Diamine monomer, preparation method of diamine monomer, polyimide film, and preparation method of polyimide film
Through the new diamine monomer preparation method, the problems of high thermal expansion coefficient and insufficient mechanical properties of polyimide films in flexible OLED processes were solved, and polyimide films with low thermal expansion coefficient and high glass transition temperature were prepared. , suitable for high-temperature polysilicon-thin film transistor processing and flexible OLED display.
Patent Information
- Application Number
- CN202211396279.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-09
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2042-11-09
AI Technical Summary
The existing polyimide films have high thermal expansion coefficient, insufficient mechanical properties in the flexible OLED preparation process, and are complex in the process, making it difficult to meet the needs of high-temperature polysilicon-thin film transistor processing process.
The new diamine monomer N,N'-(2,7-to-one) bis(2 chloro-4 aminobenzamide) is used as the synthetic raw material for polyimide films, and the reaction of nitration, reduction and organic alkali Preparation is made to form a polyimide film with a low coefficient of thermal expansion and a high glass transition temperature.
The prepared polyimide film has low thermal expansion coefficient, high glass transition temperature and excellent mechanical properties, and is suitable for flexible OLED displays and other high heat resistant coating fields.
Smart Images

Figure QLYQS_1 
Figure QLYQS_2 
Figure QLYQS_3
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of high-performance organic thin films, and in particular to a diamine monomer, a method for preparing the diamine monomer, a polyimide film, and a method for preparing the polyimide film. Background Art
[0002] Polyimide (PI) is a type of polymer material containing an imide ring in its molecular chain. Polyimide is a type of special engineering plastic and has been widely used in the fields of civil high technology and national defense industry.
[0003] Polyimide can be synthesized and processed in a variety of ways to produce a variety of material forms such as films, resins, fibers, foams, and adhesives. Among them, polyimide films have excellent heat resistance, dimensional stability, dielectric properties, insulation, and self-extinguishing properties, and are mainly used in the insulation electrical and electronic fields.
[0004] In the 1960s, DuPont of the United States first developed the homophenylene polyimide film. With the rapid development of electronic communications, aerospace and other technologies, the demand for polyimide films is increasing. Japanese companies such as Ube Industries, Kaneka Chemical, Mitsubishi Gas, Mitsui Tosu, and South Korea's SKC have successively developed different types of polyimide films. In recent years, flexible organic light-emitting display (OLED) technology has gradually developed. With its advantages of fast response, low power consumption, wearable and foldable, it is one of the most competitive new display technologies in the future.
[0005] The development of flexible substrates is a key link in realizing flexible OLED displays. Polyimide has become the most promising application material in the field of flexible substrates due to its excellent comprehensive performance. The ideal PI substrate needs to meet the following requirements: 1) High heat resistance. The PI substrate needs to withstand the high temperature (300-500°C) of the low-temperature polysilicon-thin-film transistor (LTPS-TFT) processing process. The higher the processing temperature, the more complete the polysilicon crystallization and the better the TFT performance. At the same time, thermal decomposition should be avoided to contaminate the device. 2) Low coefficient of thermal expansion (CTE). The PI substrate needs to match the CTE value of the inorganic layer and metal layer in the device to reduce delamination and curling during processing.
[0006] Chinese patents CN111793207A, CN114106324A, CN114015091A, CN101407590A, CN109762335A, etc. reported that the introduction of new monomers, the drawing of thin films, and the preparation of inorganic-organic hybrid materials are the key to improving the glass transition temperature (T g ) and an effective way to reduce CTE.
[0007] However, the stretching involved in the above patent is not applicable to the flexible OLED preparation process, and doping with inorganic materials can only improve the polymer performance to a limited extent. There are also problems such as complex process and easy agglomeration. Therefore, it is of great significance to provide a preparation method of a polyimide film with wide applicability, and the polyimide film has the advantages of low thermal expansion coefficient, high glass transition temperature and excellent mechanical properties. Summary of the invention
[0008] The technical problem solved by the present invention is to provide a diamine monomer and a polyimide film. The diamine monomer provided in the present application, as a synthetic raw material for the polyimide film, has the characteristics of low thermal expansion coefficient, high glass transition temperature and excellent mechanical properties.
