A test method for trace element contamination on the surface of highly hydrophobic and soft membranes
By using the extract to cover the surface of the filter membrane with gravity in the container, the detection problems caused by incomplete immersion of the fluorine material filter membrane and soft texture are solved, and effective detection of trace elements contamination on the surface of hydrophobic and soft membranes is achieved, ensuring that Accuracy and simplicity of detection.
Patent Information
- Application Number
- CN202211189819.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-28
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2042-09-28
AI Technical Summary
The existing integrated immersion extraction method is difficult to effectively detect the surface trace element contamination of the fluorine material filter membrane, especially due to its hydrophobicity and low density, it is difficult to fully contact the extract, and the texture is soft and easy to cause wrinkles.
The filter membrane is placed indirectly in the container, and the gravity of the extract itself is used to cover the surface of the filter membrane. After a certain period of time, the extract liquid is taken out for ICP-MS test. The difference between the two test results is calculated to determine the membrane. The surface pollutant content avoids floating and wrinkling during soaking.
It realizes effective detection of trace elements contamination on the surface of hydrophobic and soft membranes, and is easy to operate, suitable for low-density fluorine material filter membranes, avoids incomplete immersion and wrinkle problems, and improves the accuracy of analysis.
Smart Images

Figure CN115684328B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of membrane surface pollutant testing, and relates to a testing method for trace element contamination on the surface of a highly hydrophobic and soft membrane, and specifically to a testing method for trace element contamination on the surface of a filter membrane material, and especially to a testing method for surface contamination of a fluorine material filter membrane during semiconductor wet etching. Background Art
[0002] With a huge market size and prospects, semiconductor equipment, as the hardware foundation of scientific and technological innovation, has become increasingly valuable and important in the global industrial chain. In the post-Moore era, the compression space for chip manufacturing processes has gradually reached its upper limit, and economic costs are rising. Industrial chain links such as wafer manufacturing and packaging and testing will face higher technical challenges. Semiconductor companies have put forward extremely high requirements for the production environment and the cleanliness of the materials required on the machine.
[0003] In semiconductor equipment, whether through gas, chemicals or water, impurities in various materials may affect the performance, stability and yield of the final product, so pollution control is one of the most concerned issues in semiconductor equipment manufacturing. In order to achieve and maintain the high purity required in the process, the selection of appropriate filters becomes particularly critical to remove impurities and improve purity, thereby ensuring the yield of equipment processing in each link of manufacturing. However, for the core component of the filter, the filter membrane, it must not only meet the application requirements of the actual environment, such as excellent mechanical strength, high temperature resistance, acid and alkali resistance, etc., but also the surface cleanliness of its own material must be guaranteed to avoid contamination of the passing gas, chemicals or water. Therefore, when selecting a suitable filter, it is extremely important to detect the degree of contamination on the surface of the filter membrane material.
[0004] Inductively coupled plasma mass spectrometer (hereinafter referred to as ICP-MS) has the advantages of low detection limit at ppt level, high sensitivity, wide linear dynamic range and simultaneous determination of multiple element contents. Therefore, it has been widely recognized as one of the most effective methods for trace contamination detection in the semiconductor industry. For observing the surface contamination of the sample as a whole, the currently commonly used pre-treatment test method is the overall immersion extraction method, that is, first select an extraction solution of appropriate concentration according to the different materials to fully immerse the sample, recover it after a certain period of time, and use ICP-MS testing to obtain the element content of the entire sample surface. However, for fluorine material filter membranes, due to their extremely low intermolecular forces, they are non-sticky, and their soft texture and low density make it difficult to fully contact the extraction solution during the immersion test, and the surface is not completely immersed. Therefore, it is a challenge to use the immersion method to detect surface contamination of hydrophobic filter membranes.
[0005] Therefore, it is of great significance to develop a test method for trace element contamination on the surface of fluorine material membranes in filters. Summary of the invention
[0006] The present invention is carried out to solve the above technical problems, and aims to provide a testing method for trace element contamination on the surface of a highly hydrophobic and soft membrane.
[0007] The basic idea of the test method of the present invention is as follows: select a suitable container as the shell carrier, use the filter membrane indirectly as a substrate (the excess portion is left at the outer mouth of the container to prevent the entire filter membrane from being scattered inside due to excessive gravity when the extraction solution is added later), use the gravity of the extraction solution itself to fully cover the surface of the filter membrane, take out part of the extraction solution after a certain period of time, and use ICP-MS to test the content of elements in the solution to complete the element contamination test of the entire surface. This method is simple, fast and effective to operate. On the one hand, it avoids the floating phenomenon caused by hydrophobicity and low density when the filter membrane is immersed. On the other hand, it uses the gravity of the extraction solution to fully open the filter membrane to avoid the wrinkling phenomenon caused by soft texture. It is suitable for the analysis of trace element pollutants on the surface of hydrophobic, soft and low-density fluorine materials.
