Pre-lithiation method of battery negative electrode, pre-lithiation negative electrode sheet and lithium-ion battery
By using aryl lithiation reagents to pre-lithiate the negative electrode sheets of lithium-ion batteries, the problems of low efficiency and complex operation in the existing technology are solved, the energy density and cycle life of lithium-ion batteries are improved, and the process safety is high , suitable for mass production.
Patent Information
- Application Number
- CN202110804983.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-07-16
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2041-07-16
AI Technical Summary
The existing lithium-ion battery negative electrode prelithiation method is inefficient, complex to operate and has harsh environmental requirements, and cannot be mass-produced.
An aryl lithiation reagent is used to pre-lithium the negative electrode sheet. By reacting metallic lithium with aromatic hydrocarbons in an inert atmosphere, a lithium salt solution containing aromatic hydrocarbons is generated, which is used to soak the negative electrode sheet to achieve pre-lithiumization of the negative electrode active material. ization to improve the first Coulombic efficiency and cycle performance of the battery.
It improves the first Coulomb efficiency and cycle performance of lithium-ion batteries, simplifies operation, reduces environmental requirements, and has a simple process and is easy for industrial application.
Smart Images

Figure BDA0003165996800000031 
Figure BDA0003165996800000041 
Figure BDA0003165996800000051
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of lithium-ion batteries, and in particular to a pre-lithiation method for a battery negative electrode, a pre-lithiation negative electrode sheet, and a lithium-ion battery. Background Art
[0002] Lithium-ion batteries have become one of the most widely used secondary batteries due to their high energy density, long cycle life, and no memory effect. With the development of economy and technology, industries such as portable electronic devices (such as mobile phones, tablets, etc.) and electric vehicles have put forward higher requirements for the energy density and cycle life of lithium-ion batteries. Among them, pre-replenishing lithium to the positive or negative electrode of the battery can compensate for the irreversible consumption of active lithium due to the formation of a solid electrolyte film (SEI film) on the electrode surface during the first charging process, thereby improving the battery's first coulomb efficiency and battery capacity, and then improving the battery's energy density and cycle life.
[0003] At present, it is common to pre-replenish lithium to the negative electrode of the battery. Usually, lithium metal is added as a lithium replenisher when making the negative electrode sheet. However, the chemical activity of the lithium replenisher for the negative electrode is usually very high, and the water and oxygen value in the environment must be strictly controlled. It is often incompatible with the water-based binder of the negative electrode and cannot be mass-produced. Summary of the invention
[0004] In view of this, the present application provides a highly feasible battery negative electrode pre-lithiation method to solve the problems of low efficiency, complex operation and strict requirements on the operating environment of existing negative electrode pre-lithiation methods.
[0005] Specifically, the first aspect of the present application provides a method for pre-lithiation of a negative electrode of a lithium-ion battery, comprising the following steps:
[0006] (1) under an inert atmosphere, adding metallic lithium to an organic solution of an aromatic hydrocarbon substance for reaction to obtain a solution containing an aromatic hydrocarbon lithium salt, that is, obtaining an aryl lithiation reagent; wherein the aromatic hydrocarbon substance comprises at least one of substituted fluorene and substituted or unsubstituted xanthene, the substituent in the substituted fluorene comprises at least one of an alkyl group, a cyanoalkyl group, an alkoxyalkyl group, an alkoxy group, and a phenyl group, and the substituent in the substituted xanthene comprises at least one of an alkyl group, an ester group, and a phenyl group;
[0007] (2) Immersing the negative electrode sheet for lithium-ion battery in the aryl lithiation reagent to perform a pre-lithiation reaction, then taking out the negative electrode sheet after the reaction, washing and drying it to obtain a pre-lithiation negative electrode sheet.
