Boron nitride particles, boron nitride powder, resin composition, and method for producing resin composition

By loading and unloading treatment in the short side direction of the boron nitride particles, the shape recovery is ensured, and the problem of the reduction of thermal conductivity of boron nitride particles in the heat dissipation material is solved, and the thermal conductivity and elastic deformation ability of the material are improved.

CN115605428BActive Publication Date: 2024-11-15DENKA CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202180035668.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-08-20
Filing Date
2021-08-19
Publication Date
2024-11-15
Estimated Expiration
2041-08-19

AI Technical Summary

Technical Problem

When using boron nitride particles as heat dissipation material, in order to improve thermal conductivity, elongated boron nitride particles need to be able to restore their original shape during loading and unloading to avoid deformation affecting thermal conductivity.

Method used

The shortness of the boron nitride particles is ensured by gradually applying the load from 0.27 mN/s at a load speed of 0.27 mN/s at a load speed of 0.27 mN/s, and gradually unloading at a unloading speed of 0.27 mN/sec. The edge-direction length returns to its original state when unloading, and the boron nitride particles have a shell portion and a hollow portion formed of boron nitride, enhancing their elastic deformation ability.

Benefits of technology

The shape recovery of boron nitride particles during compression and pressure relief is achieved, the thermal conductivity of the heat dissipation material and the elastic deformation ability of the material are improved, and the stability of the heat conduction path and excellent heat dissipation performance are ensured.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115605428B_ABST
    Figure CN115605428B_ABST
Patent Text Reader

Abstract

Boron nitride particles have an elongated shape, and when subjected to a load-unloading test having a loading step and an unloading step in sequence, at least a portion of the length of the short-side direction of the boron nitride particles compressed in the loading step is restored in the unloading step, wherein the loading step is a step of compressing the boron nitride particles by gradually applying a load from 0.2 mN to 20 mN at a load speed of 0.27 mN / second in the short-side direction of the boron nitride particles, and the unloading step is a step of gradually unloading the load to 0.2 mN at an unloading speed of 0.27 mN / second.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to boron nitride particles, boron nitride powder, a resin composition and a method for producing the resin composition. Background Art

[0002] Boron nitride has lubricity, high thermal conductivity, and insulation properties, and is used in a variety of applications, including solid lubricants, mold release materials, raw materials for cosmetics, heat dissipation materials, and sintered bodies with heat resistance and insulation properties.

[0003] For example, Patent Document 1 discloses a hexagonal boron nitride powder that can impart high thermal conductivity and high insulation resistance to a resin composition filled with a resin, wherein the hexagonal boron nitride powder comprises aggregated particles formed of primary particles of hexagonal boron nitride and has a BET specific surface area of ​​0.7 to 1.3 m 2 / g, and the oil absorption measured based on JIS K 5101-13-1 is 80 g / 100 g or less.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2016-160134 Summary of the invention

[0007] Problems to be solved by the invention

[0008] According to the research of the inventors of the present application, when the boron nitride particles are used in, for example, a heat dissipation material (heat sink), it is desirable that the boron nitride particles have an elongated shape in order to improve the thermal conductivity in a specific direction. In addition, when the boron nitride particles are mixed with a resin and formed into a sheet for use as a heat dissipation material, a load is sometimes applied to the boron nitride particles during mixing with the resin or during forming of the heat dissipation material, causing the boron nitride particles to deform. However, it is desirable that when the load is removed, the boron nitride particles return to their original shape, or return to a shape as close to the original shape as possible.

[0009] The main purpose of the present invention is to provide novel boron nitride particles and boron nitride powder.

[0010] Means for solving problems

[0011] One aspect of the present invention is a boron nitride particle having an elongated shape. When the boron nitride particle is subjected to a load-unloading test sequentially including a loading step and an unloading step, at least a portion of the length of the short side direction of the boron nitride particle compressed in the loading step is restored in the unloading step. The loading step is a step of compressing the boron nitride particle by gradually applying a load from 0.2 mN to 20 mN at a loading speed of 0.27 mN / second in the short side direction. The unloading step is a step of gradually unloading the load to 0.2 mN at an unloading speed of 0.27 mN / second.

[0012] When the amount of displacement of the boron nitride particles in the short-side direction in the loading step is D1 and the amount of displacement of the boron nitride particles in the short-side direction in the unloading step is D2, D2 / D1 may be greater than or equal to 0.2.

[0013] The boron nitride particles may include an outer shell portion formed of boron nitride and a hollow portion surrounded by the outer shell portion.

