A fluorine-containing polyurethane emulsion and its preparation method and application
By preparing fluorine-containing polyurethane emulsions, the introduction of intermolecular hydrogen bonds and fluorine elements is solved, and the problems of self-repair and poor binding force of polyurethane topcoat are achieved, achieving efficient protection effect of metal substrates.
Patent Information
- Application Number
- CN202211420829.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-11
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2042-11-11
AI Technical Summary
The existing polyurethane topcoat does not have the ability to self-repair, has high water absorption, is prone to powder and fall off, and has poor bonding power with the primer, making it unable to effectively protect metal substrates.
By mixing fluoro-containing acrylate with polyetheramines of different molecular weights, mixing them with 1,4-butanediol and HDI trimers, a fluoro-containing polyurethane emulsion is prepared to form intermolecular hydrogen bonds, and improve self-healing performance and Water absorption, enhancing interface interaction with epoxy resin primer.
It significantly improves the self-repairing performance and density of the topcoat, reduces water absorption, enhances adhesion to the primer, extends the service time of the coating, and significantly improves the corrosion shielding ability to metal substrates.
Smart Images

Figure CN115677973B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of anti-corrosion topcoats and relates to a fluorine-containing polyurethane emulsion and a preparation method and application thereof. Background Art
[0002] In practical applications, a single coating cannot meet the protection requirements of the base material, and the protective coating mainly adopts multiple anti-corrosion matching coatings. For example, a primer coating, an intermediate coating and a topcoat coating are set on the substrate. The topcoat is located at the outermost layer of the entire protective coating, and its performance is crucial. The topcoat must have the properties of light retention and color retention, and is not easy to powder. It is the last coating of the coating system. It usually also has the functions of pollution resistance, aging resistance, chemical resistance, UV resistance, moisture resistance, etc. It must also have the characteristics of not polluting the environment, safety and non-toxicity. The topcoat used in the field of application and anti-corrosion needs to be more outstanding, and must have comprehensive application properties such as acid, alkali and salt resistance, weather resistance, aging resistance and decorativeness. At present, the main anti-corrosion topcoats used in my country's industrial field are aliphatic polyurethane coatings, fluorocarbon coatings and polysiloxane coatings. Polyurea is a kind of protective coating polyurea that is usually composed of a soft segment phase composed of structures such as polyether or polyester and a hard segment phase composed of urea groups and amino groups, and presents a microphase separation state at the microscopic level. Polyurea has a special microstructure and exhibits excellent physical and chemical properties and thermal stability at the macroscopic level. The advantage of polyurea is that it contains rigid hard domains, mainly composed of ordered aliphatic groups characterized by high glass transition (Tg), dispersed in a soft viscoelastic matrix composed of ordered aromatic segments with low Tg. The reaction mechanism of polyurea is similar to that of polyurethane, and the construction methods and application fields also overlap, so the generalized polyurethane often includes polyurea. In terms of molecular structure, polyurethane and polyurea also have similarities. Polyurea is formed by rapid cross-linking and gradual growth polymerization between aliphatic isocyanates and aromatic oligomeric diamines, so the molecule contains an urethane structure. Since polyurea resin cures quickly, it has high requirements for construction equipment. Nowadays, in practical applications, polyethers with terminal hydroxyl groups and terminal amino groups are often used in combination to achieve a win-win situation in performance and economy. However, the existing polyurethane topcoat does not have self-healing ability, has high water absorption, and has poor bonding with commonly used primers such as epoxy resins. It is easy to powder and fall off, resulting in it being unable to effectively combine with the primer and effectively protect the metal substrate. Summary of the invention
[0003] In view of the problems existing in the prior art, the present invention provides a fluorine-containing polyurethane emulsion and a preparation method and application thereof, thereby effectively solving the technical problems in the prior art that the fluorine-containing polyurethane emulsion as a topcoat material does not have self-repairing properties, has a high water absorption rate, and is easy to powder and fall off.
[0004] The present invention is achieved through the following technical solutions:
[0005] A method for preparing a fluorine-containing polyurethane emulsion comprises the following steps:
[0006] S1: adding fluorinated acrylate to two polyetheramines with different molecular weights respectively, stirring and reacting to obtain two fluorinated monomers with different molecular weights;
[0007] S2: Mix the two fluorine-containing monomers with different molecular weights obtained in step S1 with 1,4-butanediol and HDI trimer, and stir to react to obtain the fluorine-containing polyurethane emulsion.
[0008] Preferably, the molar ratio of the polyetheramines of different molecular weights to the fluorinated acrylate is (0.7-1.2):(1.4-2.5).
[0009] Preferably, in step S1, the molecular weight of the polyetheramine is any two of 230Da, 400Da and 2000Da.
[0010] Preferably, the fluorine-containing acrylate is one or more of trifluoroethyl acrylate, trifluoroethyl methacrylate, hexafluorobutyl acrylate, hexafluorobutyl methacrylate, dodecafluoroheptyl acrylate and dodecafluoroheptyl methacrylate.
[0011] Preferably, in step S2, the ratio of the molar amount of the HDI trimer to the sum of the molar amounts of the secondary amine groups on the polyetheramine and the hydroxyl groups on 1,4-butanediol is (1.0-1.3):(0.8-1.2).
[0012] Preferably, the step S1 is reacted at room temperature.
[0013] Preferably, in step S1, the addition rate of the fluorinated acrylate is (1-2) mol / h.
[0014] Preferably, in step S1, the mass ratio of the two polyetheramines with different molecular weights is (5-10):(5-15).
[0015] A fluorine-containing polyurethane emulsion is prepared by the above method.
[0016] The above-mentioned fluorine-containing polyurethane emulsion is used in anti-corrosion topcoat.
