A preparation method of non-stick roller composite coating and non-stick roller composite coating
By spraying the AT40-PFA composite coating on the surface of the metal substrate and performing heat treatment, the problem of insufficient wear resistance and surface roughness of the polytetrafluoroethylene non-stick coating was solved, and an insatiable combination of high wear resistance and low friction coefficient was achieved. Tack coating for applications such as thin film equipment.
Patent Information
- Application Number
- CN202211158128.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-22
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-09-22
AI Technical Summary
Existing non-stick coatings such as polytetrafluoroethylene have deficiencies in wear resistance and surface roughness, resulting in high wear and short service life in applications and difficulty in meeting industrial requirements.
The AT40-PFA composite coating is sprayed on the surface of the metal substrate using the atmospheric plasma spraying method, and the substrate is pre-treated and heat-treated before spraying, combined with compressed air cooling to reduce the evaporation of PFA and improve the wear resistance and wear resistance of the coating. Combining abilities.
It significantly improves the wear resistance and wettability of the non-stick coating, reduces surface roughness, and enhances the stability and service life of the coating. It is suitable for high-demand applications such as film equipment.
Smart Images

Figure CN115612968B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of coating preparation, and in particular to a preparation method of a non-stick roller composite coating and the non-stick roller composite coating. Background Art
[0002] Wettability is an important physical and chemical index of solid surface, which refers to the ability of liquid to spread on the solid surface. The size of the static contact angle is usually used to characterize the wetting properties of the material surface. When the static contact angle of the material surface is greater than 90°, it has a certain degree of non-stickiness, and when it is greater than 150°, it has super non-stickiness. Non-stick coating refers to the low surface energy material, which is compounded on the surface of the substrate in the form of a coating or film, thereby giving it the function of non-stickiness and easy cleaning. Non-stick or super non-stick coatings have broad application prospects in daily life, industrial production, national defense and aviation, etc., and can be used to prepare plastic film equipment, marine anti-fouling equipment, household appliances, etc.
[0003] The preparation technology of non-stick coatings has made significant progress in the past few decades. Traditional polytetrafluoroethylene (PTFE) super non-stick coatings are widely used in mechanical electronics, non-stick cookware, and marine antifouling fields due to their outstanding non-stick properties, excellent chemical stability, and good self-lubrication. However, they have disadvantages such as low hardness, large wear, and insufficient wear resistance. The mechanical strength of polytetrafluoroethylene is poor, only 14-32MPa. Due to its insufficient rigidity, when the load (P) and sliding speed (V) exceed certain conditions, its wear will become very large. Therefore, in application, there are certain restrictions on the PV value. For example, when used as a bearing, the PV value must not be greater than 10kg / (cm·s), otherwise the bearing must be replaced frequently, affecting normal use; in addition, the surface energy of polytetrafluoroethylene is extremely low, making it difficult to bond with the surface of other objects, which limits its industrial application to a certain extent. The polytetrafluoroethylene coating also cannot meet the technical requirements in the film equipment because of its uncontrollable surface roughness. The surface of the produced film is not smooth and the thickness is uneven.
[0004] It can be seen that the existing technology still needs to be improved and enhanced. Summary of the invention
[0005] In view of the above-mentioned deficiencies in the prior art, the object of the present invention is to provide a method for preparing a non-stick roller composite coating and a non-stick roller composite coating, aiming to improve the wear resistance of the non-stick roller coating and reduce the roughness of the coating.
[0006] In order to achieve the above object, the present invention adopts the following technical solutions:
[0007] A method for preparing a non-stick roller composite coating comprises the following steps:
[0008] Step S001. Substrate surface pretreatment: grinding, polishing, cleaning and sandblasting the surface of the metal substrate in sequence;
[0009] Step S002. Spraying a transition layer: spraying an AT40 coating on the surface of a metal substrate using an atmospheric plasma spraying method;
[0010] Step S003. Spraying the non-stick layer: spraying the AT40-PFA composite coating on the AT40 coating using an atmospheric plasma spraying method, and continuously cooling the coating using compressed air during the spraying process;
[0011] Step S004. Heat treatment: After the coating is sprayed, heat treatment is performed at 370° C. for 10 min in an atmospheric environment, and a non-stick roller composite coating is obtained after cooling.
[0012] The method for preparing the non-stick roller composite coating, wherein in the step S003, in the AT40-PFA composite coating, the weight ratio of AT40 to PFA is 1:3.