[0014] Another aspect of the present invention is a boron nitride powder, wherein the boron nitride powder is an aggregate of boron nitride particles having an elongated shape, and when subjected to a load-unloading test having the following steps (1) to (3) in sequence, at least a portion of the length in the short side direction of the boron nitride particles B compressed in the loading step is restored in the unloading step.

[0015] (1) a calculation step of applying a load at a load rate of 0.27 mN / sec in the short-side direction of each of 10 boron nitride particles A selected from the boron nitride powder to crush the boron nitride particles A, and calculating an average value F of the load;

[0016] (2) a loading step of compressing the boron nitride particles B selected from the boron nitride powder separately from the boron nitride particles A by gradually applying a load in the short-side direction at a loading rate of 0.27 mN / sec from 0.2 mN to 50% of the average value F of the load;

[0017] (3) Unloading step: The boron nitride particles B are gradually unloaded at an unloading rate of 0.27 mN / sec until the load reaches 0.2 mN.

[0018] Alternatively, when the average value of the displacement of the boron nitride particles B in the short side direction in the loading step is set to D3 and the average value of the displacement of the boron nitride particles B in the short side direction in the unloading step is set to D4, D4 / D3 is greater than 0.2.

[0019] The boron nitride powder may be an aggregate of boron nitride particles having an outer shell portion formed of boron nitride and a hollow portion surrounded by the outer shell portion.

[0020] Another aspect of the present invention is a resin composition comprising a resin and the above-mentioned boron nitride particles or the above-mentioned boron nitride powder.

[0021] Another aspect of the present invention is a method for producing a resin composition, which comprises the following steps: a step of preparing the boron nitride particles or the boron nitride powder; a step of mixing the boron nitride particles or the boron nitride powder with a resin. The method for producing a resin composition may further comprise a step of crushing the boron nitride particles or the boron nitride powder.

[0022] Effects of the Invention

[0023] According to one aspect of the present invention, novel boron nitride particles and boron nitride powder can be provided. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] [ Figure 1 ] is a schematic diagram showing the relationship between the load amount and the displacement amount of the boron nitride particles when the boron nitride particles are subjected to a load and unloading test.

[0025] [ Figure 2 ] is a graph showing the X-ray diffraction measurement results of the boron nitride particles of Example 1.

[0026] [ Figure 3 ] is a SEM image of the boron nitride particles of Example 1.

[0027] [ Figure 4 ] is a graph showing the relationship between the load amount and the displacement amount of the boron nitride particles when the boron nitride particles B (particle No. 1) of Example 1 are subjected to a load unloading test. DETAILED DESCRIPTION

[0028] Hereinafter, embodiments of the present invention will be described in detail.

[0029] (First embodiment: Boron nitride particles)

[0030] One embodiment (first embodiment) of the present invention is a boron nitride particle having an elongated shape. The boron nitride particle having an elongated shape may have an aspect ratio of, for example, 1.5 or more. The aspect ratio of the boron nitride particle may be 1.6 or more, 1.7 or more, 1.8 or more, 1.9 or more, 2.0 or more, 2.5 or more, or 3.0 or more, and may be 12.0 or less, 10.0 or less, 9.5 or less, 9.0 or less, or 8.0 or less.

[0031] The aspect ratio of a boron nitride particle is defined as the maximum length (L a), and the maximum length of the boron nitride particle in the direction perpendicular to the direction having the maximum length (L b ) ratio (L a / L b ). The maximum length of the boron nitride particle (L a ) refers to the maximum length among the straight-line distances between any two points on a boron nitride particle when the boron nitride particle is observed under a microscope. The microscope may be, for example, a microscope attached to a micro compression tester (e.g., MCT series manufactured by Shimadzu Corporation). The maximum length (L a ) can be measured by importing the observed image into image analysis software (for example, software attached to a micro compression tester). The maximum length (L) of the boron nitride particle in the direction perpendicular to the direction with the maximum length b ) can be used with a maximum length (L a ) were determined by the same method.

[0032] The larger the aspect ratio of the boron nitride particles, the more elongated the shape of the boron nitride particles. Therefore, it is believed that, for example, when the boron nitride particles are mixed with a resin as a heat dissipation material, the boron nitride particles become easy to overlap with each other. In addition, it is believed that when the boron nitride particles with an elongated shape overlap with other boron nitride particles, the boron nitride particles with an elongated shape overlap in an inclined manner. Therefore, it is believed that the number of particles arranged in the thickness direction of the heat dissipation material decreases, and the heat conduction loss between the boron nitride particles decreases, so the thermal conductivity of the heat dissipation material is more excellent.

