Preparation and application of a highly efficient, green and pollution-free ultra-high molecular weight polyethylene fiber

By adding bio-based degradation materials to the ultra-high molecular weight polyethylene fiber production process and carrying out specific process processing, the problems of easy fiber breakage and poor dispersion of nano-anti-bacterial particles are solved, and the preparation of high-efficiency and green ultra-high molecular weight polyethylene fibers is achieved. , has high strength, toughness and good degradability, suitable for a variety of applications.

CN115595684BActive Publication Date: 2024-11-01JIANGSU JONNYMA NEW MATERIALS CO TLD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210132191.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-02-14
Publication Date
2024-11-01
Estimated Expiration
2042-02-14

AI Technical Summary

Technical Problem

In the existing ultra-high molecular weight polyethylene fiber production process, the fiber is susceptible to high temperature and shear forces to cause fracture and degradation, which affects the spinning property and product quality of the spinning stock solution. The dispersion of nano-anti-bacterial particles in high viscosity fibers is poor. , affects the overall performance and degradability of fibers.

Method used

The ultra-high molecular weight polyethylene and bio-degradable material are dispersed in the solvent, and the gel wire is extruded and stretched after forming a gel wire. The specific process conditions and solvent selection are combined to ensure the fiber. Strength, toughness and degradability.

Benefits of technology

Improve the strength, toughness and degradability of ultra-high molecular weight polyethylene fibers, meet the processing and use requirements of ropes, cables, fishing nets and various fabrics, avoid spinning instability and surface defects, and improve production efficiency and product quality. .

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention relates to the field of C08L23 / 06, specifically to the preparation and application of an efficient, green, pollution-free ultra-high molecular weight polyethylene fiber. The present invention provides a process for preparing an efficient, green, pollution-free ultra-high molecular weight polyethylene fiber. By extruding in a twin-screw extruder and a single-screw extruder, the fiber is further dissolved and homogenized, thereby improving production efficiency while avoiding spinning instability, avoiding the generation of fiber surface defects, and ensuring product quality, strength, and toughness. Ultra-high molecular weight polyethylene is used in combination with specific bio-based degradable materials, and a specific dispersion process is used in combination with the use of solvents to improve the spinnability and degradability of the fiber, thereby avoiding the problem of product quality degradation caused by the aggregation of spinning solution on a spinneret and the unspinning, so that the ultra-high molecular weight polyethylene fiber prepared by the process has higher strength, toughness, and degradability, and is particularly suitable for the actual processing and use requirements of ropes, cables, fishing nets, and various fabrics.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of C08L23 / 06, and in particular to the preparation and application of a highly efficient, green and pollution-free ultra-high molecular weight polyethylene fiber. Background Art

[0002] At present, the production process of ultra-high molecular weight polyethylene fibers in the existing technology mostly adopts a single twin-screw extrusion method. However, the molecular chain of ultra-high molecular weight polyethylene resin is relatively long, and it is easy to break and degrade under the action of high temperature and shear force in the twin-screw extruder, which directly affects the spinnability of the spinning solution and the quality of the product.

[0003] Chinese patent CN106498532B discloses a method for preparing ultra-high molecular weight polyethylene fiber, which is obtained by swelling, plasticizing, extruding, and stretching ultra-high molecular weight polyethylene resin with solvents and antioxidants, and then spinning to obtain a method for preparing ultra-high molecular weight polyethylene fiber with shorter process and lower energy consumption, but it is easy to cause spinning instability, affect the strength and toughness of the fiber, and the production efficiency is also very low. Chinese patent CN112126999A discloses a method for preparing ultra-high molecular weight polyethylene antibacterial fiber, which is prepared by blending ultra-high molecular weight polyethylene powder and nano antibacterial particles to prepare ultra-high molecular weight polyethylene fiber with antibacterial effect, but it is impossible to ensure the good dispersion of nano antibacterial particles in ultra-high molecular weight polyethylene fiber with high viscosity, which not only increases the processing difficulty, but also affects the comprehensive performance of the fiber. At the same time, the obtained fiber has poor degradability and cannot meet the processing and use requirements of ropes, cables, fishing nets and various fabrics.