[0013] The method for preparing the non-stick roller composite coating, wherein in the step S002, the metal substrate is also preheated before spraying.
[0014] The method for preparing the non-stick roller composite coating, wherein in the step S002, the AT40 powder and the AT40-PFA mixed powder are dried before spraying.
[0015] The method for preparing the non-stick roller composite coating, wherein in the step S002, the thickness of the transition layer is 100-120 μm.
[0016] The method for preparing the non-stick roller composite coating, wherein in the step S003, the thickness of the non-stick layer is 50-80 μm.
[0017] In the method for preparing the non-stick roller composite coating, in the step S001, the cleaning comprises: first using kerosene as a cleaning medium, using ultrasonic waves to clean the polished metal substrate surface, and then cleaning it with clean water and alcohol respectively.
[0018] The method for preparing the non-stick roller composite coating, wherein in step S002 and step S003, the spraying parameters of the atmospheric plasma spraying are: current 590-620A, spray distance 110mm, argon gas flow rate 40-60L·min -1 , hydrogen flow rate 5L·min -1 , powder feeding rate 15g·min -1 .
[0019] The method for preparing the non-stick roller composite coating, wherein, in the step S001, the pressure range of the sandblasting roughening treatment is 0.3-0.4Mpa, the sandblasting angle is 80°-90°, and the surface roughness of the substrate after sandblasting is 3.0-5.0μm.
[0020] A non-stick roller composite coating is prepared by the preparation method of the non-stick roller composite coating.
[0021] Beneficial effects:
[0022] The present invention provides a method for preparing a non-stick roller composite coating, wherein the bonding ability of the non-stick layer material is improved by pre-treating the surface of a metal substrate and spraying a transition layer. PFA (fusible polytetrafluoroethylene) is used in the spraying of the non-stick layer to improve the wettability and compatibility of the non-stick layer, and AT40 (Al2O3-40wt.% TiO2) is added to improve the wear resistance of the non-stick layer. When the non-stick layer is sprayed by atmospheric plasma, the coating is continuously cooled by compressed air to reduce the evaporation amount of PFA, reduce the loss of PFA, and ensure the non-stickiness of the non-stick layer. After the coating is sprayed, heat treatment is used to further improve the performance of the coating and reduce its surface roughness.
[0023] The present invention also provides a non-stick roller composite coating, which is made by the above-mentioned preparation method of the non-stick roller composite coating. It has a small friction coefficient. As the friction proceeds, the friction coefficient fluctuates slightly and has good stability. It also has a large contact angle of more than 130° and can be used to make thin film equipment. It also has excellent wear resistance, less wear, and longer service life. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is a physical picture of the non-stick roller composite coating prepared by the present invention.
[0025] Figure 2 This is a coating structure diagram of the non-stick roller composite coating of the present invention before heat treatment.
[0026] Figure 3 This is a coating structure diagram of the non-stick roller composite coating after heat treatment of the present invention.
[0027] Figure 4 This is the friction coefficient variation curve during the test of the embodiment of the present invention.
[0028] Figure 5 The contact angle measurement results of Example 1 of the present invention are shown in FIG.
[0029] Figure 6 The contact angle measurement results of Example 2 of the present invention are shown. DETAILED DESCRIPTION
[0030] The present invention provides a method for preparing a non-stick roller composite coating and a non-stick roller composite coating. In order to make the purpose, technical solution and effect of the present invention clearer and more specific, the present invention is further described in detail with reference to the accompanying drawings and examples. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0031] A method for preparing a non-stick roller composite coating comprises the following steps:
[0032] Step S001. Substrate surface pretreatment: grinding, polishing, cleaning and sandblasting the surface of the metal substrate in sequence;
[0033] Specifically, the surface of the substrate can be polished with a rotary grinder to remove the machining allowance and the oxide layer to obtain a relatively smooth and clean surface. The sandblasting roughening treatment after cleaning can increase the surface roughness of the substrate so that the transition layer can be more firmly bonded.
[0034] Step S002. Spraying a transition layer: spraying an AT40 coating on the surface of a metal substrate using an atmospheric plasma spraying method;
[0035] The purpose of selecting AT40 as the transition layer is to prepare a dense ceramic coating on the surface of the metal substrate, improve the corrosion resistance of the substrate, and combine with the non-stick layer so that it can be fixed on the metal substrate. The PFA in the non-stick layer has low surface energy, large wettability with the metal substrate, thermal mismatch, and is difficult to combine with the surface of the metal substrate. By setting the transition layer, PFA can be better fixed.