[0008] In the above-mentioned pre-lithiation method, an aryl lithiation reagent is used to treat the negative electrode sheet. The aryl lithiation reagent can better reduce the negative electrode active material, embed lithium ions in the negative electrode active material, and realize the pre-lithiation of the negative electrode sheet, thereby improving the first cycle coulomb efficiency of the battery assembled by the pre-lithiation negative electrode sheet and the positive electrode sheet, and improving its energy density and cycle performance. In addition, the aryl lithiation reagent has a mild nature, so that pre-lithiation can be achieved in a relatively safe environment with low operating requirements, and the process is simple, the lithiation depth is controllable, and it is easy to apply industrially.
[0009] More importantly, the aryl lithiation reagent used in the present application is different from the existing pre-lithiation reagent. It uses at least one of substituted fluorene and substituted or unsubstituted anthracene as a preparation raw material. The polycyclic aromatic conjugated structure in the raw material molecule can delocalize the outermost electrons of lithium to form a lithiation reagent containing aromatic hydrocarbon lithium salts; and the alkyl, cyanoalkyl, alkoxyalkyl, alkoxy, phenyl and other substituents on the obtained fluorene lithium salts have an electron-pushing effect, and the heteroatom oxygen on the anthracene lithium salts and the alkyl, ester, phenyl and other substituents on them all have an electron-pushing effect, which can be used to increase the lowest unoccupied orbital energy level of the aromatic hydrocarbon lithium salts, reduce its redox potential, and significantly increase its reduction ability. Therefore, the redox potential of the aryl lithiation reagent provided in the present application is relatively low, which is lower than the average lithium insertion potential of common negative electrode active materials, so that it can pre-lithiate a variety of negative electrode active materials, and can achieve good lithiation effects, such as shortening the pre-lithiation time, improving the pre-lithiation efficiency and lithiation depth. When the aromatic hydrocarbon material is a substituted fluorene, the redox potential of the obtained aryl lithium reagent is below 0.2 V (for Li / Li + ), which is lower than other common chemical lithiation reagents except elemental lithium.
[0010] In the present application, an alkyl group is a residual group after an alkane loses a hydrogen atom, and an alkoxy group can be regarded as an alkyl group connected with an ether bond (-O-). Wherein, the carbon number of the alkyl group is 1-10, and when the carbon number of the alkyl group is greater than or equal to 3, it can be a straight chain alkyl group or a branched chain alkyl group. Specifically, the alkyl group can be, for example, a methyl group, an ethyl group, a n-propyl group, an isopropyl group, a tert-butyl group, etc. In some embodiments, the carbon number of the alkyl group is 1-6, preferably 1-4. Similarly, the carbon number of the alkoxy group can be 1-10, 1-6 or 1-4. And when there are alkyl and alkoxy groups on fluorene and xanthene, the number of the two can be 1 or more (such as 2-4).
[0011] In the present application, alkoxyalkyl and cyanoalkyl are substituted alkyl groups. 1 -OR 2 , where R 1 is an alkylene group having 1 to 6 carbon atoms, R 2is an alkyl group having 1 to 6 carbon atoms, such as methoxymethyl, methoxyethyl, etc. Cyanoalkyl can be represented by -R 1 '-CN, R 1 ' can be an alkylene group having 1 to 6 carbon atoms, and further an alkylene group having 2 to 5 carbon atoms. The ester group can be represented by -COOR 3 , R 3 is an alkyl group having 1 to 6 carbon atoms, preferably an alkyl group having 1 to 4 carbon atoms. For example, the ester group may be a methyl formate group (-COOCH 3 ) or ethyl formate (-COOCH 2 CH 3 ).
[0012] Preferably, the substituents in the substituted fluorene include at least one of an alkyl group, an alkoxyalkyl group, and a cyanoalkyl group, and the substituents in the substituted xanthene include at least one of an alkyl group and an ester group. In some embodiments, the substituents in the substituted fluorene include at least one of a methyl group, an ethyl group, a tert-butyl group, a methoxymethyl group, and a cyanoethyl group, and the number of each substituent may be one or more. The substituents in the substituted xanthene include at least one of a methyl group, a tert-butyl group, a methyl formate group, and an ethyl formate group, and the number of each substituent may be one or more.