[0008] In order to achieve the above object, the specific scheme adopted by the present invention is as follows:
[0009] The present invention provides a method for testing trace element contamination on the surface of a highly hydrophobic and soft film, comprising the following steps:
[0010] (1) Determination of trace elements in blank samples
[0011] Place a clean, corrosion-resistant empty bottle in the sampling area of a clean room of at least Class 100, add extraction liquid, and place the front end of the clean tweezers in the extraction liquid for 5 to 7 seconds, then cover the lid, record the volume of the extraction liquid used, recover the solution after soaking for a certain period of time, and test the element content in the solution with an inductively coupled plasma mass spectrometer, and record the result as the previous value;
[0012] (2) Determination of trace elements of membrane surface contamination
[0013] Place a corrosion-resistant empty bottle of the same material in a clean room sampling area with the same cleanliness level as step (1), then place the middle area of the polymer film to be tested at the mouth of the bottle, and at the same time use clean tweezers the same as step (1) to gently act on the film at the mouth of the bottle for 5 to 6 seconds, so that the film at this location extends to a certain depth; then slowly add the same volume of extraction solution as step (1) to the film at the mouth of the bottle, record the volume of extraction solution used and the surface area of the film immersed in the solution, recover the solution after a certain period of time, and test the element content in the solution with an inductively coupled plasma mass spectrometer, and record the result as the post value;
[0014] (3) Calculation of trace element concentration on membrane surface
[0015] Take the difference between the two test results and calculate the trace element contamination content on the surface of the polymer membrane material to be tested by the following formula:
[0016]
[0017] Where: C p is the concentration of the test sample (μg / L), recorded as the post-value;
[0018] C B is the concentration of the blank control (μg / L), recorded as the previous value;
[0019] V is the volume of the extract soaking the sample to be tested (L);
[0020] S is the surface area of the immersed membrane (m 2 ).
[0021] Preferably, no chemical or physical reaction, such as corrosion reaction, electrostatic reaction, etc., occurs between the tweezers and the corrosion-resistant empty bottle and the strongly hydrophobic and soft film to be tested.
[0022] Preferably, in terms of material, the corrosion-resistant empty bottle is a PFA empty bottle, the strong hydrophobicity and soft membrane to be tested is a fluorine material filter membrane, and the tweezers are made of the same fluorine material. In the embodiment of the present invention, the corrosion-resistant empty bottle is a PFA empty bottle, the strong hydrophobicity and soft membrane to be tested is a filter PTFE filter membrane, and the tweezers are also made of PTFE material as an example to verify the test effect. The results show that the detection of trace elements of membrane surface contamination can be fully realized.
[0023] The trace elements on the film surface that can be detected by the present invention include metal elements from the second period to the sixth period and five non-metal elements: B, Si, As, Se and Te.
[0024] The containers, corrosion-resistant empty bottles and tweezers used in the testing process must be soaked in a 20% by mass nitric acid solution for at least one week, rinsed with pure water at least six times, blown dry with a high-pressure air gun, and tested on the machine for verification before being used as clean equipment for standby.
[0025] The extraction liquid used is electronic grade water or electronic grade reagent. For fluorine material filter membrane, the electronic grade reagent is electronic grade 10% HCl solution.
[0026] The beneficial effects of the present invention are as follows:
[0027] The present invention uses a comprehensive and fast overall immersion extraction method to extract trace element pollutants on the surface of a highly hydrophobic and soft membrane. The container is used as a shell carrier, and the membrane is fully expanded by the gravity of the extracting liquid, so that it can be fully immersed. On the one hand, the floating phenomenon caused by hydrophobicity and low density during immersion of the filter membrane is avoided, and on the other hand, the wrinkling phenomenon caused by soft texture and low density is avoided. It is very effective for the analysis of trace element pollutants on the surface of such hydrophobic, soft and low-density membranes. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 It is a structural schematic diagram of the method for extracting trace elements on the surface of a highly hydrophobic and soft membrane of the present invention. DETAILED DESCRIPTION
[0029] In order to explain the present invention more clearly, the present invention is further described below in conjunction with preferred embodiments. It should be understood by those skilled in the art that the content described below is illustrative rather than restrictive, and should not be used to limit the scope of protection of the present invention.