[0004] Therefore, an efficient, green and pollution-free preparation process for ultra-high molecular weight polyethylene fibers is provided to ensure product quality so that the ultra-high molecular weight polyethylene fibers prepared by the process have higher strength, toughness and biodegradability, so as to better meet the actual processing and use requirements of ropes, cables, fishing nets and various fabrics, which has important practical research and application significance. Summary of the invention

[0005] On the one hand, the present invention provides a highly efficient, green and pollution-free preparation process of ultra-high molecular weight polyethylene fiber, which comprises at least the following steps:

[0006] S1, dispersing ultra-high molecular weight polyethylene and biodegradable materials in a solvent, letting them stand for 4-6 hours, and then conveying them to a twin-screw extruder for extrusion to obtain a semi-finished product;

[0007] S2, adding the semi-finished product into a single screw extruder for extrusion, and then spinning through a spinneret to form gel filaments in a water bath;

[0008] S3, extracting the gel filaments and then stretching them to obtain the product.

[0009] Ultra-high molecular weight polyethylene has excellent wear resistance, self-lubrication and chemical stability, high strength and strong anti-aging performance, and is increasingly widely used in official, military and other fields. As a preferred technical solution, the ultra-high molecular weight polyethylene in step S1 is selected from at least one of UHMWPE L1000, UHMWPE L2000, UHMWPE L3000 and UHMWPE L5000. Preferably, the ultra-high molecular weight polyethylene in step S1 is UHMWPE L5000, so that the provided stable degradable linear polyethylene fiber has high strength, wear resistance and anti-aging performance.

[0010] The UHMWPE L5000 was purchased from Yexin Plastic Raw Materials Business Department in Zhangmutou, Dongguan City.

[0011] The biodegradable material in step S1 includes polylactic acid; the intrinsic viscosity of the polylactic acid is 39.8-49.1% dL / g; the intrinsic viscosity of the polylactic acid is 39.8-49.1% dL / g when 0.1 wt% of the polylactic acid is in chloroform at 25°C.

[0012] The polylactic acid has a CAS number of 31852-84-3 and a brand number of 900293, and was purchased from Sigma-Aldrich (Shanghai) Trading Co., Ltd.

[0013] As a preferred technical solution, the bio-based degradable material in step S1 also includes one or more of polyvinyl alcohol, polycaprolactone, polybutylene succinate, and polyhydroxyalkanoate; preferably, the bio-based degradable material in step S1 also includes polyvinyl alcohol, preferably, the weight average molecular weight of the polyvinyl alcohol is 195000-205000, preferably, the weight average molecular weight of the polyvinyl alcohol is 195000; further preferably, the degree of hydrolysis of the polyvinyl alcohol is 98-99 mol%, and the content of acetate groups is 1.1-1.9 wt%, which improves the spinnability of the fiber and avoids the problem of product quality degradation due to the accumulation of spinning solution on the spinneret without spinning.

[0014] The grade of the polyvinyl alcohol is 56-98, purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.

[0015] As a preferred technical solution, the weight ratio of the ultra-high molecular weight polyethylene and the solvent is (8-10): 1; preferably, the solvent is selected from one or more of white oil, paraffin oil, decalin, water, and alcohol solvents; preferably, the solvent includes decalin and water. The applicant found during the exploration that when the weight ratio of decalin and water is (0.8-1.2): (0.15-0.3), the ultra-high molecular weight polyethylene and the bio-based degradable material can be well dispersed in the system under specific process conditions, which helps to improve processing efficiency and ensure product quality.

[0016] The CAS number of decalin is 91-17-8, which was purchased from Wuhan Hongde Yuexin Pharmaceutical Technology Co., Ltd.

[0017] As a preferred technical solution, the specific steps of dispersing in step S1 are: dispersing the ultra-high molecular weight polyethylene and the bio-based degradable material at 20-30°C for 3-6 minutes, then stirring at 58-65°C for 50-80 minutes, continuing to heat up to 65-72°C and stirring for 25-40 minutes, and continuing to heat up to 75-85°C and stirring for 20-35 minutes.