[0017] Compared with the prior art, the present invention has the following beneficial technical effects:
[0018] A method for preparing a fluorinated polyurethane emulsion, wherein trifluoroethyl methacrylate (TFMA) is used to modify polyetheramine to prepare fluorinated monomers of different molecular weights, and the fluorinated monomers are mixed with 1,4-butanediol (BDO) and HDI trimer to prepare fluorinated polyurethane (FPU), wherein intermolecular hydrogen bonds can be formed between the fluorinated polyurethanes, so that the fluorinated polyurethanes have obvious self-healing properties, and the structure of the topcoat coating formed is more compact, and the introduction of F atoms significantly reduces the water absorption of the topcoat, which can protect the coating from external damage and corrosion by corrosive ions, and prolong the service life of the coating. The fluorinated polyurethane has active functional groups, which can react with the surface and residual amine and hydroxyl groups inside the epoxy resin primer, showing better interface interaction and good adhesion. The fluorine element on the fluorine-containing polyurethane is evenly distributed in the polyurethane coating. When the emulsion is used as a topcoat and combined with an epoxy resin primer, the fluorine element can penetrate into the inherent pores left by the epoxy resin due to water volatilization. This structure makes the coating structure more complete and the combination more compact. The preparation method of the fluorine-containing polyurethane emulsion is simple and convenient, and the design is reasonable. The obtained fluorine-containing polyurethane emulsion can effectively delay the corrosion of the metal substrate and show excellent corrosion shielding ability.
[0019] Furthermore, the molar ratio of polyetheramines of different molecular weights to fluorinated acrylates is (0.7-1.2):(1.4-2.5), but sufficient fluorine atoms are introduced into the polyetheramine to effectively enhance the water barrier capability of the fluorinated polyurethane emulsion.
[0020] Furthermore, the molecular weight of the polyetheramine is any two of 230Da, 400Da and 2000Da. The polyetheramine with this molecular weight has a suitable viscosity, which is beneficial to the preparation and subsequent use of the fluorine-containing polyurethane emulsion.
[0021] Furthermore, the ratio of the molar amount of HDI trimer to the sum of the molar amounts of the secondary amine groups on the polyetheramine and the hydroxyl groups on 1,4-butanediol is (1.0-1.3):(0.8-1.2), which fully ensures the short-term and long-term corrosion resistance of the fluorinated polyurethane emulsion.
[0022] Furthermore, the addition rate of the fluorinated acrylate is (1-2) mol / h, which effectively controls the reaction rate, allowing the fluorinated acrylate to fully react with the polyetheramine, and also allows the distribution of the fluorine element to be more uniform.
[0023] Furthermore, the mass ratio of the two polyetheramines with different molecular weights is (5-10):(5-15), which can effectively control the steric hindrance when the fluorinated polyurethane emulsion forms hydrogen bonds, making it easier to form hydrogen bonds between molecules, thereby making the fluorinated polyurethane more dense after forming the topcoat. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0025] Figure 1 A schematic diagram of a process for preparing a fluorine-containing polyurethane emulsion according to the present invention;
[0026] Figure 2 is a synthetic route diagram of the fluorine-containing polyether monomer prepared in Example 9 of the present invention;
[0027] Figure 3 FT-IR spectra of the fluorinated polyether monomer, polyetheramine D230, polyetheramine D2000 and trifluoroethyl methacrylate prepared in Example 9 of the present invention;
[0028] Figure 4 is the water absorption rate of the fluorine-containing polyurethane anticorrosive topcoat formed after curing in Example 9 of the present invention;
[0029] Figure 5 The SEM images of the fluorine-containing polyurethane anticorrosive topcoat prepared in Examples 7 to 11 of the present invention are as follows: A to E correspond to Examples 7 to 11, respectively;
[0030] Figure 6 The cross-sectional morphology scanning image (A) and the EDS spectrum of the F element (B) of the composite coating formed by coating the fluorinated polyurethane (FPU) anticorrosive topcoat prepared in Example 9 of the present invention on the surface of the waterborne epoxy resin (WEP) primer;
[0031] Figure 7 The Nyquist plots of the fluorine-containing polyurethane anticorrosive topcoat samples prepared in Examples 7 to 11 of the present invention at the initial stage of salt spray erosion;
[0032] Figure 8 The Bode modulus diagram of the fluorine-containing polyurethane anticorrosive topcoat samples prepared in Examples 7 to 11 of the present invention at the initial stage of salt spray erosion;
[0033] Fig. 9 Phase diagram of the fluorine-containing polyurethane anticorrosive topcoat samples prepared in Examples 7 to 11 of the present invention at the initial stage of salt spray erosion;
[0034] Fig.10The EIS impedance spectra of the waterborne epoxy coating and the fluorinated polyurethane anticorrosive topcoat samples prepared in Example 9 of the present invention after different salt spray erosion times; wherein A-1, A-2 and A-3 are the Nyquist, Bode modulus and Phase diagrams of the waterborne epoxy coating, respectively; and B-1, B-2 and B-3 are the Nyquist, Bode modulus and Phase diagrams of the fluorinated polyurethane anticorrosive topcoat, respectively. DETAILED DESCRIPTION
[0035] In order to enable those skilled in the art to understand the characteristics and effects of the present invention, the following is a general description and definition of the terms and expressions mentioned in the specification and claims. Unless otherwise specified, all technical and scientific terms used in the text are the common meanings understood by those skilled in the art for the present invention. In the event of a conflict, the definition in this specification shall prevail.
[0036] The theories or mechanisms described and disclosed herein, whether correct or incorrect, should not limit the scope of the present invention in any way, that is, the present invention can be implemented without being limited by any specific theory or mechanism.
[0037] Herein, all features such as values, quantities, contents and concentrations defined in the form of numerical ranges or percentage ranges are for simplicity and convenience only. Accordingly, the description of numerical ranges or percentage ranges should be considered to have included and specifically disclosed all possible secondary ranges and individual values within the range (including integers and fractions).
[0038] In this document, unless otherwise specified, “includes,” “including,” “contains,” “has,” or similar terms cover the meanings of “consisting of” and “mainly consisting of,” for example, “A includes a” covers the meanings of “A includes a and other” and “A only includes a.”
