A polymer containing dynamic covalent bonds and its preparation and foam material

By introducing dynamic covalent bonds into the polyaryletherketone (sulfone) molecular chain and forming a dynamic covalent crosslinking network, the problem of insufficient mechanical properties of thermoplastic foams is solved, significantly improving the mechanical properties and density of the foams, and achieving higher levels room temperature compression strength.

CN115612091BActive Publication Date: 2024-11-26DALIAN INSTITUTE OF CHEMICAL PHYSICS CHINESE ACADEMY OF SCIENCES
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110783850.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-07-12
Publication Date
2024-11-26
Estimated Expiration
2041-07-12

AI Technical Summary

Technical Problem

The existing thermoset high-temperature resistant structure foam is difficult to recover, and the mechanical properties and creep resistance of thermoplastic polyaryletherketone (sulfone) foam are different from those of thermoset foam, making it difficult to obtain high-magnification foams.

Method used

Dynamic covalent bonds are introduced into the polyaryletherketone (sulfone) molecular chain, a dynamic covalent crosslinking network is formed by heat treatment methods of high temperature molding or extrusion, and foam materials are prepared by carbon dioxide foaming technology.

Benefits of technology

The mechanical properties of polyaryletherketone (sulfone) foam are significantly improved while maintaining its plasticity, achieving higher room temperature compression strength and density.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115612091B_ABST
    Figure CN115612091B_ABST
Patent Text Reader

Abstract

The present invention provides a polyaryletherketone (sulfone) containing dynamic covalent bonds, and a polymer foam material prepared by using the polymer as a matrix resin through a carbon dioxide foaming technology. The present invention introduces a dynamic cross-linking structure into the polyaryletherketone (sulfone) molecular chain to improve the mechanical properties of the polyaryletherketone (sulfone) foam material, while maintaining the plasticity of the polyaryletherketone (sulfone).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of polymer synthesis and molding, and specifically relates to a polyaryletherketone (sulfone) with a new structure and a foam material thereof. Technical Background

[0002] High temperature resistant structural foams are increasingly widely used in aerospace, rail transit, new energy vehicles and other fields. They play an important role in reducing weight, saving energy and improving endurance. Currently, commercial high temperature resistant structural foams are mainly thermosetting polymethacrylimide (PMI) foams and phenolic foams. However, these thermosetting foams are difficult to recycle. Therefore, the development of thermoplastic and easily recyclable high temperature resistant structural foams has become an important research direction. Polyaryletherketone (sulfone) is a high-performance foam prepared by supercritical carbon dioxide foaming technology using high-performance polyaryletherketone (sulfone) resin as raw material. It has the advantages of high temperature resistance, self-flame retardant, recyclability and radiation resistance. The foaming process is green and environmentally friendly, and has broad application prospects. However, the mechanical properties and creep resistance of this type of thermoplastic high temperature resistant structural foam are still somewhat different from those of thermosetting foams, which limits the application and promotion of this type of material. Although the mechanical properties of the foam can be enhanced by blending with inorganic fillers, the addition of a large amount of inorganic fillers affects the foaming properties of the resin, making it difficult to obtain high-ratio foams.

[0003] Dynamic covalent bond polymer materials refer to a type of polymer containing dynamic covalent bonds. This type of material has the properties of thermosetting resins at room temperature. Under external stimuli (heat, light, force, pH, etc.), the dynamic covalent bonds are reorganized, inducing dynamic adjustments in the polymer network, and have the reprocessability of thermoplastic materials. They are considered to be the third type of polymer materials after thermoplastic materials and thermosetting materials. Common dynamic covalent bonds include ester bonds, disulfide bonds, imine bonds, borate bonds, etc. Introducing dynamic covalent bonds into the polymer chain structure to construct a dynamic cross-linking network and then preparing foam materials can improve its mechanical properties and creep resistance while maintaining the plasticity of the material. Summary of the invention

[0004] The present invention provides a polymer containing dynamic covalent bonds.

