A multi-layer hard coating and its preparation method and application

CN115595532BActive Publication Date: 2024-11-12ZHUZHOU HUARUI PRECISION CUTTINGS TOOLS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211244641.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-12
Publication Date
2024-11-12
Estimated Expiration
2042-10-12

AI Technical Summary

Technical Problem

这类金属元素在高温下可以生成具有润滑性的Magnéli相氧化物,但是如专利CN108866480B和CN110907433A所述高温下这类氧化物相不稳定,容易在高温下挥发,从而导致高温耐磨性的急剧降低

Benefits of technology

[0021](1)本发明采用电弧离子镀技术沉积的多层结构硬质涂层,引入了合金元素Me(W、Mo、V),可以降低涂层摩擦系数,提高涂层的韧性。

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115595532B_ABST
    Figure CN115595532B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of surface engineering and CNC tool cutting technology, and provides a multi-layer hard coating and a preparation method and application thereof. The multi-layer hard coating deposited by the present invention using arc ion plating technology has at least three layers, including a bottom coating Al2O3 that is closely bonded to a substrate. a Cr 1‑a N, intermediate layer coating m{Al b Ti c Me 1‑b‑c N+n(Al a Cr 1‑a N / A b Ti c Me 1‑b‑c N)+Al a Cr 1‑a N+l(Al a Cr 1‑a N / A b Ti c Me 1‑b‑c N)} and the top coating Al b Ti c Me 1‑b‑c N, the introduction of alloying elements Me (W, Mo, V), can reduce the friction coefficient of the coating and improve the toughness of the coating. Under the optimization of the structure and the effect of the alloying element Me, it maintains a high hardness while having good toughness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of surface engineering and numerical control tool cutting technology, and in particular to a multi-layer structure hard coating and a preparation method and application thereof. Background Art

[0002] The application of hard coating in CNC tool cutting has a history of several decades, but with the continuous improvement of workpiece material performance, the requirements for coating performance are getting higher and higher, and the application of traditional hard coating has been limited to a certain extent. Hard coating has begun to develop in the direction of alloying and structuring.

[0003] As common nitride coatings, (Ti,Al)N coatings and (Al,Cr)N coatings are widely used in the field of CNC tool cutting. For example, in the process of machining stainless steel, the wear forms of the tool are mainly adhesive wear, diffusion wear and abrasive wear. The friction coefficient of the (Ti,Al)N coating is relatively high. During the cutting process, the cutting temperature rises rapidly, which is conducive to the development of adhesive wear and diffusion wear, resulting in rapid tool failure. In addition, the toughness of the coating is poor. During the water-cooled cutting process, the tool frequently undergoes rapid cooling, which requires certain toughness of the coating. The poor high-temperature oxidation resistance will directly cause the coating to fail at a lower temperature, and its application is subject to certain restrictions. The (Al,Cr)N coating has a great advantage in high-temperature oxidation resistance, but the friction coefficient of the coating is large, which is not conducive to chip removal during the cutting process. Poor chip removal will cause heat accumulation and more severe adhesive wear, thereby reducing the service life of the tool. Adding metal elements with lubricity to the coating can indeed improve the wear resistance and toughness of the (Ti,Al)N coating, such as W, Mo, V and other metal elements. Such metal elements can generate Magnéli phase oxides with lubricity at high temperatures, but as described in patents CN108866480B and CN110907433A, such oxides are unstable at high temperatures and easily volatilize at high temperatures, resulting in a sharp decrease in high-temperature wear resistance. In addition, as described in the document “Effect of Mo on the thermal stability, oxidation resistance, and tribo-mechanical properties of arc evaporated Ti-Al-N coatings”, the addition of such elements will also reduce the high-temperature oxidation resistance of (Ti, Al) N, and the more the amount added, the worse the high-temperature oxidation resistance of the coating. Therefore, the present invention combines the advantages of (Al, Cr) N and (Ti, Al) N coatings, and adds a small amount of metal elements with lubricity thereto, and designs a multilayer structure coating that can overcome one or several performance defects of the coating while maintaining the advantages of the (Ti, Al) N coating and the (Al, Cr) N coating. Summary of the invention

[0004] The present invention provides a multi-layer hard coating and a preparation method and application thereof, the purpose of which is to solve the above-mentioned problems existing in the background technology.

[0005] In order to achieve the above object, an embodiment of the present invention provides a multi-layer hard coating, wherein the multi-layer hard coating has at least three layers, including a bottom coating Al2O3 closely bonded to a substrate; a Cr 1-a N, intermediate layer coating m{Al bTi c Me 1-b-c N+n(Al a Cr 1-a N / A b Ti c Me 1-b-c N)+Al a Cr 1-a N+l(Al a Cr 1-a N / A b Ti c Me 1-b-c N)} and the top coating Al b Ti c Me 1-b-c N, the multilayer hard coating adopts a structural method to introduce Al with high temperature oxidation resistance a Cr 1-a N coating, wherein the atomic percentage of Al atoms is 0.2≤a≤0.8; Al b Ti c Me 1-b-c The atomic percentage of Al atoms in N is 0.4≤b≤0.7, and the atomic percentage of Ti atoms is 0.3≤c≤0.6, 2≤m≤16, 50≤n, and l≤100.

