Polishing composition

By using alumina abrasive particle composition with high and low α-degradation rate, the problem of taking into account both speed and texture when grinding hard and brittle materials is solved, and efficient grinding and surface improvement are achieved.

CN115678438BActive Publication Date: 2024-12-06FUJIMI INCORPORATED
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211428731.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-03-28
Filing Date
2019-03-14
Publication Date
2024-12-06
Estimated Expiration
2039-03-14

AI Technical Summary

Technical Problem

When the existing grinding compositions are polished with a low grinding speed and poor surface texture when grinding hard and brittle materials, it is difficult to simultaneously improve the grinding speed and improve the surface texture.

Method used

Alumina abrasive particle composition containing α-alumina A with an α-alumina A of more than 80% and α-alumina B with an α-alumina B with an α-alumina B with an α-alumina A of small diameter is used in the grinding process. The buffering effect reduces the adhesion of α-alumina B with low α-formation rate to the grinding object, improves the grinding speed and reduces scratches and marks, thereby improving the surface texture.

Benefits of technology

The high speed of high efficiency grinding of hard and brittle materials and good surface texture is achieved, reducing scratches and marks on the grinding object, and significantly improving the surface roughness and smoothness after grinding.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003944166880000141
    Figure BDA0003944166880000141
  • Figure BDA0003944166880000161
    Figure BDA0003944166880000161
Patent Text Reader

Abstract

The present invention relates to a polishing composition. The present invention provides the following method: a polishing object can be polished at a high polishing speed, and the surface quality of the polishing object can be further improved. The present invention is a polishing composition, which is a polishing composition for polishing a polishing object, comprising aluminum oxide abrasive grains and a dispersion medium, wherein the aluminum oxide abrasive grains only contain α-alumina A with an alpha rate of more than 80% and α-alumina B with an alpha rate of less than 80% as crystalline aluminum oxide, and the average particle size of the α-alumina A is smaller than the average particle size of the α-alumina B.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application of the application with application number 201980019008.3, application date March 14, 2019, and invention name “Polishing Composition”. Technical Field

[0002] The present invention relates to a polishing composition. Background Art

[0003] As substrate materials for optical devices and substrate materials for power devices, hard and brittle materials such as aluminum oxide (e.g., sapphire), zirconium oxide, aluminum nitride, silicon nitride, gallium nitride, and silicon carbide are known. Substrates or films formed from these hard and brittle materials are generally stable to chemical reactions such as oxidation, complexation, and etching, and therefore are not easily processed by grinding. Therefore, grinding and cutting using hard materials is common, but there is a problem that the grinding speed becomes low.

[0004] In order to solve such a problem, International Publication No. 2012 / 115020 (corresponding to the specification of U.S. Patent Application Publication No. 2013 / 0324015) discloses a polishing composition, characterized in that it is a polishing composition used for polishing hard and brittle materials with a Vickers hardness of 1500 Hv or more, and contains at least aluminum oxide abrasive grains and water, and has a pH of 8.5 or more, and the aluminum oxide abrasive grains have a pH of 20 m 2 International Publication No. 2012 / 115020 (corresponding to the specification of U.S. Patent Application Publication No. 2013 / 0324015) describes a method for polishing an object made of hard and brittle materials at a high polishing rate by using a polishing composition having such a structure.

[0005] In addition, Japanese Patent Publication No. 2015-120816 and Japanese Patent Publication No. 2011-121151 disclose a polishing liquid composition, which uses a magnetic disk substrate as a polishing object and mixes α-alumina with different alpha-oxidation rates. According to these technologies, a high polishing rate can be obtained and defects on the surface of the polishing object can be reduced. Summary of the invention

[0006] However, in the technology of recording in International Publication No. 2012 / 115020 (corresponding to U.S. Patent Application Publication No. 2013 / 0324015 specification), although the grinding speed becomes high, there is room for improvement in the improvement of the surface quality of the grinding object surface. In addition, the technology of recording in Japanese Patent Publication No. 2015-120816 Gazette and Japanese Patent Publication No. 2011-121151 Gazette is not suitable for the grinding object comprising hard and brittle materials, and there is room for improvement in the improvement of grinding speed, the surface quality of the grinding object surface.

[0007] Therefore, an object of the present invention is to provide a method that can polish an object to be polished at a high polishing rate and can further improve the surface quality of the object to be polished.

[0008] The present inventors have conducted intensive studies to solve the above-mentioned problems. As a result, they have found that the above-mentioned problems can be solved by using a polishing composition containing aluminum oxide abrasive grains containing only α-alumina A having an alpha-oxidation rate of 80% or more and α-alumina B having an alpha-oxidation rate of less than 80% as crystalline aluminum oxides, and the average particle size of the α-alumina A being smaller than the average particle size of the α-alumina B. And, based on the above-mentioned findings, the present invention has been completed.

