A phosphorus diffusion source and preparation method thereof
The phosphorus diffusion source is prepared through a combination of silicate, water, acids, low-carbon alcohols and ether solvents, which solves the problems of uneven diffusion and short storage time of existing phosphorus diffusion sources, achieves efficient uniform diffusion and long-term storage, and improves Improve electronic component performance and production safety.
Patent Information
- Application Number
- CN202211252873.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-13
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2042-10-13
AI Technical Summary
Existing phosphorus diffusion sources diffuse unevenly after extended storage time, resulting in reduced performance of diodes and high-power electronic components. The production process is demanding and highly toxic.
Phosphorus diffusion sources are prepared using silicate, water, acids, low-carbon alcohols and ether solvents. The phosphorus sources are evenly dispersed through the sol-gel method to form a low-viscosity latex, which extends the storage time and improves diffusion uniformity.
It achieves uniform diffusion of the phosphorus diffusion source on the silicon wafer after 12 months of storage, extending the storage time, reducing production costs, and improving the performance of electronic components.
Smart Images

Figure BDA0003888573160000061 
Figure BDA0003888573160000071 
Figure BDA0003888573160000081
Abstract
Description
Technical Field
[0001] The present application relates to the field of microelectronics industry, and more specifically to a phosphorus diffusion source and a preparation method thereof. Background Art
[0002] Diffusion source is an indispensable microelectronic chemical in the production of semiconductor devices. Diffusion sources can be divided into two categories according to different diffusion types: one is P-type diffusion source, which forms P-type semiconductor materials, mainly III-group elements, mainly boron and aluminum; the other is N-type diffusion source, which forms N-type semiconductor materials, mainly V-group elements, mainly phosphorus, also called phosphorus diffusion source.
[0003] Phosphorus diffusion sources are widely used in the production of diodes and high-power electronic components. Phosphorus is doped into the lattice of single-crystalline silicon through phosphorus diffusion sources. Phosphorus diffusion sources can greatly improve the performance of diodes and high-power electronic components, simplify the production process of electronic components, and reduce production costs.
[0004] At present, the existing phosphorus diffusion source is to dope phosphorus into single crystal silicon using phosphorus oxychloride. Since phosphorus oxychloride is highly toxic, the production process conditions of the phosphorus diffusion source are relatively high. Moreover, the existing phosphorus diffusion source is used in the production of diodes and high-power electronic components. Due to the uneven diffusion, the performance of the diodes and high-power electronic components is reduced. In addition, as the storage time increases, particles are gradually generated in the existing phosphorus diffusion source and continue to increase, and the viscosity of the phosphorus diffusion source is gradually increased. When the phosphorus diffusion source with a long storage time is used in the preparation of diodes and high-power electronic components, the phosphorus diffusion source cannot be effectively diffused and is unevenly distributed, thereby weakening the performance of the diodes and high-power electronic components. Summary of the invention
[0005] In order to improve the diffusion uniformity of a phosphorus diffusion source and prolong the storage time of the phosphorus diffusion source, the present application provides a phosphorus diffusion source and a preparation method thereof.
[0006] In a first aspect, the present application provides a phosphorus diffusion source, which comprises, by weight percentage, 15-45% silicate, 2-8% water, 0.01-1% acid, 25-50% low-carbon alcohol, 15-45% ether solvent, and 5-20% phosphorus source.
[0007] In the present application, a phosphorus diffusion source is prepared by using silicate by sol-gel method, so that the phosphorus source can be evenly dispersed in the latex, and the latex has good film-forming property and fluidity. In the present application, a phosphorus diffusion source is prepared under the action of silicate, water, acid, low-carbon alcohol and ether solvent.
[0008] At 12 months, the viscosity of the obtained phosphorus diffusion source was less than 2.3cp. At the same time, the number of fine particles in the phosphorus diffusion source was small, with the number of particles ≥0.5μm being less than 56 / mL, the number of particles ≥1.0μm being less than 2.7 / mL, and the number of particles ≥5.0μm being less than 1.9 / mL.
[0009] The phosphorus diffusion source stored for 12 months is evenly coated on the surface of the silicon wafer for preparing electronic components. Under high-temperature diffusion, the phosphorus diffusion source can form a pure substance of elemental phosphorus, which gradually diffuses into the interior of the silicon wafer, so that the square resistance and junction depth of the silicon wafer have a small difference in their respective values. In other words, the phosphorus diffusion source after storage for 12 months still has good diffusion uniformity, diffuses more evenly in the silicon wafer, and has less impact on the performance of diodes and high-power electronic components.
