Waterproofing agent composition, kit, waterproof fiber product and method for producing the same

By adjusting the molar and mass ratios of polyols and polyisocyanate compounds, a perfluoroalkyl waterproofing agent composition containing no more than 7 carbon atoms was developed, which solved the deficiencies in waterproofing and chalk mark resistance in the existing technology. solve the problem and achieve efficient waterproof fiber products without affecting other properties of fiber products.

CN115698221BActive Publication Date: 2024-10-11MEISEI CHEM WORKS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202180039852.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-06-03
Filing Date
2021-06-03
Publication Date
2024-10-11
Estimated Expiration
2041-06-03

AI Technical Summary

Technical Problem

In the existing technology, perfluorooctane sulfonate and perfluorooctanoic acid in C8 fluorine-based waterproofing agents are regarded as environmental pollutants, and their alternatives, such as C6 fluorine-based waterproofing agents and fluorine-free waterproofing agents, have poor water resistance and chalk mark resistance. It performs poorly, and commonly used softeners and pin slippage preventers will reduce the waterproofness.

Method used

Using the reactant of a polyol compound and a polyisocyanate compound, combined with a waterproofing compound, and adjusting the molar and mass ratios, a waterproofing agent composition that does not contain perfluoroalkyl groups with 7 or more carbon atoms was developed and optimized. Chalk mark resistance and preparation of water-resistant fiber products through specific kits and manufacturing methods.

Benefits of technology

It achieves excellent resistance to chalk marks while suppressing the deterioration of pin slippage and the deterioration of the adhesion of the coating agent, providing highly efficient waterproof fiber products that meet multiple performance requirements for waterproofness, feel and breathability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003972464850000391
    Figure BDA0003972464850000391
  • Figure BDA0003972464850000421
    Figure BDA0003972464850000421
  • Figure BDA0003972464850000441
    Figure BDA0003972464850000441
Patent Text Reader

Abstract

The present invention provides a waterproofing agent composition having excellent chalk mark resistance. A waterproofing agent composition, comprising at least a reactant (AB) of a polyol compound (A) and a polyisocyanate compound (B), and a water-repellent compound (C), wherein the polyol compound (A) is at least one of a polyol compound (A1) having at least one functional group selected from an ether group, a carbonate group, and an ester group, and a polyol compound (A2) having no functional group, the reactant (AB) having an isocyanate group, in the reactant (AB), when the polyol compound (A) is composed only of the polyol compound (A2), the molar ratio (B / A2) of the isocyanate group of the polyisocyanate compound (B) to the hydroxyl group of the polyol compound (A2) is 2.1 or more, the water-repellent compound (C) does not have a perfluoroalkyl group having 7 or more carbon atoms, and the mass ratio (AB / C) of the reactant (AB) to the water-repellent compound (C) is 0.05 or more.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a waterproofing agent composition, a kit, a waterproof fiber product and a method for producing the same. Background Art

[0002] Conventionally, when imparting water repellency to a substrate, a fluorine-based water repellent, particularly a C8 fluorine-based water repellent having a perfluoroalkyl group having 7 or more carbon atoms, has been used because excellent performance can be obtained with a small amount.

[0003] However, in recent years, the biological toxicity and environmental load of perfluorooctane sulfonic acid (PFOS) and perfluorooctanoic acid (PFOA) contained in C8 fluorine-based water repellents have begun to be considered as problems, and there has been a demand for the development of water repellents that do not contain or do not decompose and generate these in the environment.

[0004] Under such background, the development of C6 fluorine-based waterproofing agents without perfluoroalkyl groups having more than 7 carbon atoms and fluorine-free waterproofing agents without using fluorine compounds is being carried out. On the other hand, it is known that these waterproofing agents have many problems, for example, compared with C8 fluorine-based waterproofing agents, the waterproofing is poor. In addition, in the case of treating fiber products, softeners, anti-slip agents for stitches, etc. are used together to improve the physical properties such as the feel and stitch slippage, but it is known that this will reduce the waterproofing, and it is a problem to balance the waterproofing with other physical properties. In addition, in the process of switching from C8 fluorine-based waterproofing agents, among various physical properties, the improvement of chalk marks in particular has become a problem.

[0005] Chalk marks are a phenomenon in which the color of a portion of a fiber product changes when the surface of the fiber product is rubbed or bent, for example. This phenomenon is likely to cause complaints from users and become a problem.

[0006] As a method for improving chalk marks, for example, Patent Document 1 discloses a waterproofing agent containing a silicon-containing polymer obtained by copolymerizing a non-fluorinated (meth)acrylate monomer and an organosilicon macromer having a free radical polymerizable group as essential components. However, in the method described in Patent Document 1, in order to improve chalk marks, it is necessary to use an organosilicon macromer having an expensive free radical polymerizable group. In addition, in order to obtain a high effect, it is necessary to increase the organosilicon macromer content in the polymer, which is disadvantageous in cost, so this method is not practical. In addition, the effect is not sufficient.