[0005] The polymer containing dynamic covalent bonds has a structural formula as shown in Formula I.

[0006]

[0007] Preferably, X is selected from one of structures A and B:

[0008]

[0009] Preferably, R is selected from one of the structures ae:

[0010] (a)-H(b)-CN(c)-CH3(d)-SO3(e)-NO2

[0011] Preferably, Ar is selected from one of 1-7:

[0012]

[0013] Wherein m and n are the repeating unit ratios, wherein 0.1<m<1, 0<n<0.9, preferably 0.2<m<0.9, 0.1<n<0.8, more preferably 0.2<m<0.8, 0.2<n<0.8.

[0014] The polymer is a random copolymer structure, the polymer is 50000<M (w) <200000, 1.4 <PDI <2.5, preferably 80000 <M (w) <150000,1.6<PDI<2.2,where M (w) is the weight average molecular weight and PDI is the dispersion index.

[0015] The preparation method of the polymer containing dynamic covalent bonds is as follows: dihalogen monomer, diphenol monomer, imine monomer, carbonate, and water-carrying agent are mixed in an aprotic solvent, heated to reflux for 2-4 hours, the water-carrying agent is removed, and the reaction is continued for 2-5 hours to obtain a polymer of formula I.

[0016] Preferably, the aprotic solvent is one of dimethyl sulfoxide, N,N-dimethylacetamide, N,N-dimethylformamide and sulfolane.

[0017] Preferably, the dihalogen monomer is one or both of 4,4-difluorobenzophenone, 4,4-difluorodiphenyl sulfone and 2,5-dichlorobenzonitrile.

[0018] Preferably, the diphenol monomer is one of 1'-7':

[0019]

[0020] Preferably, the imine monomer is one of α'-ε':

[0021]

[0022] Wherein R=one or more of H, CN, NO2, CH3 or SO3.

[0023] Preferably, the carbonate is one or two of potassium carbonate, sodium carbonate and calcium carbonate.

[0024] Preferably, the water-carrying agent is toluene or xylene.

[0025] Preferably, the sum of the amounts of the dihalogen monomer and the imine monomer is equal to the amount of the diphenol monomer.

[0026] Preferably, the ratio of the amount of dihalogen monomer to the amount of imine monomer is 9:1-1:9, preferably 8:2-2:8, and more preferably 7:3-3:7.

[0027] Preferably, the amount of the carbonate is 1 to 1.5 times the amount of the diphenol monomer.

[0028] Preferably, the mass of the aprotic solvent is 2-4 times the total mass of the dihalogen monomer, the diphenol monomer and the imine monomer.

[0029] Preferably, the mass of the water-carrying agent is 15%-40% of the mass of the aprotic solvent.

[0030] The present invention also provides a polymer foam having a structure of formula I.

[0031] The preparation method of the polymer foam is as follows: a polymer having a structure of formula I is molded into a plate in a high-temperature vulcanizer to obtain a pre-foamed body, the pre-foamed body is placed in a foaming kettle and carbon dioxide is introduced, the temperature and pressure are maintained for a certain period of time, and finally the pressure is quickly released to obtain a target foam product.

[0032] Preferably, the molding temperature is 300-380° C. and the pressure is 5-20 MPa. Preferably, the holding temperature is 200-300° C., the holding pressure is 8-20 MPa, and the holding time is 30-180 min.

[0033] Beneficial effects of the present invention: The present invention provides a polymer containing dynamic covalent bonds, and the naphthalene side groups are cross-linked by a heat treatment method of high-temperature molding or extrusion to obtain a dynamic covalent cross-linked network. The foam material is prepared by carbon dioxide foaming technology. Compared with thermoplastic foams with linear structures, the mechanical properties are significantly improved.