[0010] Preferably, the phosphorus diffusion source contains 15-35% silicate, 2-5% water, 0.01-0.1% acid, 25-35% low-carbon alcohol, 15-35% ether solvent and 5-15% phosphorus source.
[0011] More preferably, the silicate is 19.68%, the water is 2.92%, the acid is 0.03%, the low-carbon alcohol is 32.3%, the ether solvent is 32.96%, and the phosphorus source is 12.11%.
[0012] In one embodiment, the silicate is methyl orthosilicate, tetraethyl orthosilicate or diethyl orthosilicate.
[0013] Preferably, the silicate is tetraethyl orthosilicate.
[0014] In the present application, silicate, as the main substance of the latex, undergoes hydrolysis and polycondensation reaction with water to gradually form a uniform sol liquid. Water is both a reactant in the hydrolysis process and a product of the polycondensation reaction, so the water content has a great influence on the entire hydrolysis and polycondensation process. When the amount of water is greater than 8%, the excess water will suppress the progress of hydrolysis, resulting in incomplete hydrolysis; when the amount of water is less than 2%, the amount of water is too little, the hydrolysis process is relatively slow, and the time of the hydrolysis and polycondensation reaction is prolonged. At the same time, when the amount of water is less than 2%, the effect of forming a sol liquid is poor.
[0015] In one embodiment, the acid is hydrochloric acid, acetic acid or sulfuric acid.
[0016] Preferably, the acid is hydrochloric acid.
[0017] In the present application, acids are added to the phosphorus diffusion source as auxiliary agents, and the acids can catalyze the hydrolysis and polycondensation process of silicate. At the same time, the acids can reduce the number of spheres formed by cross-linking reactions during the reaction process, avoid the occurrence of agglomeration, improve the diffusion uniformity of the phosphorus diffusion source, and extend the storage time of the phosphorus diffusion source.
[0018] When the amount of acid is less than 0.01%, the addition of a small amount of acid is not enough to affect the hydrolysis reaction of silicate, and the addition of a small amount of acid may lead to reaction unevenness; when the acid is greater than 0.1%, the excess acid will accelerate the cross-linking polymerization reaction between the hydrolysis products of silicate, accelerate the gelation process, and cause the electrical properties of the phosphorus diffusion source to deteriorate.
[0019] In one embodiment, the ether solvent is selected from ethylene glycol monomethyl ether and ethylene glycol ethyl ether.
[0020] Preferably, the ether solvent is ethylene glycol monomethyl ether.
[0021] In the present application, the ether solvent can be ethylene glycol monomethyl ether or ethylene glycol ethyl ether or a mixture of ethylene glycol monomethyl ether and ethylene glycol ethyl ether. Ether solvents can be used as a medium for silicate polymerization reaction, which can effectively help the polymerization reaction to be slowed down and the reaction temperature to be easy to control. Secondly, ether solvents can dissolve solid reactants in the polymerization reaction, which can effectively help the dissolution of solvent-based reactants. Finally, ether solvents can be used as diluents to allow the latex to reach a certain viscosity and have a certain degree of wettability, so that it is easy to coat on a silicon wafer, so that the phosphorus diffusion source has good diffusion uniformity.
[0022] In one embodiment, the phosphorus source is selected from phosphorus pentoxide, ammonium phosphate, diammonium hydrogen phosphate and monoammonium phosphate.
[0023] Preferably, the phosphorus source is phosphorus pentoxide.
[0024] In one embodiment, the low carbon alcohol is a C1-C4 alcohol.
[0025] Preferably, the low carbon alcohol is selected from methanol, ethanol, isopropanol and butanol.
[0026] More preferably, the low-carbon alcohol is ethanol.
[0027] In the present application, the low-carbon alcohol is a C1-C4 alcohol, which can be methanol, ethanol, isopropanol or butanol. Alcohols are added to the phosphorus diffusion source as a dispersant to increase the uniformity of the phosphorus source in the latex and avoid the occurrence of the element "clustering" phenomenon.
