Anode material and preparation method thereof, composite anode material, lithium ion battery
By using high-hardness boron nitride and silicon oxide to form a covalent bond in the lithium-ion battery anode material, and adding a carbon coating layer when necessary, the problem of structural damage of the silicon-based anode material during the charge and discharge process is solved, and the problem is improved. It improves the conductivity and cycleability of the battery and achieves higher electrochemical performance and stability.
Patent Information
- Application Number
- CN202110801123.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-07-15
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2041-07-15
AI Technical Summary
Silicon-based anode materials have a volume effect during the charge and discharge process, which leads to structural damage, increased internal resistance and a sudden drop in cycle performance, limiting its application in lithium-ion batteries.
Boron nitride with high hardness and high stability is used as a supporting frame to form a covalent bond with silicon oxide to suppress the expansion and powdering of the anode material, and when necessary, a carbon coating layer is added to improve conductivity sex.
It significantly improves the electrochemical performance of lithium-ion batteries, especially the conductivity and cyclability, simplifies the process flow, facilitates industrial production, and significantly improves the cycle stability of the battery.
Smart Images

Figure CN115621429B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of electrode materials, and in particular to an anode material and a preparation method thereof, a composite anode material and a lithium ion battery. Background Art
[0002] Silicon-based materials have a high capacity when used as anode materials, which helps to improve the energy density of electrochemical energy storage devices and is considered to be the most promising anode material to replace carbon materials for the next generation of lithium-ion batteries. However, when silicon is used as an anode material, there is a large volume effect during the charge and discharge process, which can easily lead to the destruction of the material and electrode structure, increase in internal resistance, and a sharp drop in cycle performance, which seriously limits the application and commercialization of silicon anode materials.
[0003] CN107863505A discloses a composite material composed of boron nitride nanotubes / silicon / carbon nanotubes, which is prepared by mixing the components in NMP and drying and grinding. The composite material uses silicon particles as the functional part of the material, uses boron nitride nanotubes as structural support to alleviate the volume change of silicon particles during charging and discharging, and uses carbon nanotubes to enhance the electronic conductivity and ionic conductivity of the composite material. However, the composite material has the following disadvantages: 1) the interface between the components is not tightly bonded, which will cause the composite material to fail due to volume expansion changes during use, deteriorate and deactivate; 2) boron nitride nanotubes / carbon nanotubes have the disadvantages of complex preparation process and high cost, and are prone to structural failure during use; 3) due to the structural design, the three components are simply combined together, and the material structure is disordered, so the support effect of boron nitride nanotubes on the structure is very inefficient.
[0004] Therefore, there is an urgent need for a new anode material that can overcome the problems of structural failure and disorder caused by volume expansion, thereby improving the structural stability of lithium-ion batteries of the anode material, as well as the conductivity and cyclability of lithium-ion batteries made from the anode material. Summary of the invention
[0005] The purpose of the present invention is to overcome the problems that the existing silicon / boron nitride-containing anode materials have a large volume effect during the charge and discharge process, which easily leads to the destruction of the material and electrode structure, the increase of internal resistance, and the sudden drop in cycle performance. A new anode material and its preparation method, a composite anode material, and a lithium ion battery are provided. The anode material can effectively inhibit the expansion and pulverization problems during the application process, maintain the structural stability of the anode material, thereby improving the conductivity and cyclability of the lithium ion battery.
[0006] In order to achieve the above object, the present invention provides an anode material in a first aspect, the anode material comprises a substrate, the substrate contains silicon oxide, boron nitride and optional carbon element, wherein the general formula of the silicon oxide is SiO x , where 0.5≤x≤1.7;
[0007] Wherein, based on the total weight of the substrate, the sum of the contents of silicon oxide and boron nitride is 3-100wt%;
[0008] Wherein, the configuration of the boron nitride is selected from cubic boron nitride and optional hexagonal boron nitride.
[0009] Preferably, the anode material further comprises: a carbon coating layer coated on the surface of the substrate.
[0010] A second aspect of the present invention provides a method for preparing an anode material, the method comprising the following steps:
[0011] (1) Under inert gas conditions, silicon oxide, boron powder and an optional carbon-containing additive are first mixed to obtain a precursor I;
[0012] (2) heat treating the precursor I with H2O and NH3 under inert gas conditions to obtain a substrate;
[0013] (3) Optionally, the substrate is subjected to carbon coating modification treatment to obtain an anode material;
[0014] Wherein, the general formula of the silicon oxide is SiO x , where 0.5≤x≤1.7.
[0015] A second aspect of the present invention provides a method for preparing an anode material, the method comprising the following steps:
[0016] (1′) Under inert gas conditions, silicon oxide, hexagonal boron nitride, lithium nitride and an optional carbon-containing additive are mixed for a second time to obtain a precursor II;
[0017] (2') Under inert gas conditions, the precursor II is sequentially heated and pre-pressed, and the resulting product is subjected to ultrahigh pressure treatment to obtain a matrix;
[0018] (3') Optionally, the substrate is subjected to a carbon coating modification treatment to obtain an anode material;
[0019] Wherein, the general formula of the silicon oxide is SiO x , where 0.5≤x≤1.7;
[0020] The matrix contains silicon oxide, boron nitride and optional carbon element; based on the total weight of the matrix, the sum of the content of silicon oxide and boron nitride is 3-100wt%.
