Preparation method and application of porous sheet-like cobalt tetroxide

By using a reaction method of mixing cobalt-containing reagents and alkaline reagents in the positive electrode material of lithium battery, porous sheet-like cobalt tetroxide is prepared, which solves the problem of long-term, low-cost and high-quality process in the prior art, and improves the coating performance and material performance.

CN115676908BActive Publication Date: 2024-11-22GUIZHOU YAYOU NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211450731.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-18
Publication Date
2024-11-22
Estimated Expiration
2042-11-18

AI Technical Summary

Technical Problem

The existing cobalt tetroxide preparation method has long process routes, low production efficiency and high cost, and cannot meet the coating requirements of nano-level cobalt tetroxide additives in the positive electrode materials of lithium battery.

Method used

The mixture of cobalt-containing reagents and alkaline reagents are used to react in the solvent, and after solid-liquid separation and calcination, a porous sheet-like cobalt tetroxide is formed, simplifying the process route and improving production efficiency.

Benefits of technology

The preparation of nanosheet-shaped cobalt tetroxide is realized, which improves the coating performance, reduces costs, and improves the cycleability and service life of the cathode material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115676908B_ABST
    Figure CN115676908B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for preparing porous flaky cobalt oxide and its application. The method for preparing the porous flaky cobalt oxide comprises the following steps: S1: mixing a cobalt-containing reagent and an alkaline reagent in a solvent, and performing solid-liquid separation after the reaction to obtain a solid material; S2: calcining the solid material to obtain the porous flaky cobalt oxide. The method for preparing porous flaky cobalt oxide of the present invention has the advantages of short process route, high production efficiency, low cost, simple operation and stable product quality.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field related to battery positive electrode material additives, and in particular to a preparation method and application of porous sheet-like cobalt tetroxide. Background Art

[0002] The solid phase production method is used in the production of lithium cobalt oxide and high nickel ternary materials, which are positive electrode materials for lithium batteries. In order to reduce the excess lithium elements in lithium cobalt oxide and high nickel ternary materials and improve the cyclability and service life of the positive electrode materials, the production and processing technology adopts a lithium-rich calcination process. In this process, nano-scale additives need to be added to the semi-finished products during the secondary calcination process to achieve the purpose of reducing the excess lithium in lithium cobalt oxide and high nickel ternary materials.

[0003] The existing conventional system for preparing cobalt tetroxide is mostly a conventional carbonate precipitation system, and the crystal structure is mostly spheroidized or cubic crystals, and multiple crystals are spherical large particles. If crushing and depolymerization are adopted, nanometer small particles can be obtained, but the crushing cost is high, the uniformity of the discharging particles is poor, and the physical and chemical requirements of the existing materials for the coating material cannot be met, so finding a sheet-like single crystal structure cobalt tetroxide is the best way to solve this problem. In order to adapt to the development of positive electrode materials, adding nanometer-level cobalt tetroxide additives with coating performance is becoming a trend of development. However, the existing nanometer-level cobalt tetroxide preparation method has a long process route, low production efficiency and high cost, which is not conducive to the practical application of nanometer-level cobalt tetroxide additives.

[0004] Therefore, a new method for preparing cobalt tetroxide is urgently needed to solve the above problems. Summary of the invention

[0005] The first technical problem to be solved by the present invention is:

[0006] Provided is a method for preparing porous sheet-like cobalt tetroxide.

[0007] The second technical problem to be solved by the present invention is:

[0008] Application of the method.

[0009] In order to solve the first technical problem, the technical solution adopted by the present invention is:

[0010] A method for preparing porous sheet-like cobalt oxide comprises the following steps:

[0011] S1: mixing a cobalt-containing reagent and an alkaline reagent in a solvent, and performing solid-liquid separation after the reaction to obtain a solid material;

[0012] S2: calcining the solid material to obtain the porous sheet-like cobalt oxide.

[0013] According to the embodiments of the present invention, one of the technical solutions has at least one of the following advantages or beneficial effects:

[0014] 1. The method for preparing porous sheet-like cobalt oxide of the present invention can realize unidirectional growth of particles to form nanosheets, making the cobalt oxide more suitable for rear-end coating, thereby improving the performance of the positive electrode material after coating.

[0015] 2 The method for preparing porous sheet-like cobalt tetroxide of the present invention has the advantages of short process route, high production efficiency, low cost, simple operation and stable product quality.