[0034] The invention introduces a dynamic cross-linking structure into the polyaryletherketone (sulfone) molecular chain to improve the mechanical properties of the polyaryletherketone (sulfone) foam material while maintaining the plasticity of the polyaryletherketone (sulfone). BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 The polymer obtained in Example 1 1 H-NMR spectrum

[0036] Figure 2 The scanning electron microscope image of the foam obtained in Example 1 is DETAILED DESCRIPTION

[0037] Comparative Example

[0038]

[0039] Phenolphthalein (1 mol), 4,4-difluorobenzophenone (1 mol), potassium carbonate (1.15 mol), sulfolane (1200 g), and toluene (300 ml) were added to a reaction kettle and mixed, heated to 140° C. and refluxed for 2 h, toluene was removed, and the temperature was continued to be raised to 200° C. and reacted for 1.5 h to obtain a polymer having a structure of formula II. 1 H-NMR and GPC determined the molecular structure and degree of polymerization (220) of the polymer. The polymer having the structure of Formula II was then molded into a plate in a high-temperature vulcanizer at a molding temperature of 340°C and a pressure of 10 MPa to obtain a pre-foamed body with a thickness of 4 mm. The pre-foamed body was placed in a foaming kettle and carbon dioxide was introduced. The temperature and pressure were maintained at 260°C and 10 MPa for 150 minutes, and the pressure was quickly released to obtain a density of 90 kg / m 3 Foam product, room temperature compressive strength 1.2MPa.

[0040] Example 1

[0041]

[0042] Phenolphthalein (1 mol, corresponding to the diphenol monomer is 1'), imine monomer α' (0.2 mol, R is H), 4,4-difluorobenzophenone (0.8 mol), potassium carbonate (1.15 mol), sulfolane (1200 g), and toluene (300 ml) were added into a reaction kettle and mixed, heated to 140° C. and refluxed for 2 h, toluene was removed, and the temperature was continued to be raised to 200° C. and reacted for 2.5 h to obtain a polymer having a structure of formula III. 1 H-NMR and GPC were used to determine the molecular structure and molecular weight (M (w) =84000, PDI=1.8). The polymer having the structure of formula III was molded into a plate in a high temperature vulcanizer at a molding temperature of 320°C, a pressure of 10 MPa, and a molding time of 60 min to obtain a pre-foamed body with a thickness of 4 mm. The pre-foamed body was placed in a foaming kettle and carbon dioxide was introduced. The temperature and pressure were maintained at 270°C and 12 MPa for 150 min, and finally the pressure was quickly released to obtain a density of 93 kg / m 3 Foam product, room temperature compressive strength 1.5MPa.

[0043] Example 2

[0044]

[0045] Phenolphthalein (1 mol, corresponding to diphenol monomer 1'), imine monomer α' (0.2 mol, R is CN), 4,4-difluorodiphenyl sulfone (0.8 mol), potassium carbonate (1.15 mol), cyclopentane (1200 g), toluene (300 ml) were added into a reaction kettle and mixed, heated to 140° C. and refluxed for 2 h, toluene was removed, and the temperature was continued to be raised to 200° C. and reacted for 2.5 h to obtain a polymer having a structure of formula IV. 1 H-NMR and GPC were used to determine the molecular structure and molecular weight (M (w) =94000, PDI=1.8). The polymer having the structure of Formula IV was molded into a plate in a high temperature vulcanizer at a molding temperature of 330°C, a pressure of 15 MPa, and a molding time of 60 min to obtain a pre-foamed body with a thickness of 4 mm. The pre-foamed body was placed in a foaming kettle and carbon dioxide was introduced. The temperature and pressure were maintained at 275°C and 12 MPa for 150 min, and the pressure was quickly released to obtain a density of 89 kg / m 3 Foam product, room temperature compressive strength 1.45MPa.