[0036] Step S003. Spraying the non-stick layer: spraying the AT40-PFA composite coating on the AT40 coating using an atmospheric plasma spraying method, and continuously cooling the coating using compressed air during the spraying process;
[0037] Compared with traditional PTFE, PFA has better wettability and compatibility. By combining with AT40, it can improve the wear resistance of the non-stick layer and make up for the problem of insufficient wear resistance of the non-stick material. In addition, the melting point of AT40 is relatively low, which can better match with PFA, and the compatibility of the two is better during spraying. The temperature of atmospheric plasma spraying is very high, which can melt AT40 and PFA, but PFA has a low boiling point and will evaporate if the temperature is too high. The present invention uses compressed air to continuously cool the coating during the spraying process to reduce the spraying temperature and reduce the evaporation of PFA.
[0038] Step S004. Heat treatment: After the coating is sprayed, heat treatment is performed at 370° C. for 10 min in an atmospheric environment, and a non-stick roller composite coating is obtained after cooling.
[0039] PFA will soften and remelt during the heat treatment process, thus tightly wrapping the AT40 in the coating. Through heat treatment, the interface bonding performance between AT40 and PFA can be further improved and the roughness of the coating surface can be reduced. Figure 2 and Figure 3 , Figure 2 The coating structure before heat treatment observed under an electron microscope. Figure 3 The coating structure after heat treatment observed under an electron microscope. From the two pictures, it can be seen that the composite coating presents an obvious hierarchical structure. Before heat treatment, the transition layer and the non-stick layer are combined in a clustered stacking manner, and after heat treatment, the transition layer and the non-stick layer are more tightly combined.
[0040] In the step S003, in the AT40-PFA composite coating, the weight ratio of AT40 to PFA is 1: 3. The non-stick layer obtained by adopting this composition ratio has good wear resistance, and the non-stick property will not be greatly affected.
[0041] In the step S002, the metal substrate is preheated before spraying. By preheating the metal substrate, the bonding strength between the transition layer and the surface of the metal substrate can be improved.
[0042] In step S002, the AT40 powder and the AT40-PFA mixed powder are dried before spraying to remove moisture therein. Specifically, before spraying, the AT40 powder and the AT40-PFA mixed powder are dehumidified and dried in a drying oven at 50° C. for 3-4 hours.
[0043] In the step S002, the thickness of the transition layer is 100-120 μm.
[0044] In the step S003, the thickness of the non-stick layer is 50-80 μm.
[0045] In step S001, the cleaning includes: first using kerosene as a cleaning medium, using ultrasonic waves to clean the surface of the polished metal substrate, and then cleaning it with water and alcohol respectively. The ultrasonic cavitation effect can remove grease, dirt, aluminum chips, etc. adhered to the surface of the substrate.
[0046] In step S002 and step S003, the spraying parameters of the atmospheric plasma spraying are: current 590-620A, spray distance 110mm, argon gas flow rate 40-60L·min -1 , hydrogen flow rate 5L·min -1 , powder feeding rate 15g·min -1 .
[0047] In step S001, the pressure range of the sandblasting roughening treatment is 0.3-0.4Mpa, the sandblasting angle is 80°-90°, and the surface roughness of the substrate after sandblasting is 3.0-5.0μm. Specifically, pay attention to keeping the moving speed uniform during sandblasting, and the surface of the substrate is gray after grinding without obvious metallic luster. After the sandblasting roughening treatment is completed, use compressed air to blow away the loose sand particles and debris on the surface, and finally wipe it with alcohol for cleaning.
[0048] A non-stick roller composite coating is prepared by the preparation method of the non-stick roller composite coating.
[0049] Example 1
[0050] A non-stick roller composite coating, the preparation method of which comprises the following steps:
[0051] Step S001. Pretreatment of the substrate surface: grinding the substrate surface with a rotary grinder to remove the machining allowance and the oxide layer to obtain a relatively smooth and clean surface;
[0052] Then, the surface of the substrate is cleaned, kerosene is used as the cleaning medium, the surface of the polished metal substrate is cleaned with ultrasonic waves, and then cleaned with water and alcohol, and wiped with clean filter paper for dehumidification;
[0053] The surface of the substrate that has been polished is subjected to sandblasting roughening treatment by using sandblasting equipment. The sandblasting equipment and materials are CS-600D sandblasting machine and 24# brown corundum sand. The pressure range of sandblasting roughening treatment is 0.3-0.4Mpa, the sandblasting angle is 80°-90°, and the surface roughness of the substrate after sandblasting is 3.0-5.0μm. The surface is gray and has no obvious metallic luster. After sandblasting, the loose sand and debris on the surface are blown away with compressed air, and finally wiped with alcohol for cleaning.