[0013] In the present application, the above-mentioned alkyl, cyanoalkyl, alkoxyalkyl, alkoxy, phenyl, ester and other groups will not react with metallic lithium, so that the stability of the obtained aryl lithium reagent is relatively high. Among them, the substituents in the substituted fluorene and substituted xanthene may also contain other active groups that do not react with lithium, such as hydroxyl (-OH), amino (-NH 2 ), carboxyl group (-COOH), aldehyde group (-CHO), inert groups other than halogen atoms, etc.
[0014] Exemplarily, the aromatic hydrocarbon substances may include at least one of the following (A)-(R):
[0015]
[0016]
[0017]
[0018] Among them, the substance represented by formula (A) is 1-methylfluorene, the substance represented by formula (B) is 2-ethylfluorene, the substance represented by formula (C) is 9,9-dimethylfluorene, the substance represented by formula (D) is 2,7-di-tert-butylfluorene, the substance represented by formula (E) is 9,9-dihexylfluorene, the substance represented by formula (F) is 9,9-dioctylfluorene, the substance represented by formula (G) is 9,9-di(2-cyanoethyl)fluorene, and the substance represented by formula (H) is 9-methoxy Methyl-fluorene, the substance represented by formula (I) is 9,9-bis(methoxymethyl)fluorene, the substance represented by formula (J) is 9,9-bis(methoxymethyl)-3,6-dimethylfluorene, the substance represented by formula (K) is 9,9-bis(methoxymethyl)-2,3,6,7-tetramethylfluorene, the substance represented by formula (L) is 9,9-bis(methoxymethyl)-4-tert-butylfluorene, and the substance represented by formula (M) is 2-methoxy-9,9-diphenylfluorene. The substance represented by formula (N) is xanthene (also known as oxanthene), the substance represented by formula (O) is 9,9-dimethylxanthene, the substance represented by formula (P) is 2,7-di-tert-butyl-9,9-dimethylxanthene, the substance represented by formula (Q) is xanthene-9-carboxylic acid methyl ester, and the substance represented by formula (R) is xanthene-9-carboxylic acid ethyl ester.
[0019] In the present application, the organic solution of aromatic hydrocarbons is obtained by dissolving aromatic hydrocarbons in an organic solvent. The preparation process of the organic solvent can be carried out in a dry environment to avoid introducing water into the prepared organic solution. Among them, the organic solvent is an aprotic solvent, which can specifically include one or more of tetrahydrofuran (THF), 2-methyltetrahydrofuran, N-methylpyrrolidone (NMP), ethylene glycol dimethyl ether (DME), diethylene glycol dimethyl ether, N,N-dimethylformamide (DMF), dimethyl sulfoxide (DMSO), etc., but is not limited thereto.
[0020] In step (1), the reaction of metallic lithium and aromatic hydrocarbon compounds is carried out under an inert atmosphere, and the inert atmosphere can be at least one of argon, helium, etc. The molar ratio of lithium element in the metallic lithium to the aromatic hydrocarbon compound can be (1-10):1. Preferably, the molar ratio is (1.2-10):1. In this case, the metallic lithium is excessive, which can ensure that the aromatic hydrocarbon compound is fully reacted, and the excess lithium is better removed. For example, when the metallic lithium is a lithium plate or lithium foil, the metallic lithium can be directly removed after the reaction is completed, or the reaction solution can be filtered.
[0021] Optionally, the reaction time in step (1) can be 30 min-6 h. Specifically, the reaction time can be 45 min, 1 h, 1.5 h, 2 h, 3 h, 4 h or 5 h. The reaction time can be adjusted according to the amount of metallic lithium and aromatic hydrocarbon substances. In addition, the reaction can be carried out at room temperature.
[0022] Optionally, in the aryl lithiation reagent, the concentration of the aromatic hydrocarbon lithium salt is 0.01-10 mol / L. At this concentration, the aryl lithiation reagent can fully pre-lithiate the negative electrode sheet, make the pre-lithiation uniform, and the pre-lithiation depth meets the requirements. The concentration can specifically be 0.05, 0.08, 0.1, 0.2, 0.5, 1, 2, 5, 8 or 9 mol / L.