[0033] The maximum length of the boron nitride particles (L a ) can be greater than 80μm, greater than 100μm, greater than 125μm, greater than 150μm, greater than 175μm, greater than 200μm, greater than 225μm, greater than 250μm, greater than 275μm, or greater than 300μm, and can be less than 500μm or less than 400μm.

[0034] The maximum length (L a ) direction, the maximum length (L b ) can be greater than 50 μm, greater than 60 μm, greater than 70 μm, or greater than 80 μm, and can be less than 300 μm, less than 200 μm, less than 150 μm, or less than 100 μm.

[0035] The appearance shape of the boron nitride particles is not particularly limited as long as it is an elongated shape. The boron nitride particles can be shaped or amorphous. As the appearance shape of the boron nitride particles, a rotational ellipsoid, a rod, a dumbbell, etc. can be cited. For example, the boron nitride particles can also have a branching structure that branches in two or more directions.

[0036] Boron nitride particles can be solid or hollow. When the boron nitride particles are hollow, the boron nitride particles can have an outer shell formed by boron nitride and a hollow portion surrounded by the outer shell. The hollow portion can extend along the length direction of the boron nitride particles. That is, the boron nitride particles can also be tubular. In this case, at least one of the ends in the length direction of the boron nitride particles can be an open end, or all the ends can be open ends. The open end can be connected to the above-mentioned hollow portion. The boron nitride particles are hollow, and at least one of the ends in the length direction of the boron nitride particles is an open end, so that when the boron nitride particles are mixed with a resin and used as a heat dissipation material, for example, the resin lighter than the boron nitride particles is filled in the hollow portion, so it can be expected that the thermal conductivity of the heat dissipation material will be improved, and the heat dissipation material will be lightweight.

[0037] The boron nitride particles of the present embodiment are boron nitride particles in which at least a portion of the length of the short side direction of the boron nitride particles compressed in the loading step is restored in the unloading step when being subjected to a load-unloading test having a loading step and an unloading step in sequence. The loading step is a step of compressing the boron nitride particles by gradually applying a load from 0.2 mN to 20 mN at a load speed of 0.27 mN / second in the short side direction, and the unloading step is a step of gradually unloading the load to 0.2 mN at an unloading speed of 0.27 mN / second.

[0038] In the loading process, first, boron nitride particles are set on the sample table. At this time, the boron nitride particles are set in a manner that the length direction of the boron nitride particles is along the setting surface of the sample table. Then, the indenter (for example, the indenter diameter is 200 μm) of a micro compression testing machine (for example, MCT series manufactured by Shimadzu Corporation) is lowered toward a boron nitride particle on the sample table, and a load is gradually applied to the boron nitride particles from 0.2 mN to 20 mN at a load speed of 0.27 mN / second. At this time, the size (displacement) of the displacement of the boron nitride particles relative to the applied load (load amount) is measured.

[0039] In the unloading process, the load (20 mN) in the loading process is applied to the boron nitride particles, and the load is gradually unloaded at an unloading speed of 0.27 mN / second until it reaches 0.2 mN. At this time, the displacement of the boron nitride particles relative to the load is also measured. It should be noted that the time from the end of the loading process to the start of the unloading process (maintaining the state of applying a load of 20 mN to the boron nitride particles) is less than 5 seconds.

[0040] Figure 1 FIG. 2 shows an example of the relationship between the load amount and the displacement amount of the boron nitride particles when the boron nitride particles are subjected to the load unloading test. Figure 1As shown, when the displacement amount of the boron nitride particles is set to X and the load amount is set to Y, for example, the displacement amount X and the load amount Y of the boron nitride particles in the loading process are in a relationship like the load curve L1, and the displacement amount X and the load amount Y of the boron nitride particles in the unloading process are in a relationship like the unloading curve L2.

[0041] When the amount (absolute value) of displacement of the boron nitride particles in the short side direction in the loading process is set to D1, and the amount (absolute value) of displacement of the boron nitride particles in the short side direction in the unloading process is set to D2, the so-called recovery of at least a portion of the length of the short side direction of the boron nitride particles compressed in the loading process in the unloading process means that D2>0. In addition, the larger the recovery rate (D2 / D1) indicating the degree to which the boron nitride particles compressed in the unloading process recover, the more preferred. The recovery rate (D2 / D1) can be, for example, 0.2 or more, 0.25 or more, 0.3 or more, 0.35 or more, or 0.4 or more.

[0042] A large recovery rate can also be said to be a large elastic deformation work ratio of the boron nitride particles. That is, the larger the elastic deformation work ratio of the boron nitride particles, the easier it is for the boron nitride particles to return to their original shape even if they are compressed. The elastic deformation work ratio of the boron nitride particles can be, for example, 0.1 or more, 0.15 or more, 0.2 or more, 0.25 or more, 0.3 or more, or 0.35 or more.