[0018] Preferably, the specific steps of dispersing in step S1 are: dispersing the ultra-high molecular weight polyethylene and the biodegradable material at 25°C for 5 minutes, then stirring at 60°C for 60 minutes, continuing to heat to 70°C and stirring for 30 minutes, and continuing to heat to 80°C and stirring for 30 minutes.

[0019] In order to improve the degradability of ultra-high molecular weight fibers, the applicant added some bio-based degradable materials. However, the applicant found that when the bio-based degradable material is polylactic acid, the spinnability is poor during spinning, and the spinning solution gathers on the spinning plate without being stretched into filaments. After a series of studies, the applicant unexpectedly found that when the intrinsic viscosity of polylactic acid is 39.8-49.1% dL / g, in the process of dispersing ultra-high molecular weight polyethylene and polylactic acid in the solvent, first disperse at 25°C for 5 minutes, then stir at 60°C for 1 hour, then stir at 70°C for 0.5 hours, and finally stir at 80°C for 1 hour. When stirred at 0°C for 0.5h, the spinning solution did not gather at the spinneret when it was extruded through the subsequent extruder and spun. The applicant believes that the possible reason is that in the subsequent step-by-step heating and stirring and subsequent screw extrusion process, the polylactic acid and ultra-high molecular weight polyethylene molecular chains have different degrees of folding, which improves the cohesion of the spinning solution and the poor adsorption between the spinneret, avoiding the situation where the spinning solution is not drawn into filaments, improving the strength and toughness of the fiber, and making the provided ultra-high molecular weight polyethylene fiber better suitable for the processing and use of ropes, cables, fishing nets and various fabrics.

[0020] As a preferred technical solution, the extrusion temperature of the twin-screw extruder in step S1 is 180-220°C; preferably, the feeder speed of the twin-screw extruder in step S1 is 120-150r / min;

[0021] As a preferred technical solution, the extrusion temperature of the single screw extruder in step S2 is 240-260° C., and preferably, the aperture of the spinneret in step S2 is 0.1-0.3 mm.

[0022] The applicant found in the experiment that some fibers had certain surface hole defects, and unexpectedly found that when the feeder speed of the twin-screw extruder was within the specific range in this application and cooperated with the spinneret with an aperture of 0.1-0.3mm, the problem of fiber surface defects caused by polylactic acid with a characteristic viscosity of 39.8-49.1% dL / g was solved. The applicant believes that it may be that after the ultra-high molecular weight polyethylene and polylactic acid are dispersed in the solvent, at a feeder speed of 120-150r / min, the ultra-high molecular weight polyethylene is further swollen and given a certain time for physical cross-linking with the polylactic acid. In this process, the small molecular weight polymer substance in the polylactic acid may be confined between the molecular chain segments with the specific physical cross-linking degree, which can ensure that the small molecular weight polymer substance will not migrate to the surface during the further dissolution process in the subsequent single-screw extruder. Combined with the spinneret with a specific aperture, smooth and stable drawing and filamentation can be achieved, which helps to ensure the strength and product quality of the ultra-high molecular weight polyethylene fiber.

[0023] As a preferred technical solution, the weight ratio of the bio-based degradable material to the ultra-high molecular weight polyethylene in step S1 is (0.3-0.5):1, which improves the creep resistance of the fiber to a certain extent and improves the degradation function of the ultra-high molecular weight polyethylene fiber.

[0024] When the applicant selected biodegradable materials and ultra-high molecular weight polyethylene to improve biodegradability, it was unexpectedly discovered that when the biodegradable material also includes polyvinyl alcohol, and when the content of acetate groups in the polyvinyl alcohol is 1.1-1.9wt%, and the weight ratio of the biodegradable material to the ultra-high molecular weight polyethylene is controlled to be (0.3-0.5):1, and the aperture of the spinneret is 0.1-0.3mm, the obtained fiber may reduce the molecular slippage between fibers due to the appropriate hydrogen bonding force in the composite fiber, while maintaining a certain degree of orientation, and maintaining a certain stability inside the molecular chain without affecting the biodegradability of the fiber.