[0023] In step (2), the negative electrode sheet generally includes a negative electrode current collector and a negative electrode material layer disposed on the negative electrode current collector, and the negative electrode material layer generally includes a negative electrode active material, a negative electrode binder and an optional conductive agent. Among them, the negative electrode active material includes one or more of carbon-based materials, silicon-based materials, tin-based materials, phosphorus-based materials, etc. Specifically, the carbon-based material may include graphite (such as natural graphite, artificial graphite), non-graphitized carbon (soft carbon, hard carbon), etc. Silicon-based materials may include one or more of elemental silicon, silicon-based alloys, silicon oxides, and silicon-carbon composite materials. Tin-based materials may include one or more of elemental tin, tin alloys, etc. Phosphorus-based materials may include one or more of red phosphorus, black phosphorus, and phosphorus-carbon composite materials, etc. Among them, the negative electrode binder may be selected from one or more of polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), polyacrylamide (PAM), polyacrylic acid (PAA), polyvinyl alcohol (PVA), sodium carboxymethyl cellulose (CMC), and styrene-butadiene rubber (SBR), etc., but is not limited thereto. The conductive agent may be a conventional material in the art, such as one or more of acetylene black, Ketjen black, Super P conductive carbon black, furnace black, carbon nanotubes, and the like.
[0024] In step (2), the reaction temperature of the pre-lithiation reaction can be 0-60°C, for example, 25-35°C. The reaction time of the pre-lithiation reaction can be 1 min-10 h. In some embodiments, the reaction time can be 1 min-5 h, and further can be 20 min-2 h. As mentioned earlier in this article, the aromatic lithiation reagent provided in the present application has a strong reducing ability, which can fully pre-embed lithium in the negative electrode sheet, improve the pre-lithiation efficiency and lithiation depth, and shorten the pre-lithiation time. By adjusting the temperature and reaction time of the pre-lithiation reaction, the degree of pre-lithiation can be controllably adjusted.
[0025] Optionally, in step (2), the molar ratio of the negative electrode active material in the negative electrode sheet to the lithium in the aryl lithiation reagent is 1:(1-10), ensuring that there is sufficient lithium source to achieve pre-lithiation of the negative electrode material. Specifically, the molar ratio is 1:1.2, 1:2, 1:3, 1:4, 1:5, 1:6, 1:7, 1:8 or 1:9, etc. In some embodiments, the molar ratio is 1:(1-8).
[0026] The negative electrode pre-lithiation method provided in the first aspect of the present application uses a mild and highly reducing aromatic lithiation reagent to pre-lithiate the negative electrode sheet. The pre-lithiation effect on the negative electrode sheet is good and the degree of lithiation is controllable. The pre-lithiation method has no strict requirements on the operating environment and has strong safety.
[0027] In a second aspect, the present application provides a pre-lithiation negative electrode sheet prepared by the pre-lithiation method described in the first aspect of the present application.
[0028] The pre-lithiation negative electrode sheet has been embedded with suitable lithium ions. During the first charging process of the lithium battery assembled using the pre-lithiation negative electrode sheet, the irreversible consumption of active lithium released from the positive electrode by the negative electrode can be reduced, the first coulombic efficiency and battery capacity of the battery can be improved, and thus the energy density and cycle performance of the battery can be improved.
[0029] In a third aspect, the present application provides a lithium-ion battery, comprising a positive electrode sheet, the pre-lithiated negative electrode sheet described in the second aspect, and a separator and an electrolyte located between the positive electrode sheet and the pre-lithiated negative electrode sheet.
[0030] The preparation method of the lithium ion battery comprises: stacking and assembling a positive electrode sheet, a separator and a pre-lithiated negative electrode sheet in sequence to obtain a battery core, accommodating the battery core in a battery shell, injecting an electrolyte, and then sealing the battery shell to obtain a lithium ion battery.
