Organoaminopolysiloxanes for deposition of silicon-containing films
By using an organic amino polysiloxane compound and plasma source with multiple silicon atoms and Si-O-Si bonds, the problem of impurities and high-temperature process discomfort in silicon oxide films at low temperatures is solved, and high-quality silicon oxide films are achieved. Deposition, suitable for semiconductor manufacturing.
Patent Information
- Application Number
- CN202211350727.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2018-01-30
- Filing Date
- 2018-02-06
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2038-02-06
AI Technical Summary
The prior art has impurity problems when depositing silicon oxide films at low temperatures, and the high-temperature deposition process is not suitable for conventional precursors in the semiconductor industry, resulting in poor film quality and difficult process control.
Using an organoaminopolysiloxane with three or more silicon atoms and at least two Si-O-Si bonds as a precursor, deposition at lower temperatures by thermoatomic layer deposition or plasma enhanced atomic layer deposition process A silicon-containing film uses a specific organic amino polysiloxane compound and an oxygen-containing and nitrogen-containing plasma source to form a high-quality silicon-oxygen film.
It realizes the depositing of high-density, low chemical impurities and excellent electrical properties of silicon oxide films at low temperatures, and improves the conformity and wet etching rate of the film, which is suitable for semiconductor manufacturing.
Smart Images

Figure BDA0003918745260000041 
Figure BDA0003918745260000061 
Figure BDA0003918745260000081
Abstract
Description
[0001] This application is a divisional application of a Chinese patent application with an application date of February 6, 2018, application number 201880021253.3, and invention name “Organoaminopolysiloxane for depositing silicon-containing films”.
[0002] CROSS-REFERENCE TO RELATED APPLICATIONS
[0003] This application claims the benefit of priority under 35 U.S.C. §119(e) to U.S. Provisional Application Serial No. 62 / 456,311 filed on February 8, 2017 and Provisional Application Serial No. 62 / 472,313 filed on March 16, 2017, the entire contents of which are incorporated herein by reference. Background Art
[0004] The present disclosure relates to organosilicon compounds useful for depositing films containing silicon and oxygen (e.g., silicon oxide, silicon oxycarbonitride, silicon oxycarbide, carbon-doped silicon oxide, and other films containing silicon and oxygen), methods of depositing silicon oxide-containing films using these compounds, and films obtained from the compounds and methods.
[0005] Described herein are novel organoaminopolysiloxane compounds and compositions and methods containing the organoaminooligosiloxane compounds for depositing silicon-containing films (such as, but not limited to, silicon oxide, silicon oxynitride, silicon oxycarbonitride, and carbon-doped silicon oxide) by thermal atomic layer deposition (ALD) or plasma enhanced atomic layer deposition (PEALD) processes or combinations thereof. More specifically, described herein are compositions and methods for forming stoichiometric or non-stoichiometric silicon-containing films or materials at one or more deposition temperatures of about 600° C. or less (including, for example, about 25° C. to about 300° C.).
[0006] Atomic layer deposition (ALD) and plasma enhanced atomic layer deposition (PEALD) are processes for depositing conformal films such as silicon oxide at low temperatures (<500°C). In both ALD and PEALD processes, precursors and reactive gases (such as oxygen or ozone) are pulsed separately in a certain number of cycles to form a monolayer of silicon oxide in each cycle. However, silicon oxide deposited at low temperatures using these processes may contain impurity levels that may be harmful in certain semiconductor applications, such as but not limited to carbon (C) or hydrogen (H). To address this problem, one possible solution is to increase the deposition temperature to 500°C or higher. However, at these higher temperatures, conventional precursors used by the semiconductor industry tend to self-react, thermally decompose, and deposit in chemical vapor deposition (CVD) mode rather than ALD mode. Compared with ALD deposition, CVD mode deposition has reduced conformality, especially for high aspect ratio structures required in many semiconductor applications. In addition, compared with ALD mode deposition, CVD mode deposition has less control over the thickness of the film or material.
[0007] It is known in the art that it can be used at relatively low temperatures (<300°C) and at relatively high growth rates per cycle (GPC, / cycle) by atomic layer deposition (ALD) and plasma enhanced atomic layer deposition (PEALD) processes to deposit organoaminosilane and chlorosilane precursors for silicon-containing films.
[0008] Examples of known precursors and methods are disclosed in the following publications, patents and patent applications.
[0009] US Patent No. 7,084,076 describes the use of halogen- or NCO-substituted disiloxane precursors to deposit silicon oxide films in a base-catalyzed ALD process.
[0010] US Publication No. 2015 / 0087139 describes the deposition of silicon-containing films using amino-functionalized carbosilanes by thermal ALD or PEALD processes.
[0011] US Patent No. 9,337,018 describes the use of organoaminodisilanes to deposit silicon-containing films by thermal ALD or PEALD processes.
[0012] US Patent Nos. 8,940,648, 9,005,719, and 8,912,353 describe the use of organoaminosilanes to deposit silicon-containing films by thermal ALD or PEALD processes.
[0013] US Publication No. 2015 / 0275355 describes the deposition of silicon-containing films using mono- and bis(organoamino)alkylsilanes by thermal ALD or PEALD processes.
[0014] US Publication No. 2015 / 0376211 describes the deposition of silicon-containing films using mono(organoamino)-, halido-, and pseudohalo-substituted trisilylamines by thermal ALD or PEALD processes.
[0015] Publication No. WO 2015 / 0105337 and US Pat. No. 9,245,740 describe the deposition of silicon-containing films by thermal ALD or PEALD processes using alkylated trisilylamines.
[0016] US Patent No. 7,084,076 describes the use of halogen- or NCO-substituted disiloxane precursors to deposit silicon oxide films in a base-catalyzed ALD process.
[0017] The disclosures of the above-identified patents and patent applications are incorporated herein by reference.
[0018] There is a need in the art for precursors and methods for depositing silicon and oxygen containing films at high growth per cycle (GPC) to maximize the throughput of semiconductor manufacturing facilities. / cycle GPC deposition, but these precursors have disadvantages such as low quality films (elemental contamination, low density, poor electrical properties, high wet etch rates), high process temperatures, require catalysts, are expensive, produce low conformal films, and other disadvantages. Summary of the invention
[0019] The present disclosure solves the problems associated with conventional precursors and processes by providing silicon-and-oxygen-containing precursors, particularly organoaminopolysiloxanes (which have at least three silicon atoms, oxygen atoms, and organoamino groups for anchoring the polysiloxane units to the substrate surface) as part of a process for depositing silicon-and-oxygen-containing films. The precursors disclosed in the present invention having three or more silicon atoms and at least two or more Si-O-Si bonds have novel structures compared to those described in the background of the present invention, and thus can provide advantages in one or more aspects regarding the cost or convenience of precursor synthesis, precursor physical properties (including thermal stability, reactivity, or volatility), the process for depositing silicon-containing films, or the properties of the deposited silicon-containing films.
[0020] In one embodiment, a composition comprising at least one organoaminopolysiloxane compound selected from the group consisting of Formula A, B, C, D, E, F, G, and H is disclosed:
[0021]
[0022] Where R 1 Selected from straight chain C 1 To C 10 Alkyl, branched chain C 3 To C 10 Alkyl, C 3 To C 10 Cycloalkyl, C 3 To C 10 Heterocyclic group, C 3 To C 10 Alkenyl, C 3 To C 10 Alkynyl and C 4 To C 10 Aryl; R 2 Selected from hydrogen, straight chain C 1 To C 10 Alkyl, branched chain C 3 To C 10 Alkyl, C 3 To C 10 Cycloalkyl, C 3 To C 10 Heterocyclic group, C 3 To C 10 Alkenyl, C 3 To C 10 Alkynyl and C 4To C 10 Aryl, wherein R in the formula AH 1 and R 2 connected to form an cyclic ring structure or not connected to form an cyclic ring structure.
[0023] In another aspect, a method for depositing a film comprising silicon and an oxide onto a substrate is provided, the method comprising the steps of: a) providing a substrate in a reactor; b) introducing into the reactor a composition comprising at least one organoaminopolysiloxane compound selected from the group consisting of Formula A, B, C, D, E, F, G and H:
[0024]
[0025] Where R 1 Selected from straight chain C 1 To C 10 Alkyl, branched chain C 3 To C 10 Alkyl, C 3 To C 10 Cycloalkyl, C 3 To C 10 Heterocyclic group, C 3 To C 10 Alkenyl, C 3 To C 10 Alkynyl and C 4 To C 10 Aryl; R 2 Selected from hydrogen, straight chain C 1 To C 10 Alkyl, branched chain C 3 To C 10 Alkyl, C 3 To C 10 Cycloalkyl, C 3 To C 10 Heterocyclic group, C 3 To C 10 Alkenyl, C 3 To C 10 Alkynyl and C 4 To C 10 Aryl, wherein R in the formula AH 1 and R 2 connected to form an annular ring structure or not connected to form an annular ring; c) purging the reactor with a purge gas; d) introducing at least one of an oxygen-containing source and a nitrogen-containing source into the reactor; e) purging the reactor with the purge gas, wherein steps b to e are repeated until a film of a desired thickness is deposited; and wherein the method is carried out at one or more temperatures in the range of about 25°C to 600°C.
[0026] In another aspect, a method for preparing an organoaminopolysiloxane compound having a structure shown in Formula A to H is disclosed:
[0027]
[0028] Where R 1 Selected from straight chain C 1 To C 10 Alkyl, branched chain C 3 To C 10 Alkyl, C 3 To C 10 Cycloalkyl, C 3 To C 10 Heterocyclic group, C 3 To C 10 Alkenyl, C 3 To C 10 Alkynyl and C 4 To C 10 Aryl; R 2 Selected from hydrogen, straight chain C 1 To C 10 Alkyl, branched chain C 3 To C 10 Alkyl, C 3 To C 10 Cycloalkyl, C 3 To C 10 Heterocyclic group, C 3 To C 10 Alkenyl, C 3 To C 10 Alkynyl and C 4 To C 10 Aryl, wherein R in the formula AH 1 and R 2 The method comprises the following steps: a) reacting the reactants R in the presence of a catalyst 1 R 2 NH is contacted with a polysiloxane having at least one Si-H group to form a reaction mixture wherein R 1 and R 2 as defined above; b) optionally adding a solvent to the reaction mixture; c) maintaining the reaction mixture at a temperature of about 0°C to about 300°C; and d) allowing the reaction to proceed to form the organoaminopolysiloxane compound from the reaction mixture.
[0029] The process for depositing stoichiometric or non-stoichiometric silicon and oxygen-containing materials or films (such as, but not limited to, silicon oxide, carbon-doped silicon oxide, silicon oxynitride film, or carbon-doped silicon oxynitride film) at relatively low temperatures (e.g., at one or more temperatures of 600° C. or less) can be plasma enhanced ALD (PEALD), plasma enhanced cyclic chemical vapor deposition (PECCVD), flowable chemical vapor deposition (FCVD), plasma enhanced flowable chemical vapor deposition (PEFCVD), plasma enhanced ALD-like process, or an ALD process using an oxygen-containing reactant source, a nitrogen-containing reactant source, or a combination thereof.
[0030] In some embodiments, the oxygen-containing source used in the method is selected from oxygen plasma, ozone, water vapor, water vapor plasma, nitrogen oxides with or without an inert gas (e.g., N 2 O, NO, NO 2 ) plasma, carbon oxides (e.g., CO 2 In some embodiments, the oxygen source further comprises an inert gas. In these embodiments, the inert gas is selected from argon, helium, nitrogen, hydrogen, and combinations thereof. In alternative embodiments, the oxygen source does not comprise an inert gas. In another embodiment, the oxygen-containing source comprises nitrogen, which reacts with the reagent under plasma conditions to provide a silicon oxynitride film.
[0031] In some embodiments, the nitrogen-containing source can be introduced into the reactor in the form of at least one nitrogen-containing source and / or can be incidentally present in other precursors used in the deposition process. Suitable nitrogen source gases may include, for example, ammonia, hydrazine, monoalkyl hydrazine, dialkyl hydrazine, nitrogen, nitrogen / hydrogen, nitrogen / argon plasma, nitrogen / helium plasma, ammonia plasma, nitrogen plasma, nitrogen / hydrogen plasma, organic amines such as tert-butylamine, dimethylamine, diethylamine, isopropylamine, diethylamine plasma, dimethylamine plasma, trimethyl plasma, trimethylamine plasma, ethylenediamine plasma, and alkoxyamines such as ethanolamine plasma, and mixtures thereof. In certain embodiments, the nitrogen-containing source includes ammonia plasma, a plasma comprising nitrogen and argon, a plasma comprising nitrogen and helium, or a plasma comprising hydrogen and nitrogen source gas.
[0032] In the above embodiments and throughout the present invention, the inert gas is selected from argon, helium, nitrogen, hydrogen, or a combination thereof. In an alternative embodiment, the oxygen-containing plasma source does not contain an inert gas.
[0033] The embodiments of the present invention may be used alone or in combination with each other. DETAILED DESCRIPTION
[0034] Unless otherwise specified herein or clearly contradictory to the context, the terms "a / an" and "the" and similar references in the context of describing the present invention (especially in the context of the following claims) should be interpreted as covering both the singular and the plural. Unless otherwise specified, the terms "comprising", "having", "including" and "containing" should be interpreted as open terms (i.e., "including but not limited to"). Unless otherwise specified herein, the recording of numerical ranges herein is intended only to be used as a shorthand method for individually referring to each individual value falling within the range, and each individual value is incorporated into this specification as if it is recorded separately herein. Unless otherwise specified herein or the context is clearly contradictory, all methods described herein can be performed in any suitable order. Unless otherwise stated, the use of any and all examples or exemplary language (e.g., "such as") provided herein is intended only to better illustrate the present invention without limiting the scope of the present invention. Any language in the specification should not be interpreted as indicating that any unclaimed element is necessary for the implementation of the present invention.
[0035] Preferred embodiments of the present invention are described herein. After reading the foregoing description, variations of those preferred embodiments may become apparent to those of ordinary skill in the art. The inventors expect that skilled artisans will appropriately adopt such variations, and the inventors intend that the present invention be implemented in a manner different from that specifically described herein. Therefore, the present invention includes all modifications and equivalents permitted by applicable law of the subject matter recorded in the appended claims. Moreover, unless otherwise specified herein or the context is clearly contradictory, the present invention encompasses any combination of all possible variations of the above elements.