[0043] The elastic deformation work ratio of boron nitride particles is defined as follows. Figure 1 As shown in FIG. 1 , the area of ​​a region P surrounded by the load curve L1, the unloading curve L2, and the straight line L3 indicating Y=0.2 mN is defined as the plastic deformation work W. P The area of ​​the region E surrounded by the unloading curve L2, the straight line L3, and the straight line L4 connecting the intersection of the load curve L1 and the unloading curve L2 and the straight line L3 and parallel to the Y axis is defined as the elastic deformation work W. E , W P With W E The sum of (W P +W E ) is set as the total work W T When the elastic deformation work ratio is defined as relative to the total work W T The elastic deformation work W E The ratio (W E / W T ).

[0044] Even if the boron nitride particles involved in one embodiment are deformed by applying a load from the outside, they return to a shape close to the original shape when unloading. Therefore, for example, when the boron nitride particles are mixed with a resin and formed into a sheet to make a heat dissipation material, even if the boron nitride particles are deformed during mixing with the resin or during the molding of the heat dissipation material, the boron nitride particles return to a shape close to the original shape afterwards. Therefore, compared with the previous boron nitride particles, the boron nitride particles are easy to maintain a heat conduction path in the heat dissipation material. In addition, the boron nitride particles have an elongated shape, so the thermal conductivity in a specific direction in the heat dissipation material can also be particularly improved. Thus, the boron nitride particles can be preferably used as a heat dissipation material. It should be noted that although the use of the boron nitride particles as a heat dissipation material is illustrated, the boron nitride particles are not limited to heat dissipation materials and can be used for various purposes.

[0045] (Second embodiment: Boron nitride powder)

[0046] Another embodiment (second embodiment) of the present invention is a boron nitride powder, which is an aggregate of elongated boron nitride particles (a powder composed of a plurality of elongated boron nitride particles). In the boron nitride powder involved in the second embodiment, each boron nitride particle may be the boron nitride particle involved in the first embodiment.

[0047] The boron nitride powder according to the second embodiment may be a boron nitride powder in which, when subjected to a load-unload test including the following steps (1) to (3) in sequence, at least a portion of the length in the short side direction of the boron nitride particles B compressed in the loading step is restored in the unloading step:

[0048] (1) a calculation step of applying a load at a load rate of 0.27 mN / sec in the short-side direction of each of 10 boron nitride particles A selected from the boron nitride powder and measuring the magnitude of the load required to crush the boron nitride particles A, and calculating an average value F of the magnitude of the load;

[0049] (2) a loading step of compressing the boron nitride particles B selected from the boron nitride powder separately from the boron nitride particles A by gradually applying a load in the short-side direction of each of the boron nitride particles B at a loading rate of 0.27 mN / sec from 0.2 mN to 50% of the average value F of the load;

[0050] (3) Unloading step: gradually unloading the load at a rate of 0.27 mN / s until the load reaches 0.2 mN.

[0051] In the calculation process, first, more than 10 boron nitride particles selected from boron nitride powder are set on the sample table. At this time, the boron nitride particles are set in a manner that the length direction of each boron nitride particle is along the setting surface of the sample table. Then, the indenter (for example, the indenter diameter is 200 μm) of a micro compression testing machine (for example, MCT series manufactured by Shimadzu Corporation) is lowered toward one boron nitride particle on the sample table, and a load is applied at a load speed of 0.27 mN / second. In addition, the size of the load when the displacement in the short side direction of the boron nitride particle rises sharply is measured as the size of the load required to crush the boron nitride particle. The measurement is performed in the same way for 10 boron nitride particles (the boron nitride particles are referred to as boron nitride particles A), and the average value F (mN) of the size of the load required to crush the boron nitride particles A is calculated.

[0052] Then, a loading process is performed on the boron nitride particles (these boron nitride particles are referred to as boron nitride particles B) selected separately from the boron nitride powder relative to the boron nitride particles A in the same manner as described in the first embodiment. However, the loading process in the second embodiment is different from the loading process in the first embodiment in the following respects: a load is gradually applied to the boron nitride particles B from 0.2 mN to 50% of the average value F (mN) calculated in the above calculation process at a load speed of 0.27 mN / second. Then, an unloading process is performed on the boron nitride particles B in the same manner as described in the first embodiment. In the loading process and the unloading process, the displacement of the boron nitride particles B relative to the load amount is measured in the same manner as described in the first embodiment.