[0021] The third aspect of the present invention provides a composite anode material, which comprises the anode material provided in the first aspect and / or the anode material prepared by the method provided in the second aspect and a carbonaceous material.
[0022] A fourth aspect of the present invention provides a lithium ion battery, which comprises the anode material provided in the first aspect, the anode material prepared by the method provided in the second aspect, and the composite anode material provided in the third aspect.
[0023] Compared with the prior art, the present invention has the following advantages:
[0024] (1) The anode material provided by the present invention uses boron nitride with high hardness and high stability as the supporting frame of the anode material, and uses silicon oxide as the active component. The covalent bond formed between boron nitride and silicon oxide allows the boron nitride to remain stable during the charge and discharge process of the anode material, effectively suppressing the expansion and pulverization of the anode material during the application process, thereby improving the electrochemical performance of the lithium ion battery containing the anode material, especially the conductivity and cyclability; in particular, the use of cubic boron nitride further improves the electrochemical performance of the lithium ion battery;
[0025] (2) Preferably, when the matrix of the anode material provided by the present invention further contains carbon elements, the conductivity of the anode material can be further improved; when the anode material provided by the present invention further contains a carbon coating layer, it helps to improve the initial charge and discharge coulomb efficiency and conductivity of the anode material;
[0026] (3) The method for preparing the anode material provided by the present invention forms a covalent bond between boron nitride and silicon oxide. Preferably, the boron nitride is synthesized in situ, and the contact strength between the components is higher, thereby avoiding problems such as structural failure, cracking and deactivation caused by loose interface bonding between the components. At the same time, the method simplifies the process flow and is convenient for industrial production.
[0027] (4) Using the anode material provided by the present invention in lithium-ion batteries can significantly improve the cycle stability of the batteries. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 is a schematic structural diagram of anode material S1 prepared in Example 1;
[0029] Figure 2 is a cross-sectional SEM image of the anode material S1 prepared in Example 1;
[0030] Figure 3is an XRD schematic diagram of the anode material S1 prepared in Example 1;
[0031] Figure 4 is the FT-IR graph of the anode material S1 prepared in Example 1;
[0032] Figure 5 This is the FT-IR graph of the anode material S3 prepared in Example 3. DETAILED DESCRIPTION
[0033] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0034] In the present invention, unless otherwise specified, the "first" and "second" do not represent the order of precedence, nor do they limit the materials or operations. They are only used to distinguish the materials or operations. For example, the "first" and "second" in the "first stage" and the "second stage" are only used to distinguish to indicate that they are not the same stage; the "first" and "second" in the "first mixing" and the "second mixing" are only used to distinguish to indicate that they are not the same mixing.
[0035] The first aspect of the present invention provides an anode material, the anode material comprising a substrate, the substrate containing silicon oxide, boron nitride and an optional carbon element, wherein the general formula of the silicon oxide is SiO x , where 0.5≤x≤1.7;
[0036] Wherein, based on the total weight of the substrate, the sum of the content of the silicon oxide and the cubic boron nitride is 3-100wt%;
[0037] Wherein, the configuration of the boron nitride is selected from cubic boron nitride and optional hexagonal boron nitride.
[0038] The inventors of the present invention have found that the combination of the boron nitride nanotube skeleton, silicon and carbon nanotubes in the boron nitride nanotube / silicon / carbon nanotube composite material in the prior art mainly relies on the mechanical adhesion generated by the drying and grinding of the suspension, and this mechanical adhesion is mainly the intermolecular force such as the van der Waals force. Therefore, the inventors use boron nitride (especially cubic boron nitride) with high hardness and high stability as the support frame of the anode material, so that the anode material containing the support frame maintains structural stability during the electrochemical charge and discharge process, effectively suppresses the expansion and pulverization problems of the anode material during the application process, thereby improving the electrochemical performance of the lithium ion battery containing the anode material, especially the conductivity and cyclability.
[0039] At the same time, the covalent bond formed between the boron nitride (cubic boron nitride and optional hexagonal boron nitride) and silicon oxide in the anode material provided by the present invention can further enhance the binding force between the components in the anode material, thereby significantly improving the cycle performance of the anode material by improving the structural stability of the anode material.
[0040] In some embodiments of the present invention, Figure 4 As shown in the FT-IR Fourier infrared test, the 1190cm -1 The peak of bridging oxygen in Si-OB was detected nearby, proving that silicon oxide and boron nitride are connected by covalent bonds; -1 The absorption peaks in the range correspond to the sp 3 The bonding transverse optical symmetric vibration mode indicates that the anode material contains cubic boron nitride.
[0041] In some embodiments of the present invention, Figure 5 It can be seen that in the FT-IR Fourier infrared test, the 1190cm -1 The peak of bridging oxygen in Si-OB was detected nearby, proving that silicon oxide and boron nitride are connected by covalent bonds; -1 and 790cm -1 There are obvious absorption peaks at 1062-1069cm, which correspond to the in-plane stretching vibration of the relevant BN bonds in the h-BN phase and the out-of-plane bending vibration of BNB, respectively, proving that the material does have an h-BN phase; -1 The absorption peaks in the range correspond to the sp 3 Bonding indicates that the anode material contains hexagonal boron nitride and cubic boron nitride.