[0009] In view of this, the present application provides a diamine monomer as shown in formula (IV),
[0010]
[0011] The present application also provides a method for preparing the diamine monomer, comprising the following steps:
[0012] A) dissolving xanthenone in concentrated sulfuric acid, and then subjecting it to a nitration reaction to obtain a compound 1 as shown in formula (I);
[0013] B) subjecting the compound 1 to a reduction reaction to obtain a compound 2 as represented by formula (II);
[0014] C) reacting the compound II with 2-chloro-4-nitrobenzoyl halide under the action of an organic base to obtain a compound III as shown in formula (III);
[0015] D) subjecting the compound 3 to a reduction reaction to obtain a compound 4 as shown in formula (IV);
[0016]
[0017]
[0018] Preferably, in step A), the reagent for the nitration reaction is potassium nitrate, the mass of the concentrated sulfuric acid is 5 to 30 times that of the xanthones, the molar amount of the potassium nitrate is 2 to 5 times that of the xanthones, and the time of the nitration reaction is 3 to 15 hours; in step B), the reduction reaction adopts a neutral or acidic reduction system, the molar ratio of the reduction system to the compound one is (5 to 20): 1, the reaction temperature is 50 to 100°C, and the time is 5 to 36 hours.
[0019] Preferably, in step C), the 2-chloro-4-nitrobenzoyl halide is selected from 2-chloro-4-nitrobenzoyl chloride or 2-chloro-4-nitrobenzoyl bromide, the molar ratio of the 2-chloro-4-nitrobenzoyl halide to the compound II is (2-5):1, the organic base is selected from one or more of triethylamine, pyridine and isoquinoline, the molar ratio of the organic base to the compound II is (2.0-5.0):1, the reaction temperature is 10-50°C, and the reaction time is 5-24h.
[0020] Preferably, in step D), the reduction reaction adopts a neutral or acidic reduction system, the molar ratio of the reduction system to the compound three is (5-20):1, the reaction temperature is 50-100°C, and the reaction time is 5-36h.
[0021] The present application also provides a polyimide film, which is prepared from aromatic dianhydride and aromatic diamine; the aromatic diamine includes the diamine monomer described in the above scheme or the diamine monomer prepared by the preparation method.
[0022] Preferably, the aromatic dianhydride is selected from one or two of the structures shown in formula (V1) and formula (V2);
[0023]
[0024] Preferably, the aromatic diamine further comprises one or more structures shown in formula (VI1), formula (VI2), formula (VI3), formula (VI4), formula (VI5) and formula (VI6);
[0025]
[0026]
[0027] Preferably, the molar ratio of the aromatic dianhydride to the aromatic diamine is 0.9:1 to 1:0.9.
[0028] The present application also provides a method for preparing the polyimide film, comprising the following steps:
[0029] A) mixing an aromatic dianhydride and an aromatic diamine in an organic solvent, polymerizing, and obtaining a polyamic acid solution;
[0030] B) casting the polyamic acid solution into a film, and then sequentially drying, imidizing and curing to obtain a polyimide film.
[0031] The present application provides a diamine monomer as shown in formula (IV), which is specifically N,N'-(2,7-xanthenone)bis(2-chloro-4-aminobenzamide), wherein the xanthenone structure in the diamine monomer increases the rigidity of the molecular chain, the amide structure can form hydrogen bonds between the molecular chains, and the Cl group undergoes a cross-linking reaction at high temperature, further restricting the movement of the molecular chain, thereby improving the rigidity of the molecular main chain and the intermolecular interaction. Therefore, the diamine monomer provided in the present application is used to prepare a polyimide film, which has outstanding characteristics such as low thermal expansion coefficient, high glass transition temperature and excellent mechanical properties, and has potential application prospects in the fields of flexible OLED display, enameled wire, etc. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 The diamine monomer prepared in Example 1 of the present invention 1 H NMR and 13 C NMR spectrum;
[0033] Figure 2 Dynamic mechanical analysis (DMA) curves of the polyimide films prepared in Examples 2 to 5 of the present invention;
[0034] Figure 3 Thermomechanical analysis (TMA) curves of the polyimide films prepared in Examples 2 to 5 of the present invention. DETAILED DESCRIPTION
[0035] In order to further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples. However, it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, rather than limiting the claims of the present invention.
