High-strength and plastic TB3 titanium alloy wire, heat treatment method and preparation method
Through the combined process of solid solution treatment, cold deformation, multilateral treatment and aging heat treatment, the problem of the elongation of TB3 titanium alloy wire material decreases when increasing the tensile strength, achieving a matching of high strength and good plasticity, meeting the new High-strength plastic fasteners for first-generation aircraft.
Patent Information
- Application Number
- CN202211407083.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-10
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2042-11-10
AI Technical Summary
While improving the tensile strength, the existing TB3 titanium alloy wire is difficult to maintain sufficient elongation, which cannot meet the dual requirements of high strength and shaping of the new generation of aircraft.
Using a combination of solid solution treatment, cold deformation, multilateralization treatment and aging heat treatment, including heating of rod or wire at 790-820°C, cold drawing of 30-50%, multilateralization treatment of 620-640°C and 550°C. Aging treatment, combined with air-cooling treatment, TB3 titanium alloy wire material with high tensile strength and good plasticity was prepared.
The tensile strength reaches 1280~1350MPa and the elongation rate is ≥10%, which significantly improves the strength and plasticity of the material, and meets the demand for high-strength plastic fasteners of the new generation of aircraft.
Smart Images

Figure CN115673009B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of titanium alloy preparation, and in particular to a high-strength and plastic TB3 titanium alloy wire, a heat treatment method and a preparation method. Background Art
[0002] TB3 (Ti-3.5Al-10Mo-8V-1Fe) alloy is a metastable β-type titanium alloy that can be heat-treated and strengthened. It is mainly used to manufacture 1100-1150MPa high-strength aerospace fastener materials with a service temperature below 300°C. With the implementation of the new generation of aircraft development projects, aircraft have higher and higher requirements on the mechanical properties, use functions and life of fasteners. It is hoped that the strength level can reach 1250MPa level while also having good shaping. Existing TB3 titanium alloy wire The tensile strength after solution aging is 1100-1180 MPa, and the elongation is 10-18%, which is difficult to reach the strength level required for the development of a new generation of aircraft.
[0003] Titanium alloy fasteners are widely used in aircraft bodies and aerospace vehicle connection structures. From fighter jets to transport aircraft to civil aviation aircraft, the number of titanium alloy fasteners used in a single aircraft ranges from tens of thousands to hundreds of thousands. Some aircraft use as many as 700,000 to 800,000 pieces. The amount is relatively large and it is also an important key material.
[0004] TB3 titanium alloy is a metastable β-type titanium alloy developed in China in the 1990s that can be strengthened by heat treatment. It has excellent comprehensive properties such as good corrosion resistance, high specific strength, aging strengthening and good room temperature plasticity. It is mainly used to manufacture 1100-1150MPa high-strength aerospace fasteners with a service temperature below 300°C. There are many studies on the hot processing and heat treatment process of this alloy in China, especially on the solid solution treatment and solid solution aging heat treatment process. A comparative study was also conducted on single-stage aging and double aging of wire (Liu Di, Liu Xiaohua, Zhang Chenhui, et al. Effect of aging process on the microstructure and mechanical properties of TB3 titanium alloy wire [J]. Casting Technology, 2017, 38(11): 2616-2618). The strength of single-stage aging can reach 1154MPa and the elongation can reach 12%, while the strength of double aging can reach 1127MPa and the elongation can reach 15%.
[0005] As we all know, the strength and plasticity of metal materials are in an inverse relationship, that is, increasing strength will lead to reduced plasticity, and increasing plasticity will also lead to reduced strength. Therefore, how to further significantly improve the strength of materials without reducing plasticity is not only the desired goal of material designers and users, but also the goal that material workers are constantly pursuing.