[0042] According to a preferred embodiment of the present invention, based on the total weight of the substrate, the sum of the contents of the silicon oxide and cubic boron nitride is 3-98 wt %.
[0043] In the present invention, the silicon oxide in the anode material exists in the form of particles. Preferably, the particle volume distribution D50 of the silicon oxide is 0.01-100 μm, preferably 1-30 μm.
[0044] In the present invention, the source of the silicon oxide has a wide selection range, as long as the general formula of the silicon oxide meets the above requirements. The silicon oxide can be obtained by commercial purchase or by self-production.
[0045] In some embodiments of the present invention, elemental silicon and silicon dioxide are mixed in a certain ratio to obtain a general formula of SiO x Silicon oxide, wherein 0.5≤x≤1.7.
[0046] In the present invention, the boron nitride in the anode material exists in at least one form of a layer, a wire, a tube, a particle, etc.
[0047] In some embodiments of the present invention, preferably, the weight ratio of silicon oxide to boron nitride is 1.5-99: 1, preferably 5-50: 1. The preferred weight ratio ensures that the capacity of the anode material can be fully utilized while silicon nitride plays a supporting role.
[0048] In a preferred embodiment of the present invention, the configuration of the boron nitride is cubic boron nitride.
[0049] In a preferred embodiment of the present invention, the anode material comprises a matrix, wherein the matrix is composed of silicon oxide and cubic boron nitride, wherein the general formula of the silicon oxide is SiO x , where 0.5≤x≤1.7.
[0050] In some embodiments of the present invention, preferably, the anode material comprises a matrix, wherein the matrix contains silicon oxide, cubic boron nitride and carbon element, wherein the general formula of the silicon oxide is SiO x , wherein 0.5≤x≤1.7; based on the total weight of the substrate, the carbon content is 0-97wt%, preferably 2-97wt%. In the present invention, limiting the carbon content is beneficial to improving the conductivity of the anode material, but will reduce the capacity of the material.
[0051] In the present invention, unless otherwise specified, the carbon element exists in at least one form of elemental carbon, organic matter and carbonate.
[0052] In some embodiments of the present invention, preferably, in the anode material, the particle volume distribution D50 of the matrix is 0.01-100 μm, for example, 0.01 μm, 1 μm, 5 μm, 10 μm, 15 μm, 20 μm, 25 μm, 30 μm, 40 μm, 50 μm, 70 μm, 90 μm and 100 μm, and any value in the range of any two values, preferably 1-30 μm. The present invention achieves comprehensive unification of material performance in terms of processing performance, cycle performance, expansion performance and other aspects by limiting the particle volume distribution D50 of the matrix.
[0053] In the present invention, the particle volume distribution D50 parameter of the matrix is measured according to methods such as GB / T 19077-2016 "Particle Size Distribution Laser Diffraction Method" and GB / T 14265-2017 "General Rules for Analysis of Hydrogen, Oxygen, Nitrogen, Carbon and Sulfur in Metallic Materials".
[0054] According to the present invention, preferably, the anode material further comprises: a carbon coating layer coated on the surface of the substrate. In the present invention, the anode material containing the carbon coating layer is more conducive to improving the initial charge and discharge coulomb efficiency and conductivity of the anode material.
[0055] According to a particularly preferred embodiment of the present invention, the anode material comprises: a substrate and a carbon coating layer coated on the surface of the substrate, wherein the substrate contains silicon oxide, cubic boron nitride and carbon element, wherein the general formula of the silicon oxide is SiO x , where 0.5≤x≤1.7;
[0056] Wherein, based on the total weight of the substrate, the sum of the contents of the silicon oxide and cubic boron nitride is 3-98wt%, and the content of the carbon element is 2-97wt%; wherein, the weight ratio of the silicon oxide to cubic boron nitride is 1.5-99:1.
[0057] A second aspect of the present invention provides a method for preparing an anode material, the method comprising the following steps:
[0058] (1) Under inert gas conditions, silicon oxide, boron powder and an optional carbon-containing additive are first mixed to obtain a precursor I;
[0059] (2) heat treating the precursor I with H2O and NH3 under inert gas conditions to obtain a substrate;
[0060] (3) Optionally, the substrate is subjected to carbon coating modification treatment to obtain an anode material;
[0061] Wherein, the general formula of the silicon oxide is SiO x , where 0.5≤x≤1.7;
[0062] The matrix contains silicon oxide, boron nitride and optional carbon element; based on the total weight of the matrix, the sum of the content of silicon oxide and boron nitride is 3-100wt%.
[0063] In some embodiments of the present invention, preferably, in step (1), the weight ratio of the silicon oxide, boron powder and the optional carbon-containing additive is 3-49:1:0-50, preferably 30-49:1:1:0-10. The preferred weight ratio is more advantageous in that the boron nitride generation rate of the material is higher and the particle structure is more stable while ensuring that the material has a higher capacity.