[0036] Described herein are compositions and methods involving the formation of stoichiometric or non-stoichiometric films or materials comprising silicon and oxygen, such as, but not limited to, silicon oxide, carbon-doped silicon oxide films, silicon oxynitride, or carbon-doped silicon oxynitride films, or combinations thereof, at one or more temperatures of about 600° C. or less or about 25° C. to about 600° C., and in some other embodiments, about 550° C. to about 800° C. The films described herein are deposited in a deposition process such as atomic layer deposition (ALD) or in an ALD-like process such as, but not limited to, plasma enhanced ALD (PEALD) or plasma enhanced cyclic chemical vapor deposition process (PECCVD) , flowable chemical vapor deposition (FCVD) or plasma enhanced flowable chemical vapor deposition (PEFCVD). The low temperature deposition (e.g., one or more deposition temperatures ranging from about ambient temperature to 600° C.) methods described herein provide films or materials that exhibit at least one or more of the following advantages: a density of about 2.1 g / cc or greater, low chemical impurities, high conformality in a thermal atomic layer deposition, plasma enhanced atomic layer deposition (ALD) process, or a plasma enhanced ALD-like process, the ability to tune the carbon content in the resulting film; and / or a film having a carbon content of 5 Å / s when measured in 0.5 wt. % dilute HF. For carbon doped silicon oxide films, greater than 1% carbon is desirable, in addition to other properties such as, but not limited to, a density of about 1.8 g / cc or more or about 2.0 g / cc or more, to adjust the etch rate to less than 100 % in 0.5 wt. % dilute HF. The value of .
[0037] The present invention can be implemented using equipment known in the art. For example, the method of the present invention can use a conventional reactor in the field of semiconductor manufacturing.
[0038] Without wishing to be bound by any theory or explanation, it is believed that the effectiveness of the precursors of the present invention may vary with the number of silicon atoms, and in particular the number of silicon atom bonds, within the precursors of the present invention. The precursors of the present invention have three or more silicon atoms, and at least two or more Si-O-Si bonds. The Si-O-Si bonds may play an important role during the formation of films containing silicon and oxygen.
[0039] The poly-silicon precursor proposed in the present invention has a different structure from that known in the art, and therefore, can perform better than conventional silicon-containing precursors and provide a relatively high growth per cycle (GPC), thereby producing higher quality films, having a favorable wet etch rate or having less elemental contamination.
[0040] One embodiment of the present invention relates to a composition for depositing a film selected from silicon oxide, carbon-doped silicon oxide or silicon oxycarbonitride film using a vapor deposition method, the composition comprising a compound having formula A, formula B, formula C, formula D, formula E, formula F, formula G or formula H:
[0041]
[0042] Where R 1 Independently selected from linear C 1 To C 10 Alkyl, branched chain C 3 To C 10 Alkyl, C 3 To C 10 Cycloalkyl, C 3 To C 10 Heterocyclic group, C 3 To C 10 Alkenyl, C 3 To C 10 Alkynyl and C 4 To C 10 Aryl; R 2 Selected from hydrogen, straight chain C 1 To C 10 Alkyl, branched chain C 3 To C 10 Alkyl, C 3 To C 10 Cycloalkyl, C 3 To C 10 Heterocyclic group, C 3 To C 10 Alkenyl, C 3 To C 10 Alkynyl and C 4 To C 10 Aryl, wherein R in the formula AH 1 and R 2 connected to form an cyclic ring structure or not connected to form an cyclic ring structure.
[0043] In some embodiments of the composition described herein, a solvent is also included. Exemplary solvents may include, but are not limited to, ethers, tertiary amines, alkyl hydrocarbons, aromatic hydrocarbons, siloxanes, tertiary amino ethers, and combinations thereof. In some embodiments, the difference between the boiling point of the silicon precursor and the boiling point of the solvent is 40° C. or less. The weight percent of the silicon precursor composed of formula AH in the solvent may be 1 to 99 weight percent, or 10 to 90 weight percent, or 20 to 80 weight percent, or 30 to 70 weight percent, or 40 to 60 weight percent, to 50 to 50 weight percent. In some embodiments, the composition may be delivered to a reaction chamber for a silicon-containing film by direct liquid injection.
[0044] In the above formula and throughout the specification, the term "alkyl" refers to a straight or branched functional group having 1 to 10 carbon atoms. Exemplary straight chain alkyls include, but are not limited to, methyl, ethyl, propyl, butyl, pentyl, and hexyl. Exemplary branched alkyls include, but are not limited to, isopropyl (Pr i ), isobutyl (Bui ), sec-butyl (Bu s ), tert-butyl (Bu t ), isopentyl, tert-pentyl, isohexyl and neohexyl. In certain embodiments, the alkyl group may have one or more functional groups attached thereto, such as but not limited to alkoxy, dialkylamino or a combination thereof attached thereto. In other embodiments, the alkyl group does not have one or more functional groups attached thereto. The alkyl group may be saturated or alternatively unsaturated.
[0045] In the above formula and throughout the specification, the term "cycloalkyl" refers to a cyclic functional group having 3 to 10 carbon atoms. Exemplary cycloalkyl groups include, but are not limited to, cyclobutyl, cyclopentyl, cyclohexyl, and cyclooctyl.
[0046] In the above formulae and throughout the specification, the term "alkenyl" denotes a group having one or more carbon-carbon double bonds and having 2 to 10 or 2 to 6 carbon atoms.
[0047] In the formulae described herein and throughout the specification, the term "dialkylamino", "alkylamino" or "organoamino" means a group having two alkyl groups bonded to a nitrogen atom or one alkyl group bonded to a nitrogen atom and having 1 to 10 or 2 to 6 or 2 to 4 carbon atoms. Examples include, but are not limited to, HNMe, HNEt, HNPr i 、HNPr n 、HNBu s 、HNBu i 、HNBu t 、NMe 2 、NMeEt、NEt 2 NPr i 2 、NBu s 2 In some embodiments, two alkyl groups are linked to form a ring, such as pyrrolidinyl, 2,5-dimethylpyrrolidinyl, piperidino, 2,6-dimethylpiperidino.
[0048] In the above formula and throughout the specification, the term "aryl" refers to an aromatic cyclic functional group having 4 to 10 carbon atoms, 5 to 10 carbon atoms, or 6 to 10 carbon atoms. Exemplary aryl groups include, but are not limited to, phenyl, benzyl, chlorobenzyl, tolyl, o-xylyl, 1,2,3-triazolyl, pyrrolyl, and furanyl.
[0049] Throughout the specification, the term "alkyl hydrocarbon" refers to a straight or branched C 1 To C 20 Hydrocarbon, cyclic C 6 To C 20Hydrocarbons. Exemplary hydrocarbons include, but are not limited to, hexane, heptane, octane, nonane, decane, dodecane, cyclooctane, cyclononane, cyclodecane, ethylcyclohexane, ethylcyclooctane.
[0050] Throughout this specification, the term "aromatic hydrocarbons" refers to C 6 To C 20 Aromatic hydrocarbons. Exemplary aromatic hydrocarbons include, but are not limited to, toluene, mesitylene.
[0051] In the above formula and throughout the specification, the term "heterocycle" refers to a non-aromatic saturated monocyclic or polycyclic ring system of about 3 to about 10 ring atoms, preferably about 5 to about 10 ring atoms, wherein one or more atoms in the ring system are elements other than carbon, such as nitrogen, oxygen or sulfur. Preferred heterocycles contain about 5 to about 6 ring atoms. The prefix aza, oxa or thia before the heterocycle means that at least nitrogen, oxygen or sulfur atom is present as a ring atom, respectively. The heterocyclic group is optionally substituted.
[0052] Table 1a provides exemplary organoaminopolysiloxanes having the formula AH, wherein R 1 and R 2 Independently selected from C 1 To C 4 alkyl.
[0053] Table 1a. Exemplary organoaminopolysiloxanes having formula AH
[0054]
[0055]
[0056]
[0057]
[0058] Table 1b provides exemplary organoaminopolysiloxanes having the formula AH, wherein R 1 is hydrogen and R 2 Selected from C 1 To C 4 alkyl.
[0059] Table 1b. Exemplary organoaminopolysiloxanes having formula A and C , where R 1 is hydrogen and R 2 Selected from C 1 To C 4 Alkyl, such as Me, Et, Pr n , Pr i 、Bu t 、Bu i or Bu s .
[0060]
[0061] The compound having Formula A or C can be synthesized, for example, by catalytic dehydrogenative coupling of an organic amine with a polysiloxane having at least one Si—H group (eg, Reaction Formula 1-2).
[0062]
[0063] Similarly, compounds of formula B, D, E, F, G and H can also be prepared in a similar manner to reaction formula (1) or (2) using a suitable dehydrogenative coupling catalyst.
[0064] Preferably, the molar ratio of polysiloxane to organic amine in the reaction mixture is about 1 to 1.0, 1 to 1.5, 1 to 2, 1 to 3, 1 to 4 or 1 to 10.
[0065] The catalyst used in the method of the present invention in reaction formulas (1) and (2) is a catalyst that promotes the formation of silicon-nitrogen bonds. Exemplary catalysts include, but are not limited to, tris(pentafluorophenyl)borane, BR 3 (wherein R is selected from a linear, branched or cyclic C 1 To C 10 Alkyl, C 5 To C 10 Aryl or C 1 To C 10 alkoxy), 1,3-diisopropyl-4,5-dimethylimidazol-2-ylidene, 2,2'-bipyridine, phenanthroline, Mg[N(SiMe 3 ) 2 ] 2 , [tris(4,4-dimethyl-2-oxazolinyl)phenylboronic acid]MgMe, [tris(4,4-dimethyl-2-oxazolinyl)phenylboronic acid]MgH, trimethylaluminum, triethylaluminum, aluminum chloride, Ca[N(SiMe 3 ) 2 ] 2 , dibenzyl calcium, {CH-[CMeNC 6 H 3 -2,6- i Pr 2 ] 2}CaH, triruthenium dodecacarbonyl, {CH-[CMeNC 6 H 3 -2,6- i Pr 2 ] 2}Ca[N(SiMe 3 ) 2 ], bis(cyclopentadienyl)dialkyltitanium(IV), bis(cyclopentadienyl)titanium(IV)difluoride, bis(cyclopentadienyl)titanium(IV)dichloride, bis(cyclopentadienyl)titanium(IV)dihydride, TiMe2 (dmpe) 2 [dmpe = 1,2-bis(dimethylphosphino)ethane], (C 5 H 5 ) 2 Ti(OAr) 2 [Ar=(2,6-(iPr) 2 C 6 H 3 )]、(C 5 H 5 ) 2 Ti(SiHRR')PMe 3 [wherein R, R' are each independently selected from hydrogen atom (H), methyl (Me) and phenyl (Ph)], bis(phenyl)chromium (O), hexacarbonyl chromium, decacarbonyl manganese, [Mn(CO) 4 Br] 2 , iron pentacarbonyl, (C 5 H 5 )Fe(CO) 2 Me, dicobalt octacarbonyl, nickel(II) acetate, nickel(II) chloride, [(dippe)Ni(μ-H)] 2 [dippe = 1,2-bis(diisopropylphosphino)ethane], (R-indenyl)Ni(PR' 3 )Me [wherein R is selected from 1-iPr, 1-SiMe 3 and 1,3-(SiMe 3 ) 2 ; wherein R' is selected from methyl (Me) and phenyl (Ph)], [{Ni(η-CH 2 :CHSiMe 2 ) 2 O} 2 {μ-(η-CH 2 :CHSiMe 2 ) 2 O}, Nickel(II) acetylacetonate, Nickel(cyclooctadiene) 2 , copper(II) fluoride, copper(I) chloride, copper(II) chloride, copper(I) bromide, copper(II) bromide, copper(I) iodide, copper(I) acetate, Cu(PPh 3 ) 3 Cl, zinc chloride, [tris(4,4-dimethyl-2-oxazolinyl)phenylboronic acid]ZnH, Sr[N(SiMe 3 ) 2 ] 2 , bis(cyclopentadienyl)dialkylzirconium(IV), bis(cyclopentadienyl)zirconium(IV) difluoride, bis(cyclopentadienyl)zirconium(IV) dichloride, bis(cyclopentadienyl)zirconium(IV) dihydride, [(Et 3P)Ru(2,6-dimesitylphenylthiophenol)][B[3,5-(CF 3 ) 2 C 6 H 3 ] 4 ]、(C 5 Me 5 )Ru(R 3 P) x (NCMe) 3-x ] + (wherein R is selected from a linear, branched or cyclic C 1 To C 10 Alkyl and C 5 To C 10 Aryl; x = 0, 1, 2, 3), tris(triphenylphosphine)carbonyl rhodium hydride (I), di-μ-chloro-tetracarbonyl dirhodium (I), tris(triphenylphosphine)rhodium chloride (I) (Wilkinson catalyst), hexadecyl hexarhodium, tris(triphenylphosphine)carbonyl rhodium hydride (I), bis(triphenylphosphine)carbonyl rhodium chloride (I), [RhCl(cyclooctadiene)] 2 , tris(dibenzylideneacetone)dipalladium(0), tetrakis(triphenylphosphine)palladium(0), palladium(II) acetate, palladium(II) chloride, palladium(II) iodide, cesium carbonate, (C 5 H 5 ) 2 SmH、(C 5 Me 5 ) 2 SmH、(NHC)Yb(N(SiMe 3 ) 2 ) 2 [NHC = 1,3-bis(2,4,6-trimethylphenyl)imidazol-2-ylidene)], tungsten hexacarbonyl, dirhenium decacarbonyl, triosmium dodecacarbonyl, tetrairidium dodecacarbonyl, (acetylacetonate) dicarbonyl iridium (I), (POCOP) IrHCl [(POCOP) = 2,6-(R 2 PO) 2 C 6 H 3 , R is selected from isopropyl ( i Pr), n-butyl ( n Bu) and methyl (Me)], Ir (Me) 2 (C 5 Me 5 )L[wherein L is selected from PMe 3 and PPh 3 ], [Ir(cyclooctadiene)OMe] 2 , platinum (0)-1,3-divinyl-1,1,3,3-tetramethyldisiloxane (Karstedt catalyst), H 2PtCl 6 ·nH 2 O(chloroplatinic acid), bis(tri-tert-butylphosphine)platinum(0), PtO 2 and Pt(cyclooctadiene) 2 .
[0066] The catalyst may also be present fixed on a support. A support is a solid with a high surface area. Typical support materials include, but are not limited to: alumina, MgO, zeolite, carbon, monolithic cordierite, diatomaceous earth, silica gel, silica / alumina, ZrO and TiO 2 . Preferred supports are carbon (e.g., platinum carbon, palladium carbon, rhodium carbon, ruthenium carbon), alumina, silica and MgO. The metal loading of the catalyst is in the range of about 0.01 wt % to about 50 wt %. The preferred range is about 0.5 wt % to about 20 wt %. The more preferred range is about 0.5 wt % to about 10 wt %. Catalysts that require activation can be activated by many known methods. Heating the catalyst under vacuum is a preferred method.