[0025] As a preferred technical solution, the specific steps of the stretching treatment in step S3 are: the stretching ratio is 8-10 times, and the treatment is carried out at 95-110°C for 4-8min after stretching; Preferably, the specific steps of the stretching treatment in step S3 are: the stretching ratio is 8-10 times, and the treatment is carried out at 95-110°C for 4-8min after stretching;

[0026] Generally, the fiber strength can be improved to a certain extent after heat treatment. However, the applicant unexpectedly found in the experiment that when the fiber is treated at 100°C for 5 minutes under 10 times stretching in the present application, the degradability of the obtained fiber is improved. The applicant believes that the possible reason is that the weight ratio of ultra-high molecular weight polyethylene and polylactic acid in the present application is 1: (0.3-0.5). Under specific molecular physical entanglement, under specific stretching multiples and heat treatment, the specific regularity of the macromolecular chain, when the degradation process occurs, it is easier to stimulate the inertial motion of the polyethylene chain segment when the carbon chain breaks under the action of PVC oxidase and dehydrogenase.

[0027] On the other hand, the present invention provides an application of degradable ultra-high molecular weight polyethylene fiber prepared by an efficient, green and pollution-free ultra-high molecular weight polyethylene fiber preparation process, which is particularly suitable for the processing and use of ropes, cables, fishing nets and various fabrics.

[0028] Beneficial effects:

[0029] 1. The present invention provides a highly efficient, green and pollution-free preparation process for ultra-high molecular weight polyethylene fibers, which ensures product quality and enables the ultra-high molecular weight polyethylene fibers prepared by the process to have higher strength, toughness and degradability, so as to better meet the actual processing and use requirements of ropes, cables, fishing nets and various fabrics.

[0030] 2. Through extrusion treatment in a twin-screw extruder and a single-screw extruder respectively, further dissolution and homogenization are achieved, which improves production efficiency while avoiding spinning instability and fiber surface defects, thus ensuring product quality, strength and toughness.

[0031] 3. By using ultra-high molecular weight polyethylene in combination with specific biodegradable materials and using a specific dispersion process and solvent, the spinnability of the fiber is improved, avoiding the problem of product quality degradation caused by the accumulation of spinning solution on the spinneret.

[0032] 4. Under specific processes, by controlling the weight ratio of ultra-high molecular weight polyethylene and bio-based degradable materials to (0.3-0.5):1, the creep resistance of the fiber is improved to a certain extent, and the degradation function of the ultra-high molecular weight polyethylene fiber is improved.

[0033] 5. Through specific stretching treatment, not only the high strength of polyethylene fiber is guaranteed, but also the introduction of biodegradable materials significantly improves the degradability of ultra-high molecular weight polyethylene fiber, meeting the requirements of green production. DETAILED DESCRIPTION

[0034] Example 1

[0035] Embodiment 1 of the present invention provides a process for preparing an efficient, green and pollution-free ultra-high molecular weight polyethylene fiber, comprising the following steps:

[0036] S1, dispersing ultra-high molecular weight polyethylene and biodegradable materials in a solvent, letting them stand for 5 hours, and then conveying them to a twin-screw extruder for extrusion to obtain a semi-finished product;

[0037] S2, adding the semi-finished product into a single screw extruder for extrusion, and then spinning through a spinneret to form gel filaments in a water bath;

[0038] S3, extracting the gel filaments and then stretching them to obtain the product.

[0039] The ultra-high molecular weight polyethylene in step S1 is UHMWPE L5000, and the UHMWPE L5000 is purchased from Dongguan Zhangmutou Yexin Plastic Raw Materials Business Department.

[0040] In the step S1, the biodegradable material is polylactic acid; the intrinsic viscosity of the polylactic acid is 39.8-49.1% dL / g; the intrinsic viscosity of the polylactic acid is 39.8-49.1% dL / g when 0.1 wt% of the polylactic acid is in chloroform at 25°C.

[0041] The polylactic acid has a CAS number of 31852-84-3 and a brand number of 900293, and was purchased from Sigma-Aldrich (Shanghai) Trading Co., Ltd.