[0064] In the present invention, the carbon-containing auxiliary agent has a wide selection range, as long as the carbon-containing auxiliary agent contains carbon. Preferably, the carbon-containing auxiliary agent is selected from at least one of carbon, organic matter and carbonate, preferably organic matter. For example, the weight average molecular weight of the organic matter is greater than 70 g / mol, and is selected from glucose, sucrose, hydrocarbons, etc., but is not limited thereto.
[0065] In some embodiments of the present invention, the inert gas is selected from at least one of nitrogen, helium, argon and neon, preferably nitrogen.
[0066] In the present invention, in step (1), there is a wide range of options for the first mixing method, as long as the silicon oxide, boron powder and the optional carbon-containing additive are mixed.
[0067] In the present invention, the first mixed product is subjected to spray drying, crushing, grinding, ball milling, etc. according to the type of carbon-containing additive in step (1) and the particle size control of the precursor I. Preferably, the first mixed product in step (1) is ball milled in a high-speed ball mill for 1-5 hours to obtain the precursor I.
[0068] In some embodiments of the present invention, preferably, the volume distribution D50 of the precursor I is 0.01-100 μm, preferably 1-30 μm.
[0069] In the present invention, in step (2), the conditions for the heat treatment have a wide range of selection. Preferably, the conditions for the heat treatment include: a temperature of 1000-2000°C, preferably 1300-1500°C; a time of 0.5-12h, preferably 0.5-5h.
[0070] In some embodiments of the present invention, the precursor I is introduced with H2O and NH3 under inert gas conditions, heated to 1000-2000°C for heat treatment for 0.5-12h, and then cooled to room temperature to obtain a substrate I.
[0071] In the present invention, unless otherwise specified, the room temperature refers to 20-25°C, preferably 25°C.
[0072] According to the present invention, preferably, in step (2), the heat treatment includes: a first stage and a second stage, wherein the process of the first stage includes: first contacting the precursor I with H2O; and the process of the second stage includes: second contacting the product of the first contact with NH3. The use of a segmented heat treatment method is conducive to uniform distribution of H2O in the equipment atmosphere, slight hydroxylation and adsorption of the material and H2O, facilitating in-situ synthesis of cubic boron nitride, promoting the bonding between the components through covalent bonds, and improving the structural stability of the anode material.
[0073] In the present invention, the first contacting realizes that H2O is evenly distributed in the reaction equipment, and the precursor I contacts with H2O to form micro-hydroxylation and adsorption, and at the same time, H2O reacts with boron powder to generate B2O2 gas. Preferably, the conditions of the first contacting include: a temperature of 1000-2000°C, preferably 1300-1500°C.
[0074] In the present invention, the second contact is to achieve NH3, H2O, SiO x The reaction between A and B includes:
[0075] 2B+2H2O→B2O2+2H2
[0076] B2O2+2NH3→2BN+2H2O+H2.
[0077] According to the present invention, preferably, the conditions for the second contact include: a temperature of 1000-2000° C., preferably 1300-1500° C.; and a time of 0.5-12 h, preferably 0.5-5 h.
[0078] In the present invention, in step (2), the heat-treated product can be subjected to pulverization, classification and other treatments according to the particle volume distribution D50 range of the matrix, preferably classification treatment. In the present invention, the classification treatment is carried out in an air flow classifier.
[0079] In the present invention, in step (3), the modification treatment is intended to load a carbon coating layer on the surface of the substrate, thereby improving the conductivity and cyclability of the anode material.
[0080] In the present invention, there is a wide range of options for the carbon coating modification treatment, that is, the substrate can be subjected to carbon coating modification treatment with carbon-containing gas, carbon-containing liquid, or carbon-containing solid.
[0081] In a preferred embodiment of the present invention, the substrate is subjected to a carbon coating modification treatment with a carbon-containing gas to obtain an anode material.
[0082] In the present invention, the type of the carbon-containing gas has a wide range of selection, as long as the carbon-containing gas contains carbon elements, it can also be a vaporized carbon-containing liquid, such as toluene. Preferably, the carbon-containing gas is selected from at least one of ethylene, acetylene, methane, ethane, propane, propylene and formaldehyde, preferably at least one of ethylene, acetylene, methane and propane.
[0083] In some embodiments of the present invention, preferably, the conditions of the carbon coating modification treatment include: temperature of 800-1500° C., preferably 900-1200° C.; time of 0.1-5 h, preferably 0.5-3 h.
[0084] According to another embodiment of the present invention, preferably, the method for preparing the anode material comprises the following steps:
[0085] (1′) Under inert gas conditions, silicon oxide, hexagonal boron nitride, lithium nitride and an optional carbon-containing additive are mixed for a second time to obtain a precursor II;
[0086] (2') Under inert gas conditions, the precursor II is sequentially heated and pre-pressed, and the resulting product is subjected to ultrahigh pressure treatment to obtain a matrix;
[0087] (3') Optionally, the substrate is subjected to a carbon coating modification treatment to obtain an anode material;
[0088] Wherein, the general formula of the silicon oxide is SiO x , where 0.5≤x≤1.7;
[0089] The matrix contains silicon oxide, boron nitride and optional carbon element; based on the total weight of the matrix, the sum of the content of silicon oxide and boron nitride is 3-100wt%.