[0053] As described in the first embodiment, Figure 1 FIG. 2 shows an example of the relationship between the load amount and the displacement amount of the boron nitride particle B when the boron nitride particle B is subjected to a load and unload test. Figure 1 As shown, when the displacement amount of the boron nitride particle B is set to X and the load amount is set to Y, for example, the displacement amount X and the load amount Y of the boron nitride particle B in the loading process become a relationship like the load curve L1, and the displacement amount X and the load amount Y of the boron nitride particle B in the unloading process become a relationship like the unloading curve L2.

[0054] When the average value (average displacement) of the amount (absolute value) of the displacement of the boron nitride particles B in the short side direction in the loading process is set to D3, and the average value (average displacement) of the amount (absolute value) of the displacement of the boron nitride particles B in the short side direction in the unloading process is set to D4, the larger the average recovery rate (D4 / D3), the more preferred. The average recovery rate (D4 / D3) can be, for example, 0.2 or more, 0.25 or more, 0.3 or more, 0.35 or more, or 0.4 or more. The average displacement D3 and the average displacement D4 refer to the average values ​​of the displacement D1 and the displacement D2 measured for 10 boron nitride particles B in the same manner as described in the first embodiment.

[0055] A large average recovery rate can also be said to be a large average elastic deformation work ratio of the boron nitride particles B. That is, the larger the average elastic deformation work ratio of the boron nitride particles B, the easier it is for the boron nitride particles B to recover to their original shape even if compressed. The average elastic deformation work ratio of the boron nitride particles B can be, for example, greater than 0.1, greater than 0.15, greater than 0.2, greater than 0.25, greater than 0.3, or greater than 0.35. The average elastic deformation work ratio refers to the elastic deformation work ratio (W) measured for 10 boron nitride particles B using the same method as described in the first embodiment. E / W T )’s average value.

[0056] Next, the method for producing the above-mentioned boron nitride particles is described below. The above-mentioned boron nitride particles can be produced by, for example, a method for producing boron nitride particles having the following steps: a step of disposing a mixture containing boron carbide and boric acid and a substrate formed of a carbon material in a container formed of a carbon material (disposition step); a step of generating boron nitride particles on the substrate by heating and pressurizing the container in a nitrogen atmosphere (generation step). Another embodiment of the present invention is a method for producing such boron nitride particles.

[0057] The container formed by the carbon material is a container capable of accommodating the above-mentioned mixture and the substrate. The container may be, for example, a carbon crucible. The container is preferably a container that can improve airtightness by covering the opening with a lid. In the configuration step, for example, the mixture may be configured at the bottom of the container, and the substrate may be configured in a manner that is fixed to the side wall surface in the container and the inner side of the lid. The substrate formed by the carbon material may be, for example, in the form of a sheet, a plate or a rod. The substrate formed by the carbon material may be, for example, a carbon sheet (graphite sheet), a carbon plate or a carbon rod.

[0058] The boron carbide in the mixture may be in a powdered state (boron carbide powder), for example. The boric acid in the mixture may be in a powdered state (boric acid powder), for example. The mixture may be obtained by mixing boron carbide powder, boron nitride powder and boric acid powder by a known method.

[0059] Boron carbide powder can be manufactured by a known manufacturing method. As a manufacturing method of boron carbide powder, for example, the following method can be cited: after mixing boric acid and acetylene black, heating at 1800 to 2400° C. for 1 to 10 hours in an inert gas (e.g., nitrogen gas) atmosphere to obtain blocky boron carbide particles. The blocky boron carbide particles obtained by this method are appropriately crushed, sieved, cleaned, impurity removed, dried, etc. to obtain boron carbide powder.

[0060] By adjusting the pulverization time of the massive carbon-boron particles, the average particle size of the boron carbide powder can be adjusted. The average particle size of the boron carbide powder can be 5 μm or more, 7 μm or more, or 10 μm or less, 100 μm or less, 90 μm or less, 80 μm or less, or 70 μm or less. The average particle size of the boron carbide powder can be measured by laser diffraction scattering method.

[0061] The mixing ratio of boron carbide and boric acid can be appropriately selected. From the viewpoint that the boron nitride particles are easily enlarged, relative to 100 parts by mass of boron carbide, the content of boric acid in the mixture is preferably 2 parts by mass or more, more preferably 5 parts by mass or more, further preferably 8 parts by mass or more, and can be 100 parts by mass or less, 90 parts by mass or less, or 80 parts by mass or less.

[0062] The mixture containing boron carbide and boric acid may also contain other components. As other components, silicon carbide, carbon, iron oxide, etc. can be cited. By the mixture containing boron carbide and boric acid also containing silicon carbide, it is easy to obtain boron nitride particles without open ends.