[0046] Example 3

[0047]

[0048] Bisphenol fluorene (1 mol, corresponding to the diphenol monomer is 2'), imine monomer α' (0.2 mol, R is CN), 4,4-difluorodiphenyl sulfone (0.8 mol), potassium carbonate (1.15 mol), cyclopentane sulfone (1200 g), toluene (300 ml) were added into a reaction kettle for mixing, the temperature was raised to 150° C. and refluxed for 2 h, toluene was removed, the temperature was continued to be raised to 220° C. and reacted for 2.5 h to obtain a polymer having a structure of formula V, and the reaction mixture was carried out by 1 H-NMR and GPC were used to determine the molecular structure and molecular weight (M (w) =92000, PDI=1.9). The polymer having the structure of formula V was molded into a plate in a high temperature vulcanizer at a molding temperature of 350°C, a pressure of 17 MPa, and a molding time of 60 min to obtain a pre-foamed body with a thickness of 4 mm. The pre-foamed body was placed in a foaming kettle and carbon dioxide was introduced. The temperature and pressure were maintained at 280°C and 12 MPa for 150 min, and the pressure was quickly released to obtain a density of 97 kg / m 3 Foam product, room temperature compressive strength 1.7MPa.

[0049] Example 4

[0050]

[0051] Bisphenol fluorene (1 mol, corresponding to the diphenol monomer is 2'), imine monomer ε' (0.3 mol, R is CN), 4,4-difluorodiphenyl sulfone (0.7 mol), potassium carbonate (1.15 mol), cyclopentane sulfone (1200 g), toluene (300 ml) were added into a reaction kettle and mixed, heated to 150° C. and refluxed for 2 h, toluene was removed, and the temperature was continued to be raised to 210° C. and reacted for 2.5 h to obtain a polymer having a structure of formula VI. 1 H-NMR and GPC were used to determine the molecular structure and molecular weight (M (w) =120000, PDI=2.0). The polymer having the structure of Formula VI was molded into a plate in a high temperature vulcanizer at a molding temperature of 350°C, a pressure of 12 MPa, and a molding time of 60 min to obtain a pre-foamed body with a thickness of 4 mm. The pre-foamed body was placed in a foaming kettle and carbon dioxide was introduced. The temperature and pressure were maintained at 285°C and 12 MPa for 150 min, and the pressure was quickly released to obtain a density of 84 kg / m 3 Foam product, room temperature compressive strength 1.3MPa.

[0052] Example 5

[0053]

[0054] 3,3-bis(4-hydroxyphenyl)-3H-isoindolinone (1 mol, corresponding to the diphenol monomer is 3'), imine monomer α' (0.2 mol, R is H), 4,4-difluorodiphenyl sulfone (0.8 mol), potassium carbonate (1.25 mol), cyclopentane sulfone (1200 g), toluene (300 ml) were added into a reaction kettle and mixed, heated to 150° C. and refluxed for 2 h, toluene was removed, and the temperature was continued to be raised to 210° C. and reacted for 2.5 h to obtain a polymer having a structure of formula VII, and the reaction mixture was carried out by 1 H-NMR and GPC were used to determine the molecular structure and molecular weight (M (w) =140000, PDI=1.8). The polymer having the structure of Formula VII was molded into a plate in a high temperature vulcanizer at a molding temperature of 350°C, a pressure of 10 MPa, and a molding time of 60 min to obtain a pre-foamed body with a thickness of 4 mm. The pre-foamed body was placed in a foaming kettle and carbon dioxide was introduced. The temperature and pressure were maintained at 285°C and 12 MPa for 150 min, and the pressure was quickly released to obtain a density of 92 kg / m 3 Foam product, room temperature compressive strength 1.7MPa.