[0016] According to one embodiment of the present invention, the method for preparing the cobalt-containing reagent comprises the following steps: mixing a cobalt salt and a solvent in a weight ratio of 400-800:1000-1200 to obtain the cobalt-containing reagent.

[0017] According to one embodiment of the present invention, in the cobalt-containing reagent, the C O 2+ The mass concentration is greater than or equal to 100g / L.

[0018] According to one embodiment of the present invention, the C O 2+ The mass concentration is 100-120g / L.

[0019] According to one embodiment of the present invention, the alkaline agent includes at least one of sodium hydroxide, calcium hydroxide and potassium hydroxide.

[0020] According to one embodiment of the present invention, the alkaline reagent is an alkaline solution, and the mass percentage of the solute in the alkaline solution is greater than 31%; preferably, the mass percentage of the solute is 31.5-32.5%.

[0021] According to one embodiment of the present invention, when the alkaline reagent is an alkaline solution, the volume ratio of the alkaline solution to the cobalt-containing reagent is 7-9:20-30, preferably, 7-8:20-21.

[0022] According to one embodiment of the present invention, step S1 further includes a stirring step, wherein the stirring speed is greater than 300 rpm, preferably 300-400 rpm.

[0023] According to one embodiment of the present invention, in step S1, the reaction time is 0.5 to 2 hours, preferably, the reaction time is 30 to 40 minutes.

[0024] According to one embodiment of the present invention, in step S1, the reaction temperature is lower than 50°C, preferably, the reaction temperature is 30-40°C.

[0025] According to one embodiment of the present invention, the calcination temperature is less than 700°C.

[0026] According to one embodiment of the present invention, the calcination temperature is 500-600°C.

[0027] According to one embodiment of the present invention, the method further comprises the step of crushing the obtained porous flaky cobalt oxide, and the crushing equipment is a jet mill.

[0028] Another aspect of the present invention also relates to the application of the method for preparing the porous sheet-like cobalt oxide in the preparation of positive electrode materials for batteries. The method includes the method for preparing the porous sheet-like cobalt oxide as described in the first embodiment. Since the application adopts all the technical solutions of the method of the above embodiment, it at least has all the beneficial effects brought by the technical solutions of the above embodiment.

[0029] Other features and advantages of the present invention will be set forth in the description which follows, and in part will be apparent from the description, or may be learned by practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0031] Figure 1 This is a flow chart of the method for preparing porous sheet-like cobalt tetroxide in Example 1.

[0032] Figure 2 This is the SEM image of the porous sheet-like cobalt oxide prepared in Example 1.

[0033] Figure 3 The XRD pattern of the porous sheet-like cobalt tetroxide prepared in Example 1. DETAILED DESCRIPTION

[0034] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of the present invention.

[0035] In the examples, the alkaline solution is a sodium hydroxide solution purchased from Hubei Adama Pharmaceutical Co., Ltd. or Hengyang Jiantao Chemical Co., Ltd.

[0036] In the examples, cobalt chloride hexahydrate was purchased from Ganzhou Tengyuan Cobalt New Materials Co., Ltd. or Guangdong Jiana Energy Technology Co., Ltd.

[0037] In the embodiment, the reaction formula of the alkaline solution and the cobalt-containing reagent is: NaOH+CoCl 2 →Co(OH) 2 +NaCl.

[0038] In the embodiment, the filter cake material is placed in a muffle furnace with a set temperature of 550°C and calcined to obtain the chemical formula: Co(OH) 2 →Co 3 O 4 +H 2 O.

[0039] Example 1

[0040] A method for preparing porous sheet-like cobalt trioxide, such as Figure 1 As shown, the following steps are included:

[0041] (1) adding 454 g of cobalt chloride hexahydrate to 1 liter of water to prepare a cobalt-containing reagent;

[0042] (2) 800 ml of alkaline solution (mass percent concentration of 31.5%) and 1000 ml of water were used as the reaction base solution, stirred at 350 rpm at 30° C., and 2100 ml of the cobalt-containing reagent was added within 35 min;

[0043] (3) After the reaction is completed, the material is stirred for 30 minutes, and then put into a filter press for washing, and 4.5 liters of pure water is used for washing;

[0044] (4) The filter cake material is placed in a muffle furnace set at 550°C and calcined for 6 hours;

[0045] (5) The calcined material is crushed and depolymerized using a jet mill to obtain a porous flake-like cobalt oxide. The SEM image of the porous flake-like cobalt oxide is shown in FIG. Figure 2 As shown, the XRD pattern of the porous sheet-like cobalt tetraoxide is as follows Figure 3 shown.