[0063] The container is provided with a nitrogen atmosphere containing, for example, 95% by volume or more of nitrogen gas. The content of nitrogen gas in the nitrogen atmosphere is preferably 95% by volume or more, more preferably 99.9% by volume or more, and can be substantially 100% by volume. In addition to nitrogen gas, the nitrogen atmosphere may also contain ammonia gas or the like.

[0064] From the viewpoint that the boron nitride particles tend to grow larger, the heating temperature is preferably 1450° C. or higher, more preferably 1600° C. or higher, and further preferably 1800° C. or higher. The heating temperature may be 2400° C. or lower, 2300° C. or lower, or 2200° C. or lower.

[0065] From the viewpoint that the boron nitride particles are likely to grow larger, the pressure during pressurization is preferably 0.3 MPa or more, and more preferably 0.6 MPa or more. The pressure during pressurization may be 1.0 MPa or less, or 0.9 MPa or less.

[0066] From the viewpoint that the boron nitride particles are likely to grow larger, the heating and pressurizing time is preferably 3 hours or longer, more preferably 5 hours or longer. The heating and pressurizing time may be 40 hours or shorter, or 30 hours or shorter.

[0067] According to the manufacturing method, the above-mentioned boron nitride particles can be generated on a substrate formed of a carbon material. Therefore, by recovering the boron nitride particles on the substrate, boron nitride particles can be obtained. In the case where the particles generated on the substrate are boron nitride particles, it can be confirmed by recovering a part of the particles generated on the substrate from the substrate, performing X-ray diffraction measurement on the recovered particles, and detecting peaks from boron nitride.

[0068] The boron nitride particles obtained by the above method may be subjected to a step of classifying so as to obtain only boron nitride particles having a maximum length within a specific range (classification step).

[0069] The boron nitride particles obtained by the above method can be mixed with a resin to be used as a resin composition. That is, another embodiment of the present invention is a resin composition containing the above-mentioned boron nitride particles and a resin.

[0070] Examples of the resin include epoxy resins, silicone resins, silicone rubbers, acrylic resins, phenolic resins, melamine resins, urea resins, unsaturated polyesters, fluororesins, polyimides, polyamide-imides, polyetherimides, polybutylene terephthalate, polyethylene terephthalate, polyphenylene ether, polyphenylene sulfide, wholly aromatic polyesters, polysulfones, liquid crystal polymers, polyethersulfones, polycarbonates, maleimide-modified resins, ABS (acrylonitrile-butadiene-styrene) resins, AAS (acrylonitrile-acrylic rubber·styrene) resins, AES (acrylonitrile·ethylene·propylene·diene rubber-styrene) resins, and the like.

[0071] When the resin composition is used as a heat dissipation material, the content of the boron nitride particles may be 15% by volume or more, 20% by volume or more, 30% by volume or more, 40% by volume or more, 50% by volume or more, or 60% by volume or more based on the total volume of the resin composition from the viewpoint of improving the thermal conductivity of the heat dissipation material and facilitating obtaining excellent heat dissipation performance. From the viewpoint of being able to suppress the generation of voids when the resin composition is molded into a sheet-like heat dissipation material and suppressing the decrease in the insulation and mechanical strength of the sheet-like heat dissipation material, the content of the boron nitride particles may be 85% by volume or less or 80% by volume or less based on the total volume of the resin composition.

[0072] The content of the resin can be appropriately adjusted according to the application of the resin composition, required characteristics, etc. Based on the total volume of the resin composition, the content of the resin can be, for example, 15% by volume or more, 20% by volume or more, 30% by volume or more, 40% by volume or more, 50% by volume or more, or 60% by volume or more, and can be 85% by volume or less, 70% by volume or less, 60% by volume or less, 50% by volume or less, or 40% by volume or less.

[0073] The resin composition may further contain a curing agent for curing the resin. The curing agent may be appropriately selected according to the type of the resin. For example, as a curing agent used together with the epoxy resin, phenolic Novolac compounds, acid anhydrides, amino compounds, imidazole compounds, etc. may be cited. Relative to 100 parts by mass of the resin, the content of the curing agent may be, for example, 0.5 parts by mass or more or 1.0 parts by mass or less, and may be 15 parts by mass or less or 10 parts by mass or less.

[0074] The resin composition may further contain other components, such as a curing accelerator (curing catalyst), a coupling agent, a wetting and dispersing agent, and a surface conditioner.