[0042] The weight ratio of the ultra-high molecular weight polyethylene to the solvent is 9:1; the solvent includes decalin and water, and the weight ratio of the decalin to water is 1:0.2.

[0043] The CAS number of decalin is 91-17-8, which was purchased from Wuhan Hongde Yuexin Pharmaceutical Technology Co., Ltd.

[0044] The specific steps of dispersing in step S1 are: dispersing the ultra-high molecular weight polyethylene and the biodegradable material at 25° C. for 5 minutes, then stirring at 60° C. for 60 minutes, continuing to heat up to 70° C. and stirring for 30 minutes, and continuing to heat up to 80° C. and stirring for 30 minutes.

[0045] The extrusion temperature of the twin-screw extruder in step S1 is 200° C.; the feeder speed of the twin-screw extruder in step S1 is 130 r / min.

[0046] The extrusion temperature of the single screw extruder in step S2 is 250° C.; the aperture of the spinneret in step S2 is 0.2 mm.

[0047] In the step S1, the weight ratio of the bio-based degradable material to the ultra-high molecular weight polyethylene is 0.4:1.

[0048] The specific steps of the stretching treatment in step S3 are: the stretching ratio is 9 times, and the stretching is followed by treatment at 100° C. for 5 minutes.

[0049] Example 2

[0050] Embodiment 2 of the present invention provides a process for preparing an efficient, green and pollution-free ultra-high molecular weight polyethylene fiber, comprising the following steps:

[0051] S1, dispersing ultra-high molecular weight polyethylene and biodegradable materials in a solvent, letting them stand for 5 hours, and then conveying them to a twin-screw extruder for extrusion to obtain a semi-finished product;

[0052] S2, adding the semi-finished product into a single screw extruder for extrusion, and then spinning through a spinneret to form gel filaments in a water bath;

[0053] S3, extracting the gel filaments and then stretching them to obtain the product.

[0054] The ultra-high molecular weight polyethylene in step S1 is UHMWPE L5000, and the UHMWPE L5000 is purchased from Dongguan Zhangmutou Yexin Plastic Raw Materials Business Department.

[0055] In the step S1, the biodegradable material is polylactic acid; the intrinsic viscosity of the polylactic acid is 39.8-49.1% dL / g; the intrinsic viscosity of the polylactic acid is 39.8-49.1% dL / g when 0.1 wt% of the polylactic acid is in chloroform at 25°C.

[0056] The polylactic acid has a CAS number of 31852-84-3 and a brand number of 900293, and was purchased from Sigma-Aldrich (Shanghai) Trading Co., Ltd.

[0057] The weight ratio of the ultra-high molecular weight polyethylene to the solvent is 8:1; the solvent includes decalin and water, and the weight ratio of the decalin to water is 1.2:0.3.

[0058] The CAS number of decalin is 91-17-8, which was purchased from Wuhan Hongde Yuexin Pharmaceutical Technology Co., Ltd.

[0059] The specific steps of dispersing in step S1 are: dispersing the ultra-high molecular weight polyethylene and the biodegradable material at 30° C. for 4 minutes, then stirring at 65° C. for 50 minutes, continuing to heat up to 72° C. and stirring for 25 minutes, and continuing to heat up to 85° C. and stirring for 20 minutes.

[0060] The extrusion temperature of the twin-screw extruder in step S1 is 220° C.; the feeder speed of the twin-screw extruder in step S1 is 120 r / min.

[0061] The extrusion temperature of the single screw extruder in step S2 is 260° C.; the aperture of the spinneret in step S2 is 0.3 mm.

[0062] In the step S1, the weight ratio of the bio-based degradable material to the ultra-high molecular weight polyethylene is 0.5:1.

[0063] The specific steps of the stretching treatment in step S3 are: the stretching ratio is 10 times, and after stretching, the treatment is carried out at 110° C. for 4 minutes.

