A method for separating iron oxide and electrolyte in iron-rich covering material for aluminum electrolysis

Through aluminum salt leaching and multi-step processing, the problem of difficult separation of aluminum electrolytic iron-rich cover material in the prior art is solved, and efficient recycling of iron oxides and electrolytes is achieved, resource waste is avoided and operating costs are reduced.

CN115595447BActive Publication Date: 2024-11-15KUNMING UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211295534.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-21
Publication Date
2024-11-15
Estimated Expiration
2042-10-21

AI Technical Summary

Technical Problem

In the prior art, when NaOH solution is used to directly separate the iron oxide and electrolyte in the aluminum electrolytic iron-rich cover material, the fluoride and alumina are completely dissolved, making the filtrate composition complex, making it difficult to separate and waste resources.

Method used

The aluminum salt leaching method is used to separate the iron oxide and electrolyte in the aluminum electrolytic iron-rich cover material. Through ball milling, screening, aluminum salt solution leaching, alkaline leaching and inorganic acid regulation, the efficient recovery of iron oxides is achieved.

Benefits of technology

Effectively separate electrolytes and alumina, avoiding the waste of waste iron-rich covering materials, easy operation, low cost of agents, and high-value recycling of resources.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115595447B_ABST
    Figure CN115595447B_ABST
Patent Text Reader

Abstract

The present invention relates to a method for separating iron oxides and electrolytes in an aluminum electrolysis iron-rich covering material, and belongs to the technical field of aluminum electrolysis industrial waste recovery. The present invention breaks, ball-mills and screens the aluminum electrolysis iron-rich covering material to obtain aluminum electrolysis iron-rich covering material particles, and the aluminum electrolysis iron-rich covering material particles are added to an aluminum salt solution for leaching to obtain a filtrate A and a filter residue A; the filter residue A is added to an alkali solution for alkaline leaching, solid-liquid separation, and a filtrate B and a filter residue iron oxide are obtained; an inorganic acid is used to adjust the pH value of the filtrate B to 9-10 to precipitate Al(OH)3, solid-liquid separation is performed to obtain a filtrate C and an Al(OH)3 precipitate, and the filtrate C is returned to replace the filtrate B to precipitate Al(OH)3; an alkali solution is used to adjust the pH value of the filtrate A to 3-5, and solid-liquid separation is performed to obtain a filtrate D and a precipitate D; the filtrate D is returned to replace the aluminum salt solution for leaching, and after the precipitate D is dried, it is placed at a temperature of 500-800°C and an HF gas atmosphere for reaction and conversion into AlF3. The method can effectively separate the iron oxides in the iron-rich covering material and recover the electrolyte components in the form of AlF3.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for separating iron oxide and electrolyte in an iron-rich covering material for aluminum electrolysis, and belongs to the technical field of aluminum electrolysis industrial waste recycling. Background Art

[0002] As the use of aluminum in China and around the world continues to grow, the aluminum electrolysis industry is booming. At the same time, more and more aluminum electrolysis waste is generated. These wastes are hazardous wastes. The large amount of accumulated waste not only takes up a lot of space, but also wastes resources and threatens the environment. The aluminum electrolysis anode covering material is composed of electrolyte and alumina mixed in a certain proportion. The purpose is to reduce the energy consumption of the electrolytic cell, reduce the oxidation of the anode carbon block, reduce the anode consumption, absorb the anode fluorine volatiles generated during the electrolysis process, and can be recycled in aluminum electrolysis to ensure the material balance of the electrolysis process. However, in the actual process, since the replacement of the anode will cause the covering material to be taken out, the anode steel claws are severely corroded by the high-temperature electrolyte, and a lot of waste iron-rich covering materials are generated, which makes many aluminum electrolysis plants unable to recycle this part of the covering material and can only store it in large quantities, resulting in a large amount of resource waste. Therefore, the iron-rich covering material is urgently needed to be recycled.