[0090] In the present invention, the second mixing method has a wide range of options, as long as the silicon oxide, hexagonal boron nitride, lithium nitride and the optional carbon-containing additive are mixed uniformly in step (1').
[0091] In some embodiments of the present invention, preferably, in step (1'), the weight ratio of silicon oxide, hexagonal boron nitride, lithium nitride and carbon-containing additive is 70-95: 1-30: 1: 1-30, preferably 80-95: 1-15: 1: 1-15. The preferred weight ratio range is more conducive to achieving a corresponding balance between material capacity and material structural strength.
[0092] In the present invention, the second mixed product is spray dried, crushed, ground, ball milled, etc. according to the type of carbon-containing additive and the particle size of the precursor II in step (1'). Preferably, the second mixed product in step (1') is ball milled in a high-speed ball mill for 1-5 hours to obtain the precursor II.
[0093] In some embodiments of the present invention, preferably, the volume distribution D50 of the precursor II is 0.01-100 μm, for example, 0.01 μm, 1 μm, 5 μm, 10 μm, 15 μm, 20 μm, 30 μm, 40 μm, 50 μm, 70 μm, 90 μm and 100 μm, and any value in the range composed of any two values, preferably 0.1-20 μm.
[0094] In the present invention, preferably, in step (2'), the heating conditions include: temperature of 200-400°C, preferably 250-350°C; time of 0.1-5h, preferably 0.1-2h. The heating refers to heating the precursor II at a constant temperature of 200-400°C for 0.1-5h.
[0095] In some embodiments of the present invention, preferably, in step (2'), the pre-pressing pressure is ≥50 MPa, preferably 50-300 MPa.
[0096] In some embodiments of the present invention, preferably, the conditions of the ultra-high pressure treatment include: pressure ≥ 1 GPa, preferably 5-30 GPa; temperature 800-2000°C, preferably 1000-1800°C; time 0.1-2h, preferably 0.1-1h.
[0097] In the present invention, in step (2'), the treated product can be subjected to pulverization, classification and other treatments according to the particle volume distribution D50 range of the matrix, preferably classification treatment. In the present invention, the classification treatment is carried out in an air flow classifier.
[0098] In the present invention, in step (3'), the carbon coating modification treatment is carried out in accordance with the above-mentioned definition, and the present invention will not elaborate on it here.
[0099] The third aspect of the present invention provides a composite anode material, which comprises the anode material provided in the first aspect and / or the anode material prepared by the method provided in the second aspect and a carbonaceous material.
[0100] In some embodiments of the present invention, preferably, based on the total weight of the composite anode material, the content of the anode material is 1-60wt%, preferably 3-45wt%. The preferred content can simultaneously improve the cycle performance and material capacity of the composite anode material.
[0101] In the present invention, the preparation method of the composite anode material has a wide range of options, as long as the anode material and the carbonaceous material are composited. In the present invention, the composite operation method is not specifically limited.
[0102] In the present invention, the carbon-containing material has a wide selection range. Preferably, the carbon-containing material is selected from carbon elements, including but not limited to graphite, soft carbon, hard carbon and the like.
[0103] A fourth aspect of the present invention provides a lithium ion battery, which comprises the anode material provided by the first aspect, the anode material obtained by the method provided by the second aspect, and the composite material provided by the third aspect.
[0104] According to the present invention, preferably, the lithium ion battery is a lithium ion secondary battery containing a non-aqueous electrolyte, and the lithium ion battery contains the anode material provided by the present invention.
[0105] In some embodiments of the present invention, preferably, the anode material and / or composite anode material provided by the present invention, graphite, conductive carbon, SBR (styrene-butadiene rubber), CMC (sodium carboxymethyl cellulose) are mixed evenly with a certain amount of water in a weight ratio of 45:45:5:3:2, and the obtained mixed slurry is evenly coated on a copper foil, dried, and a working electrode is obtained; a lithium sheet is used as a symmetrical electrode, and a polymer diaphragm is used to separate the working electrode from the symmetrical electrode; and an electrolyte is made of 1 mol / L LiPF6 EC:PC to make a lithium ion battery. Wherein, the volume ratio of EC to PC is 1:1.
[0106] The present invention will be described in detail below through examples.
[0107] In the examples and comparative examples, unless otherwise specified, the room temperature is 25°C.
[0108] The property parameters of the anode materials obtained in Examples 1-9 and Comparative Examples 1-3 are listed in Table 1.