[0006] Preferably, the multilayer hard coating is alloyed by introducing alloying element Me, wherein Me is at least one of W, Mo, and V. b Ti c Me 1-b-c The N coating can generate lubricating oxides during the friction process, thereby effectively reducing the friction coefficient of the existing coating and improving wear resistance.

[0007] Preferably, the total thickness of the multilayer hard coating is 1.5 μm to 4.0 μm; a Cr 1- a N is a single-layer coating structure with a thickness of 0.2 μm to 1.0 μm; the top coating Al b Ti c Me 1-b-c N is a single-layer coating structure with a thickness of 0.2 μm to 1.0 μm; the intermediate layer coating m{Al b Ti c Me 1-b-c N+n(Al a Cr 1-a N / A b Ti c Me 1-b-c N)+Al a Cr1- a N+l(Al a Cr 1-a N / A b Ti c Me 1-b-c N)} is a multilayer structure with a thickness of 0.8μm to 2.5μm, wherein 0.2≤a≤0.8, 0.4≤b≤0.7, 0.3≤c≤0.6, 2≤m≤16, 50≤n, and l≤100.

[0008] More preferably, the intermediate layer coating m{Al b Ti c Me 1-b-c N+n(Al a Cr 1-a N / A b Ti c Me 1-b-c N)+Al a Cr 1- a N+l(Al a Cr 1-a N / A b Ti c Me 1-b-c N)} by Al b Ti c Me 1-b-c N、n(Al a Cr 1-a N / A b Ti c Me 1-b-c N), Al a Cr 1-a N and l (Al a Cr 1-a N / A b Ti c Me 1-b-c N) The four coating layers are deposited alternately in sequence, m, n, l are the number of alternating depositions, where 0.2≤a≤0.8, 0.4≤b≤0.7, 0.3≤c≤0.6, 2≤m≤16, 50≤n, l≤100.

[0009] More preferably, the first layer of the intermediate layer is Al b Ti c Me 1-b-c The thickness of the N coating is 0.02μm to 0.07μm; the second layer n (Al a Cr 1-a N / A b Ti c Me 1-b-cN) coating thickness is 0.01μm~0.05μm, and Al a Cr 1-a N layer and Al b Ti c Me 1-b- c The thickness ratio of the N layer is 0.2 to 3; the third layer of Al a Cr 1-a The coating thickness of N is 0.02μm~0.07μm; the fourth layer l (Al a Cr 1-a N / A b Ti c Me 1-b-c N) coating thickness is 0.01μm~0.05μm, and Al a Cr 1-a N layer and Al b Ti c Me 1-b-c The ratio of the thickness of the N layer is 0.2 to 3, wherein 0.2≤a≤0.8, 0.4≤b≤0.7, 0.3≤c≤0.6, 2≤m≤16, 50≤n, and l≤100.

[0010] Based on a general concept of the invention, the present invention also provides a method for preparing the above-mentioned multi-layer hard coating, comprising the following steps:

[0011] S1. Grinding, sandblasting, polishing, ultrasonic cleaning and drying the substrate;

[0012] S2. Start the cathode arc ion plating machine to perform ion cleaning on the substrate surface;

[0013] S3. Depositing a base coating on the substrate surface using ion plating technology;

[0014] S4. Depositing an intermediate coating on the base coating using an ion plating technique;

[0015] S5. Deposit a top coating on the middle coating using ion plating technology to obtain a multi-layer hard coating.

[0016] Preferably, the specific operation of ion cleaning in step S2 is: placing the substrate in a vacuum chamber of an ion plating machine, evacuating and heating until the temperature is stabilized at 400-600°C and the vacuum degree is less than 1.0×10 -3 Pa, and then fill with argon gas until the pressure in the vacuum chamber is 2.0-5.0 Pa, turn on the bias power supply, the DC negative bias voltage is 200-500V, turn on the ion source, the ion source current is 100-200A, and perform Ar ion glow cleaning on the substrate.

[0017] Preferably, the specific parameters for depositing the bottom coating in step S3 are: the arc current of the AlCr alloy target is 100-200A, the negative bias voltage of the substrate is 40-200V, the nitrogen pressure is 2.0-5.0Pa, the deposition temperature is 400-600°C, and the rotation speed of the workpiece rotating rack is 1.0-3.0rpm; the specific parameters for depositing the intermediate layer coating in step S4 are: the arc current of the AlCr alloy target and the AlTiMe alloy target are both 100-200A, the negative bias voltage of the substrate is 40-200V, the nitrogen pressure is 2.0-5.0Pa, the deposition temperature is 400-600°C, and the rotation speed of the workpiece rotating rack is 1.0-3.0rpm. V, nitrogen pressure is 2.0-5.0Pa, deposition temperature is 400-600°C, and the rotation speed of the workpiece rotating rack is 1.0-3.0rpm, wherein the alternation between layers is achieved by switching the target material; the specific parameters for depositing the top coating in step S5 are: the arc current of the AlTiMe alloy target is 100-200A, the negative bias voltage of the substrate is 40-200V, the nitrogen pressure is 2.0-5.0Pa, the deposition temperature is 400-600°C, and the rotation speed of the workpiece rotating rack is 1.0-3.0rpm.

[0018] Preferably, the substrate is a CNC blade made of cemented carbide or ceramic material; the purity of the alloy target material during the deposition process is not less than 99.96%.