[0046] Example 2

[0047] A method for preparing porous sheet-like cobalt oxide comprises the following steps:

[0048] (1) adding 454 g of cobalt chloride hexahydrate to 1 liter of water to prepare a cobalt-containing reagent;

[0049] (2) 800 ml of alkaline solution (mass percent concentration of 31.5%) and 1000 ml of water were used as the reaction base solution, stirred at 350 rpm at 40° C., and 2100 ml of the cobalt-containing reagent was added within 35 min;

[0050] (3) After the reaction is completed, the material is stirred for 30 minutes, and then put into a filter press for washing, and 4.5 liters of pure water is used for washing;

[0051] (4) The filter cake material is placed in a muffle furnace set at 550°C and calcined for 6 hours;

[0052] (5) The calcined material is crushed and depolymerized using a jet mill to obtain porous flake-like cobalt trioxide.

[0053] Example 3

[0054] A method for preparing porous sheet-like cobalt oxide comprises the following steps:

[0055] (1) adding 454 g of cobalt chloride hexahydrate to 1 liter of water to prepare a cobalt-containing reagent;

[0056] (2) 800 ml of alkaline solution (mass percent concentration of 32.5%) and 1000 ml of water were used as the reaction base solution, stirred at 350 rpm at 30° C., and 2100 ml of the cobalt-containing reagent was added within 35 min;

[0057] (3) After the reaction is completed, the material is stirred for 30 minutes, and then put into a filter press for washing, and 4.5 liters of pure water is used for washing;

[0058] (4) The filter cake material is placed in a muffle furnace set at 550°C and calcined for 6 hours;

[0059] (5) The calcined material is crushed and depolymerized using a jet mill to obtain porous flake-like cobalt trioxide.

[0060] Example 4

[0061] A method for preparing porous sheet-like cobalt oxide comprises the following steps:

[0062] (1) adding 454 g of cobalt chloride hexahydrate to 1 liter of water to prepare a cobalt-containing reagent;

[0063] (2) 800 ml of alkaline solution (mass percent concentration of 31.5%) and 1000 ml of water were used as the reaction base solution, stirred at 350 rpm at 30° C., and 2100 ml of the cobalt-containing reagent was added within 35 min;

[0064] (3) After the reaction is completed, the material is stirred for 30 minutes, and then put into a filter press for washing, and 4.5 liters of pure water is used for washing;

[0065] (4) The filter cake material is placed in a muffle furnace with a set temperature of 500°C and calcined for 6 hours;

[0066] (5) The calcined material is crushed and depolymerized using a jet mill to obtain porous flake-like cobalt trioxide.

[0067] Example 5

[0068] A method for preparing porous sheet-like cobalt oxide comprises the following steps:

[0069] (1) adding 454 g of cobalt chloride hexahydrate to 1 liter of water to prepare a cobalt-containing reagent;

[0070] (2) 700 ml of alkaline solution (mass percent concentration of 31.5%) and 1000 ml of water were used as the reaction base solution, stirred at 350 rpm at 30° C., and 2100 ml of the cobalt-containing reagent was added within 35 min;

[0071] (3) After the reaction is completed, the material is stirred for 30 minutes, and then put into a filter press for washing, and 4.5 liters of pure water is used for washing;

[0072] (4) The filter cake material is placed in a muffle furnace set at 550°C and calcined for 6 hours;

[0073] (5) The calcined material is crushed and depolymerized using a jet mill to obtain porous flake-like cobalt trioxide.

[0074] Example 6

[0075] A method for preparing porous sheet-like cobalt oxide comprises the following steps:

[0076] (1) adding 454 g of cobalt chloride hexahydrate to 1 liter of water to prepare a cobalt-containing reagent;

[0077] (2) 900 ml of alkaline solution (mass percent concentration of 31.5%) and 1000 ml of water were used as the reaction base solution, stirred at 350 rpm at 30°C, and 2100 ml of cobalt solution was added within 35 minutes.

[0078] (3) After the reaction is completed, the material is stirred for 30 minutes, and then put into a filter press for washing, and 4.5 liters of pure water is used for washing;

[0079] (4) The filter cake material is placed in a muffle furnace with a set temperature of 550°C and calcined for 6 hours.

[0080] (5) The calcined material is crushed and depolymerized using a jet mill to obtain porous flake-like cobalt trioxide.