[0009] That is, the present invention is a polishing composition, which is a polishing composition for polishing an object to be polished, comprising aluminum oxide abrasive grains and a dispersion medium, wherein the aluminum oxide abrasive grains contain only α-alumina A having an alpha conversion rate of 80% or more and α-alumina B having an alpha conversion rate of less than 80% as crystalline aluminum oxides, and the average particle size of the α-alumina A is smaller than the average particle size of the α-alumina B. DETAILED DESCRIPTION

[0010] The present invention is a polishing composition for polishing an object to be polished, comprising aluminum oxide abrasive grains and a dispersion medium, wherein the aluminum oxide abrasive grains contain only α-alumina A having an alpha conversion rate of 80% or more and α-alumina B having an alpha conversion rate of less than 80% as crystalline aluminum oxide, and the average particle size of the α-alumina A is smaller than the average particle size of the α-alumina B. By using the polishing composition of the present invention having such a structure, the object to be polished can be polished at a high polishing rate, and the surface quality of the surface of the object to be polished can be further improved.

[0011] The details of how the polishing composition of the present invention can achieve the above-mentioned effects are not clear, but are presumed as follows.

[0012] α-alumina with a moderately low alpha-oxidation rate also contains components such as amorphous alumina with low hardness, so it becomes easy to cause adhesion to the polishing object, etc., and also brings about the effect of improving the polishing speed, but it is easy to produce marks and scratches, etc., and there is a tendency to reduce the surface quality of the polishing object. On the other hand, α-alumina with a high alpha-oxidation rate and a particle size of the same degree is not easy to cause adhesion to the polishing object, and compared with α-alumina with a low alpha-oxidation rate, marks and scratches are reduced, making the surface quality of the polishing object good, but there is a tendency to be difficult to obtain the effect of improving the polishing speed.

[0013] In contrast, the polishing composition of the present invention uses a combination of an α-alumina A with a small diameter and an α-oxidation rate of 80% or more and an α-alumina B with a larger diameter and an α-oxidation rate of less than 80% than the α-alumina A. By using such a combination, when the α-alumina B is used for polishing, it is believed that there is a case where the α-alumina A with a small diameter and high hardness exists, and the α-alumina A plays a role like a buffer material in the contact between the α-alumina B and the polishing object. As a result, the adhesion of the α-alumina B with a low α-oxidation rate to the polishing object is reduced, and while maintaining a high polishing speed, it is believed that the effect of improving the surface quality of the polishing object can be obtained. In addition, even if scratches are generated, it is assumed that the α-alumina A with a high hardness further polishes the surface of the polishing object, so that the scratches are further reduced.

[0014] It should be noted that the above mechanism is based on speculation, and the present invention is not limited by the above mechanism in any way.

[0015] [Object to be polished]

[0016] Examples of the object to be polished include metals, semiconductors, glass, ceramics, etc., but are not particularly limited.

[0017] According to a preferred embodiment of the present invention, the grinding object comprises a hard and brittle material. Examples of hard and brittle materials include glass, ceramics, stone, and various semiconductor materials. More specifically, diamond, sapphire (aluminum oxide), zirconium oxide, silicon carbide, boron carbide, zirconium carbide, tungsten carbide, silicon nitride, titanium nitride, gallium nitride, aluminum nitride, etc. may be cited.

[0018] According to another preferred embodiment of the present invention, the polishing object includes a hard and brittle material having a Vickers hardness of 1500 Hv or more. Examples of such hard and brittle materials having a Vickers hardness of 1500 Hv or more include sapphire, silicon carbide, gallium nitride, and the like.

[0019] The above-mentioned hard and brittle materials can be used alone or in combination of two or more.

[0020] The polishing object preferably comprises at least one hard and brittle material selected from the group consisting of sapphire, silicon carbide and gallium nitride, more preferably comprises at least one hard and brittle material selected from the group consisting of silicon carbide and gallium nitride, and further preferably comprises silicon carbide. Silicon carbide can be expected to be a semiconductor substrate material with low power loss, excellent heat resistance, etc., and has a particularly great practical advantage in improving its surface properties.

[0021] Next, the structure of the polishing composition of the present invention is described in detail.

[0022] [Alumina Abrasive]

[0023] The polishing composition of the present invention contains aluminum oxide abrasive grains.

[0024] The alumina abrasive grains contain only α-alumina A having an alpha conversion rate of 80% or more and α-alumina B having an alpha conversion rate of less than 80% as crystalline alumina. As crystalline alumina grains, in addition to α-alumina, alumina grains called intermediate aluminas such as γ-alumina, δ-alumina, θ-alumina, η-alumina, κ-alumina, and χ-alumina are known. However, the alumina abrasive grains of the present invention contain only α-alumina A having an alpha conversion rate of 80% or more and α-alumina B having an alpha conversion rate of less than 80% as crystalline alumina, and do not contain intermediate alumina. The fact that the alumina abrasive grains used in the present invention do not contain intermediate alumina can be confirmed as follows: in the diffraction peaks obtained by subjecting the alumina abrasive grains to X-ray diffraction measurement, no peak derived from intermediate alumina is detected, and thus it can be confirmed.