[0030] Example 1
[0031] The present embodiment provides a method for analyzing the contamination of trace elements on the filter membrane surface used in the wet etching process. The filter membrane material is a hydrophobic and soft polytetrafluoroethylene (PTFE) material.
[0032] 1L and 20mL perfluoroalkoxy resin (PFA) and polytetrafluoroethylene (PTFE) tweezers were soaked in 20wt% nitric acid solution for one week, then rinsed with pure water six times, blown dry with a high-pressure air gun, and tested on a machine to be used as ultra-clean containers for standby use.
[0033] Place a clean empty perfluoroalkoxy resin (PFA) bottle in the sampling area of a Class 100 or higher clean room, add electronic grade water to the bottle mouth, and place the front end area of clean polytetrafluoroethylene (PTFE) tweezers in ultrapure water for 5 seconds. Finally, cover the lid, soak for a certain period of time, recover the solution, and place it in another clean empty perfluoroalkoxy resin (PFA) bottle. Use inductively coupled plasma mass spectrometry (ICP-MS) to test the element content in the solution, and the result is recorded as the "previous value" (blank sample).
[0034] Place a clean empty perfluoroalkoxy resin (PFA) bottle in the sampling area of a Class 100 or higher clean room, then place the roughly middle area of the polytetrafluoroethylene (PTFE) membrane at the mouth of the bottle, and use clean polytetrafluoroethylene (PTFE) tweezers to gently move the membrane at the mouth of the bottle downward a little (the tweezers act on the polytetrafluoroethylene (PTFE) membrane for about 5 seconds), then slowly add electronic grade water to the mouth of the bottle. Figure 1 As shown, record the volume of the extraction solution used (keep it consistent with the blank sample) and the surface area of the filter membrane immersed in it. After a certain period of time, recover the solution and place it in another clean empty perfluoroalkoxy resin (PFA) bottle. Use inductively coupled plasma mass spectrometry (ICP-MS) to test the element content in the solution, and the result is recorded as the "later value".
[0035] The difference between the two test results is taken and the result is calculated by the following formula, which is the content of trace element pollutants on the surface of the polytetrafluoroethylene (PTFE) membrane to be tested. For details, see Table 1.
[0036]
[0037] Where: C p is the concentration of the test sample (μg / L), recorded as “later value”;
[0038] C B is the concentration of the blank control (μg / L), recorded as “previous value”;
[0039] V is the volume of the sample to be tested immersed (L);
[0040] S is the surface area of the extracted sample (m 2 ).
[0041] Table 1 Test results of electronic grade water-immersed PTFE membrane
[0042]
[0043] Example 2
[0044] In the trace element contamination analysis on the filter membrane surface of the filter used in the wet etching process provided in this embodiment, the filter membrane material is also a hydrophobic and soft polytetrafluoroethylene (PTFE) material.
[0045] 1L and 20mL perfluoroalkoxy resin (PFA) and polytetrafluoroethylene (PTFE) tweezers were soaked in 20wt% nitric acid solution for one week, then rinsed with pure water six times, blown dry with a high-pressure air gun, and tested on a machine to be used as ultra-clean containers for standby use.
[0046] Place a clean empty perfluoroalkoxy resin (PFA) bottle in the sampling area of a Class 100 or higher clean room, add 10% HCL (G4 grade) solution to the bottle mouth, and place the front end area of clean polytetrafluoroethylene (PTFE) tweezers in ultrapure water for 5 seconds. Finally, cover the lid, soak for a certain period of time, recover the solution, and place it in another clean empty perfluoroalkoxy resin (PFA) bottle. Use inductively coupled plasma mass spectrometry (ICP-MS) to test the element content in the solution, and the result is recorded as the "previous value" (blank sample).
[0047] Empty bottle, then place the middle area of the PTFE membrane at the mouth of the bottle, and use clean PTFE tweezers to gently move the membrane down a little (the tweezers act on the PTFE membrane for about 5 seconds), then slowly add 10% HCl (G4 grade) to the mouth of the bottle. Figure 1 As shown, record the volume of the extraction solution used (keep it consistent with the blank sample) and the surface area of the filter membrane immersed in it. After a certain period of time, recover the solution and place it in another clean empty perfluoroalkoxy resin (PFA) bottle. Use inductively coupled plasma mass spectrometry (ICP-MS) to test the element content in the solution, and the result is recorded as the "later value".
[0048] The difference between the two test results is taken and the result is calculated by the following formula, which is the content of trace element pollutants on the surface of the polytetrafluoroethylene (PTFE) membrane to be tested. The results are shown in Table 2.