[0003] At present, most researchers focus on waste tank lining, carbon anode residue and aluminum ash in the solid waste of aluminum electrolysis production, while there are few literatures and studies on iron-rich covering materials. The main components of iron-rich covering materials are Fe2O3 and Fe3O4, Al2O3 and Na3AlF6, as well as CaF2, MgF2 and other substances with lower content.

[0004] In the prior art, directly using NaOH solution to leach waste aluminum electrolytic covering materials will completely dissolve fluoride and aluminum oxide, making the filtrate composition complex and affecting further separation of the filtrate.

[0005] Therefore, correctly separating iron oxides and electrolytes in the iron-rich covering material of aluminum electrolysis will help solve the problem of comprehensive utilization of solid waste. Summary of the invention

[0006] Aiming at the problem that when NaOH solution is directly used to separate iron oxides and electrolytes in iron-rich covering materials for aluminum electrolysis in the prior art, fluoride and aluminum oxide are completely dissolved, making the composition of the filtrate complex and making the filtrate difficult to separate, the present invention proposes a method for separating iron oxides and electrolytes in iron-rich covering materials for aluminum electrolysis, namely, separating iron oxides and electrolytes in iron-rich covering materials for aluminum electrolysis by aluminum salt leaching method, thereby realizing efficient recovery of iron oxides.

[0007] A method for separating iron oxide and electrolyte in an iron-rich covering material for aluminum electrolysis, comprising the following specific steps:

[0008] (1) breaking, ball-milling and screening the aluminum electrolysis iron-rich covering material to obtain aluminum electrolysis iron-rich covering material particles; achieving preliminary separation of cryolite, fluoride, alumina and iron oxide by ball-milling and screening to avoid mutual wrapping and affecting the salt leaching experiment effect;

[0009] (2) adding the iron-rich covering material particles of aluminum electrolysis into an aluminum salt solution to obtain a filtrate A and a filter residue A;

[0010] (3) adding the filter residue A into an alkaline solution for alkaline leaching and solid-liquid separation to obtain a filtrate B and filter residue iron oxides; the filter residue iron oxides are Fe2O3 and Fe3O4;

[0011] (4) adjusting the pH value of filtrate B to 9-10 with an inorganic acid to precipitate Al(OH)3, and performing solid-liquid separation to obtain filtrate C and Al(OH)3 precipitate, and filtrate C is returned to replace filtrate B to precipitate Al(OH)3;

[0012] (5) adjusting the pH value of the filtrate A to 3-5 with an alkali solution, and performing solid-liquid separation to obtain a filtrate D and a precipitate D; the filtrate D is returned to step (2) to replace the aluminum salt solution for leaching, and the precipitate D is dried to obtain hydrated aluminum hydroxyfluoride (AHF, Al2(OH) 2.76 F 3.24 ·H2O), placed at a temperature of 500-600°C and in an HF gas atmosphere, it reacts and converts into AlF3.

[0013] The particle size of the iron-rich covering material for aluminum electrolysis in the step (1) is 0.025-0.075 mm; the screening method is to use 200 mesh and 500 mesh sieves for step-by-step screening, taking the material under the 200 mesh sieve and the material on the 500 mesh sieve, and returning the material on the 200 mesh sieve to the ball mill for further grinding until all of them pass through the 200 mesh sieve.

[0014] The aluminum salt solution in step (2) is one or more of aluminum sulfate, aluminum nitrate, and aluminum chloride.

[0015] In the step (2), the aluminum ion concentration in the aluminum salt solution is 0.5-2.5 mol / L, the solid-liquid ratio (g:mL) of the aluminum electrolysis iron-rich covering material particles to the aluminum salt solution is 1:10-30, the leaching temperature is 70-90°C, and the leaching time is 1.5-3h.

[0016] The alkali solution in step (3) and step (5) is a NaOH solution, and the concentration of the NaOH solution is 1-3 mol / L.

[0017] The inorganic acid in step (4) is one or more of sulfuric acid, nitric acid and hydrochloric acid.