[0019] The present invention also provides application of the multi-layer hard coating in the field of tool cutting and surface protective coating.

[0020] The above scheme of the present invention has the following beneficial effects:

[0021] (1) The present invention adopts arc ion plating technology to deposit a multilayer hard coating, and introduces alloy elements Me (W, Mo, V), which can reduce the friction coefficient of the coating and improve the toughness of the coating.

[0022] (2) The multilayer hard coating prepared by the present invention, under the optimization of the structure and the effect of the alloy element Me, not only maintains a high hardness (as shown in Table 1 below), but also has good toughness (as shown in Table 2 below). Figures 1 to 6 shown).

[0023] (3) Compared with the traditional (Ti,Al)N coating, the multilayer hard coating prepared by the present invention is suitable for higher cutting speeds and feed rates, which broadens the application range of the tool and prolongs the service life of the tool. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0025] Figure 1 is a comparison diagram of the microindentation morphology of the coating with a load of 100 gf in Example 1 of the present invention;

[0026] Figure 2 is a comparison diagram of the microindentation morphology of the coating with a load of 200 gf in Example 1 of the present invention;

[0027] Figure 3 is a comparison diagram of the microindentation morphology of the coating with a load of 100 gf in Example 2 of the present invention;

[0028] Figure 4 is a comparison diagram of the microindentation morphology of the coating with a load of 200 gf in Example 2 of the present invention;

[0029] Figure 5 is a comparison diagram of the microindentation morphology of the coating with a load of 100 gf in Example 3 of the present invention;

[0030] Figure 6 is a comparison diagram of the microindentation morphology of the coating with a load of 200 gf in Example 3 of the present invention;

[0031] Figure 7 It is a comparison diagram of the microindentation morphology of the coating with a load of 100 gf in Comparative Example 1 of the present invention;

[0032] Figure 8 It is a comparison diagram of the microindentation morphology of the coating with a load of 200 gf in Comparative Example 1 of the present invention;

[0033] Fig. 9 It is a comparison diagram of the microindentation morphology of the coating with a load of 100 gf in Comparative Example 2 of the present invention;

[0034] Fig.10 It is a comparison diagram of the microindentation morphology of the coating with a load of 200 gf in Comparative Example 2 of the present invention. DETAILED DESCRIPTION

[0035] In order to make the technical problems, technical solutions and advantages to be solved by the present invention more clear, a detailed description will be given below with reference to the accompanying drawings and specific embodiments.

[0036] Unless otherwise defined, all professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.

[0037] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.

[0038] (Ti,Al)N coating and (Al,Cr)N coating are common nitride coatings and are widely used in the field of CNC tool cutting. For example, in the process of machining stainless steel, the wear forms of the tool are mainly adhesive wear, diffusion wear and abrasive wear. The friction coefficient of the (Ti,Al)N coating is relatively high. During the cutting process, the cutting temperature rises rapidly, which is conducive to the development of adhesive wear and diffusion wear, resulting in rapid tool failure. In addition, the toughness of the coating is poor. During the water-cooled cutting process, the tool frequently undergoes rapid cooling, which places certain requirements on the toughness of the coating. The poor high-temperature oxidation resistance will directly cause the coating to fail at a lower temperature, and its application is subject to certain restrictions. The (Al,Cr)N coating has a great advantage in high-temperature oxidation resistance, but the friction coefficient of the coating is large, which is not conducive to chip removal during the cutting process. Poor chip removal will cause heat accumulation and more severe adhesive wear, thereby reducing the service life of the tool.

[0039] In view of the existing problems, the present invention provides a multi-layer hard coating and a preparation method and application thereof.

[0040] The embodiment of the present invention provides a multi-layer hard coating, wherein the multi-layer hard coating has at least three layers, including a bottom coating Al2O3 closely bonded to a substrate; a Cr 1-a N, intermediate layer coating m{Al b Ti c Me 1-b-c N+n(Al a Cr 1-a N / A b Ti c Me 1-b-c N)+Al a Cr 1-a N+l(Al a Cr 1-a N / A b Ti c Me 1-b-c N)} and the top coating Al b Ti c Me 1-b-c N, the multilayer hard coating adopts a structural method to introduce Al with high temperature oxidation resistance a Cr 1-a N coating, wherein the atomic percentage of Al atoms is 0.2≤a≤0.8; Al b Ti c Me 1-b-c The atomic percentage of Al atoms in N is 0.4≤b≤0.7, and the atomic percentage of Ti atoms is 0.3≤c≤0.6, 2≤m≤16, 50≤n, and l≤100.

[0041] Preferably, the multilayer hard coating is alloyed by introducing alloying element Me, wherein Me is at least one of W, Mo, and V. b Ti c Me 1-b-c The N coating can generate lubricating oxides during the friction process, thereby effectively reducing the friction coefficient of the existing coating and improving wear resistance.

[0042] Preferably, the total thickness of the multilayer hard coating is 1.5 μm to 4.0 μm; a Cr 1- a N is a single-layer coating structure with a thickness of 0.2 μm to 1.0 μm; the top coating Al b Ti c Me 1-b-c N is a single-layer coating structure with a thickness of 0.2 μm to 1.0 μm; the intermediate layer coating m{Al b Ti c Me 1-b-c N+n(Al a Cr 1-a N / A b Ti c Me 1-b-c N)+Al a Cr 1- a N+l(Al a Cr 1-a N / A b Ti c Me 1-b-c N)} is a multilayer structure with a thickness of 0.8μm to 2.5μm, wherein 0.2≤a≤0.8, 0.4≤b≤0.7, 0.3≤c≤0.6, 2≤m≤16, 50≤n, and l≤100.