[0039] In this document, in order to make the description concise, not all possible combinations of various technical features in various embodiments or examples are described. Therefore, as long as there is no contradiction in the combination of these technical features, the various technical features in various embodiments or examples can be combined arbitrarily, and all possible combinations should be considered to be within the scope of this specification.
[0040] The present invention provides a method for preparing a fluorine-containing polyurethane emulsion, comprising the following steps:
[0041] S1: Add fluorinated acrylate to two polyetheramines with different molecular weights at a rate of (1-2) mol / h, respectively, and react by stirring at room temperature to obtain two fluorinated monomers with different molecular weights. The molecular weight of the polyetheramine is any two of 230Da, 400Da and 2000Da; the molar ratio of the polyetheramine with different molecular weights to the fluorinated acrylate is (0.7-1.2):(1.4-2.5); the fluorinated acrylate is one or more of trifluoroethyl acrylate, trifluoroethyl methacrylate, hexafluorobutyl acrylate, hexafluorobutyl methacrylate, dodecafluoroheptyl acrylate and dodecafluoroheptyl methacrylate; the mass ratio of the two polyetheramines with different molecular weights is (5-10):(5-15);
[0042] S2: Mix the two fluorinated monomers with different molecular weights obtained in step S1 with 1,4-butanediol (BDO) and HDI trimer, and stir to react to obtain the fluorinated polyurethane emulsion. The ratio of the molar amount of HDI trimer to the sum of the molar amounts of the secondary amine groups on the polyetheramine and the hydroxyl groups on 1,4-butanediol is (1.0-1.3):(0.8-1.2), and the secondary amine groups on the polyetheramine and the hydroxyl groups on 1,4-butanediol are both active hydrogens of the system, that is, the molar ratio of HDI trimer to active hydrogen (secondary amine groups and hydroxyl groups) is (1.0-1.3):(0.8-1.2).
[0043] The preparation method uses trifluoroethyl methacrylate (TFMA) to modify polyetheramine to prepare fluorinated monomers of different molecular weights, and mixes the fluorinated monomers with 1,4-butanediol (BDO) and HDI trimer to prepare fluorinated polyurethane (FPU). The fluorinated polyurethane can form intermolecular hydrogen bonds, so that the fluorinated polyurethane has obvious self-healing properties. At the same time, the structure of the topcoat coating is more compact. With the introduction of F atoms, the water absorption rate of the topcoat is significantly reduced, which can protect the coating from external damage and corrosion of corrosive ions, and extend the service life of the coating. The fluorinated polyurethane has active functional groups, which can react with the surface and residual amine and hydroxyl groups inside the epoxy resin primer, showing better interface interaction and good adhesion. The fluorine element on the fluorine-containing polyurethane is evenly distributed in the polyurethane coating. When the emulsion is used as a topcoat and combined with an epoxy resin primer, the fluorine element can penetrate into the inherent pores left by the epoxy resin due to water volatilization. This structure makes the coating structure more complete and the combination more compact. The preparation method of the fluorine-containing polyurethane emulsion is simple and convenient, and the design is reasonable. The obtained fluorine-containing polyurethane emulsion can effectively delay the corrosion of the metal substrate and show excellent corrosion shielding ability. The product has excellent mechanical properties, the FPU film has good room temperature hydrogen bond self-repairing ability, and the coating has excellent shielding performance against corrosive media, effectively delaying the corrosion of the metal to the substrate, providing a new method for subsequent solvent-free resin research.
[0044] In addition, the present invention also discloses that the obtained fluorinated polyurethane emulsion is used in an anticorrosive topcoat. Compared with other coating topcoats currently used, the prepared fluorinated polyurethane coating has excellent physical and chemical properties and hydrophobic properties, which can protect the coating from external damage and corrosion of corrosive ions, and prolong the service life of the coating. In addition, there is a strong interfacial force between the fluorinated polyurethane and the lower coating layer, and the fluorinated polyurethane coating acts as a barrier to prevent the corrosion of the corrosive medium, prolong the invasion of the lower corroded medium, and further effectively delays the corrosion of the metal substrate, showing excellent corrosion shielding ability. Fluorinated polymer coatings have excellent surface properties, can create miracles in the fields of corrosion, and also provide new methods for the subsequent research of solvent-free resins. The present invention is designed by molecular structure, and when the prepared product is used for coating topcoat, the hard segment of the polyurethane provides the necessary enhancement for the underlying microstructure and acts as a physical crosslink, while the soft segment provides it with inherent flexibility; fluorinated polymers, as a typical low surface energy coating material, have the performance of super hydrophobic coatings, and also have high-strength heat resistance, weather resistance, chemical resistance and corrosion resistance. The polymer structure designed by the present invention can achieve the unity of excellent physical and chemical properties, thermal stability, hydrophobicity and corrosion resistance, and solve the common technical problems in the industry such as coating corrosion resistance. When the invention is used for metal corrosion protection, it can greatly improve the physical and chemical properties of the coating and the ability to prevent corrosive substances from entering (especially water), broadening the research scope of anti-corrosion materials.
[0045] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.
[0046] The following examples use conventional instruments and equipment in the art. The experimental methods in the following examples where specific conditions are not specified are usually carried out under conventional conditions or under conditions recommended by the manufacturer. The various raw materials used in the following examples are conventional commercial products unless otherwise specified, and their specifications are conventional specifications in the art. In the specification of the present invention and the following examples, unless otherwise specified, "%" means weight percentage, "part" means weight part, and ratio means weight ratio.
[0047] Example 1
[0048] 1 mol of polyetheramine D230 was added to a three-necked flask with stirring and temperature control, and 2 mol of trifluoroethyl methacrylate was added dropwise at 25°C for 1 hour. The reaction end point was monitored by infrared spectroscopy, that is, when the primary amino peak in the infrared spectrum disappeared, the reaction was completed. This was recorded as product I.
[0049] 1 mol of polyetheramine D2000 was added into a three-necked flask with stirring and temperature control, and 2 mol of trifluoroethyl methacrylate was added dropwise at 25°C for 1 hour. The reaction end point was monitored by infrared spectroscopy. This was recorded as product II.