[0067] The catalyst can be activated before being added to the reaction vessel or before reactants are added to the reaction vessel. The catalyst can contain a promoter. A promoter is a substance that is not a catalyst itself, but increases their efficiency (activity and / or selectivity) when mixed with an active catalyst in a small amount. Promoters are typically metals such as Mn, Ce, Mo, Li, Re, Ga, Cu, Ru, Pd, Rh, Ir, Fe, Ni, Pt, Cr, Cu and Au and / or their oxides. They can be added to the reaction vessel alone, or they can be part of the catalyst itself. For example, Ru / Mn / C (ruthenium carbon promoted by manganese) or Pt / CeO 2 / Ir / SiO 2 (Platinum-silicon oxide promoted by cerium dioxide and iridium). Some promoters can be used as catalysts by themselves, but they can improve the activity of the main catalyst when used in combination with the main catalyst. Catalysts can act as promoters for other catalysts. In this case, the catalyst can be called a bimetallic (or multimetallic) catalyst. For example, Ru / Rh / C can be called a ruthenium rhodium-carbon bimetallic catalyst, or rhodium promoted ruthenium carbon. An active catalyst is a substance that acts as a catalyst in a specific chemical reaction.
[0068] The molar ratio of catalyst to polysiloxane in the reaction mixture is in the range of 0.1 to 1, 0.05 to 1, 0.01 to 1, 0.005 to 1, 0.001 to 1, 0.0005 to 1, 0.0001 to 1, 0.00005 to 1, or 0.00001 to 1. In one embodiment, 0.05 to 0.07 equivalents of catalyst are used per equivalent of polysiloxane. In another embodiment, 0.00008 equivalents of catalyst are used per equivalent of polysiloxane.
[0069] In certain embodiments, the reaction mixture comprising polysiloxane, organic amine and catalyst further comprises an anhydrous solvent. Exemplary solvents may include, but are not limited to, linear-, branched-, cyclic- or poly-ethers (e.g., tetrahydrofuran (THF), diethyl ether, diethylene glycol dimethyl ether and / or tetraethylene glycol dimethyl ether); linear, branched or cyclic alkanes, olefins, aromatic hydrocarbons and halogenated hydrocarbons (e.g., pentane, hexane, toluene and dichloromethane). If added, the selection of one or more solvents may be affected by the compatibility with the reagents contained in the reaction mixture, the solubility of the catalyst and / or the separation process of the selected intermediate product and / or final product. In other embodiments, the reaction mixture does not comprise a solvent.
[0070] In the methods described herein, the reaction between the polysiloxane and the organic amine occurs at one or more temperatures ranging from about 0°C to about 100°C. Exemplary temperatures for the reaction include ranges having any one or more of the following endpoints: 0, 10, 20, 30, 40, 50, 60, 70, 80, 90, or 100°C. Suitable temperature ranges for the reaction can be determined by the physical properties of the reagents and optional solvents. Examples of specific reactor temperature ranges include, but are not limited to, 0°C to 80°C or 0°C to 30°C.
[0071] In certain embodiments of the methods described herein, the reaction pressure may range from about 1 to about 115 psia or from about 15 to about 45 psia. In some embodiments where the polysiloxane is a liquid at ambient conditions, the reaction is carried out at atmospheric pressure. In some embodiments where the polysiloxane is a gas at ambient conditions, the reaction is carried out at a pressure greater than 15 psia.
[0072] In some embodiments, one or more reagents can be introduced into the reaction mixture as liquid or steam.In the embodiment where one or more reagents are added as steam, non-reactive gases such as nitrogen or inert gas can be used as carrier gas to transport steam to the reaction mixture.In the embodiment where one or more reagents are added as liquid, pure reagent can be added, or reagent can be diluted with solvent.Reagent is fed to the reaction mixture until the conversion of the crude mixture or crude liquid containing product as desired is realized.In some embodiments, reaction can be carried out in a continuous manner by supplementing reactants and removing reaction product and crude liquid from reactor.
[0073] The crude mixture comprising the compound of formula AH, the catalyst and possible residual organic amine, solvent or undesirable product may require a separation process. Examples of suitable separation processes include, but are not limited to, distillation, evaporation, membrane separation, filtration, gas phase transfer, extraction, fractionation using a reverse phase column and combinations thereof.
[0074] The compound having formula A or C can be synthesized using reaction formula (3) or (4).
[0075]
[0076] Similarly, Formula B, D, E, F, G and H can also be prepared in a manner similar to Reaction Formula (3) or (4).
[0077] Compounds of formulae A to H can also be synthesized by attaching an organic amino group to a chloropolysiloxane by reacting a Si-Cl bond with an alkali metal amide reagent.
[0078] Furthermore, the compounds having formulae A to H can also be synthesized by attaching an organic amino group to a hydrogenated polysiloxane by reacting a Si-H bond with an imine in the presence of a suitable hydrosilylation catalyst.
[0079] Furthermore, the compounds having formulae A to H can also be synthesized by reacting Si-Ph bonds with a strong acid such as HCl or trifluoromethanesulfonic acid and then adding a suitable organic amine to replace the phenyl group bonded to the polysiloxane unit with an organic amino group.
[0080] Therefore, the present disclosure provides a method for preparing an organoaminopolysiloxane compound having a structure shown in Formulas A to H:
[0081]
[0082] Where R 1 Selected from straight chain C 1 To C 10 Alkyl, branched chain C 3 To C 10 Alkyl, C 3 To C 10 Cycloalkyl, C 3 To C 10 Heterocyclic group, C 3 To C 10 Alkenyl, C 3 To C 10 Alkynyl and C 4 To C 10 Aryl; R 2 Selected from hydrogen, straight chain C 1 To C 10 Alkyl, branched chain C 3 To C 10 Alkyl, C 3 To C 10 Cycloalkyl, C 3 To C 10 Heterocyclic group, C 3 To C 10 Alkenyl, C 3 To C 10 Alkynyl and C4 To C 10 Aryl, wherein R in the formula AH 1 and R 2 The method comprises the following steps: a) reacting the reactants R in the presence of a catalyst 1 R 2 NH is contacted with a polysiloxane having at least one Si-H group to form a reaction mixture wherein R 1 and R 2 as defined above; b) optionally adding a solvent to the reaction mixture; c) maintaining the reaction mixture at a temperature of about 0°C to about 300°C; and d) allowing the reaction to proceed to form the organoaminopolysiloxane compound from the reaction mixture.
[0083] The organoaminopolysiloxane precursor compounds of formula A to H according to the present invention and compositions comprising the organoaminopolysiloxane precursor compounds of formula A to H according to the present invention are preferably substantially free of halide ions. As used herein, the term "substantially free" when it relates to halide ions (or halides) (e.g., chlorides and fluorides, bromides and iodides) means less than 5 ppm (by weight) as measured by ICP-MS, preferably less than 3 ppm as measured by ICP-MS, more preferably less than 1 ppm as measured by ICP-MS, and most preferably 0 ppm as measured by ICP-MS. Chlorides are known to act as decomposition catalysts for organoaminopolysiloxane precursor compounds of formulas A to H. Significant levels of chloride in the final product can lead to degradation of the organoaminopolysiloxane precursor compounds. The gradual degradation of the organoaminopolysiloxane precursor compounds can directly affect the film deposition process, making it difficult for semiconductor manufacturers to meet film specifications. In addition, the higher degradation rate of the organoaminopolysiloxane precursor compounds has a negative impact on the shelf life or stability, making it difficult to guarantee a shelf life of 1-2 years. Therefore, the accelerated decomposition of the organoaminopolysiloxane precursor compounds raises safety and performance issues related to the formation of these flammable and / or self-igniting gaseous byproducts. The organoaminopolysiloxane precursor compounds of formulas A to H are preferably substantially free of metal ions or metals, such as Li, Mg, Ca, K, Al, Fe, Ni, Cr, as measured by ICP-MS or other analytical methods for measuring metals. As used herein, the term "substantially free" when it refers to Li, Mg, Ca, K, Al, Fe, Ni, Cr refers to less than 5ppm (by weight) measured by ICP-MS, preferably less than 3ppm, more preferably less than 1ppm, and most preferably 0.1ppm. In some embodiments, the organoaminopolysiloxane precursor compounds of formulas A to H are free of metals, such as Li, Mg, Ca, K, Al, Fe, Ni, Cr. As used herein, the term "free of" metal ions or metal impurities as it relates to Li, Mg, Ca, K, Al, Fe, Ni, Cr, precious metals such as volatile Ru or Pt complexes from ruthenium or platinum catalysts used in the synthesis means less than 1 ppm, preferably 0.1 ppm (by weight) as measured by ICP-MS or other analytical methods for measuring metals.
[0084] For those embodiments in which at least one organoaminopolysiloxane precursor of formula A to H is used in a composition comprising a solvent, the selected solvent or mixture thereof does not react with the organoaminopolysiloxane precursor. The amount of solvent in the composition by weight percentage ranges from 0.5 wt % to 99.5 wt % or 10 wt % to 75 wt % to adjust the physical properties of the resulting composition for direct liquid injection, such as viscosity. In this or other embodiments, the solvent has a boiling point (bp) similar to that of the organoaminopolysiloxane precursor of formula A to H, or the difference between the bp of the solvent and the bp of the organoaminopolysiloxane precursor of formula A to H is 40°C or less, 30°C or less, or 20°C or less, or 10°C. Alternatively, the difference between the boiling points is within the boiling point range of any one or more of the following endpoints: 0, 10, 20, 30 or 40°C. Examples of suitable ranges of bp differences include, but are not limited to, 0 to 40°C, 20°C to 30°C, or 10°C to 30°C. Examples of suitable solvents in the composition include, but are not limited to, ethers (e.g., 1,4-dioxane, dibutyl ether), tertiary amines (e.g., pyridine, 1-methylpiperidine, 1-ethylpiperidine, N,N'-dimethylpiperazine, N,N,N',N'-tetramethylethylenediamine), nitriles (e.g., benzonitrile), alkyl hydrocarbons (e.g., octane, nonane, dodecane, ethylcyclohexane), siloxanes (e.g., hexamethyldisiloxane, octamethyltrisiloxane), aromatic hydrocarbons (e.g., toluene, mesitylene), tertiary amino ethers (e.g., bis(2-dimethylaminoethyl) ether), or mixtures thereof.
[0085] Another embodiment of the present invention is directed to a silicon oxide film having at least one of the following characteristics: a density of at least about 2.1 g / cc; a wet etch rate of less than about 2.5 angstroms / second as measured in a dilute HF acid solution of 1:100 HF to water (0.5 wt. % dHF); a leakage current of less than about 1e-8 A / cm at up to 6 MV / cm 2 ; and a hydrogen impurity of less than about 5e20 at / cc as measured by secondary ion mass spectroscopy (SIMS).
[0086] In another aspect, a method for depositing a film comprising silicon and an oxide onto a substrate is provided, the method comprising the steps of: a) providing a substrate in a reactor; b) introducing into the reactor a composition comprising at least one organoaminopolysiloxane compound selected from the group consisting of Formula A, B, C, D, E, F, G and H:
[0087]
[0088] Where R 1 Selected from straight chain C 1 To C 10 Alkyl, branched chain C 3 To C 10 Alkyl, C3 To C 10 Cycloalkyl, C 3 To C 10 Heterocyclic group, C 3 To C 10 Alkenyl, C 3 To C 10 Alkynyl and C 4 To C 10 Aryl; R 2 Selected from hydrogen, straight chain C 1 To C 10 Alkyl, branched chain C 3 To C 10 Alkyl, C 3 To C 10 Cycloalkyl, C 3 To C 10 Heterocyclic group, C 3 To C 10 Alkenyl, C 3 To C 10 Alkynyl and C 4 To C 10 Aryl, wherein R in the formula AH 1 and R 2 connected to form an annular ring structure or not connected to form an annular ring; c) purging the reactor with a purge gas; d) introducing at least one of an oxygen-containing source and a nitrogen-containing source into the reactor; and e) purging the reactor with the purge gas, wherein steps b to e are repeated until a film of a desired thickness is deposited; wherein the method is carried out at one or more temperatures in the range of about 25°C to 600°C.
[0089] The method disclosed herein forms a silicon oxide film having at least one of the following properties: a density of at least about 2.1 g / cc; a wet etch rate of less than about 2.5 angstroms / second as measured in a dilute HF acid solution of 1:100 HF to water (0.5 wt % dHF); a leakage current of less than about 1e-8 A / cm at up to 6 MV / cm 2 ; and hydrogen impurities less than about 5e20at / cc as measured by secondary ion mass spectroscopy (SIMS).
[0090] In certain embodiments of the methods and compositions described herein, for example, a silicon-containing dielectric material layer is deposited on at least a portion of a substrate by a chemical vapor deposition (CVD) process using a reaction chamber. Suitable substrates include, but are not limited to, semiconductor materials such as gallium arsenide ("GaAs"), silicon, and silicon-containing compositions such as crystalline silicon, polycrystalline silicon, amorphous silicon, epitaxial silicon, silicon dioxide ("SiO 2”), silicon glass, silicon nitride, fused silica, glass, quartz, borosilicate glass and combinations thereof. Other suitable materials include chromium, molybdenum and other metals commonly used in semiconductor, integrated circuit, flat panel display and flexible display applications. The substrate may have additional layers such as silicon, SiO 2 , organosilicate glass (OSG), fluorinated silicate glass (FSG), boron carbonitride, silicon carbide, hydrogenated silicon carbide, silicon nitride, hydrogenated silicon nitride, silicon carbonitride, hydrogenated silicon carbonitride, boron nitride, organic-inorganic composites, photoresists, organic polymers, porous organic and inorganic materials and composites, metal oxides such as aluminum oxide and germanium oxide. Further layers can also be germanosilicates, aluminosilicates, copper and aluminum, and diffusion barrier materials such as but not limited to TiN, Ti(C)N, TaN, Ta(C)N, Ta, W or WN.
[0091] The deposition methods disclosed herein may include one or more purge gases. The purge gas used to purge away unconsumed reactants and / or reaction byproducts is an inert gas that does not react with the precursor. Exemplary purge gases include, but are not limited to, argon (Ar), nitrogen (N 2 ), helium (He), neon, hydrogen (H 2 ) and mixtures thereof. In certain embodiments, a purge gas such as Ar is supplied to the reactor at a flow rate of about 10 to about 2000 sccm for about 0.1 to 1000 seconds to purge unreacted materials and any byproducts that may remain in the reactor.
[0092] A purge gas such as argon purges the unabsorbed excess complex from the process chamber. After sufficient purging, an oxygen source can be introduced into the reaction chamber to react with the absorbed surface, followed by another gas purge to remove the reaction byproducts from the chamber. This process cycle can be repeated to achieve the desired film thickness. In some cases, pumping can replace the inert gas purge, or both can be used to remove unreacted silicon precursor.
[0093] Throughout the specification, the term "ALD or ALD-like" refers to a process including but not limited to the following processes: a) each reactant including a silicon precursor and a reactive gas is sequentially introduced into a reactor such as a single wafer ALD reactor, a semi-batch ALD reactor or a batch furnace ALD reactor; b) each reactant including a silicon precursor and a reactive gas is exposed to the substrate by moving or rotating the substrate to different sections of the reactor, and each section is separated by an inert gas curtain, i.e., a spatial ALD reactor or a roll-to-roll ALD reactor.