[0043] More preferably, the intermediate layer coating m{Al b Ti c Me 1-b-c N+n(Al a Cr 1-a N / A b Ti c Me 1-b-c N)+Al a Cr 1- a N+l(Al a Cr 1-a N / A b Ti c Me 1-b-c N)} by Al bTi c Me 1-b-c N、n(Al a Cr 1-a N / A b Ti c Me 1-b-c N), Al a Cr 1-a N and l (Al a Cr 1-a N / A b Ti c Me 1-b-c N) The four coating layers are deposited alternately in sequence, m, n, l are the number of alternating depositions, where 0.2≤a≤0.8, 0.4≤b≤0.7, 0.3≤c≤0.6, 2≤m≤16, 50≤n, l≤100.

[0044] More preferably, the first layer of the intermediate layer is Al b Ti c Me 1-b-c The thickness of the N coating is 0.02μm to 0.07μm; the second layer n (Al a Cr 1-a N / A b Ti c Me 1-b-c N) coating thickness is 0.01μm~0.05μm, and Al a Cr 1-a N layer and Al b Ti c Me 1-b- c The thickness ratio of the N layer is 0.2 to 3; the third layer of Al a Cr 1-a The coating thickness of N is 0.02μm~0.07μm; the fourth layer l (Al a Cr 1-a N / A b Ti c Me 1-b-c N) coating thickness is 0.01μm~0.05μm, and Al a Cr 1-a N layer and Al b Ti c Me 1-b-c The ratio of the thickness of the N layer is 0.2 to 3, wherein 0.2≤a≤0.8, 0.4≤b≤0.7, 0.3≤c≤0.6, 2≤m≤16, 50≤n, and l≤100.

[0045] Based on a general concept of the invention, the present invention also provides a method for preparing the above-mentioned multi-layer hard coating, comprising the following steps:

[0046] S1. Grinding, sandblasting, polishing, ultrasonic cleaning and drying the substrate;

[0047] S2. Start the cathode arc ion plating machine to perform ion cleaning on the substrate surface;

[0048] S3. Depositing a base coating on the substrate surface using ion plating technology;

[0049] S4. Depositing an intermediate coating on the base coating using an ion plating technique;

[0050] S5. Deposit a top coating on the middle coating using ion plating technology to obtain a multi-layer hard coating.

[0051] Preferably, the specific operation of ion cleaning in step S2 is: placing the substrate in a vacuum chamber of an ion plating machine, evacuating and heating until the temperature is stabilized at 400-600°C and the vacuum degree is less than 1.0×10 -3 Pa, and then fill with argon gas until the pressure in the vacuum chamber is 2.0-5.0 Pa, turn on the bias power supply, the DC negative bias voltage is 200-500V, turn on the ion source, the ion source current is 100-200A, and perform Ar ion glow cleaning on the substrate.

[0052] Preferably, the specific parameters for depositing the bottom coating in step S3 are: the arc current of the AlCr alloy target is 100-200A, the negative bias voltage of the substrate is 40-200V, the nitrogen pressure is 2.0-5.0Pa, the deposition temperature is 400-600°C, and the rotation speed of the workpiece rotating rack is 1.0-3.0rpm; the specific parameters for depositing the intermediate layer coating in step S4 are: the arc current of the AlCr alloy target and the AlTiMe alloy target are both 100-200A, the negative bias voltage of the substrate is 40-200V, the nitrogen pressure is 2.0-5.0Pa, the deposition temperature is 400-600°C, and the rotation speed of the workpiece rotating rack is 1.0-3.0rpm. V, nitrogen pressure is 2.0-5.0Pa, deposition temperature is 400-600°C, and the rotation speed of the workpiece rotating rack is 1.0-3.0rpm, wherein the alternation between layers is achieved by switching the target material; the specific parameters for depositing the top coating in step S5 are: the arc current of the AlTiMe alloy target is 100-200A, the negative bias voltage of the substrate is 40-200V, the nitrogen pressure is 2.0-5.0Pa, the deposition temperature is 400-600°C, and the rotation speed of the workpiece rotating rack is 1.0-3.0rpm.

[0053] Preferably, the substrate is a CNC blade made of cemented carbide or ceramic material; the purity of the alloy target material during the deposition process is not less than 99.96%.

[0054] The present invention also provides application of the multi-layer hard coating in the field of tool cutting and surface protective coating.

[0055] Embodiment 1:

[0056] A multi-layer hard coating, comprising a bottom coating Al2O3 closely bonded to a substrate 0.7 Cr 0.3 N, covered with Al in the bottom coating 0.7 Cr 0.3 Intermediate layer coating on N4{Al 0.60 Ti 0.32 W 0.08 N+100(Al 0.7 Cr 0.3 N / A 0.60 Ti 0.32 W 0.08 N)+Al 0.7 Cr 0.3 N+100(Al 0.7 Cr 0.3 N / A 0.60 Ti 0.32 W 0.08 N)} and the top coating Al on the intermediate coating 0.60 Ti 0.32 W 0.08 N, wherein the substrate is a CNC blade made of cemented carbide material.