[0006] In order to improve the strength and plasticity of alloys, a lot of research has been conducted at home and abroad. Among them, the deformation heat treatment of titanium alloy is an effective method. For the deformation heat treatment process of TB3 alloy, there have been studies on the influence of pre-deformation (5%, 10% and 20% pre-deformation after solid solution) on the aging precipitation behavior and mechanical properties of TB3 alloy in China (such as: Song Zhenya, Sun Qiaoyan, Xiao Lin, et al. Effect of pre-deformation on aging precipitation behavior and mechanical properties of TB3 alloy [J]. Rare Metal Materials and Engineering, 2010, 39(05): 791-795). The study shows that the aging peak strength of the 5% pre-deformed sample is about 100MPa higher than that of the single-stage aging sample (although its aging peak strength also reaches 1350MPa, its elongation is close to 5%. In addition, its aging temperature is 500℃, which is far lower than the requirement of 550℃ specified in GJB 2219. Generally, the lower the aging temperature, the higher the strengthening effect, but the elongation also decreases rapidly). Summary of the invention
[0007] In view of this, it is necessary to provide a high-strength and plastic TB3 titanium alloy wire, a heat treatment method and a preparation method.
[0008] A high-strength and plastic TB3 titanium alloy wire material, with an elongation of ≥10% and a tensile strength of ≥1280MPa.
[0009] A high-strength and plastic TB3 titanium alloy wire heat treatment method comprises the following steps:
[0010] Solution treatment: Heat the billet to a temperature of 790-820°C, keep warm for 10-20 minutes, and then air cool.
[0011] Cold deformation: cold drawing of 30-50% of the solution treated bar or wire blank to produce semi-finished products;
[0012] Polygonal treatment: Heat the cold-deformed semi-finished product to a temperature of 620-640°C, keep it warm for 15 minutes, and then air-cool it;
[0013] Aging heat treatment: The semi-finished product after polygonal treatment is heated to 550°C, kept at this temperature for 16 hours, and then air-cooled.
[0014] A method for preparing a high-strength and plastic TB3 titanium alloy wire comprises the following steps:
[0015] Prepare the billet: Rod or wire blank;
[0016] Solution treatment: Heat the rod or wire blank to a temperature of 790-820°C, keep warm for 10-20 minutes, and then air cool.
[0017] Cold deformation: cold drawing of 30-50% of the solution treated bar or wire blank to produce semi-finished products;
[0018] Polygonal treatment: Heat the cold-deformed semi-finished product to a temperature of 620-640°C, keep it warm for 15 minutes, and then air-cool it;
[0019] Aging heat treatment: The semi-finished product after polygonal treatment is heated to 550°C, kept at this temperature for 16 hours, and then air-cooled.
[0020] Beneficial effect: CN110773686A relates to a method for preparing TB3 titanium alloy wire for fasteners. The patent straightens the wire after solid solution treatment to obtain Although the patent records that the prepared TB3 titanium alloy wire has a tensile strength of more than 1100MPa and an elongation of more than 6%, the analysis of its embodiments (as shown in Table 1 below) shows that when the elongation is greater than 10%, the tensile strength drops to 1170MPa, and when the tensile strength is 1201, the elongation can only reach 7%. Obviously, the strength and shaping parameters of the titanium alloy wire described in the background technology are in an inverted relationship at this level. With the increase of tensile strength, the elongation decreases significantly, and its elongation can no longer meet the requirements of GJB-2219.
[0021] Table 1
[0022] Diameter / mm Tensile strength / MPa Elongation / % Example 1 3 1201 7 Example 2 3.5 1185 9 Example 3 4 1170 12 Example 4 5 1145 15
[0023] The TB3 titanium alloy wire prepared by the heat treatment process of the present invention has a tensile strength of 1250-1350 MPa under the premise of elongation ≥10%. The wire has both high strength and good plasticity, achieving a good match between high strength and good plasticity, and fully meeting the demand for high-strength plastic fasteners in the development of a new generation of aircraft.
[0024] Compared with the prior art, the present invention has the following advantages:
[0025] (1) High strength: The tensile strength reaches 1280-1350 MPa, and the tensile strength is increased by 15-23%. The national military standard "GJB2219-94 Titanium and Titanium Alloys for Fasteners" stipulates that the tensile strength of TB3 after solid solution + aging treatment is ≥1100 MPa and the elongation is ≥10%. The typical value of the tensile strength is 1140 MPa. The tensile strength of the present invention is increased by 12-18% compared with the typical value.
[0026] (2) Good shaping: elongation ≥ 10%. On the basis of a significant increase in tensile strength, the elongation decreases less. According to the embodiments, some parts still maintain the same level.