[0094] The method of the present invention is performed by an ALD process using an ozone or oxygen-containing source including a plasma, wherein the plasma may also contain an inert gas, such as one or more of the following: an oxygen plasma with or without an inert gas, a water vapor plasma with or without an inert gas, a nitrogen oxide (such as N 2 O, NO, NO 2 ) plasma, carbon oxides with or without inert gases (such as CO 2 , CO) plasma and combinations thereof.
[0095] The oxygen-containing plasma source may be generated in situ, or alternatively remotely. In a particular embodiment, the oxygen-containing source comprises oxygen and is flowed or introduced during process steps b to d along with other reagents such as, but not limited to, at least one organoaminopolysiloxane precursor and optionally an inert gas.
[0096] In one or more of the above embodiments, the oxygen-containing plasma source is selected from oxygen plasma with or without an inert gas, water vapor plasma with or without an inert gas, nitrogen oxide (N 2 O, NO, NO 2 ) plasma, carbon oxides (CO 2 , CO) plasma and combinations thereof. In certain embodiments, the oxygen-containing plasma source further comprises an inert gas. In these embodiments, the inert gas is selected from argon, helium, nitrogen, hydrogen or a combination thereof. In alternative embodiments, the oxygen-containing plasma source does not comprise an inert gas.
[0097] In certain embodiments, the silicon oxide or carbon-doped silicon oxide film deposited using the methods described herein is subjected to an atmosphere comprising ozone, water (H 2 O) (e.g., deionized water, purified water and / or distilled water), oxygen (O 2 ), oxygen plasma, NO, N 2 O、NO 2 , carbon monoxide (CO), carbon dioxide (CO 2) and combinations thereof. The oxygen-containing source is provided by, for example, an in-situ or remote plasma generator to provide an oxygen-containing plasma source comprising oxygen, such as an oxygen plasma, a plasma comprising oxygen and argon, a plasma comprising oxygen and helium, an ozone plasma, a water plasma, a nitrous oxide plasma, or a carbon dioxide plasma. In certain embodiments, the oxygen-containing plasma source comprises an oxygen source gas introduced into the reactor at a flow rate of about 1 to about 2000 standard cubic centimeters per minute (sccm) or about 1 to about 1000 sccm. The oxygen-containing plasma source can be introduced for a time of about 0.1 to about 100 seconds. In a specific embodiment, the oxygen-containing plasma source comprises water having a temperature of 10° C. or higher. In embodiments where the film is deposited by a PEALD or plasma enhanced cyclic CVD process, the precursor pulse may have a pulse duration greater than 0.01 seconds (e.g., from about 0.01 to about 0.1 seconds, from about 0.1 to about 0.5 seconds, from about 0.5 to about 10 seconds, from about 0.5 to about 20 seconds, from about 1 to about 100 seconds) depending on the volume of the ALD reactor, and the oxygen-containing plasma source may have a pulse duration less than 0.01 seconds (e.g., from about 0.001 to about 0.01 seconds).
[0098] The deposition methods disclosed herein may include one or more purge gases. The purge gas used to purge away unconsumed reactants and / or reaction byproducts is an inert gas that does not react with the precursor. Exemplary purge gases include, but are not limited to, argon (Ar), nitrogen (N 2 ), helium (He), neon, hydrogen (H 2 ) and mixtures thereof. In certain embodiments, a purge gas such as Ar is supplied to the reactor at a flow rate of about 10 to about 2000 sccm for about 0.1 to 1000 seconds to purge unreacted materials and any byproducts that may remain in the reactor.
[0099] The respective steps of supplying precursors, oxygen sources and / or other precursors, source gases and / or reagents may be performed by varying the time at which they are supplied to change the stoichiometric composition of the resulting dielectric film.
[0100] Energy is applied to at least one of the organoaminopolysiloxane precursors of formulas A to H, an oxygen-containing source, or a combination thereof to initiate a reaction and form a dielectric film or coating on a substrate. Such energy can be provided by, but is not limited to, heat, plasma, pulsed plasma, helicon plasma, high-density plasma, inductively coupled plasma, X-rays, electron beams, photons, remote plasma methods, and combinations thereof. In certain embodiments, a secondary RF radio frequency source can be used to change the plasma characteristics at the substrate surface. In embodiments where the deposition involves plasma, the plasma generation process can include a direct plasma generation process (wherein the plasma is directly generated in the reactor) or a remote plasma generation process (wherein the plasma is generated outside the reactor and supplied to the reactor).
[0101] At least one organoaminopolysiloxane precursor can be delivered to a reaction chamber, such as a plasma enhanced cyclic CVD or PEALD reactor or a batch furnace reactor, in various ways. In one embodiment, a liquid delivery system can be used. In an alternative embodiment, a combined liquid delivery and flash processing unit can be used, such as a turbo evaporator manufactured by MSP Corporation, Shoreview, MN, so that low volatility materials can be quantitatively (volumetrically) delivered, which results in repeatable delivery and deposition without thermal decomposition of the precursor. In a liquid delivery configuration, the precursor described herein can be delivered in pure liquid form, or can be used in a solvent formulation or composition comprising it. Therefore, in certain embodiments, the precursor formulation can include a solvent component with suitable properties (such as may be desired and advantageous in a given end-use application) to form a film on a substrate.
[0102] As previously described, the purity level of the at least one organoaminopolysiloxane precursor is high enough to be acceptable for reliable semiconductor manufacturing. In certain embodiments, the at least one organoaminopolysiloxane precursor described herein contains less than 2% by weight, or less than 1% by weight, or less than 0.5% by weight of one or more of the following impurities: free amine, free halide or halide ion, and higher molecular weight species. The higher purity levels of the organoaminopolysiloxane precursors described herein can be obtained by one or more of the following methods: purification, adsorption and / or distillation.
[0103] In one embodiment of the methods described herein, a plasma enhanced cyclic deposition process, such as PEALD-like or PEALD, can be used, wherein deposition is performed using at least one organoaminopolysiloxane precursor and an oxygen plasma source. A PEALD-like process is defined as a plasma enhanced cyclic CVD process, but still provides highly conformal silicon and oxygen containing films.
[0104] In certain embodiments, the gas line connecting the precursor tank to the reaction chamber is heated to one or more temperatures depending on the process requirements, and the container of at least one organoaminopolysiloxane precursor is maintained at one or more temperatures for bubbling. In other embodiments, the solution containing at least one organoaminopolysiloxane precursor is injected into a vaporizer maintained at one or more temperatures for direct liquid injection.
[0105] A flow of argon and / or other gases may be used as a carrier gas to help deliver the vapor of at least one organoaminopolysiloxane precursor to the reaction chamber during the precursor pulse. In certain embodiments, the reaction chamber process pressure is about 50 mTorr to 10 Torr. In other embodiments, the reaction chamber process pressure may be up to 760 Torr (e.g., about 50 mTorr to about 100 Torr).
[0106] In a typical PEALD or PEALD-like process (eg, PECCVD process), a substrate such as a silicon oxide substrate is heated on a heater stage in a reaction chamber that is initially exposed to an organoaminopolysiloxane precursor to allow the complex to be chemically adsorbed onto the substrate surface.
[0107] A purge gas such as argon is used to purge the unabsorbed excess complex from the process chamber. After sufficient purging, an oxygen source can be introduced into the reaction chamber to react with the absorbed surface, followed by another gas purge to remove the reaction byproducts from the chamber. This process cycle can be repeated to achieve the desired film thickness. In some cases, pumping can replace the inert gas purge, or both can be used to remove unreacted silicon precursor.
[0108] In this or other embodiments, it should be understood that the steps of the methods described herein can be performed in a variety of orders, can be performed sequentially, can be performed simultaneously (e.g., during at least a portion of another step), and any combination thereof. For example, the respective steps of supplying precursor and oxygen source gases can be performed by varying the duration of supplying them to change the stoichiometric composition of the resulting dielectric film. Moreover, the purge time after the precursor or oxidant step can be minimized to <0.1 s, thereby improving throughput.
[0109] In another embodiment, described herein is a vessel or container for using a composition for depositing silicon oxide, the composition comprising at least an organoaminopolysiloxane precursor having a structure represented by Formulas A to H and / or a solvent.
[0110] In one particular embodiment, the vessel or container (vessels and containers are interchangeable) comprises at least one pressurizable container (preferably constructed of stainless steel) equipped with appropriate valves and fittings to allow one or more precursors to be delivered to the reactor for a deposition process, such as an ALD or PEALD process. In this or other embodiments, a composition comprising at least one organoaminopolysiloxane precursor having a structure represented by Formulas A to H, and a gas selected from argon (Ar), nitrogen (N 2 ), helium (He), neon and combinations thereof are provided in a pressurizable container made of stainless steel, and the purity of the precursor is 98 wt % or higher or 99.5 % or higher, which is suitable for most semiconductor applications.
[0111] In one embodiment of the present invention, a method for depositing a film containing silicon and oxygen on at least one surface of a substrate is described herein, wherein the method comprises the following steps:
[0112] a. providing a substrate in a reactor;
[0113] b. introducing into the reactor at least one organoaminopolysiloxane precursor having formula A to H as defined above;
[0114] c. purging the reactor with a purge gas;
[0115] d. introducing into the reactor an oxygen-containing source comprising a plasma; and
[0116] e. Purge the reactor with a purge gas.
[0117] In this method, steps b to e are repeated until a film of desired thickness is deposited on the substrate.
[0118] In a particular embodiment, the method described herein deposits a high quality silicon and oxygen containing film on a substrate. The method comprises the following steps:
[0119] a. providing a substrate in a reactor;
[0120] b. introducing into the reactor at least one organoaminopolysiloxane precursor having formula A to H as described herein;
[0121] c. purging the reactor with a purge gas to remove at least a portion of the unabsorbed precursor;
[0122] d. introducing an oxygen-containing plasma source into the reactor; and
[0123] e. purging the reactor with a purge gas to remove at least a portion of the unreacted oxygen source,
[0124] Steps b to e are repeated until a silicon-containing film of a desired thickness is deposited.
[0125] In another particular embodiment, the method described herein deposits a high quality silicon and oxygen containing film on a substrate at a temperature above 600° C. The method comprises the following steps:
[0126] a. providing a substrate in a reactor;
[0127] b. introducing into the reactor at least one organoaminopolysiloxane precursor having formula A or C as described herein;
[0128] c. purging the reactor with a purge gas to remove at least a portion of the unabsorbed precursor;
[0129] d. introducing an oxygen-containing plasma source into the reactor; and
[0130] e. purging the reactor with a purge gas to remove at least a portion of the unreacted oxygen source,
[0131] wherein steps b to e are repeated until a silicon-containing film of the desired thickness is deposited. It is believed that organoaminopolysiloxane precursors of formula A and C are preferred for use in this method because they do not contain any Si-H groups, which may decompose at temperatures above 600° C. and may potentially lead to undesirable chemical vapor deposition. However, it is possible that under certain conditions, such as using short precursor pulses or low reactor pressures or rotating the substrate, the method can be carried out at temperatures above 600° C. using organoaminopolysiloxane precursors of formula B, D, E, F, G or H without significant undesirable chemical vapor deposition.
[0132] Another method disclosed herein forms a carbon-doped silicon oxide film using an organoaminopolysiloxane precursor compound having a chemical structure represented by Formulae A to H as defined above plus an oxygen source.
[0133] Another exemplary method is described as follows:
[0134] a. providing a substrate in a reactor;
[0135] b. contacting the vapor generated from at least one organoaminopolysiloxane precursor compound having a structure represented by Formulas A to H as defined above with or without a co-flowing oxygen source to chemically absorb the precursor onto the heated substrate;
[0136] c. Purge any unabsorbed precursor;
[0137] d. introducing an oxygen source onto the heated substrate to react with the absorbed precursor; and
[0138] e. Purge any unreacted oxygen source,
[0139] Steps b to e are repeated until the desired thickness is reached.
[0140] In another specific embodiment, the method described herein deposits a high quality silicon oxynitride film on a substrate. The method comprises the following steps:
[0141] a. providing a substrate in a reactor;
[0142] b. introducing into the reactor at least one organoaminopolysiloxane precursor having formula A to H as described herein;
[0143] c. purging the reactor with a purge gas to remove at least a portion of the unabsorbed precursor;
[0144] d. introducing a nitrogen-containing plasma source into the reactor; and
[0145] e. purging the reactor with a purge gas to remove at least a portion of the unreacted nitrogen source,
[0146] Steps b to e are repeated until a silicon oxynitride-containing film having a desired thickness is deposited.
[0147] Another exemplary method is described as follows:
[0148] a. providing a substrate in a reactor;
[0149] b. contacting the vapor generated from at least one organoaminopolysiloxane precursor compound having a structure represented by Formulas A to H as defined above with or without a co-flowing nitrogen source to chemically absorb the precursor onto the heated substrate;
[0150] c. Purge any unabsorbed precursors;
[0151] d. introducing a nitrogen source onto the heated substrate to react with the absorbed precursor; and
[0152] e. Purge any unreacted nitrogen source,
[0153] Steps b to e are repeated until the desired thickness is reached.
[0154] Another exemplary method is described as follows:
[0155] a. providing a substrate in a reactor;
[0156] b. contacting the vapor generated from at least one organoaminopolysiloxane precursor compound having a structure represented by Formulas A to H as defined above with or without a co-flowing nitrogen source to chemically absorb the precursor onto the heated substrate;
[0157] c. Purge any unabsorbed precursors;
[0158] d. introducing a nitrogen source onto the heated substrate to react with the absorbed precursor; and
[0159] e. Purge any unreacted nitrogen source,
[0160] f. introducing an oxygen source onto the heated substrate to react with the absorbed precursor; and
[0161] g. Purge any unreacted nitrogen source,
[0162] Steps b to g are repeated until a desired thickness of the silicon oxynitride-containing film is achieved. In other embodiments, step f may be performed instead of step d, ie, an oxygen source is introduced before a nitrogen source to provide a film containing silicon oxynitride.
[0163] Various commercial ALD reactors such as single wafer, semi-batch, batch furnaces or roll-to-roll reactors can be used to deposit solid silicon oxide, silicon oxynitride, carbon-doped silicon oxynitride or carbon-doped silicon oxide.
[0164] The process temperatures of the methods described herein use one or more of the following temperatures as endpoints: 0°C, 25°C, 50°C, 75°C, 100°C, 125°C, 150°C, 175°C, 200°C, 225°C, 250°C, 275°C, 300°C, 325°C, 350°C, 375°C, 400°C, 425°C, 450°C, 500°C, 525°C, 550°C, 600°C, 650°C, 700°C, 750°C, 760°C, and 800°C. Exemplary low temperature ranges include, but are not limited to, about 0°C to about 300°C; or about 25°C to about 300°C; or about 50°C to about 290°C; or about 25°C to about 250°C, or about 25°C to about 200°C. Exemplary high temperature ranges include, but are not limited to, about 600°C to about 800°C, about 700°C to 800°C.