[0064] Example 3

[0065] Embodiment 3 of the present invention provides a process for preparing an efficient, green and pollution-free ultra-high molecular weight polyethylene fiber, comprising the following steps:

[0066] S1, dispersing ultra-high molecular weight polyethylene and biodegradable materials in a solvent, letting them stand for 5 hours, and then conveying them to a twin-screw extruder for extrusion to obtain a semi-finished product;

[0067] S2, adding the semi-finished product into a single screw extruder for extrusion, and then spinning through a spinneret to form gel filaments in a water bath;

[0068] S3, extracting the gel filaments and then stretching them to obtain the product.

[0069] The ultra-high molecular weight polyethylene in step S1 is UHMWPE L5000, and the UHMWPE L5000 is purchased from Dongguan Zhangmutou Yexin Plastic Raw Materials Business Department.

[0070] In the step S1, the biodegradable material is polylactic acid; the intrinsic viscosity of the polylactic acid is 39.8-49.1% dL / g; the intrinsic viscosity of the polylactic acid is 39.8-49.1% dL / g when 0.1 wt% of the polylactic acid is in chloroform at 25°C.

[0071] The polylactic acid has a CAS number of 31852-84-3 and a brand number of 900293, and was purchased from Sigma-Aldrich (Shanghai) Trading Co., Ltd.

[0072] The weight ratio of the ultra-high molecular weight polyethylene to the solvent is 8:1; the solvent includes decalin and water, and the weight ratio of the decalin to water is 0.8:0.15.

[0073] The CAS number of decalin is 91-17-8, which was purchased from Wuhan Hongde Yuexin Pharmaceutical Technology Co., Ltd.

[0074] The specific steps of dispersing in step S1 are: dispersing the ultra-high molecular weight polyethylene and the biodegradable material at 20° C. for 6 minutes, then stirring at 58° C. for 65 minutes, continuing to heat up to 65° C. and stirring for 40 minutes, and continuing to heat up to 75° C. and stirring for 35 minutes.

[0075] The extrusion temperature of the twin-screw extruder in step S1 is 180° C.; the feeder speed of the twin-screw extruder in step S1 is 150 r / min;

[0076] The extrusion temperature of the single screw extruder in step S2 is 240° C.; the aperture of the spinneret in step S2 is 0.1 mm.

[0077] In the step S1, the weight ratio of the bio-based degradable material to the ultra-high molecular weight polyethylene is 0.3:1.

[0078] The specific steps of the stretching treatment in step S3 are: the stretching ratio is 8 times, and after stretching, the treatment is carried out at 95° C. for 6 minutes;

[0079] Comparative Example 1

[0080] Comparative Example 1 of the present invention provides a highly efficient, green and pollution-free preparation process for ultra-high molecular weight polyethylene fiber, and its specific implementation method is the same as that of Example 1, except that the bio-based degradable material is polybutylene succinate, which is purchased from Beijing Hengye COSCO Chemical Co., Ltd.

[0081] Comparative Example 2

[0082] Comparative Example 2 of the present invention provides a preparation process for an efficient, green and pollution-free ultra-high molecular weight polyethylene fiber, and its specific implementation method is the same as that of Example 1, except that the specific steps of dispersion in step S1 are: dispersing the ultra-high molecular weight polyethylene and the bio-based degradable material at 100°C for 50 minutes.

[0083] Comparative Example 3

[0084] Comparative Example 3 of the present invention provides a highly efficient, green and pollution-free preparation process for ultra-high molecular weight polyethylene fiber, and its specific implementation method is the same as that of Example 1, except that the extrusion temperature of the twin-screw extruder in step S1 is 250°C, and the feeder speed of the twin-screw extruder in step S1 is 200r / min.

[0085] Comparative Example 4

[0086] Comparative Example 4 of the present invention provides a process for preparing an efficient, green, pollution-free ultra-high molecular weight polyethylene fiber, and its specific implementation method is the same as that of Example 1, except that the weight ratio of the bio-based degradable material to the ultra-high molecular weight polyethylene is 1:1.

[0087] Performance Testing Methods

[0088] (1) Fiber quality: The ultra-high molecular weight polyethylene fibers prepared in the examples and comparative examples were cut into fiber samples of 0.5 mm×0.5 mm, and the surfaces of the fiber samples were observed using SEM to determine whether there were any defects.