[0027] (3) Good matching of strength and plasticity: A good match between high strength and good plasticity is achieved, with excellent overall performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 , heat treatment system curve diagram of the present invention. DETAILED DESCRIPTION
[0029] The method for preparing the TB3 titanium alloy wire proposed in the present invention comprises the following steps:
[0030] Preparation of rod blanks (or wire blanks): The preparation of blank specifications must be based on the finished product specifications Calculate forward and consider the 0.02mm margin removed by grinding and polishing, so the blank should be processed according to the 30-50% cold deformation amount. The semi-finished product size is calculated forward. Therefore, the size range of the calculated blank is
[0031] Solution treatment (ST): The bar billet is heated to a temperature of 790-820°C, kept warm for 10-20 minutes, and then air-cooled;
[0032] Cold work (CW): For solution treated The rod or wire blank is cold drawn 30-50% to the semi-finished product size
[0033] Polygonization heat treatment (PHT): The cold-deformed semi-finished product is heated to a temperature of 620-640°C, kept warm for 15 minutes, and then air-cooled;
[0034] Aging heat treatment (A): The semi-finished product after polygonal treatment is heated to 550°C, kept at this temperature for 16 hours, and then air cooled (AC).
[0035] Finishing: Straighten the aged wire and then grind and polish it to the finished size After further sawing, flattening and collection, the finished straight wire is obtained.
[0036] The diameter range of the TB3 titanium alloy wire of the present invention is 1.88 to 7.88 mm (for example, the typical diameter specifications of the wire are φ4.88, φ6.88, φ7.88mm), elongation ≥10%, and tensile strength ≥1280MPa.
[0037] Example 1 TB3 wire Wire
[0038] (1) Billet preparation: Billet specifications must be prepared based on finished product specifications Calculate forward and consider the 0.02mm margin removed by grinding and polishing. According to the 50% cold deformation of the blank, The semi-finished product size is calculated forward. Therefore, the calculated size of the blank is
[0039] (2) Solution treatment: The rod blank is heated to 820°C, kept warm for 20 minutes and then air-cooled.
[0040] (3) Cold deformation: for solution treated The bar blank is cold drawn 50% to semi-finished product size
[0041] (4) Polygonalization: The 7.9 mm semi-finished product was heated to 640°C, kept at this temperature for 15 minutes, and then air-cooled.
[0042] (5) Aging heat treatment: The semi-finished product after polygonal treatment is heated to 550°C, kept at this temperature for 16 hours, and then air-cooled.
[0043] (6) Finishing: Straighten the wire after aging, and then grind and polish it to the finished size Then it is sawed, flattened and collected as finished straight wire strips.
[0044] (7) Finished product performance testing: Room temperature mechanical properties: tensile strength is 1349 MPa, elongation is 11.6%.
[0045] Example 2 TB3 wire Wire
[0046] (1) Billet preparation: Billet specifications must be prepared based on finished product specifications Calculate forward and consider the 0.02mm margin removed by grinding and polishing. According to the 40% cold deformation of the blank, The semi-finished product size is calculated forward. Therefore, the calculated size of the blank is
[0047] (2) Solution treatment: The billet is heated to 800°C, kept at this temperature for 16 minutes and then air-cooled.
[0048] (3) Cold deformation: for solution treated The bar blank is cold drawn 40% to semi-finished product size
[0049] (4) Polygonalization: The 5.9 mm semi-finished product was heated to 630°C, kept at this temperature for 15 minutes, and then air-cooled.
[0050] (5) Aging heat treatment: The semi-finished product after polygonal treatment is heated to 550°C, kept at this temperature for 16 hours, and then air-cooled.
[0051] (6) Finishing: Straighten the wire after aging, and then grind and polish it to the finished size Then it is sawed, flattened and collected as finished straight wire strips.
[0052] (7) Finished product performance testing: Room temperature mechanical properties: tensile strength is 1318 MPa, elongation is 12.1%.
[0053] Example 3 TB3 wire Wire
[0054] (1) Billet preparation: Billet specifications must be prepared based on finished product specifications Calculate forward and consider the 0.02mm margin removed by grinding and polishing. According to the 30% cold deformation of the blank, The semi-finished product size is calculated forward. Therefore, the calculated size of the blank is
[0055] (2) Solution treatment: The rod blank is heated to 790°C, kept warm for 10 minutes and then air-cooled.