[0165] In another aspect, there is provided a method of depositing a film comprising silicon and oxygen by flowable chemical vapor deposition (FCVD), the method comprising:
[0166] placing a substrate comprising surface features in a reactor, wherein the substrate is maintained at one or more temperatures in the range of about -20°C to about 400°C and the pressure of the reactor is maintained at 100 Torr or less;
[0167] Introducing at least one compound selected from formulae A to H:
[0168] providing an oxygen source into the reactor to react with the at least one compound to form a film and cover at least a portion of the surface feature;
[0169] annealing the film at one or more temperatures of about 100° C. to 1000° C. to coat at least a portion of the surface features; and
[0170] The substrate is treated with an oxygen source at one or more temperatures in a range of about 20° C. to about 1000° C. to form the silicon-containing film on at least a portion of the surface features.
[0171] In another aspect, there is provided a method of depositing a film comprising silicon, oxygen, and nitrogen by flowable chemical vapor deposition (FCVD), the method comprising:
[0172] placing a substrate comprising surface features in a reactor, wherein the substrate is maintained at one or more temperatures in the range of about -20°C to about 400°C and the pressure of the reactor is maintained at 100 Torr or less;
[0173] Introducing at least one compound selected from formulae A to H:
[0174] providing a nitrogen source into the reactor to react with the at least one compound to form a film and cover at least a portion of the surface feature;
[0175] annealing the film at one or more temperatures in the range of about 100° C. to 1000° C. to coat at least a portion of the surface features; and
[0176] The substrate is treated with an oxygen source at one or more temperatures ranging from about 20° C. to about 1000° C. to form the silicon-containing film on at least a portion of the surface features.
[0177] In certain embodiments, the oxygen source is selected from water vapor, water plasma, ozone, oxygen, oxygen plasma, oxygen / helium plasma, oxygen / argon plasma, nitrogen oxide plasma, carbon dioxide plasma, hydrogen peroxide, organic peroxides, and mixtures thereof. In other embodiments, the nitrogen source is selected from, for example, ammonia, hydrazine, monoalkylhydrazine, dialkylhydrazine, nitrogen, nitrogen / hydrogen, nitrogen / argon plasma, nitrogen / helium plasma, ammonia plasma, nitrogen plasma, nitrogen / hydrogen plasma, organic amines such as tert-butylamine, dimethylamine, diethylamine, isopropylamine, diethylamine plasma, dimethylamine plasma, trimethyl plasma, trimethylamine plasma, ethylenediamine plasma, and alkoxyamines such as ethanolamine plasma, and mixtures thereof. In yet other embodiments, the nitrogen-containing source includes ammonia plasma, a plasma comprising nitrogen and argon, a plasma comprising nitrogen and helium, or a plasma comprising hydrogen and nitrogen source gas. In this or other embodiments, the method steps are repeated until the surface features are filled with a silicon-containing film. In embodiments in which water vapor is used as an oxygen source in a flowable chemical vapor deposition process, the substrate temperature is from about -20°C to about 40°C or from about -10°C to about 25°C.
[0178] In yet another embodiment of the methods described herein, the film deposited by ALD, ALD-like, PEALD, PEALD-like, or FCVD, or the film so deposited, is subjected to a treatment step (post-deposition). The treatment step can be performed during at least a portion of the deposition step, after the deposition step, and combinations thereof. Exemplary treatment steps include, but are not limited to, treatment by high temperature thermal annealing; plasma treatment; ultraviolet (UV) light treatment; laser; electron beam treatment, and combinations thereof, to affect one or more properties of the film.
[0179] Films deposited with the organoaminopolysiloxane precursors of Formulae A to H described herein have improved properties, such as, but not limited to, a wet etch rate that is lower than the wet etch rate of the film prior to the treatment step, or a density that is higher than the density prior to the treatment step, compared to films deposited with previously disclosed silicon precursors under the same conditions. In a particular embodiment, the films so deposited are treated intermittently during the deposition process. These intermittent or mid-deposition treatments can be performed, for example, after each ALD cycle, after each certain number of ALD cycles (such as, but not limited to, one (1) ALD cycle, two (2) ALD cycles, five (5) ALD cycles, or after every ten (10) or more ALD cycles).
[0180] The precursors of formula A to H exhibit / cycle or higher growth rate.
[0181] In embodiments where the film is treated with a high temperature annealing step, the annealing temperature is at least 100°C or above the deposition temperature. In this or other embodiments, the annealing temperature is in the range of about 400°C to about 1000°C. In this or other embodiments, the annealing process can be performed in a vacuum (<760 Torr), an inert environment, or an oxygen-containing environment (e.g., H 2 O、N 2 O、NO 2 or 2 ) is carried out in
[0182] In embodiments where the film is UV treated, the film is exposed to broadband UV, or alternatively a UV source having a wavelength in the range of about 150 nanometers (nm) to about 400 nm. In a particular embodiment, after the desired film thickness is reached, the film so deposited is exposed to UV in a chamber different from the deposition chamber.
[0183] In embodiments where the film is treated with plasma, a passivation layer (e.g., SiO 2 or carbon-doped SiO 2 ) to prevent chlorine and nitrogen contaminants from penetrating into the film during subsequent plasma processing. The passivation layer can be deposited using atomic layer deposition or cyclic chemical vapor deposition.
[0184] In embodiments where the film is treated with plasma, the plasma source is selected from hydrogen plasma, plasma containing hydrogen and helium, plasma containing hydrogen and argon. Hydrogen plasma reduces the dielectric constant of the film and enhances damage resistance to subsequent plasma ashing processes while still keeping the bulk carbon content nearly unchanged.
[0185] Without intending to be bound by a particular theory, it is believed that the organoaminopolysiloxane precursor compound having a chemical structure represented by Formulas A to H as defined above can be anchored by reacting the organoamino group with the hydroxyl group on the surface of the substrate to provide a plurality of Si-O-Si fragments, thereby increasing the growth rate of silicon oxide or carbon-doped silicon oxide compared to conventional silicon precursors having only one silicon atom, such as bis(tert-butylamino)silane or bis(diethylamino)silane.
[0186] In certain embodiments, the organoaminopolysiloxane precursors of formulas A to H as defined above may also be used as dopants for metal-containing films (e.g., but not limited to, metal oxide films or metal oxynitride films). In these embodiments, metal alkoxides, metal amides, or volatile organometallic precursors are used to deposit the metal-containing film using an ALD or CVD process (e.g., those described herein). Examples of suitable metal alkoxide precursors that can be used with the methods disclosed herein include, but are not limited to, Group 3 to 6 metal alkoxides, Group 3 to 6 metal complexes with both alkoxy and alkyl-substituted cyclopentadienyl ligands, Group 3 to 6 metal complexes with both alkoxy and alkyl-substituted pyrrolyl ligands, Group 3 to 6 metal complexes with both alkoxy and diketonate ligands, and Group 3-6 metal complexes with both alkoxy and ketoester ligands.
[0187] Examples of suitable metal amide precursors that can be used with the methods disclosed herein include, but are not limited to, tetrakis(dimethylamino)zirconium (TDMAZ), tetrakis(diethylamino)zirconium (TDEAZ), tetrakis(ethylmethylamino)zirconium (TEMAZ), tetrakis(dimethylamino)hafnium (TDMAH), tetrakis(diethylamino)hafnium (TDEAH), and tetrakis(ethylmethylamino)hafnium (TEMAH), tetrakis(dimethylamino)titanium (TDMAT), tetrakis(diethylamino)titanium (TDEAT), tetrakis(ethylmethylamino)titanium (TEMAT), tert-butyliminotris(diethylamino)tantalum (TBTDET), tert-butyliminotris(dimethylamino)tantalum (TBTDET), and tert-butyliminotris(dimethylamino)tantalum (TBTDET). Tantalum (MT), tert-butyliminotris(ethylmethylamino)tantalum (TBTEMT), ethyliminotris(diethylamino)tantalum (EITDET), ethyliminotris(dimethylamino)tantalum (EITDMT), ethyliminotris(ethylmethylamino)tantalum (EITEMT), tert-amyliminotris(dimethylamino)tantalum (TAIMAT), tert-amyliminotris(diethylamino)tantalum, penta(dimethylamino)tantalum, tert-amyliminotris(ethylmethylamino)tantalum, bis(tert-butylimino)bis(dimethylamino)tungsten (BTBMW), bis(tert-butylimino)bis(diethylamino)tungsten, bis(tert-butylimino)bis(ethylmethylamino)tungsten, and combinations thereof. Examples of suitable organometallic precursors that can be used with the methods disclosed herein include, but are not limited to, Group 3 metal cyclopentadienyls or alkyl cyclopentadienyls. Exemplary Group 3 to 6 metals herein include, but are not limited to, Y, La, Ce, Pr, Nd, Sm, Eu, Gd, Tb, Dy, Er, Yb, Lu, Ti, Hf, Zr, V, Nb, Ta, Cr, Mo, and W.
[0188] In certain embodiments, the silicon-containing films described herein have a dielectric constant of 6 or less, 5 or less, 4 or less, and 3 or less. In these or other embodiments, the film may have a dielectric constant of about 5 or less, or about 4 or less, or about 3.5 or less. However, it is contemplated that films having other dielectric constants (e.g., higher or lower) may be formed depending on the desired end use of the film. Examples of silicon-containing films formed using organoaminopolysiloxane precursors having precursors of Formulas A to H and the methods described herein have a dielectric constant of about 5 or less, or about 4 or less, or about 3.5 or less. However, it is contemplated that films having other dielectric constants (e.g., higher or lower) may be formed depending on the desired end use of the film. x O y C z N v H w, wherein Si is in the range of about 10% to about 40%; O is in the range of about 0% to about 65%; C is in the range of about 0% to about 75% or about 0% to about 50%; N is in the range of about 0% to about 75% or about 0% to 50%; and H is in the range of about 0% to about 50% (atomic weight %), wherein x+y+z+v+w=100 atomic weight %, as determined, for example, by XPS or other methods. Another example of a silicon-containing film formed using the organoaminopolysiloxane precursors of Formulas A to H and the methods described herein is a silicon oxycarbonitride, wherein the carbon content measured by XPS is 1 atomic % to 80 atomic %. Yet another example of a silicon-containing film formed using the organoaminopolysiloxane precursors having Formulas A to H and the methods described herein is an amorphous silicon film, wherein the sum of both nitrogen and carbon contents measured by XPS is <10 atomic %, preferably <5 atomic %, and most preferably <1 atomic %.
[0189] As previously mentioned, the methods described herein can be used to deposit a silicon-containing film on at least a portion of a substrate. Examples of suitable substrates include, but are not limited to, silicon, SiO 2 、Si 3 N 4 , OSG, FSG, silicon carbide, hydrogenated silicon oxycarbide, hydrogenated silicon oxynitride, silicon oxycarbonitride, hydrogenated silicon oxycarbonitride, anti-reflective coatings, photoresists, germanium, germanium-containing, boron-containing, Ga / As, flexible substrates, organic polymers, porous organic and inorganic materials, metals such as copper and aluminum and diffusion barriers such as but not limited to TiN, Ti(C)N, TaN, Ta(C)N, Ta, W or WN. The film is compatible with various subsequent processing steps such as chemical mechanical planarization (CMP) and anisotropic etching processes.
[0190] The deposited films have applications including, but not limited to, computer chips, optical devices, magnetic information storage, coatings on support materials or substrates, microelectromechanical systems (MEMS), nanoelectromechanical systems, thin film transistors (TFT), light emitting diodes (LED), organic light emitting diodes (OLED), IGZO, and liquid crystal displays (LCD). Potential uses of the resulting solid silicon oxide or carbon-doped silicon oxide include, but are not limited to, shallow trench isolation, interlayer dielectric layers, passivation layers, etch stop layers, portions of dual spacers, and sacrificial layers for patterning.
[0191] The methods described herein provide high quality silicon oxide, silicon oxynitride, carbon-doped silicon oxynitride, or carbon-doped silicon oxide films. The term "high quality" refers to films that exhibit one or more of the following characteristics: a density of about 2.1 g / cc or more, 2.2 g / cc or more, 2.25 g / cc or more; a density as measured in a dilute HF acid solution of 1:100 HF to water (0.5 wt % dHF); or lower, or lower, or lower, or lower, or lower, or lower, or lower, Or lower wet etch rate; up to about 1e-8A / cm at 6MV / cm 2 or less; and hydrogen impurities of about 5e20at / cc or less as measured by SIMS; and combinations thereof. With respect to etch rate, thermally grown silicon oxide films have an etch rate of about 1.040 wt. % HF. The etching rate.
[0192] In certain embodiments, one or more organoaminopolysiloxane precursors having Formulae A to H described herein may be used to form silicon and oxygen containing films that are solid and non-porous or substantially non-porous.
[0193] Therefore, the present invention provides at least the following:
[0194] 1. A composition comprising at least one organoaminopolysiloxane compound selected from the group consisting of formula A, B, C, D, E, F, G and H:
[0195]
[0196] in,
[0197] R 1 Selected from straight chain C 1 To C 10 Alkyl, branched chain C 3 To C 10 Alkyl, C 3 To C 10 Cycloalkyl, C 3 To C 10 Heterocyclic group, C 3 To C 10 Alkenyl, C 3 To C 10 Alkynyl and C 4 To C 10 aryl; and
[0198] R 2 Selected from hydrogen, straight chain C 1 To C 10 Alkyl, branched chain C 3 To C 10 Alkyl, C 3 To C 10 Cycloalkyl, C 3 To C 10 Heterocyclic group, C 3 To C 10 Alkenyl, C 3 To C10 Alkynyl and C 4 To C 10 Aryl,
[0199] The R in the formula AH 1 and R 2 connected to form an cyclic ring structure or not connected to form an cyclic ring structure.
[0200] 2. The composition according to item 1, comprising at least one compound selected from formula A and formula C.
[0201] 3. The composition according to item 1, further comprising at least one member selected from a solvent and a purge gas.
[0202] 4. A composition according to item 3, wherein the solvent is selected from hexamethyldisiloxane and octamethyltrisiloxane.
[0203] 5. The composition according to item 3, wherein the solvent is selected from hexane, heptane, octane, nonane, decane, dodecane, cyclooctane, cyclononane, cyclodecane, ethylcyclohexane and ethylcyclooctane.
[0204] 6. A composition according to item 1, wherein R 1 and R 2 Each is C 1 To C 4 alkyl.
[0205] 7. A composition according to claim 1, wherein the composition is substantially free of one or more impurities selected from halides, metal ions, metals and combinations thereof.