[0050] Weigh 5g of product I, product II and 5g of 1,4-butanediol and HDI trimer respectively, and mix them at a molar ratio of HDI trimer to active hydrogen (secondary amine group and hydroxyl group) of 1.1:1, which is recorded as product III. Product III is a fluorine-containing polyurethane emulsion. Product III can be coated on epoxy resin primer and formed into topcoat after curing.
[0051] Example 2
[0052] Add 1 mol of polyetheramine D230 to a three-necked flask with stirring and temperature control, add 2 mol of trifluoroethyl methacrylate dropwise at 25°C for 1 hour, and monitor the reaction end point by infrared spectroscopy. This is recorded as product I. Add 1 mol of polyetheramine D2000 to a three-necked flask with stirring and temperature control, add 2 mol of trifluoroethyl methacrylate dropwise at 25°C for 1 hour, and monitor the reaction end point by infrared spectroscopy. This is recorded as product II.
[0053] Weigh 10g of product I, 5g of product II and 8g of 1,4-butanediol and HDI trimer, mix them at a molar ratio of HDI trimer to active hydrogen (secondary amine and hydroxyl) of 1.1:1, and record them as product III. Product III is a fluorine-containing polyurethane emulsion. Product III can be coated on epoxy resin primer and form a topcoat after curing.
[0054] Example 3
[0055] Add 1 mol of polyetheramine D230 to a three-necked flask with stirring and temperature control, add 2 mol of trifluoroethyl methacrylate dropwise at 25°C for 1 hour, and monitor the reaction end point by infrared spectroscopy. This is recorded as product I. Add 1 mol of polyetheramine D2000 to a three-necked flask with stirring and temperature control, add 2 mol of trifluoroethyl methacrylate dropwise at 25°C for 1 hour, and monitor the reaction end point by infrared spectroscopy. This is recorded as product II.
[0056] Weigh 5g of product I, 10g of product II and 2g of 1,4-butanediol and HDI trimer, mix them at a molar ratio of HDI trimer to active hydrogen (secondary amine and hydroxyl) of 1.1:1, and record them as product III. Product III is a fluorine-containing polyurethane emulsion. Product III can be coated on epoxy resin primer and form a topcoat after curing.
[0057] Example 4
[0058] Add 1 mol of polyetheramine D230 to a three-necked flask with stirring and temperature control, add 2 mol of trifluoroethyl methacrylate dropwise at 25°C for 1 hour, and monitor the reaction end point by infrared spectroscopy. This is recorded as product I. Add 1 mol of polyetheramine D2000 to a three-necked flask with stirring and temperature control, add 2 mol of trifluoroethyl methacrylate dropwise at 25°C for 1 hour, and monitor the reaction end point by infrared spectroscopy. This is recorded as product II.
[0059] Weigh 10g of product I, 10g of product II and 5g of 1,4-butanediol and HDI trimer and mix them at a molar ratio of HDI trimer to active hydrogen (secondary amine and hydroxyl) of 1.1:1, and record them as product III. Product III is a fluorine-containing polyurethane emulsion. Product III can be coated on epoxy resin primer and form a topcoat after curing.
[0060] Example 5
[0061] Add 1 mol of polyetheramine D230 to a three-necked flask with stirring and temperature control, add 2 mol of trifluoroethyl methacrylate dropwise at 25°C for 1 hour, and monitor the reaction end point by infrared spectroscopy. This is recorded as product I. Add 1 mol of polyetheramine D2000 to a three-necked flask with stirring and temperature control, add 2 mol of trifluoroethyl methacrylate dropwise at 25°C for 1 hour, and monitor the reaction end point by infrared spectroscopy. This is recorded as product II.
[0062] Weigh 5g of product I, 15g of product II and 8g of 1,4-butanediol and HDI trimer, mix them at a molar ratio of HDI trimer to active hydrogen (secondary amine group and hydroxyl group) of 1.1:1, and record them as product III. Product III is a fluorine-containing polyurethane emulsion. Product III can be coated on epoxy resin primer and form a topcoat after curing.
[0063] Example 6
[0064] Add 1 mol of polyetheramine D230 to a three-necked flask with stirring and temperature control, add 2 mol of trifluoroethyl methacrylate dropwise at 25°C for 1 hour, and monitor the reaction end point by infrared spectroscopy. This is recorded as product I. Add 1 mol of polyetheramine D2000 to a three-necked flask with stirring and temperature control, add 2 mol of trifluoroethyl methacrylate dropwise at 25°C for 1 hour, and monitor the reaction end point by infrared spectroscopy. This is recorded as product II.
[0065] Weigh 10g of product I, 15g of product II and 2g of 1,4-butanediol and HDI trimer, mix them at a molar ratio of HDI trimer to active hydrogen (secondary amine and hydroxyl) of 1.1:1, and record them as product III. Product III is a fluorine-containing polyurethane emulsion. Product III can be coated on epoxy resin primer and form a topcoat after curing.
[0066] Example 7
[0067] Add 1 mol of polyetheramine D230 to a three-necked flask with stirring and temperature control, add 2 mol of trifluoroethyl methacrylate dropwise at 25°C for 1 hour, and monitor the reaction end point by infrared spectroscopy. This is recorded as product I. Add 1 mol of polyetheramine D2000 to a three-necked flask with stirring and temperature control, add 2 mol of trifluoroethyl methacrylate dropwise at 25°C for 1 hour, and monitor the reaction end point by infrared spectroscopy. This is recorded as product II.
[0068] Weigh 5g of product I, 10g of product II and 8g of 1,4-butanediol and HDI trimer, mix them at a molar ratio of HDI trimer to active hydrogen (secondary amine and hydroxyl) of 1.1:1, and record them as product III. Product III is a fluorine-containing polyurethane emulsion. Product III can be coated on epoxy resin primer and form a topcoat after curing.