[0018] The beneficial effects of the present invention are:

[0019] (1) The present invention uses aluminum salt to leach the iron-rich covering material of aluminum electrolysis, effectively separates the electrolyte and alumina, and prepares the electrolyte into high-value aluminum fluoride, thereby avoiding the waste of waste iron-rich covering materials in aluminum electrolysis plants;

[0020] (2) The electrolyte in the iron-rich covering material for aluminum electrolysis of the present invention reacts with an aluminum salt solution and is finally recovered in the form of aluminum fluoride;

[0021] (3) The method of the present invention is simple to operate, and the reagents used are low-cost and easy to purchase. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 It is a process flow chart of the present invention;

[0023] Figure 2 This is the XRD pattern of iron oxide in the filter residue of Example 1;

[0024] Figure 3 This is the XRD pattern of precipitate D from Example 1. DETAILED DESCRIPTION

[0025] The present invention is further described in detail below in conjunction with specific implementation modes, but the protection scope of the present invention is not limited to the described contents.

[0026] The iron-rich covering material for aluminum electrolysis in the embodiment of the present invention is the same, containing about 14wt% of aluminum oxide, about 28wt% of iron oxide, about 11wt% of ferrosoferric oxide, about 33wt% of cryolite, and other fluorides totaling about 14wt%.

[0027] Example 1: A method for separating iron oxide and electrolyte in an iron-rich covering material for aluminum electrolysis, the specific steps are as follows:

[0028] (1) crushing the iron-rich covering material of aluminum electrolysis, grinding it with a dry ball mill, and then sieving it step by step with 200-mesh to 500-mesh screens, the material under the 200-mesh screen and the material on the 500-mesh screen enter the leaching process, and the material on the 200-mesh screen is returned and re-ground until all of them pass through the 200-mesh screen;

[0029] (2) 50 g of the ground raw material was added to 750 mL of aluminum sulfate solution, and leached at 70° C. for 2.5 h to obtain filtrate A and 25.47 g of residue A; wherein the aluminum ion concentration in the aluminum sulfate solution was 1.5 mol / L;

[0030] (3) The filter residue A was added to an excess of 2 mol / L NaOH solution for alkaline leaching and solid-liquid separation to obtain filtrate B and 18.47 g of filter residue iron oxide; the XRD pattern of the filter residue iron oxide is shown in Figure 2 ,from Figure 2 It can be seen that the filter residue is Fe2O3 and Fe3O4, and the recovery effect of iron oxide is more obvious;

[0031] (4) adjusting the pH value of filtrate B to 9.5 with sulfuric acid to precipitate Al(OH)3, performing solid-liquid separation to obtain filtrate C and Al(OH)3 precipitate, and returning filtrate C to replace filtrate B to precipitate Al(OH)3; and recovering alumina in the iron-rich covering material of aluminum electrolysis in the form of Al(OH)3;

[0032] (5) Slowly add 1 mol / L NaOH solution to the filtrate A to adjust the pH value of the filtrate A to 4.0 to obtain a white precipitate. The solid-liquid separation obtains the filtrate D and the precipitate D. The XRD pattern of the precipitate D is shown in FIG. Figure 3 The filtrate D is returned to step (2) to replace the aluminum salt solution for leaching, and the precipitate D is dried to obtain hydrated hydroxyaluminum fluoride (AHF, Al2(OH) 2.76 F 3.24 ·H2O), and then placed in a HF gas atmosphere at 520°C to react and convert into AlF3.

[0033] Example 2: A method for separating iron oxide and electrolyte in an iron-rich covering material for aluminum electrolysis, the specific steps are as follows:

[0034] (1) crushing the iron-rich covering material of aluminum electrolysis, grinding it with a dry ball mill, and then sieving it step by step with 200-mesh to 500-mesh screens, the material under the 200-mesh screen and the material on the 500-mesh screen enter the leaching process, and the material on the 200-mesh screen is returned and re-ground until all of them pass through the 200-mesh screen;

[0035] (2) 50 g of the ground raw material was added to 750 mL of aluminum sulfate solution, and leached at 90° C. for 2.0 h to obtain filtrate A and 26.08 g of residue A; wherein the aluminum ion concentration in the aluminum sulfate solution was 2.0 mol / L;