[0025] In addition, the aluminum oxide abrasive grains may contain amorphous aluminum oxide as long as the effects of the present invention are not impaired.

[0026] The alpha conversion rate of α-alumina A is 80% or more, preferably 82% or more, more preferably 85% or more, from the viewpoint of polishing speed and improving surface quality. The upper limit of the alpha conversion rate of α-alumina A is preferably 100% or less, more preferably 95% or less. It should be noted that as long as the alpha conversion rate is within the above range, a variety of α-alumina A can be used.

[0027] In addition, the alpha conversion rate of α-alumina B is lower than 80%, and from the viewpoint of polishing speed and improving surface quality, it is preferably 79% or less, and more preferably 78% or less. In addition, the lower limit of the alpha conversion rate of α-alumina B is preferably 60% or more, and more preferably 70% or more. It should be noted that as long as the alpha conversion rate is within the above range, a variety of α-alumina B can be used.

[0028] In this specification, the alpha conversion rate is a value obtained from the integrated intensity of a diffraction peak (2θ=57.5°) specific to α-alumina in an X-ray diffraction spectrum. More specifically, it can be obtained by the method described in the Examples.

[0029] In the present invention, the average particle size of α-alumina A is smaller than the average particle size of α-alumina B. When the average particle size of α-alumina A is equal to or larger than the average particle size of α-alumina B, although a tendency to improve the polishing rate is seen, there is a tendency for the marks and scratches originating from α-alumina A to increase. In a preferred embodiment, the average particle size of α-alumina A is preferably less than 0.9 times the average particle size of α-alumina B, more preferably less than 0.8 times, and further preferably less than 0.75 times.

[0030] In another preferred embodiment of the present invention, the average particle size of α-alumina A is preferably less than 0.4 μm, more preferably 0.35 μm or less, and further preferably 0.32 μm or less. The lower limit of the average particle size of α-alumina A is preferably 0.1 μm or more, and more preferably 0.2 μm or more.

[0031] In a preferred embodiment of the present invention, the average particle size of α-alumina B is preferably 0.4 μm or more, more preferably 0.41 μm or more, and further preferably 0.43 μm or more. The upper limit of the average particle size of α-alumina B is preferably 5 μm or less, and more preferably 2.5 μm or less.

[0032] In this specification, the average particle size of α-alumina A and α-alumina B is the volume-based median particle size (D50) (volume average particle size) measured by a laser diffraction scattering method. More specifically, it can be measured using a laser diffraction / scattering particle size distribution analyzer (trade name "LA-950") manufactured by Horiba, Ltd.

[0033] In a preferred embodiment of the present invention, the crystallite size of at least one of α-alumina A and α-alumina B is preferably greater than 42 nm, more preferably greater than 45 nm. In another preferred embodiment of the present invention, the crystallite size of α-alumina A is preferably less than 40 nm, more preferably less than 38 nm, and further preferably less than 35 nm. In another preferred embodiment of the present invention, the crystallite size of α-alumina B is preferably greater than 45 nm, more preferably greater than 50 nm, and further preferably greater than 60 nm.

[0034] It should be noted that the crystallite of α-alumina refers to a single crystal constituting secondary particles of α-alumina. The crystallite size can be calculated according to the Scherrer equation based on data obtained from an X-ray diffraction spectrum, and more specifically, can be determined by the method described in the Examples.

[0035] The content of aluminum oxide abrasive grains in the polishing composition (i.e., the total content of α-alumina A and α-alumina B) is not particularly limited, but is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, further preferably 1% by mass or more, and particularly preferably 3% by mass or more from the viewpoint of shortening the processing time. From the viewpoint of polishing stability and cost reduction, the content of the above-mentioned aluminum oxide abrasive grains is appropriately 20% by mass or less, preferably 15% by mass or less, more preferably 12% by mass or less, and further preferably 10% by mass or less. The technology disclosed herein can be preferably implemented, for example, in a manner in which the content of aluminum oxide abrasive grains in the polishing composition is 0.1% by mass or more and 20% by mass or less (preferably 3% by mass or more and 10% by mass or less).

[0036] The mass ratio of α-alumina A to α-alumina B (α-alumina A / α-alumina B) is not particularly limited, and is preferably 5 / 95 or more and 95 / 5 or less. In a preferred embodiment of the present invention, from the viewpoint of obtaining a higher polishing speed, the mass ratio of α-alumina A to α-alumina B (α-alumina A / α-alumina B) is more preferably 7 / 93 or more and 30 / 70 or less, and further preferably 10 / 90 or more and 20 / 80 or less. In another preferred embodiment of the present invention, from the viewpoint of making the surface quality of the polishing object better, the mass ratio of α-alumina A to α-alumina B (α-alumina A / α-alumina B) is more preferably 70 / 30 or more and 93 / 7 or less, and further preferably 80 / 20 or more and 90 / 10 or less.