[0055] Example 6

[0056]

[0057] Hydroquinone (1 mol, corresponding to the diphenol monomer is 4'), imine monomer α' (0.2 mol, R is H), 4,4-difluorodiphenyl sulfone (0.8 mol), potassium carbonate (1.25 mol), cyclopentane (1200 g), toluene (300 ml) were added into a reaction kettle and mixed, heated to 150° C. and refluxed for 2 h, toluene was removed, and the temperature was continued to be raised to 210° C. and reacted for 2.5 h to obtain a polymer having a structure of formula VIII, and the reaction mixture was carried out by 1 H-NMR and GPC were used to determine the molecular structure and molecular weight (M (w) =89000, PDI=1.6). The polymer having the structure of formula VIII was molded into a plate in a high temperature vulcanizer at a molding temperature of 350°C, a pressure of 10 MPa, and a molding time of 60 min to obtain a pre-foamed body with a thickness of 4 mm. The pre-foamed body was placed in a foaming kettle and carbon dioxide was introduced. The temperature and pressure were maintained at 275°C and 12 MPa for 150 min, and the pressure was quickly released to obtain a density of 79 kg / m 3 Foam product, room temperature compressive strength 1.5MPa.

[0058] Example 7

[0059]

[0060] Bisphenol A (1 mol, corresponding to the diphenol monomer is 6'), imine monomer α' (0.2 mol, R is NO2), 4,4-difluorodiphenyl sulfone (0.8 mol), potassium carbonate (1.15 mol), cyclopentane (1000 g), toluene (250 ml) were added into a reaction kettle for blending, heated to 150° C. and refluxed for 2 h, toluene was removed, and the temperature was continued to be raised to 210° C. for reaction for 2.5 h to obtain a polymer having a structure of formula VII, and the reaction mixture was carried out by 1 H-NMR and GPC were used to determine the molecular structure and molecular weight (M (w) =84000, PDI=2.2). The polymer having the structure of Formula IX was molded into a plate in a high temperature vulcanizer at a molding temperature of 340°C, a pressure of 10 MPa, and a molding time of 60 min to obtain a pre-foamed body with a thickness of 4 mm. The pre-foamed body was placed in a foaming kettle and carbon dioxide was introduced. The temperature and pressure were maintained at 265°C and 15 MPa for 150 min, and the pressure was quickly released to obtain a density of 95 kg / m 3 Foam product, room temperature compressive strength 1.71MPa.

[0061] Example 8

[0062]

[0063] Hexafluorobisphenol A (1 mol, corresponding to the diphenol monomer is 7'), imine monomer α' (0.4 mol, R is SO3), 4,4-difluorobenzophenone (0.6 mol), potassium carbonate (1.15 mol), sulfolane (1000 g), and toluene (250 ml) were added into a reaction kettle and mixed, heated to 150° C. and refluxed for 2 h, toluene was removed, and the temperature was continued to be raised to 190° C. and reacted for 2.5 h to obtain a polymer having a structure of formula X. 1 H-NMR and GPC were used to determine the molecular structure and molecular weight (M (w) =69000, PDI=1.8). The polymer having the structure of formula X was molded into a sheet in a high temperature vulcanizer at a molding temperature of 340°C, a pressure of 10 MPa, and a molding time of 60 min to obtain a pre-foamed body with a thickness of 4 mm. The pre-foamed body was placed in a foaming kettle and carbon dioxide was introduced. The temperature and pressure were maintained at 255°C and 15 MPa for 150 min, and the pressure was quickly released to obtain a density of 115 kg / m 3 Foam product, room temperature compressive strength 1.79MPa.

[0064] Example 9

[0065]

[0066] Hexafluorobisphenol A (1 mol, corresponding to the diphenol monomer is 7'), imine monomer γ' (0.4 mol, R is CN), 4,4-difluorobenzophenone (0.6 mol), potassium carbonate (1.15 mol), sulfolane (1000 g), and toluene (250 ml) were added into a reaction kettle for mixing, heated to 150° C. and refluxed for 2 h, toluene was removed, and the temperature was continued to be raised to 190° C. for reaction for 2.5 h to obtain a polymer having a structure of formula XI. 1 H-NMR and GPC were used to determine the molecular structure and molecular weight (M (w) =114000, PDI=2.3). The polymer having the structure of formula XI was molded into a plate in a high temperature vulcanizer at a molding temperature of 340°C, a pressure of 8MPa, and a molding time of 60min to obtain a pre-foamed body with a thickness of 4mm. The pre-foamed body was placed in a foaming kettle and carbon dioxide was introduced. The temperature and pressure were maintained at 255°C and 15MPa for 150min, and the pressure was quickly released to obtain a density of 105kg / m 3 Foam product, room temperature compressive strength 1.68MPa.