[0109] Example 1
[0110] (1) In a nitrogen atmosphere, silicon oxide particles (SiO x , x=1), boron powder and glucose were mixed in a weight ratio of 35:1:8, and the mixed product was ball-milled in a high-speed ball mill for 2 h to obtain a precursor I-1 with a volume distribution D50 of 4 μm;
[0111] (2) Under nitrogen atmosphere, the precursor I-1 was placed in a tubular rotary kiln, H2O was introduced at a flow rate of 1 L / min, the temperature was raised to 1350°C and kept constant for 0.5 h, and then NH3 was introduced at a flow rate of 0.5 L / min, and the temperature was kept at 1350°C for 1 h, and then the introduction of NH3 was stopped, and the product was cooled to room temperature, and the product was classified in an air flow classifier to obtain a matrix with a particle volume distribution D50 of 4 μm;
[0112] (3) placing the substrate in a CVD furnace, introducing acetylene to perform carbon coating modification treatment, so as to coat a carbon coating layer on the surface of the substrate to obtain anode material S1; wherein the conditions of the carbon coating modification treatment include: temperature of 900°C and time of 2h.
[0113] The structural diagram of the anode material S1 is as follows: Figure 1 As shown by Figure 1 It can be seen that the anode material S1 includes a substrate and a carbon coating layer supported on the surface of the substrate.
[0114] The cross-sectional SEM image of the anode material S1 is as follows: Figure 2 As shown by Figure 2 It can be seen that the boron nitride, carbon element and silicon oxide in the anode material S1 are tightly combined.
[0115] Among them, the XRD pattern of the anode material S1 is as follows Figure 3 As shown by Figure 3 It can be seen that the anode material S1 contains cubic boron nitride, silicon and carbon elements.
[0116] The FT-IR image of the anode material S1 is as follows: Figure 4 As shown by Figure 4 It can be seen that in the FT-IR Fourier infrared test, the 1190cm -1 The peak of bridging oxygen in Si-OB was detected nearby, proving that silicon and boron nitride are connected by covalent bonds; -1 The absorption peaks in the range correspond to the sp 3 Bonding transverse optical symmetric vibration mode, that is, the anode material S1 contains cubic boron nitride.
[0117] Example 2
[0118] (1) In a nitrogen atmosphere, silicon oxide particles (SiO x , x=0.95), boron powder and sucrose were mixed in a weight ratio of 40:1:5, and the mixed product was ball-milled in a high-speed ball mill for 1.5 h to obtain a precursor I-2 with a volume distribution D50 of 6 μm;
[0119] (2) Under nitrogen atmosphere, the precursor I-2 was placed in a tubular rotary kiln, H2O was introduced at a flow rate of 1 L / min, the temperature was raised to 400°C and kept constant for 0.5 h, and then NH3 was introduced at a flow rate of 1 L / min, the temperature was raised to 1200°C and kept constant for 1.5 h, and then the introduction of NH3 was stopped, the mixture was cooled to room temperature, and the product was classified in an air flow classifier to obtain a matrix with a particle volume distribution D50 of 6 μm;
[0120] (3) placing the above substrate into a CVD furnace, introducing ethylene to perform carbon coating modification treatment, so as to coat a carbon coating layer on the surface of the substrate to obtain anode material S2; wherein the conditions of the carbon coating modification treatment include: temperature of 1000°C and time of 2h.
[0121] Among them, the structural schematic diagram of the anode material S2 is Figure 1 Similar; the cross-sectional SEM image of the anode material S2 is Figure 2 Similar; the XRD pattern of the anode material S2 is Figure 3 Similar; the FT-IR graph of the anode material S2 is Figure 4 similar.
[0122] Example 3
[0123] (1) In a nitrogen atmosphere, silicon oxide particles (SiO x , x=1.05), hexagonal boron nitride, lithium nitride and glucose were mixed in a weight ratio of 80:1:1:10, and the mixed product was ball-milled in a high-speed ball mill for 1 h to obtain a precursor II-1 with a volume distribution D50 of 8 μm;
[0124] (2) In a nitrogen atmosphere, the precursor II-1 was heated to 300°C for 1 hour, placed in an isostatic press and pre-pressed to 200 MPa, and then subjected to ultra-high pressure treatment by a six-sided top press. The treatment conditions included: pressure of 6 GPa, temperature of 1400°C, time of 10 min, cooled to room temperature, and the product was classified in an air flow classifier to obtain a matrix with a particle volume distribution D50 of 8 μm;
[0125] (3) placing the above substrate into a CVD furnace, introducing ethylene to perform carbon coating modification treatment, so as to coat a carbon coating layer on the surface of the substrate to obtain anode material S3; wherein the conditions of the carbon coating modification treatment include: temperature of 1000°C and time of 2h.
[0126] The FI-IR image of the anode material S3 is as follows: Figure 5 As shown by Figure 5 It can be seen that the 1190cm -1The peak of bridging oxygen in Si-OB was detected nearby, proving that silicon oxide and boron nitride are connected by covalent bonds; -1 and 790cm -1 There are obvious absorption peaks at 1062-1069cm, which correspond to the in-plane stretching vibration of the relevant BN bonds in the h-BN phase and the out-of-plane bending vibration of BNB, respectively, proving that the material does have an h-BN phase; -1 The absorption peaks in the range correspond to the sp 3 Bonding, that is, the anode material S3 contains hexagonal boron nitride and cubic boron nitride.
[0127] Example 4
[0128] The method of Example 1 is followed, except that in step (1), glucose is not added, and the remaining steps are the same to obtain anode material S4.