[0028] In the presence of alcohols, the phosphorus source is evenly dispersed into the solvent to form a low-viscosity solution. Therefore, molecular-level uniformity can be achieved in a very short time. When forming the latex, the reactants are evenly mixed at the molecular level. Therefore, the formed latex has good film-forming properties and fluidity, is easy to coat, and can form a uniform film.
[0029] In one embodiment, the shelf life of the phosphorus diffusion source is more than 12 months.
[0030] In the present application, a phosphorus diffusion source is prepared by mixing silicate, acids, lower alcohols, ether solvents, a phosphorus source, and water according to corresponding weight ratios. With the mutual cooperation of the above several raw materials, the formation rate of particles in the phosphorus diffusion source can be slowed down, thereby extending the storage time of the phosphorus diffusion source to up to more than 12 months.
[0031] When the storage time is 12 months, the viscosity of the obtained phosphorus diffusion source is less than 2.3 cp, the number of particles ≥ 0.5 μm is below 56 per mL, the number of particles ≥ 1.0 μm is below 2.7 per mL, and the number of particles ≥ 5.0 μm is below 1.9 per mL.
[0032] When the obtained phosphorus diffusion source is used in silicon wafers, the sheet resistance of the silicon wafers is between 1.52 - 1.74 Ω / square, and the PN junction depth is between 5.0 - 5.7 μm, indicating that it has high diffusion uniformity. After storing the phosphorus diffusion source for 12 months and then using it in silicon wafers, the sheet resistance of the silicon wafers is between 1.51 - 1.77 Ω / square, and the PN junction depth is between 5.0 - 5.7 μm, indicating that the obtained phosphorus diffusion source still has good uniformity after being stored for 12 months and can achieve a uniformly distributed effect.
[0033] In a second aspect, the present application provides a method for preparing a phosphorus diffusion source, including the following steps,
[0034] (1) Mix the ether solvent and the phosphorus source to obtain a base solution A;
[0035] (2) Mix the silicate, the water, and the lower alcohol, and add the acids dropwise to obtain a base solution B;
[0036] (3) Then mix the base solution A and the base solution B according to a weight ratio of 1:(1 - 1.1), and after pressure filtration, obtain the phosphorus diffusion source.
[0037] In the present application, an ether solvent and a phosphorus source are added to a reactor in corresponding proportions, the temperature in the reactor is adjusted to 15-50°C, and stirred for 0.5-4h to obtain a base liquid A; silicate, water and low-carbon alcohol are added to another reactor for mixing, the temperature in the reactor is adjusted to 15-50°C, and stirred for 0.5-4h. During the stirring process, the acid is gradually added dropwise to obtain a base liquid B.
[0038] The obtained A base liquid and B base liquid are pressure filtered respectively, then mixed at a weight ratio of 1:(1-1.1), stirred for 0.5-4 hours, and then pressure filtered again to obtain a phosphorus diffusion source.
[0039] In the application, the temperature in the reactor is 15-50° C. When the temperature in the reactor is higher than 50° C., the solvent in the reactor will volatilize excessively, which is not conducive to the formation of colloid; when the temperature in the reactor is lower than 15° C., it is not conducive to the reaction.
[0040] In summary, this application has the following beneficial effects:
[0041] 1. The present application uses silicate, water, acid, low-carbon alcohol and ether solvent to prepare phosphorus diffusion source. The obtained phosphorus diffusion source has a long storage time and high diffusion uniformity, so that the storage time is up to more than 12 months;
[0042] 2. After storage for 12 months, the viscosity of the phosphorus diffusion source obtained in the present application is less than 2.3 cp, the number of particles ≥0.5 μm in the phosphorus diffusion source is less than 56 pieces / mL, the number of particles ≥1.0 μm is less than 2.7 pieces / mL, and the number of particles ≥5.0 μm is less than 1.9 pieces / mL.
[0043] 3. The preparation method of the phosphorus diffusion source of the present application is relatively simple, easy to control, and can achieve batch production. DETAILED DESCRIPTION
[0044] The present application is further described in detail below with reference to the embodiments.
[0045] raw material
[0046] Unless otherwise specified, the raw materials described in this application can be obtained commercially.