Claims

1. A polymer containing dynamic covalent bonds, Features: Its structural formula is shown in Formula I, Formula I Wherein X is selected from one or two of structures A and B: R is selected from one or more of the structures ae: (a)-H (b)-CN (c)-CH 3 (d)-SO 3 (e)-NO 2 Ar is selected from one or more of 1-8: The polymer is a random copolymer structure, where m and n are the molar ratios of the corresponding repeating units in the polymer, m+n=1, 0.1 <m<1, 0<n<0.9; Polymer 50000< <200000,1.4<PDI<2.5 is the weight average molecular weight and PDI is the polymer dispersibility index.

2. The polymer according to claim 1, Features: The polymer is a random copolymer structure, where m and n are the molar ratios of the corresponding repeating units in the polymer, m+n=1, 0.2 <m<0.9, 0.1<n<0.8; Polymer 80000< <150000,1.6<PDI<2.2,where is the weight average molecular weight and PDI is the polymer dispersibility index.

3. A method for preparing a polymer containing dynamic covalent bonds according to claim 1, Features: The dihalogen monomer, diphenol monomer, imine monomer, carbonate and water-carrying agent are mixed in an aprotic solvent, heated to reflux for 2-4 hours, the water-carrying agent is removed, and the reaction is continued for 2-5 hours to obtain a polymer of formula I.

4. The preparation method according to claim 3, Features: The aprotic solvent is one or more of dimethyl sulfoxide, N,N-dimethylacetamide, N,N-dimethylformamide and sulfolane; the water-carrying agent is one or more of toluene and xylene.

5. The preparation method according to claim 3, Features: The dihalogen monomer is one or more of 4,4-difluorobenzophenone, 4,4-difluorodiphenyl sulfone or 2,5-dichlorobenzonitrile; The diphenol monomer is one or more than two of 1'-7': The imine monomer is one or more of α'-ε': Where R=H, CN, NO 2 , CH 3 or SO 3 One or more of the following.

6. The preparation method according to claim 3, Features: The carbonate is one or more of potassium carbonate, sodium carbonate and calcium carbonate.

7. The preparation method according to any one of claims 3 to 6, Features: The sum of the amounts of the dihalogen monomer and the imine monomer is equal to the amount of the diphenol monomer, wherein the ratio of the amounts of the dihalogen monomer to the imine monomer is 9:1-1:9; The amount of carbonate is 1 to 1.5 times the amount of diphenol monomer The mass of the aprotic solvent is 2-4 times the total mass of the dihalogen monomer, the diphenol monomer and the imine monomer; The mass of the aqueous agent is 25%-50% of the mass of the aprotic solvent.

8. The preparation method according to claim 7, Features: The sum of the amounts of the dihalogen monomer and the imine monomer is equal to the amount of the diphenol monomer, wherein the ratio of the amounts of the dihalogen monomer to the imine monomer is 8:2-2:

8.

9. A foam material obtained by using the polymer according to claim 1 or the polymer foamed by the preparation method according to any one of claims 2 to 6.

10. The foam material according to claim 9, wherein the preparation method is as follows: the polymer is molded into a plate in a high-temperature vulcanizer at a molding temperature of 300-380° C. and a pressure of 5-20 MPa, or is extruded into a plate or pellets through an extruder to obtain a pre-foamed body, the pre-foamed body is placed in a foaming kettle and carbon dioxide is introduced, and the pre-foamed body is kept warm at 200-300° C. and 8-20 MPa for 30-180 min, and finally the pressure is released to obtain the target foam product.