[0057] The method for preparing the multi-layer hard coating comprises the following steps:

[0058] (1) After grinding, sandblasting and polishing, the substrate is placed on the production line, ultrasonically cleaned with an alkaline cleaning agent for 20 minutes, and then baked at 150°C for 20 minutes. After cooling, it is clamped on a rotating rack and placed in a vacuum chamber.

[0059] (2) Evacuate and heat until the temperature stabilizes at 520°C and the vacuum degree is 1.0×10 -3 Pa, and then fill with argon until the pressure in the vacuum chamber is 3.5Pa, turn on the bias power supply, the DC negative bias is 200V, turn on the ion source, the ion source current is 180A, and perform Ar ion glow cleaning on the substrate for 45min.

[0060] (3) Deposition of base coating Al 0.7 Cr 0.3 The specific parameters of N are: the arc current of the AlCr alloy target is 150A, the negative bias voltage of the substrate is 60V, the nitrogen pressure is 4.0Pa, the deposition temperature is 520℃, the rotation speed of the workpiece turntable is 1.6rpm, and the deposition time is 18min.

[0061] (4) Deposition of intermediate layer coating 4{Al 0.60 Ti 0.32 W 0.08 N+100(Al0.7 Cr 0.3 N / A 0.60 Ti 0.32 W 0.08 N)+Al 0.7 Cr 0.3 N+100(Al 0.7 Cr 0.3 N / A 0.60 Ti 0.32 W 0.08 The specific parameters of the deposition method are as follows: AlCr alloy target and arc current are 150A, AlTiW alloy target arc current is 200A, substrate negative bias voltage is 150V, nitrogen pressure is 4.0Pa, deposition temperature is 520℃, workpiece rotating speed is 1.6rpm: 0.60 Ti 0.32 W 0.08 N, turn on the AlTiW alloy target, the deposition time is 5min; deposit the second coating 100 (Al 0.7 Cr 0.3 N / A 0.60 Ti 0.32 W 0.08 N), turn on the AlCr alloy target, the deposition time is 6min; deposit the third coating Al 0.7 Cr 0.3 N, turn off the AlTiW alloy target, the deposition time is 6min; deposit the fourth coating 100 (Al 0.7 Cr 0.3 N / A 0.60 Ti 0.32 W 0.08 N), turn on the AlTiW alloy target, the deposition time is 4 min, and the above four layers are alternately deposited 4 times.

[0062] (5) Deposition of top coating Al 0.60 Ti 0.32 W 0.08 The specific parameters of N are: the arc current of the AlTiW alloy target is 200A, the negative bias voltage of the substrate is 60V, the nitrogen pressure is 4.0Pa, the deposition temperature is 520℃, the rotation speed of the workpiece turntable is 1.6rpm, and the deposition time is 50min.

[0063] (6) Turn off the AlTiW alloy target, turn off the gas, turn off the bias power supply, turn off the vacuum pump, wait for the vacuum chamber to cool down to below 200° C., and then take out the substrate.

[0064] The purity of AlTiW and AlCr alloy targets is 99.97%.

[0065] Embodiment 2:

[0066] A multi-layer hard coating, comprising a bottom coating Al2O3 closely bonded to a substrate 0.7 Cr 0.3 N, covered with Al in the bottom coating 0.7 Cr 0.3 Intermediate layer coating on N4{Al 0.60 Ti 0.32 W 0.08 N+100(Al 0.7 Cr 0.3 N / A 0.60 Ti 0.32 W 0.08 N)+Al 0.7 Cr 0.3 N+100(Al 0.7 Cr 0.3 N / A 0.60 Ti 0.32 W 0.08 N)} and the top coating Al on the intermediate coating 0.60 Ti 0.32 W 0.08 N, wherein the substrate is a CNC blade made of cemented carbide material.

[0067] The method for preparing the multi-layer hard coating comprises the following steps:

[0068] (1) After grinding, sandblasting and polishing, the substrate is placed on the production line, ultrasonically cleaned with an alkaline cleaning agent for 20 minutes, and then baked at 150°C for 20 minutes. After cooling, it is clamped on a rotating rack and placed in a vacuum chamber.

[0069] (2) Evacuate and heat until the temperature stabilizes at 520°C and the vacuum degree is 1.0×10 -3 Pa, and then fill with argon until the pressure in the vacuum chamber is 3.5Pa, turn on the bias power supply, the DC negative bias is 200V, turn on the ion source, the ion source current is 180A, and perform Ar ion glow cleaning on the substrate for 45min.

[0070] (3) Deposition of the base coating Al 0.7 Cr 0.3 The specific parameters of N are: the arc current of the AlCr alloy target is 150A, the negative bias voltage of the substrate is 60V, the nitrogen pressure is 4.0Pa, the deposition temperature is 520℃, the rotation speed of the workpiece turntable is 1.6rpm, and the deposition time is 18min.