[0047] Example
[0048] Example 1
[0049] Preparation of phosphorus diffusion source:
[0050] (1) 32.96 kg of ethylene glycol monomethyl ether (ether solvent) and 12.11 kg of phosphorus pentoxide (phosphorus source) were added to a reaction kettle, the temperature in the reaction kettle was controlled to 50° C., and stirred for 3 hours to obtain base liquid A;
[0051] (2) Add 19.68 kg of diethyl orthosilicate (silicate), 2.92 kg of water, and 32.3 kg of ethanol (low-carbon alcohol) into another reaction kettle, adjust the temperature in the reaction kettle to 50° C., and stir for 3 hours. During the stirring process, gradually add hydrochloric acid (acid) dropwise, and the total amount of hydrochloric acid used is 0.03 kg to obtain base liquid B;
[0052] (3) The obtained base liquid A and base liquid B are pressure filtered through a 0.2 μm filter element respectively, and then the filtered base liquid A and base liquid B are mixed in a weight ratio of 1:1, stirred for 3 hours, and pressure filtered again with a 0.2 μm filter element to obtain a phosphorus diffusion source.
[0053] Embodiment 2-5
[0054] The differences between Examples 2-7 and Example 1 are shown in Table 1.
[0055] Comparative Examples 1-4
[0056] The differences between Comparative Examples 1-4 and Example 1 are shown in Table 1.
[0057] Table 1 The difference parameters between Examples 1-7 and Comparative Examples 1-4 (unit: kg)
[0058] Group Ethylene glycol monomethyl ether Phosphorus pentoxide Diethyl orthosilicate water Ethanol hydrochloric acid Example 1 32.96 12.11 19.68 2.92 32.3 0.03 Example 2 32.98 12.11 19.68 2.92 32.3 0.01 Example 3 32.89 12.11 19.68 2.92 32.3 0.1 Example 4 31.99 12.11 19.68 2.92 32.3 1 Example 5 39.96 5.11 19.68 2.92 32.3 0.03 Example 6 39.96 12.11 19.68 2.92 25.3 0.03 Example 7 19.96 12.11 19.68 2.92 45.3 0.03 Comparative Example 1 32.99 12.11 19.68 2.92 32.3 0 Comparative Example 2 31.94 12.11 19.68 2.92 32.3 1.05 Comparative Example 3 43.76 19.11 19.68 2.92 14.5 0.03 Comparative Example 4 15.5 11.37 19.68 2.92 50.5 0.03
[0059] Example 8
[0060] The difference between Example 8 and Example 1 is that the acid in Example 8 is acetic acid.
[0061] Example 9
[0062] The difference between Example 9 and Example 1 is that the silicate in Example 9 is methyl orthosilicate.
[0063] Example 10
[0064] The difference between Example 10 and Example 1 is that the ether solvent in Example 10 is ethylene glycol ethyl ether.
[0065] Performance testing
[0066] 1. Shelf life test
[0067] The performance of the phosphorus diffusion source affects the quality of silicon wafers. During the storage of the phosphorus diffusion source, as the placement time increases, fine particles are generated in the phosphorus diffusion source, and the viscosity of the phosphorus diffusion source gradually increases. When the viscosity is greater than 2.3cp (25℃), it cannot meet the use requirements, resulting in uneven phosphorus diffusion source.
[0068] The particle content was tested in accordance with Q / HG 033 0101-2009 "General Method for Determination of Particle Number", mainly using the laser scattering method;
[0069] The viscosity test is carried out in accordance with Q / HG033 2303-2015.
[0070] The phosphorus diffusion sources prepared in Examples 1-10 and Comparative Examples 1-4 were tested to determine the number of fine particles in the phosphorus diffusion sources and the viscosity of the phosphorus diffusion sources at different time periods. The specific test results are shown in Table 2.
[0071] Table 2 Test results of shelf life
[0072]
[0073]
[0074]
[0075] Combining Examples 1-10 and Comparative Examples 1-4 and Table 2, it can be seen that as time goes by, the viscosity and the number of particles of the phosphorus diffusion sources obtained in Examples 1-10 and Comparative Examples 1-4 increase to varying degrees.
[0076] When the time is 12 months, the viscosity of the phosphorus diffusion source obtained in Example 1-10 is ≤2.3cp, the number of particles ≥0.5μm is less than 56 / mL, the number of particles ≥1.0μm is less than 2.7 / mL, and the number of particles ≥5.0μm is less than 1.9 / mL. The viscosity of the phosphorus diffusion source obtained in Comparative Example 1-4 is ≥42.7cp, the number of particles ≥0.5μm is more than 6992 / mL, the number of particles ≥1.0μm is more than 967 / mL, and the number of particles ≥5.0μm is more than 252 / mL.