[0037] α-Alumina A and α-alumina B may use commercial products or synthetic products. There is no particular limitation on the manufacturing method (synthesis method) of α-alumina A and α-alumina B, and they can be manufactured by referring to the general manufacturing method of α-alumina. The alpha-ization rate of α-alumina A and α-alumina B can be controlled, for example, by the roasting temperature and roasting time during manufacturing. Generally, the higher the roasting temperature and the longer the roasting time, the higher the alpha-ization rate. Furthermore, the average particle size of α-alumina A and α-alumina B can be controlled, for example, according to the conditions when the raw powder is pulverized.

[0038] <Abrasive grains other than aluminum oxide abrasive grains>

[0039] The polishing composition of the present invention may contain abrasive grains formed of materials other than the above-mentioned aluminum oxide abrasive grains (hereinafter also referred to as non-aluminum oxide abrasive grains) within a range not impairing the effects of the present invention. Examples of such non-aluminum oxide abrasive grains include: abrasive grains substantially composed of any of oxide particles such as silicon dioxide particles (silicon oxide particles), cerium oxide particles, chromium oxide particles, titanium oxide particles, zirconium oxide particles, magnesium oxide particles, manganese oxide particles, zinc oxide particles, and iron oxide particles; nitride particles such as silicon nitride particles and boron nitride particles; carbide particles such as silicon carbide particles and boron carbide particles; diamond particles; and carbonates such as calcium carbonate and barium carbonate.

[0040] In a preferred embodiment of the present invention, the content ratio of the above-mentioned non-aluminum oxide abrasive is preferably less than 20 mass %, more preferably less than 10 mass %, further preferably less than 5 mass %, and particularly preferably 0 mass %, in the total mass of the abrasive contained in the grinding composition, that is, no non-aluminum oxide abrasive is contained.

[0041] In a preferred embodiment of the present invention, the content of the aluminum oxide abrasive is preferably 80 mass % or more, more preferably 90 mass % or more, further preferably 95 mass % or more, particularly preferably 100 mass % of the total mass of the abrasive contained in the polishing composition.

[0042] [Dispersion medium]

[0043] The dispersion medium used in the grinding composition of the present invention is not particularly limited as long as it can disperse the aluminum oxide abrasive grains. As the dispersion medium, water can be preferably used. From the viewpoint of suppressing the effects of other components, it is preferred to use water that does not contain impurities as much as possible, and specifically, ion exchange water (deionized water), pure water, ultrapure water, distilled water, etc. are more preferably used. The dispersion medium may also contain organic solvents such as lower alcohols and lower ketones that can be uniformly mixed with water as needed. Usually, it is preferred that 90% by volume or more of the dispersion medium contained in the grinding composition is water, and more preferably 95% by volume or more (typically 99% by volume or more) is water.

[0044] [pH]

[0045] According to a preferred embodiment of the present invention, the lower limit of the pH of the polishing composition is preferably 1 or more, more preferably 3 or more, further preferably 5 or more, and particularly preferably 7 or more.

[0046] According to a preferred embodiment of the present invention, the upper limit of the pH of the polishing composition is preferably 12 or less, more preferably 11 or less, and even more preferably 10 or less.

[0047] According to another preferred embodiment of the present invention, the pH of the polishing composition is preferably 7 or more, more preferably 8 or more, and further preferably 8.5 or more, and is preferably 12 or less, more preferably 11 or less, and further preferably 10 or less. Within such a range, the effects of the present invention can be more effectively exerted.

[0048] In order to be adjusted to the desired pH, a pH adjusting agent can be used. As the pH adjusting agent, known acid, alkali or their salts can be used. The pH adjusting agent can be used alone or mixed with two or more. In addition, the addition amount of the pH adjusting agent is not particularly limited yet, and can be suitably adjusted to make the grinding composition become the desired pH.

[0049] In addition, the pH adopts the value measured by the method described in the Examples.

[0050] [Oxidants]

[0051] The polishing composition of the present invention preferably contains an oxidant. The oxidant is a component used to enhance the effect based on polishing, and a water-soluble oxidant is typically used. The oxidant is not particularly limited in interpretation, and it embodies the effect of oxidizing and deteriorating the surface of the polishing object during polishing, resulting in the brittleness of the polishing object surface, which is considered to be beneficial to the polishing based on abrasive grains.