[0054] Step S002. Spraying transition layer: First, dehumidify and dry AT40 powder and AT40-PFA mixed powder in a drying oven at 50°C for 3-4 hours. After drying, pour AT40 powder into the powder feeding device, install the pre-treated metal substrate on the fixture of the workpiece table, enter the corresponding spraying parameters in the control console of the spraying device, and start the spraying work. The spraying parameters of atmospheric plasma spraying are: current 590A, spray distance 110mm, argon gas flow rate 60L·min -1 , hydrogen flow rate 5L·min -1 , powder feeding rate 15g·min -1 ; Use flame to preheat the metal substrate before feeding the powder, and use atmospheric plasma spraying method to spray AT40 coating on the surface of the metal substrate;
[0055] Step S003. Spraying the non-stick layer: spraying the AT40-PFA composite coating on the AT40 coating using an atmospheric plasma spraying method. During the spraying process, the coating is continuously cooled using compressed air. After the spraying is completed, the sample is removed after it is completely cooled.
[0056] Step S004. Heat treatment: After the coating is sprayed and completely cooled, the sample is placed in a box-type resistance furnace for heat treatment at 370° C. for 10 min in an atmospheric environment. After cooling, a non-stick roller composite coating product is obtained.
[0057] Example 2
[0058] A non-stick roller composite coating, the preparation method of which comprises the following steps:
[0059] Step S001. Pretreatment of the substrate surface: grinding the substrate surface with a rotary grinder to remove the machining allowance and the oxide layer to obtain a relatively smooth and clean surface;
[0060] Then, the surface of the substrate is cleaned, kerosene is used as the cleaning medium, the surface of the polished metal substrate is cleaned with ultrasonic waves, and then cleaned with water and alcohol, and wiped with clean filter paper for dehumidification;
[0061] The surface of the substrate that has been polished is subjected to sandblasting roughening treatment by using sandblasting equipment. The sandblasting equipment and materials are CS-600D sandblasting machine and 24# brown corundum sand. The pressure range of sandblasting roughening treatment is 0.3-0.4Mpa, the sandblasting angle is 80°-90°, and the surface roughness of the substrate after sandblasting is 3.0-5.0μm. The surface is gray and has no obvious metallic luster. After sandblasting, the loose sand and debris on the surface are blown away with compressed air, and finally wiped with alcohol for cleaning.
[0062] Step S002. Spraying transition layer: First, dehumidify and dry AT40 powder and AT40-PFA mixed powder in a drying oven at 50°C for 3-4 hours. After drying, pour AT40 powder into the powder feeding device, install the pre-treated metal substrate on the fixture of the workpiece table, enter the corresponding spraying parameters in the control console of the spraying device, and start the spraying work. The spraying parameters of atmospheric plasma spraying are: current 620A, spray distance 110mm, argon gas flow rate 40L·min -1 , hydrogen flow rate 5L·min -1 , powder feeding rate 15g·min -1 ; Use flame to preheat the metal substrate before feeding the powder, and use atmospheric plasma spraying method to spray AT40 coating on the surface of the metal substrate;
[0063] Step S003. Spraying the non-stick layer: spraying the AT40-PFA composite coating on the AT40 coating using an atmospheric plasma spraying method. During the spraying process, the coating is continuously cooled using compressed air. After the spraying is completed, the sample is removed after it is completely cooled.
[0064] Step S004. Heat treatment: After the coating is sprayed and completely cooled, the sample is placed in a box-type resistance furnace for heat treatment at 370° C. for 10 min in an atmospheric environment. After cooling, a non-stick roller composite coating product is obtained.
[0065] The wear resistance, friction coefficient, contact angle and rolling angle of the non-stick roller composite coating prepared in Example 1 and Example 2 were measured.
[0066] The wear resistance and friction coefficient were measured using a friction and wear testing machine.
[0067] The contact angle and sliding angle were measured using an automatic contact angle meter.