[0069] Example 8
[0070] Add 1 mol of polyetheramine D230 to a three-necked flask with stirring and temperature control, add 2 mol of trifluoroethyl methacrylate dropwise at 25°C for 1 hour, and monitor the reaction end point by infrared spectroscopy. This is recorded as product I. Add 1 mol of polyetheramine D2000 to a three-necked flask with stirring and temperature control, add 2 mol of trifluoroethyl methacrylate dropwise at 25°C for 1 hour, and monitor the reaction end point by infrared spectroscopy. This is recorded as product II.
[0071] Weigh 5g of product I, 10g of product II and 9g of 1,4-butanediol and HDI trimer, mix them at a molar ratio of HDI trimer to active hydrogen (secondary amine and hydroxyl) of 1.1:1, and record them as product III. Product III is a fluorine-containing polyurethane emulsion. Product III can be coated on epoxy resin primer and form a topcoat after curing.
[0072] Example 9
[0073] Add 1 mol of polyetheramine D230 to a three-necked flask with stirring and temperature control, and add 2 mol of trifluoroethyl methacrylate (TFMA) at 25°C for 1 hour, and monitor the reaction end point by infrared spectroscopy. Recorded as product I (D230-F). Add 1 mol of polyetheramine D2000 to a three-necked flask with stirring and temperature control, and add 2 mol of trifluoroethyl methacrylate at 25°C for 1 hour, and monitor the reaction end point by infrared spectroscopy. Recorded as product II (D2000-F).
[0074] Weigh 5g of product I, 10g of product II and 10g of 1,4-butanediol and HDI trimer, mix them at a molar ratio of HDI trimer to active hydrogen (secondary amine and hydroxyl) of 1.1:1, and record them as product III. Product III is a fluorine-containing polyurethane emulsion. Product III can be coated on epoxy resin primer and form a topcoat after curing.
[0075] The synthetic route of the fluorinated polyether monomer in this example is shown in Figure 2 In order to verify the successful synthesis of the fluorinated polyether monomer, the infrared spectroscopy (FT-IR) test results of the products I and II prepared in this example are as follows: Figure 3 As shown by Figure 3 It can be seen that in the structure of polyetheramine D230, the -1 There are multiple absorption bands of primary amine ν-NH, which disappear in the product fluorinated monomer D230-F and are replaced by the absorption peak of -NH-. -1 The unsaturated CH absorption peak and 1680-1620cm -1 of ν C=C The absorption peak disappeared in the product fluorinated monomer D230-F, and a peak less than 3000 cm -1 The saturated CH absorption peak of the fluorinated monomer D230-F is also at 1750cm -1 and 560cm -1 The absorption peaks of C=O and -CF3 appeared, proving that the Michael addition reaction of polyetheramine D230 and TFMA was sufficient and the fluorinated monomer D230-F was successfully synthesized. Since polyetheramine D2000 and D230 have similar structures, the synthesized fluorinated monomer D2000-F has the same peak position as the fluorinated monomer D230-F except for the difference in absorption peak strength, indicating that the fluorinated monomer D2000-F was also successfully synthesized.
[0076] The fluorinated polyurethane emulsion (FPU) prepared in this example was coated on the surface of a waterborne epoxy resin (WEP) primer to form a composite coating, and the morphology of the composite coating was tested. The test results are shown in FIG. Figure 6 As shown by Figure 6 It can be seen that the F element is evenly distributed in the polyurethane coating. In addition, the polyurethane coating can wet the epoxy resin surface during the coating process and penetrate into the inherent pores left by the epoxy resin due to water evaporation. Figure 6 (B) It can be clearly seen that the polyurethane emulsion is filled in the epoxy resin, and the distribution of the F element corresponds one to one with the defects of the epoxy resin. This structure makes the structure of the composite coating more complete and the bonding force between the topcoat and the primer is tighter.
[0077] Example 10
[0078] Add 1 mol of polyetheramine D230 to a three-necked flask with stirring and temperature control, add 2 mol of trifluoroethyl methacrylate dropwise at 25°C for 1 hour, and monitor the reaction end point by infrared spectroscopy. This is recorded as product I. Add 1 mol of polyetheramine D2000 to a three-necked flask with stirring and temperature control, add 2 mol of trifluoroethyl methacrylate dropwise at 25°C for 1 hour, and monitor the reaction end point by infrared spectroscopy. This is recorded as product II.
[0079] Weigh 5g of product I, 10g of product II and 11g of 1,4-butanediol and HDI trimer, mix them at a molar ratio of HDI trimer to active hydrogen (secondary amine group and hydroxyl group) of 1.1:1, and record them as product III. Product III is a fluorine-containing polyurethane emulsion. Product III can be coated on epoxy resin primer and form a topcoat after curing.
[0080] Embodiment 11
[0081] 1 mol of polyetheramine D230 was added to a three-necked flask with stirring and temperature control, and 2 mol of trifluoroethyl methacrylate was added dropwise at 25°C for 1 hour. The reaction end point was monitored by infrared spectroscopy. This was recorded as product I.
[0082] 1 mol of polyetheramine D2000 was added into a three-necked flask with stirring and temperature control, and 2 mol of trifluoroethyl methacrylate was added dropwise at 25°C for 1 hour. The reaction end point was monitored by infrared spectroscopy. This was recorded as product II.
[0083] Weigh 5g of product I, 10g of product II and 12g of 1,4-butanediol and HDI trimer, mix them at a molar ratio of HDI trimer to active hydrogen (secondary amine group and hydroxyl group) of 1.1:1, and record them as product III. Product III is a fluorine-containing polyurethane emulsion. Product III can be coated on epoxy resin primer and form a topcoat after curing.