[0206] 8. The composition according to item 1, wherein the organoaminopolysiloxane compound is selected from 3-dimethylamino-1,1,1,3,5,5,5-heptamethyltrisiloxane, 3-diethylamino-1,1,1,3,5,5,5-heptamethyltrisiloxane, 3-ethylmethylamino-1,1,1,3,5,5,5-heptamethyltrisiloxane, 3-diisopropylamino-1,1,1,3,5,5,5-heptamethyltrisiloxane, 3-dimethylamino-1,1,3,5,5,5-pentamethyltrisiloxane, 3-diethylamino-1,1,3,5,5,5-pentamethyltrisiloxane. -pentamethyltrisiloxane, 3-dimethylamino-3-(trimethylsiloxy)-1,1,1,5,5,5-hexamethyltrisiloxane, 3-diethylamino-3-(trimethylsiloxy)-1,1,1,5,5,5-hexamethyltrisiloxane, 3-ethylmethylamino-3-(trimethylsiloxy)-1,1,1,5,5,5-heptamethyltrisiloxane, 3-diisopropylamino-3-(trimethylsiloxy)-1,1,1,5,5,5-hexamethyltrisiloxane, 3-dimethylamino-3-(dimethylsiloxy)-1,1,5,5-tetramethyltrisiloxane, 3-diethylamino-3-(dimethylsiloxy)-1,1,5,5-tetramethyltrisiloxane, 3-Ethylmethylamino-3-(dimethylsilyloxy)-1,1,5,5-tetramethyltrisiloxane, 3-Diisopropylamino-3-(dimethylsilyloxy)-1,1,5,5-tetramethyltrisiloxane, 1-Dimethylamino-3-(dimethylsilyloxy)-1,1,3,5,5-pentamethyltrisiloxane, 1-Diethylamino-3-(dimethylsilyloxy)-1,1,3,5,5-pentamethyltrisiloxane, 1-Ethylmethylamino-3-(dimethylsilyloxy)-1,1,3,5,5-pentamethyltrisiloxane, 1-Diisopropylamino-3-(dimethylsilyloxy)-1,1,3,5,5-pentamethyltrisiloxane, 3-Dimethylamino-1,1,1,5 ,5,5-hexamethyltrisiloxane, 3-diethylamino-1,1,1,5,5,5-hexamethyltrisiloxane, 3-ethylmethylamino-1,1,1,5,5,5-hexamethyltrisiloxane, 3-diisopropylamino-1,1,1,3,5,5,5-hexamethyltrisiloxane, 3-dimethylamino-1,1,5,5-tetramethyltrisiloxane, 3-diethylamino-1,1,5,5-tetramethyltrisiloxane, 3-ethylmethylamino-1,1,5,5-tetramethyltrisiloxane, 3-diisopropylamino-1,1,5,5-tetramethyltrisiloxane, 1-dimethylamino-3,3-bis(dimethylsiloxy)-1,1,5,5-tetramethyltrisiloxane, 1-diethylamino-3,3-Bis(dimethylsiloxy)-1,1,5,5-tetramethyltrisiloxane, 1-ethylmethylamino-3,3-bis(dimethylsiloxy)-1,1,5,5-tetramethyltrisiloxane, 1-diisopropylamino-3,3-bis(dimethylsiloxy)-1,1,5,5-tetramethyltrisiloxane, 3-methylamino-1,1,1,3,5,5,5-heptamethyltrisiloxane, 3-ethylamino-1,1,1,3,5,5,5-heptamethyltrisiloxane, 3-isopropylamino-1,1,1,3,5,5,5-heptamethyltrisiloxane Siloxane, 3-tert-butylamino-1,1,1,3,5,5,5-heptamethyltrisiloxane, 3-methylamino-3-(trimethylsiloxy)-1,1,1,5,5,5-hexamethyltrisiloxane, 3-ethylamino-3-(trimethylsiloxy)-1,1,1,5,5,5-hexamethyltrisiloxane, 3-isopropylamino-3-(trimethylsiloxy)-1,1,1,5,5,5-hexamethyltrisiloxane, 3-tert-butylamino-3-(trimethylsiloxy)-1,1,1,5,5,5-hexamethyltrisiloxane.
[0207] 9. A method for depositing a film comprising silicon and an oxide onto a substrate, the method comprising the steps of:
[0208] a) providing a substrate in a reactor;
[0209] b) introducing into the reactor a composition comprising at least one organoaminopolysiloxane compound selected from the group consisting of formula A, B, C, D, E, F, G and H:
[0210]
[0211] in,
[0212] R 1 Selected from straight chain C 1 To C 10 Alkyl, branched chain C 3 To C 10 Alkyl, C 3 To C 10 Cycloalkyl, C 3 To C 10 Heterocyclic group, C 3 To C 10 Alkenyl, C 3 To C 10 Alkynyl and C 4 To C 10 aryl; and
[0213] R 2 Selected from hydrogen, straight chain C 1 To C 10 Alkyl, branched chain C3 To C 10 Alkyl, C 3 To C 10 Cycloalkyl, C 3 To C 10 Heterocyclic group, C 3 To C 10 Alkenyl, C 3 To C 10 Alkynyl and C 4 To C 10 Aryl,
[0214] The R in the formula AH 1 and R 2 connected to form an annular ring structure or not connected to form an annular ring;
[0215] c) purging the reactor with a purge gas;
[0216] d) introducing at least one of an oxygen-containing source and a nitrogen-containing source into the reactor; and
[0217] e) purging the reactor with the purge gas,
[0218] wherein steps b to e are repeated until a film of desired thickness is deposited; and
[0219] wherein the method is carried out at one or more temperatures ranging from about 25°C to 600°C.
[0220] 10. The method according to item 9, wherein the organoaminopolysiloxane compound is selected from 3-dimethylamino-1,1,1,3,5,5,5-heptamethyltrisiloxane, 3-diethylamino-1,1,1,3,5,5,5-heptamethyltrisiloxane, 3-ethylmethylamino-1,1,1,3,5,5,5-heptamethyltrisiloxane, 3-diisopropylamino-1,1,1,3,5,5,5-heptamethyltrisiloxane, 3-dimethylamino-1,1,3,5,5,5-pentamethyltrisiloxane, 3-diethylamino-1,1,3,5,5,5-pentamethyltrisiloxane, 3-ethylmethylamino-1,1,1,3,5,5,5-heptamethyltrisiloxane. -pentamethyltrisiloxane, 3-dimethylamino-3-(trimethylsiloxy)-1,1,1,5,5,5-hexamethyltrisiloxane, 3-diethylamino-3-(trimethylsiloxy)-1,1,1,5,5,5-hexamethyltrisiloxane, 3-ethylmethylamino-3-(trimethylsiloxy)-1,1,1,5,5,5-heptamethyltrisiloxane, 3-diisopropylamino-3-(trimethylsiloxy)-1,1,1,5,5,5-hexamethyltrisiloxane, 3-dimethylamino-3-(dimethylsiloxy)-1,1,5,5-tetramethyltrisiloxane, 3-diethylamino-3-(dimethylsiloxy)-1,1,5,5-tetramethyltrisiloxane, 3-Ethylmethylamino-3-(dimethylsilyloxy)-1,1,5,5-tetramethyltrisiloxane, 3-Diisopropylamino-3-(dimethylsilyloxy)-1,1,5,5-tetramethyltrisiloxane, 1-Dimethylamino-3-(dimethylsilyloxy)-1,1,3,5,5-pentamethyltrisiloxane, 1-Diethylamino-3-(dimethylsilyloxy)-1,1,3,5,5-pentamethyltrisiloxane, 1-Ethylmethylamino-3-(dimethylsilyloxy)-1,1,3,5,5-pentamethyltrisiloxane, 1-Diisopropylamino-3-(dimethylsilyloxy)-1,1,3,5,5-pentamethyltrisiloxane, 3-Dimethylamino-1,1,1,5 ,5,5-hexamethyltrisiloxane, 3-diethylamino-1,1,1,5,5,5-hexamethyltrisiloxane, 3-ethylmethylamino-1,1,1,5,5,5-hexamethyltrisiloxane, 3-diisopropylamino-1,1,1,3,5,5,5-hexamethyltrisiloxane, 3-dimethylamino-1,1,5,5-tetramethyltrisiloxane, 3-diethylamino-1,1,5,5-tetramethyltrisiloxane, 3-ethylmethylamino-1,1,5,5-tetramethyltrisiloxane, 3-diisopropylamino-1,1,5,5-tetramethyltrisiloxane, 1-dimethylamino-3,3-bis(dimethylsiloxy)-1,1,5,5-tetramethyltrisiloxane, 1-diethylamino-3,3-Bis(dimethylsiloxy)-1,1,5,5-tetramethyltrisiloxane, 1-ethylmethylamino-3,3-bis(dimethylsiloxy)-1,1,5,5-tetramethyltrisiloxane, 1-diisopropylamino-3,3-bis(dimethylsiloxy)-1,1,5,5-tetramethyltrisiloxane, 3-methylamino-1,1,1,3,5,5,5-heptamethyltrisiloxane, 3-ethylamino-1,1,1,3,5,5,5-heptamethyltrisiloxane, 3-isopropylamino-1,1,1,3,5,5,5-heptamethyltrisiloxane Siloxane, 3-tert-butylamino-1,1,1,3,5,5,5-heptamethyltrisiloxane, 3-methylamino-3-(trimethylsiloxy)-1,1,1,5,5,5-hexamethyltrisiloxane, 3-ethylamino-3-(trimethylsiloxy)-1,1,1,5,5,5-hexamethyltrisiloxane, 3-isopropylamino-3-(trimethylsiloxy)-1,1,1,5,5,5-hexamethyltrisiloxane, 3-tert-butylamino-3-(trimethylsiloxy)-1,1,1,5,5,5-hexamethyltrisiloxane.
[0221] 11. The method according to item 9, wherein the composition further comprises at least one member selected from a solvent and a purge gas.
[0222] 12. The method according to item 11, wherein the solvent is selected from hexamethyldisiloxane and octamethyltrisiloxane.
[0223] 13. The method according to item 11, wherein the solvent is selected from hexane, heptane, octane, nonane, decane, dodecane, cyclooctane, cyclononane, cyclodecane, ethylcyclohexane and ethylcyclooctane.
[0224] 14. The method according to item 9, wherein R 1 and R 2 Each is C 1 To C 4 alkyl.
[0225] 15. The method of claim 8, wherein the composition is substantially free of one or more impurities selected from halides, metal ions, metals, and combinations thereof.
[0226] 16. A method for depositing a film comprising silicon and an oxide onto a substrate, the method comprising the steps of:
[0227] a) providing a substrate in a reactor;
[0228] b) introducing into the reactor a composition comprising at least one organoaminopolysiloxane compound selected from the group consisting of formula A and formula C:
[0229]
[0230] in,
[0231] R 1 Independently selected from linear C 1 To C 10 Alkyl, branched chain C 3 To C 10 Alkyl, C 3 To C 10 Cycloalkyl, C 3 To C 10 Heterocyclic group, C 3 To C 10 Alkenyl, C 3 To C 10 Alkynyl and C 4 To C 10 aryl; and
[0232] R 2 Selected from hydrogen, straight chain C 1 To C 10 Alkyl, branched chain C 3 To C 10 Alkyl, C 3 To C 10 Cycloalkyl, C 3 To C 10 Heterocyclic group, C 3 To C 10 Alkenyl, C 3 To C 10 Alkynyl and C 4 To C 10 Aryl,
[0233] Where R in Formula A and Formula C 1 and R 2 connected to form an annular ring structure or not connected to form an annular ring;
[0234] c) purging the reactor with a purge gas;
[0235] d) introducing at least one of an oxygen-containing source and a nitrogen-containing source into the reactor; and
[0236] e) purging the reactor with the purge gas,
[0237] wherein steps b to e are repeated until a film of desired thickness is deposited; and
[0238] The method is carried out at one or more temperatures in the range of about 600°C to 800°C.
[0239] 17. The method according to item 16, wherein the organoaminopolysiloxane compound is selected from 3-dimethylamino-1,1,1,3,5,5,5-heptamethyltrisiloxane, 3-diethylamino-1,1,1,3,5,5,5-heptamethyltrisiloxane, 3-ethylmethylamino-1,1,1,3,5,5,5-heptamethyltrisiloxane, 3-diisopropylamino-1,1,1,3,5,5,5-heptamethyltrisiloxane, 3-dimethylamino-1,1,3,5,5-pentamethyltrisiloxane, 3-diethylamino-1,1,3,5,5-pentamethyltrisiloxane, 3-ethylmethylamino-1,1,1,3,5,5,5-heptamethyltrisiloxane. trisiloxane, 3-dimethylamino-3-(trimethylsiloxy)-1,1,1,5,5,5-hexamethyltrisiloxane, 3-ethylmethylamino-3-(trimethylsiloxy)-1,1,1,5,5,5-hexamethyltrisiloxane, and 3-diisopropylamino-3-(trimethylsiloxy)-1,1,1,5,5,5-hexamethyltrisiloxane.
[0240] 18. The method according to item 16, wherein the composition further comprises at least one member selected from a solvent and a purge gas.
[0241] 19. The method according to item 18, wherein the solvent is selected from hexamethyldisiloxane and octamethyltrisiloxane.
[0242] 20. The method according to item 18, wherein the solvent is selected from hexane, heptane, octane, nonane, decane, dodecane, cyclooctane, cyclononane, cyclodecane, ethylcyclohexane and ethylcyclooctane.
[0243] 21. The method according to item 16, wherein R 1 and R 2 Each is C 1 To C 4 alkyl.
[0244] 22. The method of claim 16, wherein the composition is substantially free of one or more impurities selected from halides, metal ions, metals, and combinations thereof.
[0245] 23. A silicon-and-oxygen-containing film formed by the method of claim 9, having at least one of the following characteristics: a density of at least about 2.1 g / cc; a wet etch rate of less than about 2.5 angstroms / second as measured in a dilute HF acid solution of 1:100 HF to water (0.5 wt. % dHF); a leakage current of less than about 1e-8 A / cm at up to 6 MV / cm 2; and a hydrogen impurity of less than about 5e20 at / cc as measured by secondary ion mass spectroscopy (SIMS).
[0246] 24. A silicon-and-oxygen-containing film formed by the method of claim 16, having at least one of the following characteristics: a density of at least about 2.1 g / cc; a wet etch rate of less than about 2.5 angstroms / second as measured in a dilute HF acid solution of 1:100 HF to water (0.5 wt. % dHF); a leakage current of less than about 1e-8 A / cm at up to 6 MV / cm 2 ; and a hydrogen impurity of less than about 5e20 at / cc as measured by secondary ion mass spectroscopy (SIMS).