[0075] Examples of the curing accelerator (curing catalyst) include phosphorus-based curing accelerators such as tetraphenylphosphine tetraphenylborate and triphenylphosphate, imidazole-based curing accelerators such as 2-phenyl-4,5-dihydroxymethylimidazole, and amine-based curing accelerators such as boron trifluoride monoethylamine.

[0076] Examples of the coupling agent include silane coupling agents, titanate coupling agents, and aluminate coupling agents, etc. Examples of the chemical bonding groups contained in these coupling agents include vinyl groups, epoxy groups, amino groups, methacryloyl groups, and mercapto groups.

[0077] Examples of the wetting and dispersing agent include phosphate ester salts, carboxylic acid esters, polyesters, acrylic acid copolymers, and block copolymers.

[0078] Examples of the surface conditioner include acrylic surface conditioners, silicone surface conditioners, vinyl surface conditioners, and fluorine surface conditioners.

[0079] The resin composition can be manufactured, for example, by a method for manufacturing a resin composition having the following steps: a step of preparing boron nitride particles according to one embodiment or a boron nitride powder according to one embodiment (preparation step); a step of mixing the boron nitride particles or the boron nitride powder with a resin (mixing step). Another embodiment of the present invention is a method for manufacturing such a resin composition. In the mixing step, in addition to the boron nitride particles and the resin, the above-mentioned curing agent and other components may also be mixed.

[0080] The method for producing a resin composition according to one embodiment may further include a step of crushing the boron nitride particles or boron nitride powder (crushing step). The crushing step may be performed between the preparation step and the mixing step, or may be performed simultaneously with the mixing step (the boron nitride particles or boron nitride powder may also be crushed while mixing the boron nitride particles or boron nitride powder with the resin).

[0081] The resin composition can be used as a heat dissipation material, for example. The heat dissipation material can be manufactured, for example, by curing the resin composition. The method for curing the resin composition can be appropriately selected according to the type of resin (and curing agent used as needed) contained in the resin composition. For example, when the resin is an epoxy resin and the curing agent is used in combination, the resin can be cured by heating.

[0082] Example

[0083] Hereinafter, the present invention will be described in more detail by way of examples, but the present invention is not limited to the following examples.

[0084] <Manufacturing of Boron Nitride Particles (Powder)>

[0085] The blocky boron carbide particles were crushed by a pulverizer to obtain boron carbide powder with an average particle size of 10 μm. 100 parts by mass of the obtained boron carbide powder was mixed with 9 parts by mass of boric acid, and the obtained mixture was filled into a carbon crucible, and the opening of the carbon crucible was covered with a carbon sheet (manufactured by NeoGraf), and the carbon sheet was fixed by sandwiching the carbon sheet between the carbon crucible and the carbon crucible. The carbon crucible with the lid on was heated in a resistance heating furnace at 2000°C and 0.85MPa for 10 hours under a nitrogen atmosphere, thereby generating particles on the carbon sheet.

[0086] A portion of the particles generated on the carbon sheet was recovered and subjected to X-ray diffraction measurement using an X-ray diffractometer (manufactured by Rigaku Corporation, "ULTIMA-IV"). The X-ray diffraction measurement results and the X-ray diffraction measurement results of boron nitride powder (GP grade) manufactured by Denka Co., Ltd. as a comparative object are shown in Figure 2 .Depend on Figure 2 It can be seen that only the peak derived from boron nitride was detected, confirming that boron nitride particles were generated. The SEM image of the obtained boron nitride powder is shown in FIG. Figure 3 .

[0087] <Evaluation of Boron Nitride Particles>

[0088] Ten boron nitride particles A in the obtained boron nitride powder were crushed by gradually applying a load at a load rate of 0.27 mN / sec in the short side direction using a micro compression tester (manufactured by Shimadzu Corporation, MCT series). The average value F of the load required to crush each boron nitride particle A was 40 mN.

[0089] Then, the maximum length (L) of each of the other 10 boron nitride particles B relative to the boron nitride particles A in the obtained boron nitride powder was measured by observation using a microscope attached to a micro compression tester (MCT series, manufactured by Shimadzu Corporation).a ), and perpendicular to the maximum length (L a ) direction, the maximum length (L b ). In addition, the maximum length L a and L b Calculate the aspect ratio (L a / L b The results are shown in Table 1.

[0090] In addition, using a micro compression tester (manufactured by Shimadzu Corporation, MCT series), a load was gradually applied to each of the 10 boron nitride particles B in the short side direction at a load speed of 0.27 mN / sec from 0.2 mN to 20 mN (50% of the average value F (40 mN) of the load required to crush the above-mentioned boron nitride particles A) to compress the boron nitride particles (loading process), and then the load was unloaded at an unloading speed of 0.27 mN / sec until it reached 0.2 mN (unloading process). For one of the boron nitride particles B provided for the load unloading test (particle No. 1), Figure 4 The relationship between the load amount and the displacement amount of the boron nitride particles in the load unloading test is shown.