[0052] Examples of the oxidizing agent include: peroxides such as hydrogen peroxide; nitric acid compounds such as nitric acid, ferric nitrate as its salt, silver nitrate, aluminum nitrate, and cerium ammonium nitrate as its complex; persulfuric acid compounds such as potassium peroxymonosulfate and peroxodisulfuric acid, and persulfuric acid compounds such as ammonium persulfate and potassium persulfate as its salt; chloric acid compounds such as chloric acid, its salt, perchloric acid, and potassium perchlorate as its salt; bromine compounds such as bromic acid and potassium bromate as its salt; iodic acid compounds such as ammonium iodate and periodic acid as its salt; Iodine compounds such as sodium periodate and potassium periodate as salts; ferric acid and its salts such as potassium ferrite; permanganic acid and its salts such as sodium permanganate and potassium permanganate; chromic acid and its salts such as potassium chromate and potassium dichromate; vanadic acid and its salts such as ammonium vanadate, sodium vanadate and potassium vanadate; ruthenic acid such as perruthenic acid or its salts; molybdic acid and its salts such as ammonium molybdate and disodium molybdate; rhenic acid such as perrhenium or its salts; tungstic acid and its salts such as disodium tungstate.

[0053] These oxidants can be used alone or in combination of two or more. Among them, from the viewpoint of grinding efficiency, permanganic acid or its salt, peroxide, vanadic acid or its salt, periodic acid or its salt are preferred, and sodium permanganate and potassium permanganate are more preferred.

[0054] In a preferred embodiment, the polishing composition comprises a composite metal oxide as an oxidant. As the composite metal oxide, metal nitrates, ferric acids, permanganic acids, chromic acids, vanadic acids, ruthenic acids, molybdic acids, rhenic acids, and tungstic acids can be cited. Among them, ferric acids, permanganic acids, and chromic acids are more preferred, and permanganic acids are further preferred.

[0055] In a further preferred embodiment, as the above-mentioned composite metal oxide, a composite metal oxide CMO having a univalent or divalent metal element (wherein, excluding transition metal elements) and a 4th period transition metal element of the periodic table can be used. Suitable examples of the above-mentioned univalent or divalent metal element (wherein, excluding transition metal elements) include Na, K, Mg, and Ca. Among them, Na and K are more preferred. Suitable examples of the 4th period transition metal element of the periodic table include Fe, Mn, Cr, V, and Ti. Among them, Fe, Mn, and Cr are more preferred, and Mn is further preferred.

[0056] When the polishing composition of the present invention includes a composite metal oxide (preferably a composite metal oxide CMO) as an oxidant, it may also include an oxidant other than the composite metal oxide, or it may not include an oxidant other than the composite metal oxide. The technology disclosed herein may also be preferably implemented in a manner that substantially does not contain an oxidant (such as hydrogen peroxide) other than the composite metal oxide (preferably a composite metal oxide CMO) as an oxidant.

[0057] The content (concentration) of the oxidant in the polishing composition is preferably 0.1% by mass or more. From the viewpoint of highly and effectively taking into account both the polishing speed and the surface quality, the content of the oxidant is more preferably 0.3% by mass or more, further preferably 0.5% by mass or more, and particularly preferably 0.8% by mass or more. In addition, from the viewpoint of improving smoothness, the content of the above-mentioned oxidant is preferably 10% by mass or less, more preferably 8% by mass or less, further preferably 6% by mass or less, further preferably 5% by mass or less, and particularly preferably 3% by mass or less.

[0058] [Other ingredients]

[0059] The polishing composition of the present invention may further contain, as required, known additives that can be used in polishing compositions (typically high hardness material polishing compositions, such as silicon carbide substrate polishing compositions) such as chelating agents, thickeners, dispersants, surface protective agents, wetting agents, surfactants, organic acids, organic acid salts, inorganic acids, inorganic acid salts, rust inhibitors, preservatives, and mildew inhibitors, within the range that does not impair the effects of the present invention. The content of the above additives can be appropriately set according to the purpose of their addition.

[0060] [Method for producing polishing composition]

[0061] The method for producing the polishing composition is not particularly limited, but preferably comprises the step of mixing α-alumina A having an alpha-oxidation rate of 80% or more and α-alumina B having an alpha-oxidation rate of less than 80% in a dispersion medium together with other components included as required. That is, the present invention provides a method for producing a polishing composition, comprising the step of mixing α-alumina A having an alpha-oxidation rate of 80% or more and α-alumina B having an alpha-oxidation rate of less than 80% in a dispersion medium, wherein the average particle size of the α-alumina A is smaller than the average particle size of the α-alumina B.

[0062] There is no particular limitation on the method for mixing α-alumina A, α-alumina B, and other components included as needed, and for example, they can be mixed using a known mixing device such as a wing stirrer, an ultrasonic disperser, or a homomixer. There is no particular limitation on the manner in which these components are mixed, and for example, all the components can be mixed at once or in a suitably set order.

[0063] The temperature when mixing the components is not particularly limited, but is preferably 10° C. or higher and 40° C. or lower, and heating may be performed to increase the dissolution rate. The mixing time is also not particularly limited.