[0247] 25. A method for preparing an organoaminopolysiloxane compound having a structure represented by Formulas A to H:
[0248]
[0249] in,
[0250] R 1 Selected from straight chain C 1 To C 10 Alkyl, branched chain C 3 To C 10 Alkyl, C 3 To C 10 Cycloalkyl, C 3 To C 10 Heterocyclic group, C 3 To C 10 Alkenyl, C 3 To C 10 Alkynyl and C 4 To C 10 aryl; and
[0251] R 2 Selected from hydrogen, straight chain C 1 To C 10 Alkyl, branched chain C 3 To C 10 Alkyl, C 3 To C 10 Cycloalkyl, C 3 To C 10 Heterocyclic group, C 3 To C 10 Alkenyl, C 3 To C 10 Alkynyl and C 4 To C 10 Aryl,
[0252] The R in the formula AH 1 and R 2connected to form an annular ring structure or not connected to form an annular ring,
[0253] The method comprises the following steps:
[0254] a) reactant R in the presence of a catalyst 1 R 2 NH is contacted with a polysiloxane having at least one Si-H group to form a reaction mixture wherein R 1 and R 2 As defined above;
[0255] b) optionally adding a solvent to the reaction mixture;
[0256] c) maintaining the reaction mixture at a temperature of about 0°C to about 300°C; and
[0257] d) allowing a reaction to proceed to form the organoaminopolysiloxane compound from the reaction mixture.
[0258] The following examples are provided to illustrate certain aspects of the invention and should not be construed to limit the scope of the appended claims.
[0259] Example
[0260] Thermal atomic layer deposition of silicon oxide film was performed on a laboratory-scale ALD processing equipment. The silicon precursor was delivered to the chamber by vapor extraction. All gases (such as purge and reactant gases or precursors and oxygen sources) were preheated to 100°C before entering the deposition area. The flow rates of gases and precursors were controlled with an ALD diaphragm valve with high-speed actuation. The substrate used for deposition was a 12-inch long silicon strip. A thermocouple was connected to the sample holder to confirm the substrate temperature. Ozone was used as the oxygen source gas for deposition. The normal deposition process and parameters are shown in Table 2. When multiple precursor pulses are used, steps 2a to 2c are repeated. Steps 1 to 6 are repeated until the desired thickness is reached.
[0261] Table 2: Thermal atomic layer deposition of silicon oxide films using ozone as the oxygen source on a lab-scale ALD process process.
[0262]
[0263]
[0264] Plasma enhanced ALD (PEALD) was performed on a commercial side flow reactor (300mm PEALD equipment manufactured by ASM) equipped with a 27.1MHz direct plasma capability and a fixed spacing of 3.5mm between electrodes. The laminar flow chamber design utilizes an outer chamber and an inner chamber with independent pressure settings. The inner chamber is a deposition reactor where all reactant gases (e.g., precursors, argon) are mixed in a manifold and transported to the process reactor. Argon is used to maintain the reactor pressure in the outer chamber. The precursor is a liquid maintained at room temperature in a stainless steel bubbler and is transported to the chamber with an Ar carrier gas (usually set to a 200sccm flow) or vapor suction. The normal deposition process and parameters are shown in Table 3.
[0265] Table 3. Process for PEALD silicon oxide deposition in a commercial side-stream PEALD reactor using oxygen plasma.
[0266]
[0267]
[0268] All depositions reported in this study were done on native oxide-containing Si substrates of 8-12 Ohm-cm. The thickness and refractive index of the films were measured using a FilmTek2000SE ellipsometer by fitting the reflection data from the films to a pre-set physical model (e.g., the Lorentz oscillator model). The growth rate per cycle was calculated by dividing the measured thickness of the resulting silicon oxide film by the total number of ALD / PEALD cycles. Wet etch rate (WER) measurements were performed using a 1:99 diluted hydrofluoric acid (HF) solution. Thermal oxide wafers were used as standards for each set of experiments to confirm the activity of the etching solution. Before starting to collect the WER of the bulk film, the sample was fully etched for 15 seconds to remove any surface layers. With this procedure, the wet etch rate of a typical thermal oxide wafer for a 1:99 dHF aqueous solution is All density measurements were measured by the X-ray reflectivity (XRR) method. Compositional analysis was performed using secondary ion mass spectroscopy (D-SIMS) or X-ray photoelectron spectroscopy (XPS).
[0269] Example 1 . Preparation of 3-dimethylamino-1,1,1,3,5,5,5-heptamethyltrisiloxane.
[0270] To 2.26 mL (4.52 mmol) of a 2.0 M solution of dimethylamine in THF (dried over molecular sieves) was added 30 mg of Ru 3 (CO) 12, then bubbling of the catalyst was observed as it slowly dissolved. The dark orange solution was then added dropwise to a colorless solution of 0.84 g (3.77 mmol) of bis (trimethylsiloxy) methylsilane in 5 mL of hexane under a nitrogen atmosphere. The resulting dark orange solution was allowed to ventilate while stirring at room temperature overnight. GC-MS showed evidence of the desired dimethylamino-1,1,1,3,5,5,5-heptamethyltrisiloxane product, with peaks at m / z=265 (M+), 250 (M-15), 221, 207, 191, 176, 162, 147, 133, 119, 103, 73.
[0271] Example 2 . Preparation of 3-dimethylamino-1,1,1,3,5,5,5-heptamethyltrisiloxane (predicted).
[0272] A solution containing 3-chloro-1,1,1,3,5,5,5-heptamethyltrisiloxane is treated with a solution of dimethylamine in THF in the presence of triethylamine to provide a mixture which is stirred for a period of time. The resulting amine hydrochloride solid is removed by filtration and the dimethylamino-1,1,1,3,5,5,5-heptamethyltrisiloxane product is purified by vacuum distillation.
[0273] Example 3 . Preparation of 3-dimethylamino-3-(trimethylsiloxy)-1,1,1,5,5,5-hexamethyltrisiloxane (prophetic).
[0274] A solution containing 3-(trimethylsilyloxy)-1,1,1,5,5,5-hexamethyltrisiloxane is treated with a solution of dimethylamine in THF in the presence of a catalyst such as Ru, Pt, Pd or Rh or a complex thereof to provide a mixture which is stirred for a period of time. The resulting 3-dimethylamino-3-(trimethylsilyloxy)-1,1,1,5,5,5-hexamethyltrisiloxane product is purified by vacuum distillation.
[0275] Example 4 . Synthesis of 3-dimethylamino-3-(trimethylsilyloxy)-1,1,1,5,5,5-hexamethyltrisiloxane.
[0276] In a 2L three-necked round-bottom flask equipped with a mechanical stirrer, a condenser and an additional funnel, 97.5g (294.47mmol) of tris (trimethylsiloxy) chlorosilane was added, followed by 800mL of hexane. It was 0°C that the mixture was cooled to an internal temperature, and 36.0g (355.77mmol) of triethylamine was added dropwise through an addition funnel. Next, an additional funnel was loaded with a THF solution of 2.0M dimethylamine of 220mL (440mmol), and was added dropwise while maintaining an internal reaction temperature of 0°C. After addition, the reaction was removed from the cold bath and allowed to reach room temperature under stirring. After 16 hours, the resulting white slurry was filtered through a mesoporous 300mL filter funnel. About 45g of salt was collected. The filtrate was rotary evaporated to remove volatiles (150 Torr, 50°C). The crude product was purified by vacuum distillation (65°C / <1 Torr) to obtain 73.7 g of 3-dimethylamino-3-(trimethylsilyloxy)-1,1,1,5,5,5-hexamethyltrisiloxane. DSC analysis showed a boiling point of 219°C. GC-MS analysis showed the following peaks: m / z=339 (M+), 324 (M-15), 279, 265, 250, 236, 207, 193, 177, 163, 147, 133, 119, 102, 73.
[0277] Example 5 . Synthesis of 3-diethylamino-1,1,1,5,5,5-hexamethyltrisiloxane.
[0278] In a 100 mL round-bottom flask equipped with a magnetic stirrer, 1,1,1,5,5,5-hexamethyltrisiloxane (3.6 g, 0.017 mol) and diethylamine (2.5 g, 0.034 mol) were combined and stirred. 30 mg of Ru was added under nitrogen protection. 3 (CO) 12 The solid catalyst was stirred and reacted for 16 hours while allowing ventilation. The resulting reaction solution was analyzed by GC-MS and found to contain 3-diethylamino-1,1,1,5,5,5-hexamethyltrisiloxane as the main product. GC-MS showed the following peaks: m / z=279 (M+), 264 (M-15), 248, 234, 220, 207, 193, 176, 163, 147, 133, 119, 103, 89, 73.
[0279] Example 6 . Synthesis of 1-dimethylamino-3,3-bis(dimethylsiloxy)-1,1,5,5-tetramethyltrisiloxane.
[0280] 2.0 M dimethylamine THF solution (0.75 mL, 0.0015 mol), tetrakis(dimethylsiloxy)silane (1.00 g, 0.00304 mol) and Ru 3 (CO) 12 (0.04 g, 6.0 × 10 -5 mol) were combined in a 20 mL scintillation vial, and the mixture was stirred at room temperature under nitrogen protection for 1 day. The resulting reaction solution was analyzed by GC-MS and found to contain 1-dimethylamino-3,3-bis(dimethylsilyloxy)-1,1,5,5-tetramethyltrisiloxane as the main product. GC-MS showed the following peaks: m / z=371 (M+), 356 (M-15), 341, 327, 311, 296, 281, 267, 253, 239, 223, 207, 193, 179, 162, 148, 133, 119, 102, 88, 73.
[0281] Comparative Example 7a : Thermal atomic layer deposition of silicon oxide films using dimethylaminotrimethylsilane (DMATMS).
[0282] Atomic layer deposition of silicon oxide film was performed using the following precursor DMATMS. Deposition was performed on a laboratory scale ALD processing equipment. The silicon precursor was delivered to the chamber by vapor extraction. The deposition process and parameters are provided in Table 2. Steps 1 to 6 were repeated until the desired thickness was reached. At 500°C, the DMATMS precursor feed time was 8 seconds and the ozone flow was 4 seconds, the measured film growth rate per cycle was 1.24 angstroms / cycle, and the film refractive index was 1.43.
[0283] Comparative Example 7b : Plasma enhanced atomic layer deposition (PEALD) of silicon oxide films using dimethylaminotrimethylsilane (DMATMS).
[0284] The following precursor DMATMS is used to carry out plasma enhanced atomic layer deposition of silicon oxide film. Deposition is carried out on a commercial side flow reactor (300mm PEALD equipment manufactured by ASM) equipped with a 27.1MHz direct plasma. The silicon precursor is transported to the chamber by vapor suction. The deposition process and parameters are provided in Table 3. Steps 1 to 6 are repeated until the desired thickness is reached. At 100°C, the DMATMS precursor feed time is 4 seconds and the oxygen plasma time is 2 seconds, and the measured film growth rate per cycle is 0.88 angstroms / cycle, and the film refractive index is 1.49.
[0285] Example 8 : Silicon-containing film deposition by plasma-enhanced ALD deposition using the silicon precursor 3-dimethylamino-1,1,1,3,5,5,5-heptamethyltrisiloxane and oxygen plasma.
[0286] Under the conditions given in Table 3, 3-dimethylamino-1,1,1,3,5,5,5-heptamethyltrisiloxane was used as the Si precursor and O 2 Plasma deposition was performed. 3-Dimethylamino-1,1,1,3,5,5,5-heptamethyltrisiloxane was delivered as Si precursor by carrier gas at ambient temperature (25°C). Steps b to e were repeated 150 times to obtain the desired thickness of silicon oxide for metrology. The film growth rate and refractive index are shown in Table 4.
[0287] Table 4. Summary of PEALD process parameters and results for dimethylamino-1,1,1,3,5,5,5-heptamethyltrisiloxane Knot.
[0288]
[0289]
[0290] It can be seen that 3-dimethylamino-1,1,1,3,5,5,5-heptamethyltrisiloxane having Si-O-Si bonds gives a higher growth rate per cycle than dimethylaminotrimethylsilane having no Si-O-Si bonds.
[0291] Example 9 : Silicon-containing film deposition by plasma enhanced ALD deposition using the silicon precursor 3-dimethylamino-3-(trimethylsiloxy)-1,1,1,5,5,5-hexamethyltrisiloxane and oxygen plasma.
[0292] Under the conditions given in Table 3, 3-dimethylamino-3-(trimethylsiloxy)-1,1,1,5,5,5-hexamethyltrisiloxane and O 2 Plasma deposition was performed. 3-Dimethylamino-3-(trimethylsilyloxy)-1,1,1,5,5,5-hexamethyltrisiloxane was used as a Si precursor at 60°C for 100°C deposition by 200 sccm Ar carrier gas and at 70°C for 300°C deposition by 200 sccm Ar carrier gas. Steps b to e were repeated 150 times to obtain the desired thickness of silicon oxide for metrology. The film growth rate and refractive index are shown in Table 5.
[0293] Table 5. 3-Dimethylamino-3-(trimethylsilyloxy)-1,1,1,5,5,5-hexamethyltrisiloxane Summary of PEALD process parameters and results.
[0294]
[0295]
[0296] It can be seen that 3-dimethylamino-3-(trimethylsiloxy)-1,1,1,5,5,5-hexamethyltrisiloxane having Si-O-Si bonds gives a higher growth rate per cycle than the precursor dimethylaminotrimethylsilane having no Si-O-Si bonds.
[0297] Example 10 : Silicon-containing film deposition by thermal ALD deposition using the organoaminopolysiloxane precursor 3-dimethylamino-3-(trimethylsiloxy)-1,1,1,5,5,5-hexamethyltrisiloxane and ozone.
[0298] Atomic layer deposition of silicon oxide film was performed using the following precursor: 3-dimethylamino-3-(trimethylsiloxy)-1,1,1,5,5,5-hexamethyltrisiloxane. Deposition was performed on a laboratory scale ALD processing equipment. The silicon precursor was delivered to the chamber by vapor extraction. The deposition process and parameters are provided in Table 2. When multiple precursor pulses were used, steps 2a to 2c were repeated. Steps 1 to 6 were repeated until the desired thickness was reached. The process parameters, deposition rate and refractive index of the deposition are provided in Table 6.
[0299] Table 6: Processing of 3-dimethylamino-3-(trimethylsiloxy)-1,1,1,5,5,5-hexamethyltrisiloxane Summary of process parameters and results.
[0300]
[0301] It can be seen that the precursor 3-dimethylamino-3-(trimethylsiloxy)-1,1,1,5,5,5-hexamethyltrisiloxane having Si-O-Si bonds gave a higher growth rate per cycle than the precursor DMATMS having no Si-O-Si bonds.
