermal insulation material is 0.1-0.14 g / cm 3 .
4. The multifunctional thermal insulation material according to claim 1, characterized in that: The fiber preform is formed by needle punching; the density of the fiber preform is 0.08-0.15 g / cm 3 The fiber preform is formed from at least one of high silica fiber, quartz fiber, aluminum silicate fiber, alumina fiber or mullite fiber.
5. The multifunctional thermal insulation material according to claim 4, characterized in that: The catalyst is at least one of hydrochloric acid, ammonia water or ammonium fluoride.
6. The multifunctional thermal insulation material according to claim 1, characterized in that: The surface density of the fiber cloth is 90-400 g / m 2 ; The thickness of the fiber cloth is 0.1~0.3mm.
7. The multifunctional thermal insulation material according to claim 1, characterized in that: The flexible thermal insulation material is connected to at least one side of the rigid thermal insulation material.
8. A method for preparing a multifunctional thermal insulation material according to any one of claims 1 to 7, characterized in that: The preparation method comprises the following steps: (1) Preparing a rigid thermal insulation material and a flexible thermal insulation material; and providing a perforated structure on the rigid thermal insulation material; (2) sewing and fixing the flexible thermal insulation material and the rigid thermal insulation material together by passing the fiber yarn through the perforated structure to obtain a composite thermal insulation material; (3) Wrapping the composite thermal insulation material with fiber cloth to obtain the multifunctional thermal insulation material.
9. The preparation method according to claim 8, characterized in that: In step (3), after wrapping the composite thermal insulation material with fiber cloth, the method further includes the step of sewing with fiber yarn.
10. The preparation method according to claim 8, characterized in that: The fiber yarn is at least one of quartz fiber yarn, mullite fiber yarn or alumina fiber yarn; the linear density of the fiber yarn is 150-250 tex; in step (3), the suture spacing is 10-30 mm.