[0071] (4) Deposition of intermediate layer coating 4{Al 0.60 Ti 0.32 W 0.08 N+100(Al 0.7Cr 0.3 N / A 0.60 Ti 0.32 W 0.08 N)+Al 0.7 Cr 0.3 N+100(Al 0.7 Cr 0.3 N / A 0.60 Ti 0.32 W 0.08 The specific parameters of the deposition method are as follows: AlCr alloy target and arc current are 150A, AlTiW alloy target arc current is 200A, substrate negative bias voltage is 150V, nitrogen pressure is 4.0Pa, deposition temperature is 520℃, workpiece rotating speed is 1.6rpm: 0.60 Ti 0.32 W 0.08 N, turn on the AlTiW alloy target, the deposition time is 5min; deposit the second coating 100 (Al 0.7 Cr 0.3 N / A 0.60 Ti 0.32 W 0.08 N), turn on the AlCr alloy target, the deposition time is 6min; deposit the third coating Al 0.7 Cr 0.3 N, turn off the AlTiW alloy target, the deposition time is 6min; deposit the fourth coating 100 (Al 0.7 Cr 0.3 N / A 0.60 Ti 0.32 W 0.08 N), turn on the AlTiW alloy target, the deposition time is 4 min, and the above four layers are alternately deposited 4 times.

[0072] (5) Deposition of top coating Al 0.60 Ti 0.32 W 0.08 The specific parameters of N are: the arc current of the AlTiW alloy target is 200A, the negative bias voltage of the substrate is 60V, the nitrogen pressure is 4.0Pa, the deposition temperature is 520℃, the rotation speed of the workpiece turntable is 1.6rpm, and the deposition time is 50min.

[0073] (6) Turn off the AlTiW alloy target, turn off the gas, turn off the bias power supply, turn off the vacuum pump, wait for the vacuum chamber to cool down to below 200° C., and then take out the substrate.

[0074] The purity of AlTiW and AlCr alloy targets is 99.97%.

[0075] Embodiment 3:

[0076] A multi-layer hard coating, comprising a bottom coating Al2O3 closely bonded to a substrate 0.7 Cr 0.3 N, covered with Al in the bottom coating 0.7 Cr 0.3 Intermediate layer coating on N8{Al 0.60 Ti 0.32 W 0.08 N+60(Al 0.7 Cr 0.3 N / A 0.60 Ti 0.32 W 0.08 N)+Al 0.7 Cr 0.3 N+60(Al 0.7 Cr 0.3 N / A 0.60 Ti 0.32 W 0.08 N)} and the top coating Al on the intermediate coating 0.60 Ti 0.32 W 0.08 N, wherein the substrate is a CNC blade made of cemented carbide material.

[0077] The method for preparing the multi-layer hard coating comprises the following steps:

[0078] (1) After grinding, sandblasting and polishing, the substrate is placed on the production line, ultrasonically cleaned with an alkaline cleaning agent for 20 minutes, and then baked at 150°C for 20 minutes. After cooling, it is clamped on a rotating rack and placed in a vacuum chamber.

[0079] (2) Evacuate and heat until the temperature stabilizes at 520°C and the vacuum degree is 1.0×10 -3 Pa, and then fill with argon until the pressure in the vacuum chamber is 3.5Pa, turn on the bias power supply, the DC negative bias is 200V, turn on the ion source, the ion source current is 180A, and perform Ar ion glow cleaning on the substrate for 45min.

[0080] (3) Deposition of the base coating Al 0.7 Cr 0.3 The specific parameters of N are: the arc current of the AlCr alloy target is 150A, the negative bias voltage of the substrate is 60V, the nitrogen pressure is 4.0Pa, the deposition temperature is 520℃, the rotation speed of the workpiece turntable is 1.6rpm, and the deposition time is 18min.

[0081] (4) Deposition of intermediate layer coating 8{Al 0.60 Ti 0.32 W 0.08 N+60(Al 0.7 Cr 0.3N / A 0.60 Ti 0.32 W 0.08 N)+Al 0.7 Cr 0.3 N+60(Al 0.7 Cr 0.3 N / A 0.60 Ti 0.32 W 0.08 The specific parameters of the deposition method are as follows: AlCr alloy target and arc current are 150A, AlTiW alloy target arc current is 200A, substrate negative bias voltage is 150V, nitrogen pressure is 4.0Pa, deposition temperature is 520℃, workpiece rotating speed is 1.6rpm: 0.60 Ti 0.32 W 0.08 N, turn on the AlTiW alloy target, the deposition time is 5min; deposit the second coating 60 (Al 0.7 Cr 0.3 N / A 0.60 Ti 0.32 W 0.08 N), turn on the AlCr alloy target, the deposition time is 3min; deposit the third coating Al 0.7 Cr 0.3 N, turn off the AlTiW alloy target, the deposition time is 6min; deposit the fourth coating 60 (Al 0.7 Cr 0.3 N / A 0.60 Ti 0.32 W 0.08 N), turn on the AlTiW alloy target, the deposition time is 2 min, and the above four layers are alternately deposited 8 times.

[0082] (5) Deposition of top coating Al 0.60 Ti 0.32 W 0.08 The specific parameters of N are: the arc current of the AlTiW alloy target is 200A, the negative bias voltage of the substrate is 60V, the nitrogen pressure is 4.0Pa, the deposition temperature is 520℃, the rotation speed of the workpiece turntable is 1.6rpm, and the deposition time is 50min.

[0083] (6) Turn off the AlTiW alloy target, turn off the gas, turn off the bias power supply, turn off the vacuum pump, wait for the vacuum chamber to cool down to below 200° C., and then take out the substrate.