[0084] In order to verify the hydrophobicity of the fluorine-containing polyurethane anticorrosive topcoat prepared in the present invention, the water absorption rate of the topcoat formed after curing in Examples 7 to 11 was tested. The results are as follows: Figure 4 As shown. Figure 4 It can be seen that after the five groups of samples in Examples 7 to 11 were immersed in deionized water for 20 days, their water absorption rates were 0.72%, 0.53%, 0.30%, 0.43% and 0.68%, respectively. It can be seen that their water absorption rates are relatively low. This is because the fluorine-containing polyurethane anti-corrosion topcoat has a dense structure and the fluorine atom has excellent hydrophobic properties, which makes the water absorption rate of the coating low. This structure effectively blocks corrosive media, such as water, from penetrating into the coating and damaging the coating.
[0085] Furthermore, in order to characterize the morphological characteristics of the fluorinated polyurethane anticorrosive topcoat, field emission scanning electron microscopy (SEM) tests were performed on the target products in Examples 7 to 11. The test results are as follows: Figure 5 As shown by Figure 5 It can be seen that Figure 5 (A~E) The fracture is smooth, and there are cracks of varying degrees on the cross section. Figure 5 (A~D) The cracks on the cross section gradually become sparse. Figure 5 (E) The cross section cracks are obvious. This is because 1,4-butanediol (BDO) is a rigid segment and fluorinated polyetheramine is a flexible segment. As the amount of BDO increases, the microphase separation structure of fluorinated polyurethane (FPU) becomes more obvious. When the amount of BDO is 8g, the dense lines produced by flexible tearing are mainly shown, and the coating has good flexibility. When the amount of BDO is 9g, 10g, and 11g, the fracture surface becomes smoother and the fracture lines become fewer and fewer, showing the morphology of the BDO hard segment. When the amount of BDO is 12g, due to the excessive amount of BDO, the coating has serious phase separation. The cross section has irregular lines and particles shown by the soft segment, and there are also smooth cross sections of the hard segment. The density between the faults is reduced.
[0086] Further, in order to verify the anti-corrosion performance of the fluorinated polyurethane emulsion prepared in the present invention, the fluorinated polyurethane prepared in Examples 7 to 11 of the present invention was coated on the surface of the waterborne epoxy resin primer to form a composite coating, the composite coating was composed of 50 μm epoxy primer and 50 μm fluorinated polyurethane topcoat, and the composite coating was subjected to corrosion electrochemical performance test. The electrochemical results are as follows: Figures 7-8 As shown in Table 1. Figure 7 It can be seen that at the initial stage of 3.5wt% NaCl salt spray corrosion, the low-frequency impedance of the coatings with different BDO dosages exceeded 10 10 Ω·cm 2 , and the Nyquist semicircle radius is large, both showing excellent anti-corrosion performance. Figure 8 From the Bode modulus graph, it can be seen that the topcoats of Example 10 and Example 11 have resistance plateaus to varying degrees, but no resistance plateaus are observed in the EIS graphs of the topcoats of Example 7, Example 8, and Example 9. Generally, a resistance plateau means that the electrolyte solution has reached the coating / metal interface and formed a connected permeation channel in the coating. By analyzing Fig. 9From the Phase diagram, it can be seen that one time constant in the high-frequency region is related to the coating on the surface of the substrate, and the other time constant in the low-frequency region is related to the charge transfer reaction generated by the electrochemical corrosion activity on the surface of the substrate. Each additional time constant corresponds to an interface. In the present invention, the corresponding coating is the interface between the fluorinated polyurethane coating and the waterborne epoxy resin. Due to the difference in hydrophilicity between BDO and fluorinated monomers, the hydrophilicity of the coating increases when the amount of BDO increases. This will cause the corrosive solution to penetrate into the coating and reach the interface between the fluorinated polyurethane anti-corrosion topcoat and the waterborne epoxy resin. In particular, for the sample in Example 11, the electrochemical impedance data is completely consistent with the quadratic time constant model. In addition, from Figures 7-8 It can be seen that the fitting data is highly consistent with the experimental data, and the fitting model is appropriately selected.
[0087] Figures 7 to 9 The fitting data in is shown in Table 1, where R coat is the coating resistance, CPE coat is the non-ideal capacitance of the coating, R coat and CPE coat Usually used to characterize the protective ability of coatings. coat Reduce CPE coat When the R increases, the barrier performance of the coating deteriorates and the protective ability weakens. ct is the charge transfer resistance, CPE dl is the non-ideal capacitance of the double layer. "n" is the empirical index of CPE. The constant phase element (CPE) is a non-ideal capacitor behavior equivalent element used to fit the EIS curve. Capacitance is exhibited on non-uniform electrodes due to electrode porosity, non-uniform current distribution and coating variations. The impedance formula for calculating CPE is
[0088] Z CPE =γ(jω) (-n) (1)
[0089] In the formula, Z CPE is the impedance of the CPE, γ is the proportionality coefficient, j is the imaginary part, ω is the angular frequency, and n is the exponent of the CPE.
[0090] It can be seen from the fitting data in Table 1 that the electrochemical impedance value of the composite coating prepared by the present invention is greater than 10 7 , and even better can reach 10 8 , so the composite coating has good corrosion resistance.
[0091] Table 1 Electrochemical impedance fitting parameters of the fluorinated polyurethane anticorrosive topcoat obtained in Examples 7-11 of the present invention
[0092]
[0093] Furthermore, in order to better verify the change of the anti-corrosion performance of the topcoat prepared by the present invention with the salt spray corrosion, the attenuation change of the anti-corrosion performance of the coating with the corrosion time was studied by comparing the 100μm epoxy resin coating primer with the 100μm composite coating obtained in Example 9 (50μm epoxy resin primer and 50μm fluorine-containing polyurethane topcoat). At the same time, the electrochemical properties of the coating were tested, and the test results are shown in Fig.10 The dotted line in the figure is the fitting curve, which is almost completely consistent with the test data, indicating that the corrosion fitting model is suitable. Fig.10 It can be seen from A-1 that the coating is in the shape of a quarter arc at the beginning of immersion. After immersion for 200 hours, it becomes semicircular and the radius of the capacitive reactance arc is significantly reduced, which means that the coating is corroded by the corrosive medium. After immersion for 400 hours, the radius of the capacitive reactance arc is further reduced. At this time, the low-frequency area shrinks, which may be due to a small amount of corrosive medium corroding the coating, causing local corrosion and forming corrosion products. However, this stage still presents a single capacitive reactance arc, indicating that corrosion occurs at the coating / substrate interface and the corrosion is not serious. After immersion for 600 hours, the Nyquist diagram of the coating shows an obvious double capacitive reactance arc, indicating that the coating is corroded by the corrosive medium and obvious corrosion reactions occur in the substrate. In contrast, Fig.10 B-1 is the Nyquist plot of fluorinated polyurethane anticorrosive topcoat. In the figure, the radius of the capacitance arc decreases with the increase of immersion time, but it still shows a single capacitance arc at 600h. The shielding effect of the composite coating on the corrosive medium is much better than that of the waterborne epoxy resin coating (WEP).