[0077] 2. Sheet resistance and junction depth detection
[0078] The phosphorus diffusion sources prepared in Examples 1-10 and Comparative Examples 1-4 were subjected to performance tests. The obtained phosphorus diffusion sources were used in silicon wafers. The phosphorus diffusion sources were coated on the surface of the silicon wafers by coating, and then the silicon wafers were heated (generally at about 1000° C.) to allow them to diffuse thermally.
[0079] The sheet resistance and PN junction depth of the silicon wafer after coating the phosphorus diffusion source are detected. The sheet resistance is measured by the DC two-probe method, referring to GB / T1551-2021 "Determination of resistivity of silicon single crystals by in-line four-probe method and DC two-probe method"; the PN junction depth test method is the angle grinding and staining method, referring to YS / T15-2015 "Determination of thickness of silicon epitaxial layer and diffusion layer by angle grinding and staining method". The specific test results are shown in Table 3.
[0080] Table 3 Test Results
[0081]
[0082] Combined with Examples 1-10 and Comparative Examples 1-4 and Table 3, it can be seen that the phosphorus diffusion sources prepared from Examples 1-10 and Comparative Examples 1-4 are stored for 0 days and used to prepare semiconductors in silicon wafers; for the phosphorus diffusion sources prepared in Examples 1-10, the sheet resistance of the silicon wafers is between 1.52-1.74 Ω / square, and the PN junction depth is between 5.0-5.7 μm, indicating that the obtained phosphorus diffusion source has high diffusion uniformity.
[0083] The phosphorus diffusion sources prepared from Examples 1-10 and Comparative Examples 1-4 are stored for 12 months and used to prepare semiconductors in silicon wafers; for the phosphorus diffusion sources obtained in Examples 1-10, the sheet resistance of the silicon wafers is between 1.51-1.77 Ω / square, and the PN junction depth is between 5.0-5.7 μm. This shows that the obtained phosphorus diffusion source still has good uniformity after being stored for 12 months, indicating that the phosphorus diffusion source has a long shelf life.
[0084] It can be understood that the above embodiments are merely exemplary embodiments adopted to illustrate the principle of the present application. However, the present application is not limited thereto. For those skilled in the art, various modifications and improvements can be made without departing from the spirit and essence of the present application, and these modifications and improvements are also regarded as the protection scope of the present invention.
Claims
1. A phosphorus diffusion source, characterized in that: According to weight percentage, it includes 15-35% silicate, 2-5% water, 0.01-0.1% acid, 25-35% low-carbon alcohol, 15-35% ether solvent, and 5-15% phosphorus source. The acid is hydrochloric acid, acetic acid or sulfuric acid; the ether solvent is selected from ethylene glycol monomethyl ether and ethylene glycol ethyl ether.
2. The phosphorus diffusion source according to claim 1, characterized in that: In terms of weight percentage, the silicate accounts for 19.68%, the water accounts for 2.92%, the acid accounts for 0.03%, the low-carbon alcohol accounts for 32.3%, the ether solvent accounts for 32.96%, and the phosphorus source accounts for 12.11%.
3. The phosphorus diffusion source according to any one of claims 1 to 2, characterized in that: The silicate is methyl orthosilicate, tetraethyl orthosilicate or diethyl orthosilicate.
4. The phosphorus diffusion source according to any one of claims 1 to 2, characterized in that: The phosphorus source is selected from phosphorus pentoxide, ammonium phosphate, diammonium hydrogen phosphate and monoammonium phosphate.
5. The phosphorus diffusion source according to any one of claims 1 to 2, characterized in that: The low-carbon alcohol is selected from methanol, ethanol, isopropanol and butanol.
6. The phosphorus diffusion source according to any one of claims 1 to 2, characterized in that: The phosphorus diffusion source has a shelf life of more than 12 months.
7. A method for preparing a phosphorus diffusion source according to any one of claims 1 to 6, characterized in that: The following steps are included: (1) mixing the ether solvent and the phosphorus source to prepare a base liquid A; (2) mixing the silicate, the water and the low-carbon alcohol, and adding the acid dropwise to obtain a base liquid B; (3) The base liquid A and the base liquid B are mixed at a weight ratio of 1:(1-1.1), and pressure filtered to obtain a phosphorus diffusion source.