[0084] The purity of AlTiW and AlCr alloy targets is 99.97%.

[0085] Comparative Example 1:

[0086] (Ti,Al)N is a single-layer structural coating, in which the substrate is a CNC blade made of cemented carbide material.

[0087] The preparation method of the (Ti,Al)N coating comprises the following steps:

[0088] (1) After grinding, sandblasting and polishing, the substrate is placed on the production line, ultrasonically cleaned with an alkaline cleaning agent for 20 minutes, and then baked at 150°C for 20 minutes. After cooling, it is clamped on a rotating rack and placed in a vacuum chamber.

[0089] (2) Evacuate and heat until the temperature stabilizes at 520°C and the vacuum degree is 1.0×10 -3 Pa, and then fill with argon until the pressure in the vacuum chamber is 3.5Pa, turn on the bias power supply, the DC negative bias is 200V, turn on the ion source, the ion source current is 180A, and perform Ar ion glow cleaning on the substrate for 45min.

[0090] (3) The specific parameters for depositing the (Ti,Al)N coating are as follows: the arc current of the AlTi (atomic ratio Al:Ti = 67:33) alloy target is 200 A, the negative bias voltage of the substrate is 80 V, the nitrogen pressure is 3.5 Pa, the deposition temperature is 500 °C, the rotation speed of the workpiece turret is 1.6 rpm, and the deposition time is 160.2 min.

[0091] (4) Turn off the AlTi alloy target, turn off the gas, turn off the bias power supply, turn off the vacuum pump, wait for the vacuum chamber to cool down to below 200° C., and then take out the substrate.

[0092] The purity of the AlTi alloy targets is 99.96%.

[0093] Comparative Example 2:

[0094] (Al,Cr)N is a single-layer structural coating, in which the substrate is a CNC blade made of cemented carbide material.

[0095] The preparation method of the (Al, Cr) N coating comprises the following steps:

[0096] (1) After grinding, sandblasting and polishing, the substrate is placed on the production line, ultrasonically cleaned with an alkaline cleaning agent for 20 minutes, and then baked at 150°C for 20 minutes. After cooling, it is clamped on a rotating rack and placed in a vacuum chamber.

[0097] (2) Evacuate and heat until the temperature stabilizes at 520°C and the vacuum degree is 1.0×10-3Pa, then fill with argon gas until the pressure in the vacuum chamber is 3.5Pa, turn on the bias power supply, the DC negative bias voltage is 200V, turn on the ion source, the ion source current is 180A, and perform Ar ion glow cleaning on the substrate for 45min.

[0098] (3) The specific parameters for depositing the (Al,Cr)N coating are as follows: the arc current of the AlCr (atomic ratio Al:Cr = 70:30) alloy target is 150 A, the negative bias voltage of the substrate is 150 V, the nitrogen pressure is 4.0 Pa, the deposition temperature is 520 °C, the rotation speed of the workpiece turret is 2.0 rpm, and the deposition time is 140 min.

[0099] (4) Turn off the AlCr alloy target, turn off the gas, turn off the bias power supply, turn off the vacuum pump, wait for the vacuum chamber to cool down to below 200° C., and then take out the substrate.

[0100] The purity of the AlCr alloy targets is 99.97%.

[0101] Test example:

[0102] The hardness of the coatings prepared in the embodiment and the comparative example was tested using a nanoindenter. The obtained coating hardness data are shown in Table 1.

[0103] Table 1 Hardness data of coatings prepared in Examples and Comparative Examples

[0104] coating Comparative Example 1 Comparative Example 2 Example 1 Example 2 Example 3 Nanohardness [GPa] 34.2±2.3 31.7±2.5 37.1±2.9 36.8±2.0 35.6±3.0

[0105] It can be seen from Table 1 that the hardness of the multi-layer hard coating tool of the present application is increased by about 5% to 15% compared with the hardness of the comparative coating tool, indicating that the multi-layer hard coating of the present application has a higher hardness.

[0106] The toughness of the coatings prepared in the embodiment and the comparative example was characterized by a micro-Vickers hardness tester, and the micro-indentation morphology of the coatings was observed by a scanning electron microscope. Figures 1 to 10 As shown, when the load is 100 gf, annular cracks appear around the indentation of the coating of Comparative Example 1, while no cracks appear around the indentation of the coatings of Comparative Example 2 and Examples 1 to 3. When the load is 200 gf, cracks appear around the indentation of the coatings of Comparative Examples 1 to 2 and Example 1, while no cracks appear around the indentation of the coatings of Examples 2 and 3. The results show that under the combined effect of alloying and structuring, the toughness of the coatings obtained in the examples is improved, and the toughness of the coatings prepared in Examples 2 and 3 is relatively better.

[0107] The friction coefficients of the coatings obtained in the examples and comparative examples were characterized by a reciprocating friction and wear device, and the obtained coating friction coefficients are shown in Table 2 below. The average friction coefficient of the coating in comparative example 1 in the stable friction stage is about 0.67, the friction coefficient of the coating in comparative example 2 is 0.71, and the friction coefficients of the coatings in examples 1 to 3 are 0.60, 0.53 and 0.49, respectively. The results show that under the effect of alloying, the friction coefficient of the coating obtained in the example is reduced.