[0094] Fig.10 Figure A-2 and Figure B-2 are the Bode modulus graphs of WEP and fluorinated polyurethane anticorrosive topcoat. Generally speaking, low-frequency impedance (|Z| f=0.01Hz ) value, the stronger the coating's ability to resist permeability and the better its anti-corrosion performance. In the initial immersion period, the low-frequency impedance of WEP |Z| f=0.01Hz =3.200×10 10 Ω·cm 2 , low frequency impedance of fluorinated polyurethane anticorrosive topcoat |Z| f=0.01Hz =2.854×10 11 Ω·cm 2 , the difference between the two is less than one order of magnitude. However, after immersion for 600h, the low-frequency impedance |Z| of WEP f=0.01Hz =6.666×10 6 Ω·cm 2 , low frequency impedance of fluorinated polyurethane anticorrosive topcoat |Z| f=0.01Hz =2.530×10 8 Ω·cm 2 The difference between the two is nearly two orders of magnitude. The low-frequency impedance fully demonstrates that the fluorine-containing polyurethane anti-corrosion topcoat can better shield the corrosion of the corrosive medium on the substrate than pure WEP.
[0095] Fig.10 A-3 and B-3 are the Phase diagrams of WEP and fluorinated polyurethane anticorrosive topcoats. The phase angle platform area in the figure is a time constant and the response of the coating on the surface of the substrate. The wider the corresponding frequency range of this area, the better the barrier performance of the coating. The low-frequency area where the phase angle decays rapidly in the figure is another time constant, which is related to the charge transfer reaction generated by the electrochemical corrosion activity on the surface of the substrate. When the frequency range of this area increases, the phase angle decays severely. This means that the corrosion reaction occurs, and an obvious second capacitive reactance arc will appear in the Nyquist diagram. Fig.10 The variation of the Phase diagrams of A-3 and B-3 is consistent with the trend of the Nyquist and Bode modulus diagrams. The fluorinated polyurethane anticorrosive topcoat exhibits excellent corrosion resistance.
[0096] According to the electrochemical experimental results, a suitable model was selected and the electrochemical impedance was fitted and analyzed using ZSimpWin software. The corrosion process was simulated by an equivalent circuit diagram. Fig.10 The analysis and fitting data in are shown in Table 2. It can be found from Table 2 that the WEP coating has a CPE of coat and CPE dl All are 10 -11 Ω -1 cm -2 s n , are of the same order of magnitude. However, R coat But R ct The difference is two orders of magnitude. This is due to the pores left by the volatilization of water in the curing process of waterborne epoxy resin. Therefore, the waterborne epoxy resin coating is easily infiltrated and eroded by the corrosive medium. However, the thickness of the waterborne epoxy coating makes it impossible for the electrolyte to completely wet the coating and reach the surface of the substrate in a short time, so the waterborne epoxy coating can be simplified into the infiltrated part and the uninfiltrated part. The waterborne epoxy resin forms an interface due to the erosion of the corrosive medium, so R coat Always less than R ct Until the coating is corroded for 400h, R coat and R ct At this point, the coating is completely corroded by the corrosive medium, and part of the corrosive medium reaches the coating / substrate interface. dl >CPE coat , the coating impedance is 10 7 Ω·cm 2 , the coating will lose its protective function. After the coating has been subjected to a 600h salt spray test, the coating impedance is only 10 6 Ω·cm 2, and there is obvious Warburg diffusion, severe corrosion, and the coating almost loses its shielding effect. The Rcoat value of the fluorinated polyurethane anticorrosive topcoat at 0h is 7.075×10 11 Ω·cm 2 , than the WEP coating R coat 2.024×10 8 Ω·cm 2 The fluorinated polyurethane anti-corrosion topcoat has a three-order-of-magnitude higher protective effect against corrosive media than the WEP coating of the same thickness. At the same time, after the 400h salt spray test, the corrosive media only eroded the FPU layer and reached the interface between FPU and WEP. At this time, the R ct and CPE dl It is at the same order of magnitude as the 200h WEP coating. When the fluorinated polyurethane anticorrosion topcoat was corroded by salt spray for 600h, Nyquist still could not observe the second capacitive reactance arc, and the charge transfer resistance R ct Still more than 10 8 Ω·cm 2 The coating did not fail in its salt spray barrier effect and showed good shielding effect.
[0097] Table 2 Electrochemical impedance fitting parameters of WEP and fluorinated polyurethane anticorrosive topcoat obtained in Example 9
[0098]
[0099]
[0100] Example 12
[0101] A method for preparing a fluorine-containing polyurethane emulsion comprises the following steps:
[0102] S1: adding trifluoroethyl acrylate to polyetheramine D230 and D400 at a rate of 1 mol / h, respectively, and reacting by stirring at 25°C to obtain F-D230 and F-D400, wherein the mass ratio of polyetheramine D230 to D400 is 5:5, and the molar ratios of polyetheramine D230 and D400 to trifluoroethyl acrylate are both 0.7:1.4;
[0103] S2: Mix the F-D230 and F-D400 obtained in step S1 with BDO and HDI trimer, and stir to react to obtain a fluorinated polyurethane emulsion, wherein the ratio of the molar amount of HDI trimer to the molar amount of the secondary amine group on the polyetheramine and the hydroxyl group on 1,4-butanediol is 1.0:0.8.