[0068] The results of each measurement index are as follows:
[0069] The non-stick roller composite coating obtained in Example 1 was measured to have a wear form mainly of adhesive wear, a friction coefficient of 0.12, a wear scar width of 0.67 mm, and a wear rate of 17.36 mm. 3 / (N·m), the wear scar depth is 29.3μm, the contact angle is 131.4°, and the rolling angle is 4°.
[0070] The non-stick roller composite coating obtained in Example 2 was tested and found to be mainly adhesive wear, with a friction coefficient of 0.14, a wear scar width of 0.99 mm, and a wear rate of 8.31 mm. 3 / (N·m), the wear scar depth is 15.66μm; the contact angle is 135.3°, and the rolling angle is 5°.
[0071] It can be seen from the above results that the friction coefficient of the non-stick roller composite coating prepared by the present invention is low, which reflects the low surface roughness of the coating. Figure 4 It can be seen from the results that in the friction test, the friction coefficient of the coating maintains a small fluctuation and good stability, which reflects the uniform structure of the coating. It can be applied to film equipment with high requirements on surface roughness, ensuring that the produced film has a smooth surface and uniform thickness.
[0072] In addition, the above results also show that the non-stick roller composite coating prepared by the present invention has good wear resistance. From the results of contact angle and rolling angle, it can be seen that the non-stick roller composite coating prepared by the present invention has good hydrophobicity and good non-stickiness.
[0073] It is understandable that those skilled in the art can make equivalent substitutions or changes based on the technical solution and inventive concept of the present invention, and all these changes or substitutions should fall within the protection scope of the claims attached to the present invention.
Claims
1. A method for preparing a non-stick roller composite coating, characterized in that: The following steps are involved: Step S001. Pretreatment of the substrate surface: grinding and polishing, cleaning and sandblasting the surface of the metal substrate in sequence; in the step S001, the pressure range of the sandblasting roughening treatment is 0.3-0.4Mpa, the sandblasting angle is 80°-90°, and the surface roughness of the substrate after sandblasting is 3.0-5.0μm; after the sandblasting roughening treatment is completed, the loose sand particles and debris on the surface are blown away with compressed air, and finally the surface is wiped and cleaned with alcohol; Step S002. Spraying a transition layer: spraying an AT40 coating on the surface of a metal substrate using an atmospheric plasma spraying method; Step S003. Spraying a non-stick layer: spraying an AT40-PFA composite coating on the AT40 coating by an atmospheric plasma spraying method, and continuously cooling the coating by compressed air during the spraying process; in the AT40-PFA composite coating, the weight ratio of AT40 to PFA is 1:3; In step S002 and step S003, the spraying parameters of the atmospheric plasma spraying are: current 590-620A, spray distance 110mm, argon gas flow rate 40-60L·min -1 , hydrogen flow rate 5L·min -1 , powder feeding rate 15g·min -1 ; Step S004. Heat treatment: After the coating is sprayed, heat treatment is performed at 370° C. for 10 min in an atmospheric environment, and a non-stick roller composite coating is obtained after cooling.
2. The method for preparing the non-stick roller composite coating according to claim 1, characterized in that: In the step S002, the metal substrate is also preheated before spraying.
3. The method for preparing the non-stick roller composite coating according to claim 1, characterized in that: In the step S002, the AT40 powder and the AT40-PFA mixed powder are dried before spraying.
4. The method for preparing the non-stick roller composite coating according to claim 1, characterized in that: In the step S002, the thickness of the transition layer is 100-120 μm.
5. The method for preparing the non-stick roller composite coating according to claim 1, characterized in that: In the step S003, the thickness of the non-stick layer is 50-80 μm.
6. The method for preparing a non-stick roller composite coating according to claim 1, characterized in that: In the step S001, the cleaning includes: firstly using kerosene as a cleaning medium, using ultrasonic waves to clean the surface of the polished metal substrate, and then cleaning it with clean water and alcohol respectively.
7. A non-stick roller composite coating, characterized in that: The non-stick roller composite coating is prepared by the preparation method of any one of claims 1 to 6.
Citation Information
Patent Citations
Non-stick coating and preparation method thereof as well as cooking utensils and cooking device
CN109136817A
Hydrophobic anti-corrosion coating material and preparation method thereof
CN112080716A
Cited By
Optical-grade non-stick roller and manufacturing method
CN116816805A
Optical grade non-stick roll and method of manufacture
CN116816805B