[0049]
[0050] Where: C p is the concentration of the test sample (μg / L), recorded as “later value”;
[0051] C B is the concentration of the blank control (μg / L), recorded as “previous value”;
[0052] V is the volume of the sample to be tested immersed (L);
[0053] S is the surface area of the extracted sample (m 2 ).
[0054] Table 2 Test results of PTFE membrane soaked in 10% HCl
[0055]
[0056]
[0057] The preferred embodiments of the present invention have been specifically described above, but the present invention is not limited to the embodiments. Those skilled in the art may make various equivalent modifications or substitutions without violating the spirit of the present invention. These equivalent modifications or substitutions are all included in the scope defined by the claims of this application.
Claims
1. A method for testing trace element contamination on the surface of a highly hydrophobic and soft membrane, characterized in that: The steps include: (1) Determination of trace elements in blank samples Place a clean, corrosion-resistant empty bottle in the sampling area of a clean room of at least Class 100, add extraction liquid, and place the front end of the clean tweezers in the extraction liquid for 5 to 7 seconds, then cover the lid, record the volume of the extraction liquid used, recover the solution after soaking for a certain period of time, and test the element content in the solution with an inductively coupled plasma mass spectrometer, and record the result as the previous value; (2) Determination of trace elements of membrane surface contamination Place a corrosion-resistant empty bottle of the same material in a clean room sampling area with the same cleanliness level as step (1), then place the middle area of the polymer film to be tested at the mouth of the bottle, and at the same time use clean tweezers the same as those in step (1) to gently act on the film at the mouth of the bottle for a certain period of time, so that the film at this location extends to a certain depth; then slowly add the same volume of extraction solution as in step (1) to the film at the mouth of the bottle, record the volume of extraction solution used and the surface area of the film immersed in the solution, recover the solution after a certain period of time, and test the element content in the solution with an inductively coupled plasma mass spectrometer, and record the result as the post value; (3) Calculation of trace element concentration on membrane surface Take the difference between the two test results and calculate the trace element contamination content on the surface of the polymer membrane material to be tested by the following formula: Where: C p is the concentration of the test sample, in μg / L, recorded as the latter value; C B is the concentration of the blank control, in μg / L, recorded as the previous value; V is the volume of the extract used to immerse the sample to be tested, in L; S is the surface area of the immersed membrane, unit is m 2 , Among them, the corrosion-resistant empty bottle is a PFA empty bottle, the strongly hydrophobic and soft membrane to be tested is a fluorine material filter membrane, and the tweezers are made of the same fluorine material.
2. The method for testing trace element contamination on the surface of a highly hydrophobic and soft film according to claim 1, characterized in that: in, There is no chemical or physical reaction between the tweezers and the corrosion-resistant empty bottle and the strongly hydrophobic and soft membrane to be tested.
3. The method for testing trace element contamination on the surface of a highly hydrophobic and soft film according to claim 1, characterized in that: in, The corrosion-resistant empty bottle is a PFA empty bottle, the strongly hydrophobic and soft membrane to be tested is a PTFE filter membrane, and the tweezers are also made of PTFE material.
4. The method for testing trace element contamination on the surface of a highly hydrophobic and soft film according to claim 1, characterized in that: in, The trace elements on the film surface include metal elements from the second period to the sixth period and five non-metal elements: B, Si, As, Se and Te.
5. The method for testing trace element contamination on the surface of a highly hydrophobic and soft film according to claim 1, characterized in that: in, The containers, corrosion-resistant empty bottles and tweezers used in the testing process must be soaked in a 20% by mass nitric acid solution for at least one week, rinsed with pure water at least six times, blown dry with a high-pressure air gun, and tested on the machine for verification before being used as clean equipment for standby.
6. The method for testing trace element contamination on the surface of a highly hydrophobic and soft film according to claim 1, characterized in that: in, The extracting liquid used in steps (1) and (2) is electronic grade water or electronic grade reagent.
7. The method for testing trace element contamination on the surface of a highly hydrophobic and soft film according to claim 5, characterized in that: in, When the highly hydrophobic and soft membrane to be tested is a fluorine material filter membrane, the extraction liquid used is electronic grade water or electronic grade 10% HCl.
8. The method for testing trace element contamination on the surface of a highly hydrophobic and soft film according to claim 5, characterized in that: in, In step (2), the membrane at the bottle mouth is gently acted on with tweezers for 5 to 6 seconds to extend the membrane at that location to a certain depth.