[0064] The polishing composition of the present invention may be a single-component type or a multi-component type represented by a two-component type. For example, it may be composed as follows: a liquid A containing a part of the components of the polishing composition (typically components other than the dispersion medium) is mixed with a liquid B containing the remaining components so that it can be used for polishing an object to be polished.

[0065] <Concentrate>

[0066] The polishing composition may be in a concentrated form (i.e., in the form of a concentrated polishing liquid) before being supplied to the polishing object. Such a concentrated polishing composition is advantageous from the viewpoints of convenience, cost reduction, etc. during manufacture, circulation, storage, etc. The concentration ratio may be, for example, about 2 to 5 times in terms of volume conversion.

[0067] The grinding composition in the form of such a concentrated liquid can be used in a manner of diluting at a desired time to prepare a grinding liquid and supplying the grinding liquid to the grinding object. The above-mentioned dilution is typically performed as follows: the above-mentioned dispersion medium is added to the above-mentioned concentrated liquid and mixed, so that it can be performed. In addition, when the above-mentioned dispersion medium is a mixture, only a part of the components of the dispersion medium can be added and diluted, or a mixed dispersion medium containing these components in a different amount ratio from the above-mentioned dispersion medium can be added and diluted. In addition, as described later, in a multi-dose grinding composition, a part of the agents can be diluted and mixed with other agents to prepare a grinding liquid, or a plurality of agents can be mixed and the mixture can be diluted to prepare a grinding liquid.

[0068] The content of the abrasive in the above-mentioned concentrated solution is preferably 40% by mass or less. From the viewpoint of the stability of the polishing composition (e.g., the dispersion stability of the abrasive) and filterability, it is more preferably 30% by mass or less, further preferably 20% by mass or less, and particularly preferably 15% by mass or less. In addition, from the viewpoint of convenience during production, circulation, storage, etc., cost reduction, etc., the content of the abrasive in the concentrated solution is preferably 0.2% by mass or more, more preferably 1% by mass or more, further preferably 5% by mass or more, and particularly preferably 10% by mass or more.

[0069] [Grinding method]

[0070] The polishing composition of the present invention can be used for polishing an object to be polished in a mode including the following operations, for example.

[0071] That is, a polishing liquid (slurry) containing any polishing composition disclosed herein is prepared. When preparing the above-mentioned polishing liquid, it may include: applying concentration adjustment (such as dilution), pH adjustment and other operations to the polishing composition to prepare the polishing liquid. Alternatively, the above-mentioned polishing composition may be directly used as a polishing liquid. In addition, in the case of a multi-liquid polishing composition, when preparing the above-mentioned polishing liquid, the following steps may be included: mixing these agents, diluting one or more agents before the mixing, diluting the mixture after the mixing, etc.

[0072] Next, the grinding liquid is supplied to the surface of the grinding object, and grinding is performed by conventional methods. For example, the grinding object is mounted on a general grinding device, and the grinding liquid is supplied to the surface (grinding object surface) of the grinding object through the grinding pad of the grinding device. Typically, the grinding liquid is continuously supplied, and the grinding pad is pressed against the surface of the grinding object so that the two move relative to each other (for example, rotate and move). After the above-mentioned polishing process, the grinding of the grinding object is completed.

[0073] According to one embodiment of the present invention, there is provided: a grinding method for grinding a grinding object containing a hard and brittle material and a method for manufacturing a grinding object that has been ground using the grinding method. The grinding method is characterized in that it includes the following steps: grinding the grinding object using the grinding composition disclosed herein. A preferred embodiment of the grinding method includes the following steps: a step of pre-polishing (pre-polishing step) and a step of finishing polishing (finishing polishing step). The so-called pre-polishing step here refers to a step of pre-polishing the grinding object. In a typical embodiment, the pre-polishing step is a polishing step arranged before the finishing polishing step is about to be performed. The pre-polishing step can be a single-step polishing step or a multi-step polishing step of more than two steps. In addition, the so-called finishing polishing step here refers to a step of finishing polishing the grinding object that has been pre-polished, and is a grinding step arranged at the end (i.e., the most downstream side) in the polishing step performed with a polishing slurry containing abrasive grains. Thus, in a polishing method including a preliminary polishing step and a final polishing step, the polishing composition disclosed herein can be used in the preliminary polishing step, in the final polishing step, or in both the preliminary polishing step and the final polishing step.

[0074] In a preferred embodiment, the polishing process using the above-mentioned grinding composition can be a pre-polishing process. From the aspect that a high grinding speed can be achieved, the grinding composition disclosed herein is suitable for the grinding composition (pre-polishing composition) used in the pre-polishing process of the grinding object surface. In the case where the pre-polishing process includes a multi-step polishing process of more than 2 steps, the polishing process of more than 2 steps in them can also be implemented using any grinding composition disclosed herein. The grinding composition disclosed herein can be preferably used for the pre-polishing of the front section (above-mentioned side). For example, it can also be preferably used in the initial pre-polishing process (typically 1 grinding process) of the grinding process described later.