[0007] Patent Document 2 discloses that chalk marks can be improved by using an alkyl-modified silicone having an alkyl group having 23 to 40 carbon atoms in a fluorine-based water repellent or a fluorine-free water repellent, but the effect is not sufficient.

[0008] Prior art literature

[0009] Patent Literature

[0010] Patent Document 1: Japanese Patent Application Publication No. 2018-095879

[0011] Patent Document 2: International Publication No. 2019 / 163570A1 Summary of the invention

[0012] Problems to be solved by the invention

[0013] The main object of the present invention is to provide a waterproofing agent composition which does not contain a compound containing a perfluoroalkyl group having 7 or more carbon atoms and has excellent chalk mark resistance. Furthermore, the present invention also aims to provide a kit for preparing the waterproofing agent composition, a waterproof fiber product using the waterproofing agent composition, and a method for producing the same.

[0014] Means of solving problems

[0015] The present inventors have conducted intensive research to solve the above-mentioned problems. As a result, it was found that in a waterproofing agent composition comprising at least a reactant (AB) of a polyol compound (A) and a polyisocyanate compound (B), and a water-repellent compound (C), the polyol compound (A) is at least one of a polyol compound (A1) having at least one functional group selected from an ether group, a carbonate group, and an ester group and a polyol compound (A2) having no functional group, the reactant (AB) has an isocyanate group, and in the reactant (AB), when the polyol compound (A) is composed only of the polyol compound (A2), the molar ratio (B / A2) of the isocyanate group of the polyisocyanate compound (B) to the hydroxyl group of the polyol compound (A2) is 2.1 or more, the water-repellent compound (C) does not have a perfluoroalkyl group having 7 or more carbon atoms, and the water-repellent agent composition having a mass ratio (AB / C) of the reactant (AB) to the water-repellent compound (C) of 0.05 or more has excellent chalk mark resistance. The present invention has been completed through further studies based on these findings.

[0016] That is, the present invention provides the inventions of the aspects disclosed below.

[0017] Item 1. A water repellent composition comprising at least a reaction product (AB) of a polyol compound (A) and a polyisocyanate compound (B), and a water repellency imparting compound (C), wherein:

[0018] The polyol compound (A) is at least one of a polyol compound (A1) having at least one functional group selected from the group consisting of an ether group, a carbonate group and an ester group, and a polyol compound (A2) having no functional group.

[0019] The above-mentioned reactant (AB) has an isocyanate group,

[0020] In the reactant (AB), when the polyol compound (A) is composed only of the polyol compound (A2), the molar ratio (B / A2) of the isocyanate group of the polyisocyanate compound (B) to the hydroxyl group of the polyol compound (A2) is 2.1 or more,

[0021] The water repellency-imparting compound (C) does not have a perfluoroalkyl group having 7 or more carbon atoms,

[0022] The mass ratio (AB / C) of the reactant (AB) to the water repellency-imparting compound (C) is 0.05 or more.

[0023] Item 2. The water repellent composition according to Item 1, wherein the polyol compound (A1) is a polymer polyol compound having at least one group selected from the group consisting of an ether group, a carbonate group, and an ester group as a main chain-forming bonding group.

[0024] Item 3. The waterproofing agent composition according to Item 1 or 2, wherein, in the reactant (AB), when the polyol compound (A) consists only of the polyol compound (A1), the ratio of the number of moles of isocyanate groups of the polyisocyanate compound (B) to the number of moles of hydroxyl groups of the polyol compound (A1) (molar ratio B / A1) is in the range of 1 to 25.

[0025] Item 4. The waterproofing agent composition according to Item 1 or 2, wherein in the reactant (AB), the ratio of the number of moles of isocyanate groups of the polyisocyanate compound (B) to the total number of moles of hydroxyl groups of the polyol compound (A1) and the polyol compound (A2) (molar ratio B / (A1+A2)) is in the range of 1 to 25.

[0026] Item 5. The water repellent composition according to any one of Items 1 to 4, wherein the isocyanate group in the structure of the reactant (AB) is a blocked isocyanate group.

[0027] Item 6. The water repellent composition according to Item 5, wherein the reactant (AB) has a hydroxyl group in its structure.

[0028] Item 7. The water repellent composition according to any one of Items 1 to 6, wherein the reactant (AB) has at least one group selected from the group consisting of a nonionic hydrophilic group, a cationic hydrophilic group, and an anionic hydrophilic group.

[0029] Item 8. The water repellent composition according to any one of Items 1 to 7, comprising a crosslinking agent (D).

[0030] Item 9. A water repellent composition as described in any one of Items 1 to 8, wherein the water repellency imparting compound (C) comprises at least one selected from the group consisting of a fluorine compound having a perfluoroalkyl group having 1 to 6 carbon atoms, a non-fluorine compound having a hydrocarbon group having 7 to 40 carbon atoms, and an organosilicon compound having at least an alkyl group having 3 to 50 carbon atoms.