[0129] Example 5
[0130] The method of Example 1 is as follows, except that in step (1), silicon oxide particles (SiO x , x=1), the weight ratio of boron powder and glucose was replaced from 35:1:8 to 50:15:8, and the remaining steps were the same to obtain anode material S5.
[0131] Example 6
[0132] The method of Example 1 is as follows, except that in step (1), silicon oxide particles (SiO x , x = 1) is replaced by silicon oxide particles (SiO x , x=1.5), and the remaining steps are the same to obtain anode material S6.
[0133] Example 7
[0134] The method of Example 1 is followed, except that in step (2), under a nitrogen atmosphere, the precursor I-1 is placed in a tubular rotary kiln, H2O at a flow rate of 1 L / min and NH3 at a flow rate of 0.5 L / min are introduced, the temperature is raised to 1350°C and maintained at a constant temperature for 1.5 hours, the product is cooled to room temperature, and the product is classified in an air flow classifier to obtain a matrix with a particle volume distribution D50 of 6 μm; the remaining steps are the same to obtain the anode material S7.
[0135] Example 8
[0136] The method of Example 1 is followed, except that step (3) is omitted, that is, the matrix with a particle volume distribution D50 of 6 μm obtained in step (2) is used as anode material S8.
[0137] Example 9
[0138] The method of Example 1 is followed, except that the anode material S1 obtained in step (3) is compounded with a carbon-containing material (graphite) to obtain a composite anode material S9.
[0139] Based on the total weight of the composite material S9, the content of the anode material S1 is 10 wt%.
[0140] Comparative Example 1
[0141] The method of Example 1 is as follows, except that in step (1), silicon oxide particles (SiO x , x = 1) is replaced by silicon oxide particles (SiO x , x=2), and the remaining steps are the same to obtain the anode material DS1.
[0142] Comparative Example 2
[0143] According to the method disclosed in CN107863505A, silicon particles (chemical formula Si), boron nitride nanotubes, and carbon nanotubes are mixed in a weight ratio of 1:2:2, ultrasonically vibrated for 3 hours, dried, dried at 100°C for 15 hours, and ground to obtain the anode material DS2, that is, a boron nitride nanotube / silicon / carbon nanotube composite material with a silicon content of 20wt%.
[0144] Comparative Example 3
[0145] The method of Example 1 is followed, except that NH3 is not introduced in step (2). The remaining steps are the same, and the obtained anode material D3 does not contain boron nitride. Based on the total weight of the anode material D3, the content of silicon oxide is 91.6wt%, and the content of carbon is 8.4wt%.
[0146] Table 1
[0147]
[0148]
[0149] Note: 1- the sum of the contents of silicon oxide and boron nitride in the matrix; 2- the content of carbon in the matrix; 3- the weight ratio of silicon oxide and boron nitride in the matrix; 4- the expansion coefficient is the value of the volume ratio of the material before and after lithium insertion in the half-cell divided by the material capacity (Ah / g) (for example, in Example 1, the volume ratio after lithium insertion is 1.92 compared to the volume ratio before lithium insertion, then the coefficient is 1.92 / 1.2099=1.59).
[0150] It can be seen from the data in Table 1 that the present invention is more conducive to improving the material capacity and first coulombic efficiency of the anode material and reducing the expansion coefficient of the anode material after lithium insertion by limiting the sum of the contents of silicon oxide and boron nitride in the matrix of the anode material, the content of carbon element in the matrix, and the weight ratio of silicon oxide and boron nitride in the matrix within the preferred condition range.
[0151] Compared with Comparative Example 2, the anode material prepared in Example 1 has a higher material capacity and first coulombic efficiency, and a lower expansion coefficient after lithium insertion; compared with Comparative Example 3, the anode material prepared in Example 1 has a higher first coulombic efficiency, and a lower expansion coefficient after lithium insertion. Therefore, the anode material provided by the present invention has a higher material capacity and first coulombic efficiency, and a lower expansion coefficient after lithium insertion.
[0152] Test Case
[0153] The anode materials (S1-S9 and DS1-DS3) prepared in Examples 1-9 and Comparative Examples 1-3 were subjected to electrochemical performance tests.
[0154] Assembling lithium-ion secondary batteries: Anode materials (S1-S9 and DS1-DS3), graphite, conductive carbon, SBR (styrene-butadiene rubber), and CMC (sodium carboxymethyl cellulose) were mixed in water at a weight ratio of 45:45:5:3:2, and the obtained mixed slurry was evenly coated on copper foil and dried to obtain a working electrode; lithium sheets were used as symmetrical electrodes, and the working electrode and the symmetrical electrode were separated by a polymer diaphragm; the electrolyte used was 1 mol / L LiPF6 EC:PC to make lithium-ion secondary batteries (Q1-Q9 and DQ1-DQ3). Among them, the volume ratio of EC and PC was 1:1.