[0036] (3) The filter residue A was added to an excess of 3 mol / L NaOH solution for alkaline leaching and solid-liquid separation to obtain filtrate B and 19.71 g of filter residue iron oxide; the filter residue was Fe2O3 and Fe3O4, and the recovery effect of iron oxide was more obvious;

[0037] (4) adjusting the pH value of filtrate B to 9.0 with sulfuric acid to precipitate Al(OH)3, performing solid-liquid separation to obtain filtrate C and Al(OH)3 precipitate, and returning filtrate C to replace filtrate B to precipitate Al(OH)3; and recovering alumina in the iron-rich covering material of aluminum electrolysis in the form of Al(OH)3;

[0038] (5) Slowly adding 2 mol / L NaOH solution to the filtrate A to adjust the pH value of the filtrate A to 4.0 to obtain a white precipitate, and separating the solid and liquid to obtain a filtrate D and a precipitate D; the filtrate D returns to step (2) to replace the aluminum salt solution for leaching, and the precipitate D is dried to obtain hydrated hydroxyaluminum fluoride (AHF, Al2(OH) 2.76 F 3.24 ·H2O), and then reacted in HF gas atmosphere at 600℃ to convert into AlF3.

[0039] Example 3: A method for separating iron oxide and electrolyte in an iron-rich covering material for aluminum electrolysis, the specific steps are as follows:

[0040] (1) crushing the iron-rich covering material of aluminum electrolysis, grinding it with a dry ball mill, and then sieving it step by step with 200-mesh to 500-mesh screens, the material under the 200-mesh screen and the material on the 500-mesh screen enter the leaching process, and the material on the 200-mesh screen is returned and re-ground until all of them pass through the 200-mesh screen;

[0041] (2) 50 g of the ground raw material was added to 500 mL of aluminum chloride solution, and leached at 80° C. for 1.5 h to obtain filtrate A and 27.85 g of residue A; wherein the aluminum ion concentration in the aluminum chloride solution was 2.5 mol / L;

[0042] (3) The filter residue A was added to an excess of 1.5 mol / L NaOH solution for alkaline leaching and solid-liquid separation to obtain filtrate B and 21.04 g of filter residue iron oxide; the filter residue was Fe2O3 and Fe3O4, and the recovery effect of iron oxide was more obvious;

[0043] (4) using hydrochloric acid to adjust the pH value of filtrate B to 10.0 to precipitate Al(OH)3, and performing solid-liquid separation to obtain filtrate C and Al(OH)3 precipitate, and filtrate C is returned to replace filtrate B to precipitate Al(OH)3; the alumina in the iron-rich covering material of aluminum electrolysis is recovered in the form of Al(OH)3;

[0044] (5) Slowly adding 1.5 mol / L NaOH solution to the filtrate A to adjust the pH value of the filtrate A to 4.5 to obtain a white precipitate, and separating the solid and liquid to obtain a filtrate D and a precipitate D; the filtrate D returns to step (2) to replace the aluminum salt solution for leaching, and the precipitate D is dried to obtain hydrated aluminum hydroxyfluoride (AHF, Al2(OH) 2.76 F 3.24 ·H2O), and is placed at a temperature of 760°C in an HF gas atmosphere to react and convert into AlF3.

[0045] Example 4: A method for separating iron oxide and electrolyte in an iron-rich covering material for aluminum electrolysis, the specific steps are as follows:

[0046] (1) crushing the iron-rich covering material of aluminum electrolysis, grinding it with a dry ball mill, and then sieving it step by step with 200-mesh to 500-mesh screens, the material under the 200-mesh screen and the material on the 500-mesh screen enter the leaching process, and the material on the 200-mesh screen is returned and re-ground until all of them pass through the 200-mesh screen;

[0047] (2) 50 g of the ground raw material was added to 1000 mL of aluminum chloride solution, and leached at 90° C. for 2.0 h to obtain filtrate A and 25.96 g of residue A; wherein the aluminum ion concentration in the aluminum chloride solution was 1.5 mol / L;