[0081] Example 7

[0082] A method for preparing porous sheet-like cobalt oxide comprises the following steps:

[0083] (1) adding 454 g of cobalt chloride hexahydrate to 1 liter of water to prepare a cobalt-containing reagent;

[0084] (2) 700 ml of alkaline solution (mass percent concentration of 31.5%) and 1000 ml of water were used as the reaction base solution, stirred at 350 rpm at 30°C, and 2100 ml of cobalt solution was added within 35 minutes.

[0085] (3) After the reaction is completed, the material is stirred for 30 minutes, and then put into a filter press for washing, and 4.5 liters of pure water is used for washing;

[0086] (4) The filter cake material is placed in a muffle furnace with a set temperature of 550°C and calcined for 6 hours.

[0087] (5) The calcined material is crushed and depolymerized using a jet mill to obtain porous flake-like cobalt trioxide.

[0088] Example 8

[0089] A method for preparing porous sheet-like cobalt oxide comprises the following steps:

[0090] (1) adding 454 g of cobalt chloride hexahydrate to 1 liter of water to prepare a cobalt-containing reagent;

[0091] (2) 800 ml of alkaline solution (mass percent concentration of 31.5%) and 1000 ml of water were used as the reaction base solution, stirred at 350 rpm at 50°C, and 2100 ml of cobalt solution was added within 35 minutes.

[0092] (3) After the reaction is completed, the material is stirred for 30 minutes, and then put into a filter press for washing, and 4.5 liters of pure water is used for washing;

[0093] (4) The filter cake material is placed in a muffle furnace with a set temperature of 550°C and calcined for 6 hours.

[0094] (5) The calcined material is crushed and depolymerized using a jet mill to obtain porous flake-like cobalt trioxide.

[0095] Example 9

[0096] A method for preparing porous sheet-like cobalt oxide comprises the following steps:

[0097] (1) adding 454 g of cobalt chloride hexahydrate to 1 liter of water to prepare a cobalt-containing reagent;

[0098] (2) 800 ml of alkaline solution (mass percent concentration of 31.5%) and 1000 ml of water were used as the reaction base solution, stirred at 350 rpm at 50°C, and 2100 ml of cobalt solution was added within 35 minutes.

[0099] (3) After the reaction is completed, the material is stirred for 30 minutes, and then put into a filter press for washing, and 4.5 liters of pure water is used for washing;

[0100] (4) The filter cake material is placed in an oven set at 80°C for 48 hours to reduce the moisture content of the material to below 2%.

[0101] (5) The calcined material is crushed and depolymerized using a jet mill to obtain porous flake-like cobalt trioxide.

[0102] Performance Testing:

[0103] The products of Example 1 and Examples 6-9 were tested, and the test results are shown in Table 1.

[0104] Table 1

[0105] Example Cobalt content Moisture D50 Example 1 72.20% 0.33% 0.26μm Example 6 72.25% 0.50% 0.27μm Example 7 72.31% 0.41% 0.25μm Example 8 72.19% 0.63% 0.28μm Example 9 72.10% 0.56% 0.24μm

[0106] It can be seen from Table 1 that the physical and chemical indicators of the products corresponding to the above embodiments all meet the requirements and satisfy the material requirements.

[0107] The above are only embodiments of the present invention, and are not intended to limit the patent scope of the present invention. Any equivalent transformations made using the contents of the present invention specification, or directly or indirectly applied in related technical fields, are also included in the patent protection scope of the present invention.

Claims

1. A method for preparing porous sheet-like cobalt trioxide, characterized in that: The following steps are involved: S1. Add 454 g of cobalt chloride hexahydrate to 1 L of water to prepare a cobalt-containing reagent; S2: using 700-900 mL of an alkaline solution with a mass percentage concentration of 31.5% and 1000 mL of water as the reaction base liquid, stirring at 350 rpm at a temperature of 30-50° C., and adding 2100 mL of the cobalt-containing reagent within 35 minutes; S3: Continue stirring the materials after the reaction for 30 minutes, then put them into the filter press for washing, and use 4.5L of pure water for washing; The S4 filter cake material was placed in a muffle furnace set at 550°C and calcined for 6 hours; After calcination in S5, the material is crushed and depolymerized using a jet mill to obtain porous flake-like cobalt trioxide; The alkaline solution is a sodium hydroxide solution.

2. Application of the method according to claim 1 in the preparation of positive electrode materials for batteries.