[0031] Compared with a battery assembled using a non-pre-lithiated negative electrode sheet, the first-cycle coulombic efficiency of the lithium-ion battery provided in the third aspect of the present application is greatly improved, which is beneficial to improving the battery capacity, energy density and cycle performance.
[0032] Advantages of the embodiments of the present application will be explained in the following description, and some of them are obvious from the description or can be learned through the implementation of the embodiments of the present application. DETAILED DESCRIPTION
[0033] The embodiments of the present application are further described below with reference to a plurality of embodiments.
[0034] Example 1
[0035] A method for pre-lithiation of a negative electrode sheet, comprising:
[0036] (1) in a dry environment, dispersing 1-methylfluorene in a solvent of ethylene glycol dimethyl ether (DME) to obtain a solution, adding metallic lithium in an amount equal to that of 1-methylfluorene to the solution, stirring and reacting at room temperature for 2 hours, and obtaining a DME solution of 1-methylfluorene lithium with a concentration of 1 mol / L, that is, obtaining an aryl lithium reagent;
[0037] (2) mixing a negative electrode active material (specifically carbon-coated silicon oxide), a conductive agent (specifically Super P), and a binder (specifically a mixture of SBR, CMC, and PAA) in a mass ratio of 90:5:5 to obtain a negative electrode slurry, coating the negative electrode slurry on a copper foil, and drying to obtain a negative electrode sheet;
[0038] (3) Under an argon atmosphere, immerse the above-mentioned negative electrode sheet in the aryl lithium reagent of step (1), control the molar ratio of the negative electrode active material to 1-methylfluorene lithium to be 1:2, and carry out a pre-lithiation reaction at a temperature of 25°C for 30 minutes. Take out the negative electrode sheet after the reaction, wash it with DME solvent for 3 times, and vacuum dry it to obtain a pre-lithiation negative electrode sheet.
[0039] An assembly of a lithium-ion battery, comprising:
[0040] Provide a lithium cobalt oxide positive electrode sheet, which is formed by coating LiCoO on an aluminum foil 2 , a conductive agent (specifically Super P), and a binder (specifically PVDF) are prepared in a mass ratio of 96:2:2 to form a positive electrode slurry, which is dried and pressed into sheets; the lithium cobalt oxide positive electrode sheet, the separator, and the pre-lithiation negative electrode sheet of Example 1 are stacked and assembled in sequence to form a battery cell, and the battery cell is contained in a battery housing, and an electrolyte is injected, and then the battery housing is sealed to obtain a full battery. After the formation and capacity division processes of the full battery are completed, the following electrochemical performance tests are carried out: first, charge to 4.1V at 1.3C, and charge to 1.0C at a constant voltage; then charge to 4.2V at 1.0C, and charge to 0.7C at a constant voltage; then charge to 4.3V at 0.7C, and charge to 0.4C at a constant voltage; then charge to 4.45V at 0.4C, and charge to 0.025C at a constant voltage; then discharge to 3.0V at 0.2C, and test its first-week coulomb efficiency and cycle performance.
[0041] After testing, the lithium-ion battery assembled with the pre-lithiated negative electrode sheet prepared in Example 1 has a first-week coulombic efficiency of 88.6%, and a capacity retention rate of 85.1% after 500 cycles at 25°C. However, the lithium-ion battery assembled with the negative electrode sheet that was not pre-lithiated under the same conditions has a first-week coulombic efficiency of only 65.7%, and a capacity retention rate of only 75.3% after 500 cycles at 25°C.