Claims
1. A method of depositing a film containing silicon and oxygen by flowable chemical vapor deposition (FCVD), the method comprising: placing a substrate comprising surface features in a reactor, wherein the substrate is maintained at one or more temperatures in the range of -20°C to 400°C and the pressure of the reactor is maintained at 100 Torr or less; Introducing at least one organoaminopolysiloxane compound selected from Formulae A to H: in, R 1 Selected from straight chain C1 to C 10 Alkyl, branched C3 to C 10 Alkyl, C3 to C 10 Cycloalkyl, C3 to C 10 Heterocyclic group, C3 to C 10 Alkenyl, C3 to C 10 Alkynyl and C4 to C 10 aryl; and R 2 Selected from hydrogen, straight chain C1 to C 10 Alkyl, branched C3 to C 10 Alkyl, C3 to C 10 Cycloalkyl, C3 to C 10 Heterocyclic group, C3 to C 10 Alkenyl, C3 to C 10 Alkynyl and C4 to C 10 Aryl, The R in the formula AH 1 and R 2 connected to form an annular ring structure or not connected to form an annular ring structure; providing an oxygen source into the reactor to react with the at least one compound to form a film and cover at least a portion of the surface feature; annealing the film at one or more temperatures from 100°C to 1000°C to coat at least a portion of the surface features; and The substrate is treated with an oxygen source at one or more temperatures in the range of 20° C. to 1000° C. to form the silicon and oxygen containing film on at least a portion of the surface features.
2. The method according to claim 1, wherein the organoaminopolysiloxane compound is selected from the group consisting of 3-dimethylamino-1,1,1,3,5,5,5-heptamethyltrisiloxane, 3-diethylamino-1,1,1,3,5,5,5-heptamethyltrisiloxane, 3-ethylmethylamino-1,1,1,3,5,5,5-heptamethyltrisiloxane, 3-diisopropylamino-1,1,1,3,5,5,5-heptamethyltrisiloxane, 3-dimethylamino-1,1,3,5,5-pentamethyltrisiloxane, 3-diethylamino-1,1,3,5,5-pentamethyltrisiloxane, 3-ethylmethylamino-1,1,1,3,5,5,5-heptamethyltrisiloxane. ,5-pentamethyltrisiloxane, 3-dimethylamino-3-(trimethylsiloxy)-1,1,1,5,5,5-hexamethyltrisiloxane, 3-diethylamino-3-(trimethylsiloxy)-1,1,1,5,5,5-hexamethyltrisiloxane, 3-ethylmethylamino-3-(trimethylsiloxy)-1,1,1,5,5,5-heptamethyltrisiloxane, 3-diisopropylamino-3-(trimethylsiloxy)-1,1,1,5,5,5-hexamethyltrisiloxane, 3-dimethylamino-3-(dimethylsiloxy)-1,1,5,5-tetramethyltrisiloxane, 3-diethylamino-3-(dimethylsiloxy)-1,1,5,5-tetramethyltrisiloxane , 3-ethylmethylamino-3-(dimethylsilyloxy)-1,1,5,5-tetramethyltrisiloxane, 3-diisopropylamino-3-(dimethylsilyloxy)-1,1,5,5-tetramethyltrisiloxane, 1-dimethylamino-3-(dimethylsilyloxy)-1,1,3,5,5-pentamethyltrisiloxane, 1-diethylamino-3-(dimethylsilyloxy)-1,1,3,5,5-pentamethyltrisiloxane, 1-ethylmethylamino-3-(dimethylsilyloxy)-1,1,3,5,5-pentamethyltrisiloxane, 1-diisopropylamino-3-(dimethylsilyloxy)-1,1,3,5,5-pentamethyltrisiloxane, 3-dimethylamino-1,1,1, 5,5,5-hexamethyltrisiloxane, 3-diethylamino-1,1,1,5,5,5-hexamethyltrisiloxane, 3-ethylmethylamino-1,1,1,5,5,5-hexamethyltrisiloxane, 3-diisopropylamino-1,1,1,3,5,5,5-hexamethyltrisiloxane, 3-dimethylamino-1,1,5,5-tetramethyltrisiloxane, 3-diethylamino-1,1,5,5-tetramethyltrisiloxane, 3-ethylmethylamino-1,1,5,5-tetramethyltrisiloxane, 3-diisopropylamino-1,1,5,5-tetramethyltrisiloxane, 1-dimethylamino-3,3-bis(dimethylsiloxy)-1,1,5,5-tetramethyltrisiloxane, 1-diethylamino-3,3-Bis(dimethylsiloxy)-1,1,5,5-tetramethyltrisiloxane, 1-ethylmethylamino-3,3-bis(dimethylsiloxy)-1,1,5,5-tetramethyltrisiloxane, 1-diisopropylamino-3,3-bis(dimethylsiloxy)-1,1,5,5-tetramethyltrisiloxane, 3-methylamino-1,1,1,3,5,5,5-heptamethyltrisiloxane, 3-ethylamino-1,1,1,3,5,5,5-heptamethyltrisiloxane, 3-isopropylamino-1,1,1,3,5,5,5-heptamethyltrisiloxane Siloxane, 3-tert-butylamino-1,1,1,3,5,5,5-heptamethyltrisiloxane, 3-methylamino-3-(trimethylsiloxy)-1,1,1,5,5,5-hexamethyltrisiloxane, 3-ethylamino-3-(trimethylsiloxy)-1,1,1,5,5,5-hexamethyltrisiloxane, 3-isopropylamino-3-(trimethylsiloxy)-1,1,1,5,5,5-hexamethyltrisiloxane, 3-tert-butylamino-3-(trimethylsiloxy)-1,1,1,5,5,5-hexamethyltrisiloxane.
3. The method according to claim 1, wherein R 1 and R 2 Each is a C1 to C4 alkyl group.
4. The method of claim 1, wherein the at least one organoaminopolysiloxane compound is selected from Formula A and Formula C.
5. The method according to claim 4, wherein the organoaminopolysiloxane compound is selected from the group consisting of 3-dimethylamino-1,1,1,3,5,5,5-heptamethyltrisiloxane, 3-diethylamino-1,1,1,3,5,5,5-heptamethyltrisiloxane, 3-ethylmethylamino-1,1,1,3,5,5,5-heptamethyltrisiloxane, 3-diisopropylamino-1,1,1,3,5,5,5-heptamethyltrisiloxane, 3-dimethylamino-1,1,3,5,5-pentamethyltrisiloxane, 3-diethylamino-1,1,3,5,5-pentamethyltrisiloxane, 3-ethylmethylamino-1,1,1,3,5,5,5-heptamethyltrisiloxane. trisiloxane, 3-dimethylamino-3-(trimethylsiloxy)-1,1,1,5,5,5-hexamethyltrisiloxane, 3-ethylmethylamino-3-(trimethylsiloxy)-1,1,1,5,5,5-hexamethyltrisiloxane, and 3-diisopropylamino-3-(trimethylsiloxy)-1,1,1,5,5,5-hexamethyltrisiloxane.
6. The method according to any one of claims 1 to 5, wherein the oxygen source is selected from water vapor, water plasma, ozone, oxygen, oxygen plasma, oxygen / helium plasma, oxygen / argon plasma, nitrogen oxide plasma, carbon dioxide plasma, hydrogen peroxide, organic peroxides and mixtures thereof.
7. The method according to claim 6, wherein water vapor is used as the oxygen source, and the substrate temperature is -20°C to 40°C or -10°C to 25°C.
8. A method of depositing a film containing silicon, oxygen and nitrogen by flowable chemical vapor deposition (FCVD), the method comprising: placing a substrate comprising surface features in a reactor, wherein the substrate is maintained at one or more temperatures in the range of -20°C to 400°C and the pressure of the reactor is maintained at 100 Torr or less; Introducing at least one organoaminopolysiloxane compound selected from Formulae A to H: in, R 1 Selected from straight chain C1 to C 10 Alkyl, branched C3 to C 10 Alkyl, C3 to C 10 Cycloalkyl, C3 to C 10 Heterocyclic group, C3 to C 10 Alkenyl, C3 to C 10 Alkynyl and C4 to C 10 aryl; and R 2 Selected from hydrogen, straight chain C1 to C 10 Alkyl, branched C3 to C 10 Alkyl, C3 to C 10 Cycloalkyl, C3 to C 10 Heterocyclic group, C3 to C 10 Alkenyl, C3 to C 10 Alkynyl and C4 to C 10 Aryl, The R in the formula AH 1 and R 2 connected to form an annular ring structure or not connected to form an annular ring structure; providing a nitrogen source into the reactor to react with the at least one compound to form a film and cover at least a portion of the surface feature; annealing the film at one or more temperatures in the range of 100° C. to 1000° C. to coat at least a portion of the surface features; and The substrate is treated with an oxygen source at one or more temperatures in the range of 20° C. to 1000° C. to form the film comprising silicon, oxygen, and nitrogen on at least a portion of the surface features.
9. The method according to claim 8, wherein the organoaminopolysiloxane compound is selected from the group consisting of 3-dimethylamino-1,1,1,3,5,5,5-heptamethyltrisiloxane, 3-diethylamino-1,1,1,3,5,5,5-heptamethyltrisiloxane, 3-ethylmethylamino-1,1,1,3,5,5,5-heptamethyltrisiloxane, 3-diisopropylamino-1,1,1,3,5,5,5-heptamethyltrisiloxane, 3-dimethylamino-1,1,3,5,5-pentamethyltrisiloxane, 3-diethylamino-1,1,3,5,5-pentamethyltrisiloxane, 3-ethylmethylamino-1,1,1,3,5,5,5-heptamethyltrisiloxane. ,5-pentamethyltrisiloxane, 3-dimethylamino-3-(trimethylsiloxy)-1,1,1,5,5,5-hexamethyltrisiloxane, 3-diethylamino-3-(trimethylsiloxy)-1,1,1,5,5,5-hexamethyltrisiloxane, 3-ethylmethylamino-3-(trimethylsiloxy)-1,1,1,5,5,5-heptamethyltrisiloxane, 3-diisopropylamino-3-(trimethylsiloxy)-1,1,1,5,5,5-hexamethyltrisiloxane, 3-dimethylamino-3-(dimethylsiloxy)-1,1,5,5-tetramethyltrisiloxane, 3-diethylamino-3-(dimethylsiloxy)-1,1,5,5-tetramethyltrisiloxane , 3-ethylmethylamino-3-(dimethylsilyloxy)-1,1,5,5-tetramethyltrisiloxane, 3-diisopropylamino-3-(dimethylsilyloxy)-1,1,5,5-tetramethyltrisiloxane, 1-dimethylamino-3-(dimethylsilyloxy)-1,1,3,5,5-pentamethyltrisiloxane, 1-diethylamino-3-(dimethylsilyloxy)-1,1,3,5,5-pentamethyltrisiloxane, 1-ethylmethylamino-3-(dimethylsilyloxy)-1,1,3,5,5-pentamethyltrisiloxane, 1-diisopropylamino-3-(dimethylsilyloxy)-1,1,3,5,5-pentamethyltrisiloxane, 3-dimethylamino-1,1,1, 5,5,5-hexamethyltrisiloxane, 3-diethylamino-1,1,1,5,5,5-hexamethyltrisiloxane, 3-ethylmethylamino-1,1,1,5,5,5-hexamethyltrisiloxane, 3-diisopropylamino-1,1,1,3,5,5,5-hexamethyltrisiloxane, 3-dimethylamino-1,1,5,5-tetramethyltrisiloxane, 3-diethylamino-1,1,5,5-tetramethyltrisiloxane, 3-ethylmethylamino-1,1,5,5-tetramethyltrisiloxane, 3-diisopropylamino-1,1,5,5-tetramethyltrisiloxane, 1-dimethylamino-3,3-bis(dimethylsiloxy)-1,1,5,5-tetramethyltrisiloxane, 1-diethylamino-3,3-Bis(dimethylsiloxy)-1,1,5,5-tetramethyltrisiloxane, 1-ethylmethylamino-3,3-bis(dimethylsiloxy)-1,1,5,5-tetramethyltrisiloxane, 1-diisopropylamino-3,3-bis(dimethylsiloxy)-1,1,5,5-tetramethyltrisiloxane, 3-methylamino-1,1,1,3,5,5,5-heptamethyltrisiloxane, 3-ethylamino-1,1,1,3,5,5,5-heptamethyltrisiloxane, 3-isopropylamino-1,1,1,3,5,5,5-heptamethyltrisiloxane Siloxane, 3-tert-butylamino-1,1,1,3,5,5,5-heptamethyltrisiloxane, 3-methylamino-3-(trimethylsiloxy)-1,1,1,5,5,5-hexamethyltrisiloxane, 3-ethylamino-3-(trimethylsiloxy)-1,1,1,5,5,5-hexamethyltrisiloxane, 3-isopropylamino-3-(trimethylsiloxy)-1,1,1,5,5,5-hexamethyltrisiloxane, 3-tert-butylamino-3-(trimethylsiloxy)-1,1,1,5,5,5-hexamethyltrisiloxane.
10. The method according to claim 8, wherein R 1 and R 2 Each is a C1 to C4 alkyl group.
11. The method of claim 8, wherein the at least one organoaminopolysiloxane compound is selected from Formula A and Formula C.
12. The method according to claim 8, wherein the organoaminopolysiloxane compound is selected from the group consisting of 3-dimethylamino-1,1,1,3,5,5,5-heptamethyltrisiloxane, 3-diethylamino-1,1,1,3,5,5,5-heptamethyltrisiloxane, 3-ethylmethylamino-1,1,1,3,5,5,5-heptamethyltrisiloxane, 3-diisopropylamino-1,1,1,3,5,5,5-heptamethyltrisiloxane, 3-dimethylamino-1,1,3,5,5-pentamethyltrisiloxane, 3-diethylamino-1,1,3,5,5-pentamethyltrisiloxane, 3-ethylmethylamino-1,1,1,3,5,5,5-heptamethyltrisiloxane. Amino-1,1,3,5,5-pentamethyltrisiloxane, 3-diisopropylamino-1,1,3,5,5-pentamethyltrisiloxane, 3-dimethylamino-3-(trimethylsiloxy)-1,1,1,5,5,5-hexamethyltrisiloxane, 3-diethylamino-3-(trimethylsiloxy)-1,1,1,5,5,5-hexamethyltrisiloxane, 3-ethylmethylamino-3-(trimethylsiloxy)-1,1,1,5,5,5-heptamethyltrisiloxane and 3-diisopropylamino-3-(trimethylsiloxy)-1,1,1,5,5,5-hexamethyltrisiloxane.
13. The method according to any one of claims 8 to 12, wherein the nitrogen source is selected from ammonia, hydrazine, monoalkylhydrazine, dialkylhydrazine, nitrogen, nitrogen / hydrogen, nitrogen / argon plasma, nitrogen / helium plasma, ammonia plasma, nitrogen plasma, nitrogen / hydrogen plasma, organic amines, diethylamine plasma, dimethylamine plasma, trimethyl plasma, trimethylamine plasma, ethylenediamine plasma and alkoxyamine plasma, and mixtures thereof.
14. The method of claim 13, wherein the organic amine comprises tert-butylamine, dimethylamine, diethylamine, isopropylamine, and mixtures thereof.
15. The method of claim 13, wherein the alkoxyamine plasma comprises ethanolamine plasma.