[0091] For each of the ten boron nitride particles B, the displacement amount D1 in the short side direction of the boron nitride particle in the loading process was calculated, and the displacement amount D2 in the short side direction of the boron nitride particle in the unloading process was calculated from the length of the short side of the boron nitride particle. 2、 And the recovery rate D2 / D1. In addition, for each of the 10 boron nitride particles B, Figure 1 The area of ​​a region P surrounded by the load curve L1, the unloading curve L2, and the straight line L3 indicating Y = 0.2 mN is defined as the plastic deformation work W. P The area of ​​the region E surrounded by the unloading curve L2, the straight line L3, and the straight line L4 connecting the intersection of the load curve L1 and the unloading curve L2 and the straight line L3 and parallel to the Y axis is defined as the elastic deformation work W. E , W P With W E The sum of (W P +W E ) is set as the total work W T When the elastic deformation work ratio W is calculated E / W T The results are shown in Table 1.

[0092] [Table 1]

[0093]

Claims

1. Boron nitride particles having an elongated shape, the boron nitride particles having an outer shell portion formed of boron nitride and a hollow portion surrounded by the outer shell portion, When subjected to a load-unloading test including a loading step and an unloading step in sequence, at least a portion of the length in the short-side direction of the boron nitride particles compressed in the loading step is restored in the unloading step. in, The loading step is a step of gradually applying a load from 0.2 mN to 20 mN at a loading rate of 0.27 mN / sec in the short-side direction of the boron nitride particles to perform compression, and the unloading step is a step of gradually unloading the load to 0.2 mN at an unloading rate of 0.27 mN / sec.

2. The boron nitride particles according to claim 1, wherein When the amount of displacement of the boron nitride particles in the short-side direction in the loading step is D1 and the amount of displacement of the boron nitride particles in the short-side direction in the unloading step is D2, D2 / D1 is 0.2 or more.

3. Boron nitride powder, the boron nitride powder being an aggregate of elongated boron nitride particles, the elongated boron nitride particles having an outer shell portion formed of boron nitride and a hollow portion surrounded by the outer shell portion, When subjected to a load-unloading test including the following steps (1) to (3) in sequence, at least a portion of the length in the short side direction of the boron nitride particles B compressed in the loading step is restored in the unloading step: (1) a calculation step of applying a load at a load rate of 0.27 mN / sec in the short-side direction of each of 10 boron nitride particles A selected from the boron nitride powder, measuring the magnitude of the load required to crush the boron nitride particles A, and calculating an average value F of the magnitude of the load; (2) a loading step of compressing the boron nitride particles B selected from the boron nitride powder separately from the boron nitride particles A by gradually applying a load in the short-side direction thereof at a loading rate of 0.27 mN / sec from 0.2 mN to 50% of an average value F of the load; (3) Unloading step: gradually unloading the boron nitride particles B at an unloading rate of 0.27 mN / sec until the load reaches 0.2 mN.

4. The boron nitride powder according to claim 3, wherein When the average value of the displacement of the boron nitride particles B in the short side direction in the loading step is D3 and the average value of the displacement of the boron nitride particles B in the short side direction in the unloading step is D4, D4 / D3 is 0.2 or more. 5 . A resin composition comprising: a resin, and the boron nitride particles according to claim 1 or 2 or the boron nitride powder according to claim 3 or 4.

6. A method for producing a resin composition, comprising the following steps: A step of preparing the boron nitride particles according to claim 1 or 2 or the boron nitride powder according to claim 3 or 4; A step of mixing the boron nitride particles or the boron nitride powder with a resin. 7 . The method for producing a resin composition according to claim 6 , further comprising a step of pulverizing the boron nitride particles or the boron nitride powder.

Citation Information

Patent Citations

  • Hexagonal boron nitride powder and method for producing the same

    JP2016160134A

  • Sintered spherical BN particles with concave part, method for producing same, and polymer material

    CN104470873A

  • Aggregated boron nitride particles, composition containing said particles, and three-dimensional integrated circuit having layer comprising said composition

    CN105947997A

  • Cubic boron nitride polycrystal, cutting tool, wear resistant tool, grinding tool, and method for producing cubic boron nitride polycrystal

    CN107207364A

  • Flexible boron nitride nano-belt aerogel and preparation method therefor

    CN109704296A