[0075] In another preferred embodiment, the polishing process using the above-mentioned grinding composition is a finishing polishing process. From the aspect of effectively reducing the number of scratches on the surface after grinding, the grinding composition disclosed herein can be particularly preferably used as the grinding composition (finishing polishing composition) used in the finishing polishing process on the grinding object surface.

[0076] The pre-polishing step and the finishing polishing step can be used for either the polishing using a single-sided polishing device or the polishing using a double-sided polishing device. In the single-sided polishing device, the polishing object is attached to a ceramic plate with wax, the polishing object is held by a holding tool called a carrier, and a polishing composition is supplied while a polishing pad is pressed against a single side of the polishing object while the two are relatively moved (e.g., rotated), thereby polishing a single side of the polishing object. In the double-sided polishing device, the polishing object is held by a holding tool called a carrier, and a polishing composition is supplied from above while a polishing pad is pressed against the opposite side of the polishing object while the two are rotated in relative directions, thereby polishing both sides of the polishing object simultaneously.

[0077] The polishing pad used in each polishing step is not particularly limited, and any of nonwoven type, suede type, hard foamed polyurethane type, abrasive grain-containing type, and abrasive grain-free type can be used.

[0078] The object of grinding after grinding by the above-mentioned grinding method is typically cleaned after polishing. The cleaning can be carried out using a suitable cleaning solution. The cleaning solution used is not particularly limited and can be appropriately selected from known and commonly used ones for use.

[0079] It should be noted that the grinding method may further include any other process on the basis of the above-mentioned pre-polishing process and the finishing polishing process. As such a process, a grinding process performed before the pre-polishing process can be cited. The above-mentioned grinding process is a process for grinding the grinding object by pressing the surface of a grinding plate (such as a cast iron plate) against the grinding object. Therefore, a grinding pad is not used in the grinding process. The grinding process is typically carried out by supplying abrasive grains (typically diamond abrasive grains) between the grinding plate and the grinding object. In addition, the grinding method disclosed herein may include additional processes (cleaning process, polishing process) before the pre-polishing process and between the pre-polishing process and the finishing polishing process.

[0080] The present invention may include providing: a method for manufacturing a polished object (e.g., a method for manufacturing a silicon carbide substrate) and a polished object manufactured by the method, which includes a polishing process using the above-mentioned polishing composition. That is, according to the present invention, a method for manufacturing a polished object and a polished object manufactured by the method are provided, and the method for manufacturing a polished object includes the following steps: supplying any polishing composition disclosed herein to a polished object containing a hard and brittle material and polishing the polished object. The above-mentioned manufacturing method can be implemented by preferably applying the content of any polishing method disclosed herein. According to the above-mentioned manufacturing method, it is possible to effectively provide: a polished object (e.g., a silicon carbide substrate) having a polished surface with improved surface quality after polishing.

[0081] Example

[0082] The present invention is further described in detail by the following examples and comparative examples, but the protection scope of the present invention should not be limited to the following examples.

[0083] The volume average particle size (D50) of the aluminum oxide abrasive grains was measured using a laser diffraction / scattering particle size distribution measuring apparatus (manufactured by Horiba, Ltd., LA-950).

[0084] The alpha conversion rate and crystallite size of the aluminum oxide abrasive grains were determined by X-ray diffraction measurement under the following measurement conditions:

[0085] Equipment: Powder X-ray diffraction equipment Ultima IV manufactured by Rigaku Corporation

[0086] X-ray generating voltage: 40kV

[0087] Radiation: Cu-Kα1 line

[0088] Current: 10mA

[0089] Scanning speed: 10° / min

[0090] Measuring step: 0.01°

[0091] The alpha conversion rate was calculated based on the integrated intensity of the diffraction peak (2θ=57.5°) specific to α-alumina. The crystallite size was calculated using powder X-ray diffraction spectrum comprehensive analysis software JADE (manufactured by MDI, automatic calculation based on Scherrer's formula).

[0092] As alumina particles, three kinds shown in the following Table 1 were prepared.

[0093] [Table 1]

[0094] Table 1

[0095]

[0096] In addition, in the above-mentioned three types of aluminum oxide particles, no peak derived from crystalline aluminum oxide other than α-alumina was confirmed.

[0097] (Example 1)

[0098] Aluminum oxide A1 and aluminum oxide B1 were prepared as abrasive grains, and mixed in water in a manner such that aluminum oxide A1:aluminum oxide B1=1:9 (mass ratio) and the content of the abrasive grains as a whole was 6 mass%. Then, potassium permanganate was added to a content of 2 mass%, and stirred at room temperature (25° C.) for 30 minutes to prepare a dispersion. While checking the pH of the dispersion with a pH meter (manufactured by Horiba, Ltd.), potassium hydroxide aqueous solution (concentration 48 mass%) as an alkali was added to the dispersion to a content of 0.01 mass%, and the pH was adjusted to 9.0 to prepare a polishing composition.