[0048] (3) The filter residue A was added to an excess of 1.0 mol / L NaOH solution for alkaline leaching and solid-liquid separation to obtain filtrate B and 19.19 g of filter residue iron oxide; the filter residue was Fe2O3 and Fe3O4, and the recovery effect of iron oxide was more obvious;

[0049] (4) using hydrochloric acid to adjust the pH value of filtrate B to 10.0 to precipitate Al(OH)3, and performing solid-liquid separation to obtain filtrate C and Al(OH)3 precipitate, and filtrate C is returned to replace filtrate B to precipitate Al(OH)3; the alumina in the iron-rich covering material of aluminum electrolysis is recovered in the form of Al(OH)3;

[0050] (5) Slowly adding 1 mol / L NaOH solution to the filtrate A to adjust the pH value of the filtrate A to 4.5 to obtain a white precipitate, and separating the solid and liquid to obtain a filtrate D and a precipitate D; the filtrate D returns to step (2) to replace the aluminum salt solution for leaching, and the precipitate D is dried to obtain hydrated hydroxyaluminum fluoride (AHF, Al2(OH) 2.76 F 3.24 ·H2O), and is placed at a temperature of 690°C in an HF gas atmosphere to react and convert into AlF3.

[0051] Example 5: A method for separating iron oxide and electrolyte in an iron-rich covering material for aluminum electrolysis, the specific steps are as follows:

[0052] (1) crushing the iron-rich covering material of aluminum electrolysis, grinding it with a dry ball mill, and then sieving it step by step with 200-mesh to 500-mesh screens, the material under the 200-mesh screen and the material on the 500-mesh screen enter the leaching process, and the material on the 200-mesh screen is returned and re-ground until all of them pass through the 200-mesh screen;

[0053] (2) 50 g of the ground raw material was added to 1500 mL of aluminum sulfate solution, and leached at 80° C. for 3.0 h to obtain filtrate A and 27.37 g of residue A; wherein the aluminum ion concentration in the aluminum sulfate solution was 1.0 mol / L;

[0054] (3) The filter residue A was added to an excess of 1.5 mol / L NaOH solution for alkaline leaching and solid-liquid separation to obtain filtrate B and 20.38 g of filter residue iron oxide; the filter residue was Fe2O3 and Fe3O4, and the recovery effect of iron oxide was more obvious;

[0055] (4) using hydrochloric acid to adjust the pH value of filtrate B to 9.5 to precipitate Al(OH)3, and performing solid-liquid separation to obtain filtrate C and Al(OH)3 precipitate, and filtrate C is returned to replace filtrate B to precipitate Al(OH)3; the alumina in the iron-rich covering material of aluminum electrolysis is recovered in the form of Al(OH)3;

[0056] (5) Slowly adding 1.5 mol / L NaOH solution to the filtrate A to adjust the pH value of the filtrate A to 4.5 to obtain a white precipitate, and separating the solid and liquid to obtain a filtrate D and a precipitate D; the filtrate D returns to step (2) to replace the aluminum salt solution for leaching, and the precipitate D is dried to obtain hydrated aluminum hydroxyfluoride (AHF, Al2(OH) 2.76 F 3.24 ·H2O), and is placed at a temperature of 740°C in an HF gas atmosphere to react and convert into AlF3.

[0057] Example 6: A method for separating iron oxide and electrolyte in an iron-rich covering material for aluminum electrolysis, the specific steps are as follows:

[0058] (1) crushing the iron-rich covering material of aluminum electrolysis, grinding it with a dry ball mill, and then sieving it step by step with 200-mesh to 500-mesh screens, the material under the 200-mesh screen and the material on the 500-mesh screen enter the leaching process, and the material on the 200-mesh screen is returned and re-ground until all of them pass through the 200-mesh screen;

[0059] (2) 50 g of the ground raw material was added to 1000 mL of aluminum chloride solution, and leached at 70° C. for 2.5 h to obtain filtrate A and 26.42 g of residue A; wherein the aluminum ion concentration in the aluminum chloride solution was 0.5 mol / L;