[0036] In view of the need for further development of polyimide films in the prior art and the limited improvement of the performance of polyimide films, this application introduces a new type of diamine monomer, which improves the rigidity of the molecular main chain and the intermolecular interaction by introducing xanthones, so that the prepared polyimide film has excellent mechanical properties, heat resistance and dimensional stability, and can be applied to flexible OLED substrates, enameled wires, high heat-resistant coatings and other fields. Specifically, the embodiment of the present invention discloses a diamine monomer as shown in formula (IV),
[0037]
[0038] The above-mentioned diamine monomer can be named N,N'-(2,7-xanthenone)bis(2-chloro-4-aminobenzamide), in which the xanthenone increases the rigidity of the molecular chain, and the amide structure can form hydrogen bonds between molecular chains. The Cl group can undergo cross-linking reaction at high temperature, further restricting the movement of the molecular chain, thereby significantly improving the rigidity and intermolecular effect of the diamine monomer.
[0039] The present application also provides a method for preparing a diamine monomer, comprising the following steps:
[0040] A) dissolving xanthenone in concentrated sulfuric acid, and then subjecting it to a nitration reaction to obtain a compound 1 as shown in formula (I);
[0041] B) subjecting the compound 1 to a reduction reaction to obtain a compound 2 as represented by formula (II);
[0042] C) reacting the compound II with 2-chloro-4-nitrobenzoyl halide under the action of an organic base to obtain a compound III as shown in formula (III);
[0043] D) subjecting the compound 3 to a reduction reaction to obtain a compound 4 as shown in formula (IV);
[0044]
[0045]
[0046] In the preparation process of the diamine monomer, the present application first dissolves xanthanone in concentrated sulfuric acid, and then performs a nitration reaction to obtain a compound 1 as shown in formula (I). In this process, the concentrated sulfuric acid is used as a solvent and a dehydrating agent; the reagent for the nitration reaction is potassium nitrate. The mass of the concentrated sulfuric acid is 5 to 30 times that of the xanthanone, the molar amount of the potassium nitrate is 2 to 5 times that of the xanthanone, and the time of the nitration reaction is 3 to 15 hours; specifically, the concentrated sulfuric acid is 10 to 26 times that of the xanthanone, the molar amount of the potassium nitrate is 3 to 5 times that of the xanthanone, and the time of the nitration reaction is 6 to 10 hours.
[0047] According to the present invention, the compound 1 is then subjected to a reduction reaction to obtain a compound 2 as shown in formula (II). In this process, the reduction reaction adopts a neutral or acidic reduction system, more specifically stannous chloride; the molar ratio of stannous chloride to the compound 1 is (5-20):1, specifically, the molar ratio of stannous chloride to the compound 1 is (8-12):1; the reaction temperature is 50-100°C, the time is 5-36h, specifically, the reaction temperature is 60-80°C, and the time is 10-24h. The above reduction reaction is carried out in an organic solvent, and the organic solvent is specifically selected from one or more of tetrahydrofuran, ethyl acetate, ethylene glycol dimethyl ether and 1,4-dioxane, and the mass ratio of the organic solvent to the compound 1 is (10-25):1.
[0048] Furthermore, the present application then reacts the compound II with 2-chloro-4-nitrobenzoyl halide under the action of an organic base to obtain a compound III as shown in formula (III). In this process, the 2-chloro-4-nitrobenzoyl halide is selected from 2-chloro-4-nitrobenzoyl chloride or 2-chloro-4-nitrobenzoyl bromide, and the organic base is selected from one or more of triethylamine, pyridine and isoquinoline. The molar ratio of the 2-chloro-4-nitrobenzoyl halide to the compound II is (2-5):1, specifically, the molar ratio of the 2-chloro-4-nitrobenzoyl halide to the compound II is (3-4):1; the molar ratio of the organic base to the compound II is (2.0-5.0):1, specifically, the molar ratio of the organic base to the compound II is (3.0-4.0):1; the reaction temperature is 10-50°C, and the reaction time is 5-24h, specifically, the reaction temperature is 20-30°C, and the reaction time is 10-24h.