[0056] (3) Cold deformation: for solution treated The bar blank is cold drawn by 30% to the semi-finished product size
[0057] (4) Polygonalization: The 1.9 mm semi-finished product was heated to 620°C, kept at this temperature for 15 minutes, and then air-cooled.
[0058] (5) Aging heat treatment: The semi-finished product after polygonal treatment is heated to 550°C, kept at this temperature for 16 hours, and then air-cooled.
[0059] (6) Finishing: Straighten the wire after aging, and then grind and polish it to the finished size Then it is sawed, flattened and collected as finished straight wire strips.
[0060] (7) Finished product performance testing: Room temperature mechanical properties: tensile strength is 1312MPa, elongation is 12.3%.
[0061] Comparative Example 1 TB3 wire Wire
[0062] The process used in this comparative example is the process of Example 1, without cold deformation and polygonization treatment, and the product formation test obtains the data shown in the following table.
[0063] Comparative Example 2 TB3 wire Wire
[0064] The process used in this comparative example is the process of Example 2, without cold deformation and polygonization treatment, and the product formation test obtains the data shown in the following table.
[0065] Comparative Example 3 TB3 wire Wire
[0066] The process used in this comparative example is the process in Example 3, without cold deformation and polygonization treatment, and the product formation test obtained the data shown in the following table.
[0067] Figure 1 The heat treatment system curve diagram of the present invention is shown in Table 2.
[0068]
[0069] Note: In the table, ST is solution treatment; STA is solution treatment + aging treatment; CW is cold deformation; PHT is polygonal heat treatment; A is aging treatment.
[0070] As can be seen from the figure, the heat treatment method adopted in the embodiment of the present invention is solution treatment + cold deformation (pre-deformation) + polygonal treatment + aging treatment. On the basis of the existing technology, cold deformation and polygonal heat treatment processes are added, and the deformation amount of cold deformation reaches 30-50%, which is much greater than the level of existing technology research. Through the research of this heat treatment process, under the premise of achieving elongation ≥10%, the tensile strength reaches 1280-1350MPa. The prepared wire has both high strength and good plasticity, achieving a good match between high strength and good plasticity, and forming a titanium alloy wire with excellent comprehensive performance.
[0071] What is disclosed above is only a preferred embodiment of the present invention, which certainly cannot be used to limit the scope of rights of the present invention. A person skilled in the art can understand that all or part of the processes of the above embodiments and equivalent changes made according to the claims of the present invention still fall within the scope of the invention.
Claims
1. A high-strength and plastic TB3 titanium alloy wire heat treatment method, characterized in that The following steps are involved: Solution treatment: Heat the billet to a temperature of 790-820°C, keep warm for 10-20 minutes, and then air cool. Cold deformation: 30~50% cold drawing is performed on the solution treated bar blank to process it into semi-finished products; Polygonal treatment: Heat the cold-deformed semi-finished product to a temperature of 620-640°C, keep it warm for 15 minutes, and then air-cool it; Aging heat treatment: The semi-finished product after polygonal treatment is heated to 550°C, kept at this temperature for 16 hours, and then air-cooled.
2. A method for preparing high-strength and plastic TB3 titanium alloy wire, characterized in that: Prepare the bar blank: select the bar blank of φ2.28~φ11.15mm; Solution treatment: Heat the billet to 790-820°C, keep warm for 10-20 minutes and then air cool. Cold deformation: 30~50% cold drawing is performed on the solution treated bar blank to process it into semi-finished products; Polygonal treatment: Heat the cold-deformed semi-finished product to a temperature of 620-640°C, keep it warm for 15 minutes, and then air-cool it; Aging heat treatment: The semi-finished product after polygonal treatment is heated to 550°C, kept at this temperature for 16 hours, and then air-cooled.
3. The method for preparing the high-strength and plastic TB3 titanium alloy wire according to claim 2, characterized in that: The selection method of the rod blank is: calculate forward from the finished product specification φ1.88~φ7.88mm, consider the 0.02mm margin removed by grinding and polishing, and calculate forward according to the blank being processed by 30~50% cold deformation to the semi-finished product size of φ1.9~φ7.9mm.