[0104] Example 13
[0105] A method for preparing a fluorine-containing polyurethane emulsion comprises the following steps:
[0106] S1: adding trifluoroethyl methacrylate to polyetheramine D230 and D2000 at a rate of 1.3 mol / h, respectively, and reacting by stirring at 25°C to obtain F-D230 and F-D2000, wherein the mass ratio of polyetheramine D230 to D2000 is 7:5, and the molar ratios of polyetheramine D230 and D2000 to trifluoroethyl methacrylate are both 0.8:1.6;
[0107] S2: Mix the F-D230 and F-D2000 obtained in step S1 with BDO and HDI trimer, and stir to react to obtain a fluorinated polyurethane emulsion, wherein the ratio of the molar amount of HDI trimer to the molar amount of the secondary amine group on the polyetheramine and the hydroxyl group on 1,4-butanediol is 1.1:1.2.
[0108] Embodiment 15
[0109] A method for preparing a fluorine-containing polyurethane emulsion comprises the following steps:
[0110] S1: adding hexafluorobutyl acrylate to polyetheramine D230 and D2000 at a rate of 1.5 mol / h, respectively, and reacting by stirring at 25°C to obtain F-D230 and F-D2000, wherein the mass ratio of polyetheramine D230 to D2000 is 10:15, and the molar ratios of polyetheramine D230 and D2000 to trifluoroethyl methacrylate are both 1.1:2.0;
[0111] S2: Mix the F-D230 and F-D2000 obtained in step S1 with BDO and HDI trimer, and stir to react to obtain a fluorinated polyurethane emulsion, wherein the ratio of the molar amount of HDI trimer to the molar amount of the secondary amine group on the polyetheramine and the hydroxyl group on 1,4-butanediol is 1.3:1.2.
[0112] Example 16
[0113] A method for preparing a fluorine-containing polyurethane emulsion comprises the following steps:
[0114] S1: adding hexafluorobutyl methacrylate to polyetheramine D400 and D2000 at a rate of 2 mol / h, respectively, and reacting by stirring at 25°C to obtain F-D400 and F-D2000, wherein the mass ratio of polyetheramine D400 to D2000 is 5:5, and the molar ratios of polyetheramine D400 and D2000 to hexafluorobutyl methacrylate are both 1.2:2.5;
[0115] S2: Mix the F-D400 and F-D2000 obtained in step S1 with BDO and HDI trimer, and stir to react to obtain a fluorinated polyurethane emulsion, wherein the ratio of the molar amount of HDI trimer to the molar amount of the secondary amine group on the polyetheramine and the hydroxyl group on 1,4-butanediol is 1.3:1.1.
[0116] Example 16
[0117] The difference between this embodiment and embodiment 10 is that the fluorine-containing acrylate is hexafluorobutyl methacrylate.
[0118] Embodiment 17
[0119] The difference between this embodiment and embodiment 10 is that the fluorine-containing acrylate is dodecafluoroheptyl acrylate.
[0120] Embodiment 18
[0121] The difference between this embodiment and embodiment 10 is that the fluorine-containing acrylate is dodecafluoroheptyl methacrylate.
[0122] Embodiment 19
[0123] The difference between this embodiment and embodiment 10 is that the fluorine-containing acrylate is a mixture of trifluoroethyl acrylate and trifluoroethyl methacrylate.
[0124] Embodiment 20
[0125] The difference between this embodiment and embodiment 10 is that the fluorine-containing acrylate is a mixture of hexafluorobutyl methacrylate and dodecafluoroheptyl acrylate.
[0126] Embodiment 21
[0127] The difference between this embodiment and embodiment 10 is that the fluorine-containing acrylate is a mixture of hexafluorobutyl acrylate, hexafluorobutyl methacrylate and dodecafluoroheptyl methacrylate.
[0128] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
[0129] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A method for preparing a fluorinated polyurethane emulsion, characterized in that: The following steps are involved: S1: adding fluorinated acrylate to two polyetheramines with different molecular weights respectively, stirring and reacting to obtain two fluorinated monomers with different molecular weights; S2: mixing the two fluorine-containing monomers with different molecular weights obtained in step S1 with 1,4-butanediol and HDI trimer, and stirring to react to obtain the fluorine-containing polyurethane emulsion; In step S1, the molecular weight of the polyetheramine is any two of 230Da, 400Da and 2000Da; In the step S1, the mass ratio of the two polyetheramines with different molecular weights is (5-10):(5-15); In step S1, the reaction is stopped when the primary amino group peak in the polyetheramine disappears; In step S2, the ratio of the molar amount of the HDI trimer to the sum of the molar amounts of the secondary amine groups on the polyetheramine and the hydroxyl groups on 1,4-butanediol is (1.0-1.3):(0.8-1.2).
2. The method for preparing a fluorinated polyurethane emulsion according to claim 1, characterized in that: The molar ratio of the polyetheramines with different molecular weights to the fluorinated acrylate is (0.7-1.2):(1.4-2.5).
3. The method for preparing a fluorinated polyurethane emulsion according to claim 1, characterized in that: The fluorine-containing acrylate is one or more of trifluoroethyl acrylate, trifluoroethyl methacrylate, hexafluorobutyl acrylate, hexafluorobutyl methacrylate, dodecafluoroheptyl acrylate and dodecafluoroheptyl methacrylate.
4. The method for preparing a fluorinated polyurethane emulsion according to claim 1, characterized in that: The step S1 is reacted at room temperature.
5. The method for preparing a fluorinated polyurethane emulsion according to claim 1, characterized in that: In the step S1, the addition rate of the fluorinated acrylate is (1-2) mol / h.
6. A fluorinated polyurethane emulsion, characterized in that: Prepared by the method according to any one of claims 1 to 5.
7. Use of the fluorine-containing polyurethane emulsion described in claim 6 in anti-corrosion topcoat.