[0049] Finally, the compound three is subjected to a reduction reaction to obtain a compound four as shown in formula (IV). In this process, the reduction reaction adopts a neutral or acidic reduction system, and specifically uses stannous chloride as a reducing agent. The molar ratio of stannous chloride to the compound three is (5-20):1, specifically, the molar ratio of stannous chloride to the compound three is (8-15):1; the reaction temperature is 50-100°C, the time is 5-36h, specifically, the reaction temperature is 60-80°C, and the time is 10-24h. The above reduction reaction is carried out in an organic solvent, and the organic solvent is specifically selected from one or more of tetrahydrofuran, ethyl acetate, ethylene glycol dimethyl ether and 1,4-dioxane, and the mass ratio of the organic solvent to the compound one is (10-25):1.
[0050] Furthermore, the present application also provides a polyimide film, which is prepared from aromatic dianhydride and aromatic diamine; the aromatic diamine includes the diamine monomer described in the above scheme or the diamine monomer prepared by the preparation method described in the above scheme.
[0051] In the polyimide film, the aromatic dianhydride is selected from one or two of the structures shown in formula (V1) and formula (V2);
[0052]
[0053] The aromatic diamine also includes one or more structures shown in formula (VI1), formula (VI2), formula (VI3), formula (VI4), formula (VI5) and formula (VI6);
[0054]
[0055] Furthermore, in the present application, the molar ratio of the aromatic dianhydride to the aromatic diamine is 0.9:1 to 1:0.9. More specifically, the molar ratio of the aromatic dianhydride to the aromatic diamine is 1:1.
[0056] The present application also provides a method for preparing a polyimide film, comprising the following steps:
[0057] A) mixing an aromatic dianhydride and an aromatic diamine in an organic solvent, polymerizing, and obtaining a polyamic acid solution;
[0058] B) casting the polyamic acid solution into a film, and then sequentially drying, imidizing and curing to obtain a polyimide film.
[0059] In the preparation process of the polyimide film, the polymerization temperature is -10 to 50°C and the time is 5 to 72 hours; specifically, the polymerization temperature is 20 to 40°C and the time is 10 to 36 hours. The organic solvent is a solvent for the resin of a person skilled in the art, and can be selected from polar aprotic solvents, more specifically one or more of DMF, DMAc, DMSO and NMP. The solid content of the polyamic acid solution is 5 to 25%.
[0060] After obtaining the polyamic acid solution, the film is cast and then heat treated. The heat treatment is divided into three stages. The first stage is the solvent volatilization stage. The treatment temperature is lower than 150°C. In this stage, the solvent volatilization mainly occurs. The second stage is the imidization stage. The treatment temperature is lower than 300°C. In this stage, the residual solvent volatilization and imidization reaction mainly occur. The third stage is the curing stage. The treatment temperature is higher than 300°C. In this stage, the molecular chain orientation rearrangement and intermolecular cross-linking reaction mainly occur. There is no special restriction on the heating temperature and heating time of the solvent volatilization stage and the imidization stage, while the temperature of the film curing stage is 320-380°C and the curing time is 0.5-1.5h.
[0061] In order to further understand the present invention, the preparation method of the diamine monomer, the polyimide film and the preparation method thereof provided by the present invention are described in detail below in conjunction with the embodiments. The protection scope of the present invention is not limited by the following embodiments.