[0089] (2) Spinnability: Observe whether the spinneret surface is blocked during the preparation of ultra-high molecular weight polyethylene fibers in the examples and comparative examples.

[0090] (3) Breaking strength: The polyethylene fiber samples prepared in the examples and comparative examples were cut into fiber samples of 10 mm×5 mm, and the breaking strength of the fiber samples was measured at room temperature with a tensile rate of 15 mm / min according to GB-T 3916-2013.

[0091] (4) Biodegradation rate: Referring to GB / T19277, the polyethylene fibers prepared in the examples and comparative examples were made into 10 μm fiber samples. The fiber samples were mixed with compost inoculants and placed in a composting container. Oxygen was introduced at a temperature of 58±2°C and a humidity of 50-55% for sufficient composting. The final release of CO2 after 45 days of degradation was measured. The biodegradation rate is the ratio of the actual CO2 release to its theoretical maximum release. The detection reference material was cellulose with a particle size of 10 μm. The degradation rate of the reference material after 45 days was 85%.

[0092] Test items Fiber quality Spinnability Breaking strength (cN / dtex) Biodegradation rate (%) Example 1 No defects Not blocked 25 15 Example 2 No defects Not blocked 24.6 14.5 Example 3 No defects Not blocked 24.2 14 Comparative Example 1 Defective Not blocked 22.1 13 Comparative Example 2 Defective Blockage 18.5 11 Comparative Example 3 Defective Blockage 19 10 Comparative Example 4 Defective Blockage 20.8 12

Claims

1. A process for preparing an efficient, green and pollution-free ultra-high molecular weight polyethylene fiber, characterized in that: At least the following steps are included: S1, dispersing ultra-high molecular weight polyethylene and biodegradable materials in a solvent, letting them stand for 4-6 hours, and then conveying them to a twin-screw extruder for extrusion to obtain a semi-finished product; S2, adding the semi-finished product into a single screw extruder for extrusion, and then spinning through a spinneret to form gel filaments in a water bath; S3, extracting the gel filaments and then stretching them to obtain the gel filaments; In step S1, the biodegradable material includes polylactic acid, and the intrinsic viscosity of the polylactic acid is 39.8-49.1% dL / g at 25° C. for 0.1 wt % of the polylactic acid in chloroform; The specific steps of dispersing in step S1 are: dispersing the ultra-high molecular weight polyethylene and the biodegradable material at 20-30° C. for 3-6 minutes, then stirring at 58-65° C. for 50-80 minutes, continuing to heat to 65-72° C. and stirring for 25-40 minutes, and continuing to heat to 75-85° C. and stirring for 20-35 minutes; The extrusion temperature of the twin-screw extruder in step S1 is 180-220° C., and the feeder speed of the twin-screw extruder in step S1 is 120-150 r / min; The extrusion temperature of the single screw extruder in step S2 is 240-260° C., and the aperture of the spinneret in step S2 is 0.1-0.3 mm.

2. The process for preparing a highly efficient, green and pollution-free ultra-high molecular weight polyethylene fiber according to claim 1, characterized in that: The weight ratio of the ultra-high molecular weight polyethylene to the solvent is (8-10):

1.

3. The process for preparing a highly efficient, green and pollution-free ultra-high molecular weight polyethylene fiber according to claim 1, characterized in that: In the step S1, the weight ratio of the bio-based degradable material to the ultra-high molecular weight polyethylene is (0.3-0.5):

1.

4. The process for preparing a highly efficient, green and pollution-free ultra-high molecular weight polyethylene fiber according to claim 1, characterized in that: The specific steps of the stretching treatment in step S3 are: the stretching ratio is 8-10 times, and after stretching, the treatment is carried out at 95-110° C. for 4-8 minutes.

5. An application of a high-efficiency, green and pollution-free ultra-high molecular weight polyethylene fiber preparation process according to any one of claims 1 to 4, characterized in that: The high-efficiency, green and pollution-free ultra-high molecular weight polyethylene fiber is suitable for the processing and use of ropes, cables and fishing nets.