[0042] Example 2
[0043] A method for pre-lithiation of a negative electrode sheet, comprising:
[0044] (1) in a dry environment, dispersing 9,9-di(2-cyanoethyl)fluorene in a solvent of ethylene glycol dimethyl ether (DME) to obtain a solution, adding a metal lithium foil whose molar amount is twice that of the 9,9-di(2-cyanoethyl)fluorene to the solution, stirring and reacting at room temperature for 2 hours, filtering and removing the excess lithium foil, and obtaining a DME solution of 9,9-di(2-cyanoethyl)fluorene lithium with a concentration of 1 mol / L, that is, obtaining an aryl lithium reagent;
[0045] (2) mixing a negative electrode active material (specifically micron silicon), a conductive agent (specifically Super P), and a binder (specifically a mixture of SBR, CMC, and PAA) in a mass ratio of 90:5:5 to obtain a negative electrode slurry, coating the negative electrode slurry on a copper foil, and drying to obtain a negative electrode sheet;
[0046] (3) Under an argon atmosphere, immerse the above-mentioned negative electrode sheet in the aryl lithiation reagent of step (1), control the molar ratio of the negative electrode active material to 9,9-di(2-cyanoethyl)fluorene lithium to be 1:2, and carry out a pre-lithiation reaction at a temperature of 30° C. for 25 minutes. Take out the negative electrode sheet after the reaction, wash it with DME solvent for 3 times, and vacuum dry it to obtain a pre-lithiation negative electrode sheet.
[0047] According to the full battery assembly method described in Example 1, the pre-lithiated negative electrode sheet prepared in Example 2 was used to assemble a lithium-ion battery, and its first-week coulomb efficiency was measured to be 86.5%, and the capacity retention rate after 500 cycles at 25°C was 83.6%. However, the lithium-ion battery assembled using the negative electrode sheet that was not pre-lithiated under the same conditions had a first-week coulomb efficiency of only 61.3%, and a capacity retention rate after 500 cycles at 25°C was only 72.4%.
[0048] Example 3
[0049] A pre-lithiation method for a negative electrode of a lithium battery, which differs from Example 1 in that: 9,9-bis(methoxymethyl)fluorene shown in formula (I) is used to replace 1-methylfluorene; the molar ratio of the negative electrode active material to 9,9-bis(methoxymethyl)fluorene lithium is 1:4, and the pre-lithiation reaction is carried out at a temperature of 25°C for 10 minutes.
[0050] According to the full battery assembly method described in Example 1, the pre-lithiated negative electrode sheet prepared in Example 3 was used to assemble a lithium-ion battery, and its first-week coulombic efficiency was measured to be 89.1%, and the capacity retention rate after 500 cycles at 25°C was 87.8%.
[0051] Example 4
[0052] A method for pre-lithiation of a negative electrode of a lithium battery, which differs from Example 1 in that 2-methoxy-9,9-diphenylfluorene shown in formula (M) is used to replace 1-methylfluorene.
[0053] According to the full battery assembly method described in Example 1, the pre-lithiated negative electrode sheet prepared in Example 4 was used to assemble a lithium-ion battery, and its first-cycle coulombic efficiency was measured to be 87.3%.
[0054] Example 5
[0055] A method for pre-lithiation of a negative electrode of a lithium battery, which differs from Example 1 in that: 1-methylfluorene is replaced by xanthene represented by formula (N).
[0056] According to the full battery assembly method described in Example 1, the pre-lithiated negative electrode sheet prepared in Example 5 was used to assemble a lithium-ion battery, and its first-cycle coulomb efficiency was measured to be 85.2%, and the capacity retention rate after 500 cycles at 25°C was 80.8%.
[0057] Example 6
[0058] A method for pre-lithiation of a negative electrode of a lithium battery, which differs from Example 1 in that 2,7-di-tert-butyl-9,9-dimethylxanthene shown in formula (P) is used to replace 1-methylfluorene.
[0059] According to the full battery assembly method described in Example 1, the pre-lithiated negative electrode sheet prepared in Example 6 was used to assemble a lithium-ion battery, and its first-week coulombic efficiency was measured to be 86.1%, and the capacity retention rate after 500 cycles at 25°C was 83%.
[0060] Example 7
[0061] A method for pre-lithiation of a negative electrode of a lithium battery, which differs from Example 1 in that 1-methylfluorene is replaced by xanthene-9-carboxylic acid methyl ester represented by formula (Q).