[0060] (3) The filter residue A was added to an excess of 1.5 mol / L NaOH solution for alkaline leaching and solid-liquid separation to obtain filtrate B and 19.85 g of filter residue iron oxide; the filter residue was Fe2O3 and Fe3O4, and the recovery effect of iron oxide was more obvious;

[0061] (4) adjusting the pH value of filtrate B to 9.0 with sulfuric acid to precipitate Al(OH)3, performing solid-liquid separation to obtain filtrate C and Al(OH)3 precipitate, and returning filtrate C to replace filtrate B to precipitate Al(OH)3; and recovering alumina in the iron-rich covering material of aluminum electrolysis in the form of Al(OH)3;

[0062] (5) Slowly adding 2.5 mol / L NaOH solution to the filtrate A to adjust the pH value of the filtrate A to 5.0 to obtain a white precipitate, and separating the solid and liquid to obtain a filtrate D and a precipitate D; the filtrate D is returned to step (2) to replace the aluminum salt solution for leaching, and the precipitate D is dried to obtain hydrated hydroxyaluminum fluoride (AHF, Al2(OH) 2.76 F 3.24 ·H2O), and then placed at 550℃ in HF gas atmosphere to react and convert into AlF3.

[0063] The specific implementation modes of the present invention are described in detail above, but the present invention is not limited to the above implementation modes, and various changes can be made within the knowledge scope of ordinary technicians in this field without departing from the purpose of the present invention.

Claims

1. A method for separating iron oxide and electrolyte in an iron-rich covering material for aluminum electrolysis, characterized in that: The specific steps include: (1) breaking, ball-milling and sieving the aluminum electrolysis iron-rich covering material to obtain aluminum electrolysis iron-rich covering material particles; (2) adding the iron-rich covering material particles of aluminum electrolysis to an aluminum salt solution to obtain a filtrate A and a filter residue A; the aluminum ion concentration in the aluminum salt solution is 0.5-2.5 mol / L, the solid-liquid ratio of the iron-rich covering material particles of aluminum electrolysis to the aluminum salt solution is g:mL 1:10-30, the leaching temperature is 70-90°C, and the leaching time is 1.5-3h; (3) adding the filter residue A into an alkaline solution for alkaline leaching and solid-liquid separation to obtain a filtrate B and filter residue iron oxide; (4) adjusting the pH value of filtrate B to 9-10 with an inorganic acid to precipitate Al(OH)3, and performing solid-liquid separation to obtain filtrate C and Al(OH)3 precipitate, and filtrate C is returned to replace filtrate B to precipitate Al(OH)3; (5) adjusting the pH value of the filtrate A to 3-5 with an alkaline solution, and performing solid-liquid separation to obtain a filtrate D and a precipitate D; the filtrate D is returned to step (2) to replace the aluminum salt solution for leaching; after the precipitate D is dried, it is placed at a temperature of 500-800° C. and an HF gas atmosphere to react and convert into AlF 3 .

2. The method for separating iron oxide and electrolyte in an iron-rich covering material for aluminum electrolysis according to claim 1, characterized in that: The particle size of the iron-rich covering material in step (1) aluminum electrolysis is 0.025-0.075 mm.

3. The method for separating iron oxide and electrolyte in an iron-rich covering material for aluminum electrolysis according to claim 1, characterized in that: The aluminum salt solution in step (2) is one or more of aluminum sulfate, aluminum nitrate, and aluminum chloride.

4. The method for separating iron oxide and electrolyte in an iron-rich covering material for aluminum electrolysis according to claim 1, characterized in that: The alkali solution in step (3) and step (5) is a NaOH solution, and the concentration of the NaOH solution is 1-3 mol / L.

5. The method for separating iron oxide and electrolyte in an iron-rich covering material for aluminum electrolysis according to claim 1, characterized in that: The inorganic acid in step (4) is one or more of sulfuric acid, nitric acid and hydrochloric acid.