[0108] Table 2: Friction coefficients of coatings prepared in Examples and Comparative Examples

[0109] coating Comparative Example 1 Comparative Example 2 Example 1 Example 2 Example 3 Friction coefficient 0.67 0.71 0.60 0.53 0.49

[0110] The multilayer hard coating tool of the embodiment and the comparative coating tool were processed under the same cutting processing conditions, and the specific cutting parameters were as follows: the blade model was WNMG080408, the processing material was 304 stainless steel, the cutting speed Vc=240m / min, the feed rate Fz=0.25mm / rev, the cutting depth ap=1.0mm, and the cooling method was water cooling. When the blade back surface was evenly worn to 0.2mm or the tool was broken, it was judged to be failed. The cutting results are shown in Table 3:

[0111] Table 3: Cutting life of tools in the examples and comparative examples

[0112] Coated tools Flank wear width Cutting time Comparative Example 1 0.345mm 10.5min Comparative Example 2 0.296mm 10.5min Example 1 0.278mm 13.5min Example 2 0.233mm 13.5min Example 3 0.216mm 15.0min

[0113] It can be seen from Table 3 that the cutting life of the multilayer hard coating tool of the present application is increased by about 30% to 50% compared with the cutting life of the comparative coating tool, and the wear of the back tool surface is also relatively small, indicating that the multilayer hard coating of the present application has excellent cutting performance.

[0114] The above is a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A multi-layer hard coating, It is characterized in that Including the base coating Al that is closely bonded to the substrate 0.7 Cr 0.3 N, intermediate layer coating 4{Al 0.60 Ti 0.32 W 0.08 N+100(Al 0.7 Cr 0.3 N / A 0.60 Ti 0.32 W 0.08 N)+Al 0.7 Cr 0.3 N+100(Al 0.7 Cr 0.3 N / A 0.60 Ti 0.32 W 0.08 N)} and the top coating Al 0.6 Ti 0.32 W 0.08 N.

2. The multilayer hard coating according to claim 1, It is characterized in that The total thickness of the multilayer hard coating is 1.5 μm to 4.0 μm; the bottom coating Al 0.7 Cr 0.3 N is a single-layer coating structure with a thickness of 0.2 μm to 1.0 μm; the top coating Al 0.6 Ti 0.32 W 0.08 N is a single-layer coating structure with a thickness of 0.2 μm to 1.0 μm; The intermediate layer coating 4{Al 0.60 Ti 0.32 W 0.08 N+100(Al 0.7 Cr 0.3 N / A 0.60 Ti 0.32 W 0.08 N)+Al 0.7 Cr 0.3 N+100(Al 0.7 Cr 0.3 N / A 0.60 Ti 0.32 W 0.08 N)} is a multi-layer structure with a thickness of 0.8μm to 2.5μm.

3. A method for preparing a multilayer hard coating according to any one of claims 1 to 2, It is characterized in that The steps include: S1. Grinding, sandblasting, polishing, ultrasonic cleaning and drying the substrate; S2. Start the cathode arc ion plating machine to perform ion cleaning on the substrate surface; S3. Depositing a base coating on the substrate surface using ion plating technology; S4. Depositing an intermediate coating on the base coating using an ion plating technique; S5. Deposit a top coating on the middle coating using ion plating technology to obtain a multi-layer hard coating.

4. The preparation method according to claim 3, It is characterized in that The specific operation of ion cleaning in step S2 is: placing the substrate in a vacuum chamber of an ion plating machine, evacuating and heating until the temperature is stabilized at 400-600°C and the vacuum degree is less than 1.0×10 -3 Pa, and then fill with argon gas until the pressure in the vacuum chamber is 2.0-5.0 Pa, turn on the bias power supply, the DC negative bias voltage is 200-500V, turn on the ion source, the ion source current is 100-200A, and perform Ar ion glow cleaning on the substrate.

5. The preparation method according to claim 3, It is characterized in that The specific parameters for depositing the bottom layer coating in step S3 are: the arc current of the AlCr alloy target is 100-200A, the negative bias voltage of the substrate is 40-200V, the nitrogen pressure is 2.0-5.0Pa, the deposition temperature is 400-600°C, and the rotation speed of the workpiece rotating rack is 1.0-3.0rpm; the specific parameters for depositing the intermediate layer coating in step S4 are: the arc current of the AlCr alloy target and the AlTiW alloy target are both 100-200A, the negative bias voltage of the substrate is 40-200V, The nitrogen pressure is 2.0-5.0 Pa, the deposition temperature is 400-600° C., and the rotation speed of the workpiece rotating rack is 1.0-3.0 rpm, wherein the alternation between layers is achieved by switching the target material; the specific parameters for depositing the top coating in step S5 are: the arc current of the AlTiW alloy target is 100-200 A, the negative bias voltage of the substrate is 40-200 V, the nitrogen pressure is 2.0-5.0 Pa, the deposition temperature is 400-600° C., and the rotation speed of the workpiece rotating rack is 1.0-3.0 rpm.

6. The preparation method according to claim 3, It is characterized in that The substrate is a numerically controlled blade made of hard alloy or ceramic material; the purity of the alloy target material during the deposition process is not less than 99.96%.

7. Use of the multilayer hard coating according to any one of claims 1 to 2 or the multilayer hard coating obtained by the preparation method according to any one of claims 3 to 6 in the field of tool cutting and surface protective coating.