[0062] According to the full battery assembly method described in Example 1, the pre-lithiated negative electrode sheet prepared in Example 7 was used to assemble a lithium-ion battery, and its first-week coulombic efficiency was measured to be 85.8%, and the capacity retention rate after 500 cycles at 25°C was 82.5%.
[0063] From the above exemplary embodiments, it can be seen that compared with the battery assembled from the negative electrode sheet that has not been pre-lithiated, the first-cycle coulombic efficiency of the battery is greatly improved after the negative electrode sheet is pre-lithiated with the aryl lithiation reagent provided in the present application and then assembled into a battery. This shows that the pre-lithiation method provided in the present application is more effective, simple, feasible and safe.
[0064] The above is an exemplary embodiment of the present application. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made thereto without departing from the principles of the present application. These improvements and modifications are also considered to be within the scope of protection of the present application.
Claims
1. A method for pre-lithiation of a negative electrode of a battery, characterized in that: The following steps are involved: Under an inert atmosphere, adding metallic lithium to an organic solution of an aromatic hydrocarbon substance for reaction to obtain a solution containing an aromatic hydrocarbon lithium salt, that is, obtaining an aryl lithiation reagent; wherein the aromatic hydrocarbon substance comprises at least one of substituted fluorene and substituted or unsubstituted xanthene, the substituent in the substituted fluorene comprises at least one of cyanoalkyl, alkoxyalkyl, alkoxy, and phenyl, and the substituent in the substituted xanthene comprises at least one of alkyl, ester, and phenyl; The negative electrode sheet for lithium-ion battery is immersed in the aryl lithiation reagent to carry out a pre-lithiation reaction, and then the negative electrode sheet after the reaction is taken out, washed and dried to obtain a pre-lithiation negative electrode sheet; wherein the molar ratio of the negative electrode active material in the negative electrode sheet to the lithium in the aryl lithiation reagent is 1: (1-10).
2. The pre-lithiation method according to claim 1, characterized in that The carbon number of the alkyl and alkoxy groups is 1-10, and the carbon number of the cyanoalkyl group is 2-7; the alkoxyalkyl group is represented by -R1-OR2, R1 is an alkylene group with 1-6 carbon atoms, and R2 is an alkyl group with 1-6 carbon atoms; the ester group is represented by -COOR3, and R3 is an alkyl group with 1-6 carbon atoms.
3. The pre-lithiation method according to claim 1, characterized in that The substituents in the substituted fluorene include at least one of an alkoxyalkyl group and a cyanoalkyl group, and the substituents in the substituted xanthene include at least one of an alkyl group and an ester group.
4. The pre-lithiation method according to claim 1, characterized in that The molar ratio of the lithium element in the metallic lithium to the aromatic hydrocarbon compound is (1-10):
1.
5. The pre-lithiation method according to claim 1, characterized in that: In the aryl lithiation reagent, the concentration of the aromatic hydrocarbon lithium salt is 0.01-10 mol / L.
6. The pre-lithiation method according to claim 1, characterized in that: The organic solvent contained in the organic solution of the aromatic hydrocarbon substance includes one or more of tetrahydrofuran, 2-methyltetrahydrofuran, N-methylpyrrolidone, ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, N,N-dimethylformamide, and dimethyl sulfoxide.
7. The pre-lithiation method according to claim 1, characterized in that: The reaction time of the pre-lithiation reaction is 1 min-10 h.
8. The pre-lithiation method according to any one of claims 1 to 7, characterized in that: The negative electrode active material in the negative electrode sheet includes one or more of carbon-based materials, silicon-based materials, tin-based materials, and phosphorus-based materials.
9. A pre-lithiation negative electrode sheet obtained by the pre-lithiation method according to any one of claims 1 to 8.
10. A lithium ion battery, characterized in that: It comprises a positive electrode sheet, a pre-lithiation negative electrode sheet as claimed in claim 9, and a separator and an electrolyte located between the positive electrode sheet and the pre-lithiation negative electrode sheet.
Citation Information
Patent Citations
Pre-lithiation method, pre-lithiation negative plate and lithium ion battery
CN113097451A