[0099] (Examples 2 to 5)

[0100] A polishing composition was prepared in the same manner as in Example 1 except that the mass ratio of aluminum oxide A1 to aluminum oxide B1 was set to the mass ratio described in Table 2 below.

[0101] (Comparative Examples 1 to 4)

[0102] A polishing composition was prepared in the same manner as in Example 1 except that the alumina particles described in the following Table 2 were used instead of the alumina A1 and the alumina B1.

[0103] (Evaluation of polishing speed and surface quality)

[0104] 〔Grinding speed〕

[0105] Using each of the polishing compositions of Examples 1 to 5 and Comparative Examples 1 to 4, a silicon carbide substrate was polished under the following polishing conditions.

[0106] <Polishing conditions for silicon carbide substrate>

[0107] Silicon carbide (SiC) substrate: 2-inch N-type, 4H-SiC, 4° off

[0108] Polishing device: EJ-3801N (manufactured by ENGIS JAPAN Corporation)

[0109] Polishing pad: Non-woven fabric pad SUBA800 (manufactured by Nitta Haas Co., Ltd.)

[0110] Grinding load: 300g / cm 2

[0111] Plate speed: 80rpm

[0112] Grinding time: 30 minutes

[0113] After polishing with the polishing composition of each embodiment and comparative example, the mass of the SiC substrate was measured, and the difference in mass before and after polishing was divided by the polishing time to calculate the polishing rate. It should be noted that the polishing rate in Table 2 represents the ratio when the polishing rate when the polishing composition of Comparative Example 1 is used is set to 100%.

[0114] [Evaluation of surface quality (Ra, number of concave defects and number of scratches)]

[0115] The surface roughness Ra is as follows: for the surface of the polished object after grinding, an atomic force microscope (AFM, Park Systems, NX-HDM) is used to measure 4 points including the center of each substrate in a measurement field of 10 μm□ (10 μm square), and the average value of 3 substrates is obtained. It should be noted that the surface roughness Ra is a parameter representing the average amplitude of the height direction of the roughness curve, and represents the arithmetic mean of the height of the surface of the polished object in a constant field of view.

[0116] The number of concave defects (dot-shaped depressions) and scratches is as follows: For the AFM images obtained in the above measurement, each one was confirmed using the attached software, and the depth of the concave defects and scratches was also confirmed based on the statistics of 12 images in each case.

[0117] The evaluation results are shown in Table 2 below.

[0118] [Table 2]

[0119]

[0120] It is clear from Table 2 that: when using the grinding composition of the embodiment, the grinding object can be ground at a high grinding speed, and in addition, the number of concave defects is small, and even if scratches occur, it is also very shallow, and the surface roughness of the grinding object surface is also small, and a smooth surface with a high surface quality with few bends can be obtained. In particular, it is known that when using the grinding composition of Examples 1 and 2, a higher grinding speed can be obtained. In addition, it is known that when using the grinding composition of Examples 4 and 5, the surface quality of the grinding object surface is further improved.

[0121] It is found that when the polishing compositions of Comparative Examples 1 to 4 were used, the number of concave defects increased, and the surface quality of the polishing object was reduced.

[0122] It should be noted that the present application is based on Japanese Patent Application No. 2018-061561 filed on March 28, 2018, the disclosure of which is incorporated herein by reference in its entirety.

Claims

1. Use of a polishing composition for polishing hard and brittle materials having a Vickers hardness of 1500 Hv or more, The polishing composition comprises: aluminum oxide abrasive grains, a dispersion medium, and an oxidizing agent. The aluminum oxide abrasive grains contain only α-aluminum oxide A having an alpha conversion rate of 80% or more and α-aluminum oxide B having an alpha conversion rate of less than 80% as crystalline aluminum oxides, and the average particle size of the α-aluminum oxide A is smaller than the average particle size of the α-aluminum oxide B. The oxidant comprises a composite metal oxide, The content of the aluminum oxide abrasive grains, that is, the total content of α-aluminum oxide A and α-aluminum oxide B, is 0.1 mass % or more and 20 mass % or less. The content of the oxidizing agent is 0.1 mass % or more and 10 mass % or less.

2. The use according to claim 1, wherein The content mass ratio of the α-alumina A to the α-alumina B is 5 / 95 or more and 95 / 5 or less.

3. The use according to claim 1 or 2, wherein the pH of the polishing composition is 7 or higher.

4. The use according to claim 1 or 2, wherein The hard and brittle material comprises silicon carbide. 5 . The use according to claim 1 , wherein the polishing composition does not substantially contain an oxidizing agent other than the composite metal oxide. 6 . The use according to claim 1 or 2 , wherein in the polishing composition, the alpha-alumina A has an alpha-reduction rate of 85% or more, and the alpha-reduction rate of α-alumina B has an alpha-reduction rate of 78% or less and 70% or more.