[0155] Test conditions: The lithium-ion batteries (Q1-Q9 and DQ1-DQ3) were left at room temperature for 24 hours. The charging and discharging device was used. The first charge and discharge were performed at a constant current of 0.025C, and the cut-off voltage was 0.005V. The discharge was performed at a constant current of 0.025C, and the cut-off voltage was 2V; then the charging was performed at a constant current of 0.2C, and the cut-off voltage was 0.005V. The discharge was performed at a constant current of 0.2C, and the cut-off voltage was 2V; the charge and discharge were repeated 1 time, 50 times, 100 times, 150 times, and 200 times, and the results of the capacity retention rate (%) were listed in Table 2.
[0156] Table 2
[0157]
[0158] It can be seen from the data in Table 2 that, compared with Comparative Examples 1-3, using the anode material provided by the present invention in a lithium ion battery can effectively improve the cycle performance of the battery during the charge and discharge process.
[0159] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. An anode material for a lithium ion battery, characterized in that: The anode material comprises a matrix, wherein the matrix contains silicon oxide and boron nitride, wherein the silicon oxide has a general formula of SiO x , wherein 0.5≤x≤1.7; the silicon oxide and the boron nitride are connected by a Si-OB covalent bond; Wherein, based on the total weight of the substrate, the sum of the content of the silicon oxide and the boron nitride is 3-100wt%; the weight ratio of the silicon oxide to the boron nitride is 1.5-99:1; Wherein, the configuration of the boron nitride is cubic boron nitride, or cubic boron nitride and hexagonal boron nitride.
2. The anode material according to claim 1, characterized in that Based on the total weight of the substrate, the sum of the contents of the silicon oxide and the boron nitride is 3-98wt%.
3. The anode material according to claim 1, characterized in that The matrix also contains carbon; Based on the total weight of the substrate, the content of the carbon element is 0-97wt%.
4. The anode material according to claim 3, characterized in that Based on the total weight of the substrate, the content of the carbon element is 2-97wt%.
5. The anode material according to claim 1, characterized in that The particle volume distribution D50 of the matrix is 0.01-100 μm.
6. The anode material according to any one of claims 1 to 5, characterized in that: The anode material further comprises: a carbon coating layer coated on the surface of the substrate.
7. A method for preparing an anode material for a lithium ion battery, characterized in that: The method comprises the following steps: (1) Under inert gas conditions, silicon oxide and boron powder are first mixed to obtain a precursor I; (2) Under inert gas conditions, heat-treating the precursor I with H2O and NH3 to obtain a substrate; the heat-treating conditions are: temperature of 1000-2000°C, time of 0.5-12h; (3) performing carbon coating modification on the substrate; wherein the substrate or the product obtained in step (3) is used as an anode material; Wherein, the general formula of the silicon oxide is SiO x , where 0.5≤x≤1.7; The matrix contains silicon oxide and boron nitride; based on the total weight of the matrix, the sum of the content of silicon oxide and boron nitride is 3-100wt%; and the weight ratio of silicon oxide to boron nitride is 1.5-99:
1.
8. The method according to claim 7, wherein: In step (1), the silicon oxide, boron powder and carbon-containing additive are mixed in the first step; Wherein, the matrix also contains carbon element.
9. A method for preparing an anode material for a lithium ion battery, characterized in that: The method comprises the following steps: (1') Under inert gas conditions, silicon oxide, hexagonal boron nitride and lithium nitride are mixed for a second time to obtain a precursor II; the weight ratio of silicon oxide to hexagonal boron nitride is 70-95:1-30; (2') Under inert gas conditions, the precursor II is heated and pre-pressed in sequence, and the resulting product is subjected to ultra-high pressure treatment to obtain a matrix; the heating conditions are: temperature of 200-400°C, time of 0.1-5h; the ultra-high pressure treatment conditions are: pressure ≥1GPa, temperature of 800-2000°C, time of 0.1-2h; (3') subjecting the substrate to a carbon coating modification treatment; wherein the substrate or the product obtained in step (3') is used as an anode material; Wherein, the general formula of the silicon oxide is SiO x , where 0.5≤x≤1.7; The matrix contains silicon oxide and boron nitride; based on the total weight of the matrix, the sum of the contents of silicon oxide and boron nitride is 3-100wt%.
10. The method according to claim 9, wherein: In step (1'), the silicon oxide, hexagonal boron nitride, lithium nitride and carbon-containing additive are subjected to the second mixing; Wherein, the matrix also contains carbon element.
11. The method according to claim 9, characterized in that In step (2'), the pre-pressing pressure is ≥50 MPa.
12. The method according to claim 11, characterized in that The pre-pressing pressure is 50-300 MPa.
13. The method according to claim 11, characterized in that The ultra-high pressure treatment conditions are: pressure of 5-30 GPa; temperature of 1000-1800° C.; and time of 0.1-1 h.
14. A composite anode material for a lithium ion battery, characterized in that: The composite anode material contains the anode material described in any one of claims 1 to 6, or the anode material prepared by the method described in any one of claims 7 to 13 and a carbonaceous material.
Citation Information
Patent Citations
Boron nitride nanotube / silicon / carbon nanotube composite material and preparation and application
CN107863505A
Graphite powder of lithium ionic cell cathode and preparation thereof
CN101323447A
Boron-doped silicon-based composite anode material, preparation method and application thereof
CN110071272A
Negative electrode material, electrochemical device comprising negative electrode material and electronic device
CN110444750A