[0062] Example 1
[0063] Dissolve 70g (0.36mol) of xanthanone in 1000mL of concentrated sulfuric acid, slowly add 151.7g of potassium nitrate, stir and react for 6 hours, then add into 2000mL of ice water, precipitate the compound of formula (Ⅰ), filter, wash with water and dry, the yield is 82%;
[0064] 70 g (0.25 mol) of the compound represented by the formula (I), 631.8 g (2.81 mol) of stannous chloride dihydrate and 1400 mL of ethyl acetate were added to a reaction bottle in sequence, stirred and reacted at 70°C for 10 hours, cooled to room temperature and filtered to obtain the compound represented by the formula (II), with a yield of 72%;
[0065] 22.6 g (0.10 mol) of the compound of formula (II), 66.0 g (0.30 mol) of 2-chloro-4-nitrobenzoyl chloride, 40.4 g (0.40 mol) of triethylamine, and 260 g of DMAc were added to a three-necked bottle, reacted at 10° C. for 24 hours, filtered, and dried to obtain the compound of formula (III) with a yield of 51%;
[0066] 8.91 g (0.015 mol) of the compound represented by the formula (III), 33.87 g (0.15 mol) of stannous chloride dihydrate and 180 mL of dioxane were added to the reaction bottle in sequence, stirred and reacted at 80° C. for 15 hours, cooled to room temperature and filtered to obtain the compound represented by the formula (IV), with a yield of 72%;
[0067]
[0068] The obtained compound of the structure shown in formula (IV) was characterized by nuclear magnetic resonance (NMR), and the result was: 1 H NMR (400MHz, DMSO) δ10.43 (s, 2H), 8.64 (s, 2H), 8.11 (d, J=9.1Hz, 2H), 7.68 (d, J=9 .1Hz, 2H), 7.34 (d, J=8.4Hz, 2H), 6.67 (s, 2H), 6.57 (d, J=8.4Hz, 2H), 5.84 (s, 4H). 13 C NMR (101MHz, DMSO) δ165.90, 152.17, 152.06, 136.27, 131.99, 131.16, 127.90, 122.94, 121.22, 119.08, 115.30, 114.08, 112.07.
[0069] Example 2
[0070] Into a three-necked round-bottom flask equipped with mechanical stirring and nitrogen protection, 2.18 g (0.01 mol) of pyromellitic dianhydride (PMDA), 5.34 g (0.01 mol) of a diamine having a structure represented by formula (IV), and 45 mL of DMAc were added, and the mixture was reacted at 20°C for 24 hours to obtain a light yellow polyamic acid solution; after coating on a glass plate, the solution was dried and thermally imidized, and then treated at 320°C for 1 hour in the curing stage to obtain a polyimide film.
[0071] Example 3
[0072] Into a three-necked round-bottom flask equipped with mechanical stirring and nitrogen protection, 2.18 g (0.01 mol) of pyromellitic dianhydride (PMDA), 5.34 g (0.01 mol) of a diamine having a structure represented by formula (IV), and 45 mL of DMAc were added, and the mixture was reacted at 20°C for 24 hours to obtain a light yellow polyamic acid solution; after coating on a glass plate, the solution was dried and thermally imidized, and then treated at 340°C for 1 hour in the curing stage to obtain a polyimide film.
[0073] Example 4
[0074] Into a three-necked round-bottom flask equipped with mechanical stirring and nitrogen protection, 2.18 g (0.01 mol) of pyromellitic dianhydride (PMDA), 5.34 g (0.01 mol) of a diamine having a structure represented by formula (IV), and 45 mL of DMAc were added, and the mixture was reacted at 20°C for 24 hours to obtain a light yellow polyamic acid solution; after coating on a glass plate, the solution was dried and thermally imidized, and then treated at 360°C for 1 hour in the curing stage to obtain a polyimide film.
[0075] Example 5
[0076] Into a three-necked round-bottom flask equipped with mechanical stirring and nitrogen protection, 2.18 g (0.01 mol) of pyromellitic dianhydride (PMDA), 5.34 g (0.01 mol) of a diamine having a structure represented by formula (IV), and 45 mL of DMAc were added, and the mixture was reacted at 20°C for 24 hours to obtain a light yellow polyamic acid solution; after coating on a glass plate, the solution was dried and thermally imidized, and then treated at 380°C for 1 hour in the curing stage to obtain a polyimide film.
[0077] Example 6
[0078] Into a three-necked round-bottom flask equipped with mechanical stirring and nitrogen protection, 2.94 g (0.01 mol) of biphenyltetracarboxylic dianhydride (BPDA), 5.34 g (0.01 mol) of a diamine having a structure represented by formula (IV), and 50 mL of DMAc were added, and the mixture was reacted at 20°C for 24 hours to obtain a light yellow polyamic acid solution; after coating on a glass plate, the solution was dried and thermally imidized, and then treated at 320°C for 1 hour in the curing stage to obtain a polyimide film.
[0079] Example 7
[0080] Into a three-necked round-bottom flask equipped with mechanical stirring and nitrogen protection, 2.94 g (0.01 mol) of biphenyltetracarboxylic dianhydride (BPDA), 5.34 g (0.01 mol) of a diamine having a structure represented by formula (IV), and 50 mL of DMAc were added, and the mixture was reacted at 20°C for 24 hours to obtain a light yellow polyamic acid solution; after coating on a glass plate, the solution was dried and thermally imidized, and then treated at 360°C for 1 hour in the curing stage to obtain a polyimide film.
[0081] Example 8
[0082] Into a three-necked round-bottom flask equipped with mechanical stirring and nitrogen protection, 2.18 g (0.01 mol) of pyromellitic dianhydride (PMDA), 2.67 g (0.005 mol) of a diamine having a structure represented by formula (Ⅳ), 1.13 g (0.005 mol) of a diamine having a structure represented by formula (Ⅵ2), and 36 mL of DMAc were added, and the mixture was reacted at 20°C for 24 hours to obtain a yellow polyamic acid solution; after coating on a glass plate, the solution was dried and thermally imidized, and then treated at 340°C for 1 hour in the curing stage to obtain a polyimide film.
[0083] Example 9
[0084] Into a three-necked round-bottom flask equipped with mechanical stirring and nitrogen protection, 2.18 g (0.01 mol) of pyromellitic dianhydride (PMDA), 2.67 g (0.005 mol) of a diamine having a structure represented by formula (Ⅳ), 1.13 g (0.005 mol) of a diamine having a structure represented by formula (Ⅵ4), and 36 mL of DMAc were added, and the mixture was reacted at 20°C for 24 hours to obtain a yellow polyamic acid solution; after coating on a glass plate, the solution was dried and thermally imidized, and then treated at 340°C for 1 hour in the curing stage to obtain a polyimide film.
[0085] The performance of the polyimide films prepared in Examples 2 to 9 was tested. The results are as follows: Figure 2 , Figure 3 As shown in Table 1;
[0086] Table 1 Polyimide film performance data table
[0087]
[0088] As can be seen from Table 1, the polyimide film prepared by the present invention has a glass transition temperature greater than 349°C, a thermal expansion coefficient of less than 25.9ppm / K at 50-350°C, a tensile strength greater than 109MPa, and a tensile modulus greater than 4.6GPa, and has very excellent comprehensive properties.
[0089] The above embodiments are only used to help understand the method and core idea of the present invention. It should be noted that, for those skilled in the art, several improvements and modifications can be made to the present invention without departing from the principles of the present invention, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.
[0090] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A method for preparing a polyimide film, comprising the following steps: Into a three-necked round-bottom flask equipped with mechanical stirring and nitrogen protection, 0.01 mol of pyromellitic dianhydride, 0.005 mol of a diamine having a structure represented by formula (IV), 0.005 mol of a diamine having a structure represented by formula (VI2), and 36 mL of DMAc were added, and the mixture was reacted at 20°C for 24 hours to obtain a yellow polyamic acid solution; after coating on a glass plate, the solution was dried and thermally imidized, and then treated at 340°C for 1 hour in the curing stage to obtain a polyimide film.
2. The preparation method according to claim 1, characterized in that: The method for preparing the diamine having the structure represented by formula (IV) comprises the following steps: A) dissolving xanthenone in concentrated sulfuric acid, and then subjecting it to a nitration reaction to obtain a compound 1 as shown in formula (I); B) subjecting the compound 1 to a reduction reaction to obtain a compound 2 as represented by formula (II); C) reacting the compound II with 2-chloro-4-nitrobenzoyl halide under the action of an organic base to obtain a compound III as shown in formula (III); D) subjecting the compound 3 to a reduction reaction to obtain a compound 4 as shown in formula (IV);