[0031] Item 10. The waterproofing agent composition according to any one of Items 1 to 9, further comprising a surfactant.

[0032] Item 11. A waterproof fiber product, which is produced by treating the fiber product with the waterproofing agent composition according to any one of Items 1 to 10.

[0033] Item 12. A method for producing a water-repellent fiber product, comprising the step of bringing the water-repellent composition according to any one of Items 1 to 10 into contact with a fiber product.

[0034] Item 13. A kit for preparing a waterproofing agent composition, comprising:

[0035] A first agent comprising at least a reactant (AB) of a polyol compound (A) and a polyisocyanate compound (B); and

[0036] The second agent comprises at least a water-repellency-imparting compound (C), wherein

[0037] The polyol compound (A) is at least one of a polyol compound (A1) having at least one functional group selected from the group consisting of an ether group, a carbonate group, and an ester group, and a polyol compound (A2) having no functional group.

[0038] The reactant (AB) has an isocyanate group,

[0039] In the reactant (AB), when the polyol compound (A) is composed only of the polyol compound (A2), the molar ratio (B / A2) of the isocyanate group of the polyisocyanate compound (B) to the hydroxyl group of the polyol compound (A2) is 2.1 or more,

[0040] The water repellency-imparting compound (C) does not have a perfluoroalkyl group having 7 or more carbon atoms,

[0041] The mass ratio (AB / C) of the reactant (AB) to the water repellency imparting compound (C) is 0.05 or more,

[0042] When used, the first agent and the second agent are mixed to prepare a waterproofing agent composition.

[0043] Item 14. The kit according to Item 13, wherein the isocyanate group in the structure of the reactant (AB) is a blocked isocyanate group.

[0044] Item 15. The kit according to Item 14, wherein the reactant (AB) has a hydroxyl group in its structure.

[0045] Effects of the Invention

[0046] According to the present invention, a waterproofing agent composition that does not contain a compound containing a perfluoroalkyl group having carbon atoms of 7 or more and has excellent chalk mark resistance can be provided. Furthermore, the present invention can provide a kit for preparing the waterproofing agent composition, a waterproof fiber product using the waterproofing agent composition, and a method for producing the same.

[0047] In addition, according to the preferred aspects of the present invention described later, in addition to the chalk mark resistance, the deterioration of stitch slippage and the reduction of adhesion with the coating agent can also be effectively suppressed. As described later, examples of coating agents applied to waterproof fiber products include acrylic resins and polyurethane resins. The coating of waterproof fiber products is carried out, for example, to improve waterproofness (water resistance) and adjust air permeability. For example, if it is a windproof outerwear, the non-coated surface (outside) can be given waterproofness, and the coated surface (inside) can be given windproofness by blocking the fibers with a coating agent (resin). Similarly, if the inner side of the umbrella is coated, the water resistance is improved by blocking. In this way, in waterproof fiber products, acrylic resins, polyurethane resins (such as polycarbonate polyurethane resins, polyether polyurethane resins, polyester polyurethane resins), etc. are mainly used as coating agents according to the purpose (feel, waterproofness, air permeability, moisture permeability, etc.). It can be said that in waterproof fiber products, it is best not to reduce the adhesion with such coating agents (for example, refer to Japanese Patent Publication No. 2018-119250). DETAILED DESCRIPTION

[0048] 1. Waterproofing agent composition

[0049] The waterproofing agent composition of the present invention is a waterproofing agent composition comprising at least a reactant (AB) of a polyol compound (A) and a polyisocyanate compound (B) and a waterproofing agent composition of a compound (C). The polyol compound (A) is at least one of a polyol compound (A1) having at least one functional group selected from an ether group, a carbonate group and an ester group and a polyol compound (A2) not having any of the functional groups. In addition, the reactant (AB) has an isocyanate group. Furthermore, in the reactant (AB), when the polyol compound (A) is composed only of the polyol compound (A2), the molar ratio (B / A2) of the isocyanate group of the polyisocyanate compound (B) to the hydroxyl group of the polyol compound (A2) is 2.1 or more. The waterproofing agent compound (C) does not have a perfluoroalkyl group having more than 7 carbon atoms. The mass ratio (AB / C) of the reactant (AB) to the waterproofing agent compound (C) is 0.05 or more. The waterproofing agent composition of the present invention exhibits excellent chalk mark resistance by having these structures. The waterproofing agent composition of the present invention is described in detail below.

[0050] In the following description, the description will be centered on a one-part waterproofing agent composition comprising a reaction product (AB) of a polyol compound (A) and a polyisocyanate compound (B) and a waterproofing compound (C), but as described later, in the present invention, a two-part kit may be used. The envisioned kit is shown below.

[0051] (Reagent test kit)

[0052] A two-component kit for preparing a waterproofing agent composition, comprising a first component of a reactant (AB) containing at least a polyol compound (A) and a polyisocyanate compound (B) and a second component containing at least a water-repellency-imparting compound (C), wherein the polyol compound (A) is at least one of a polyol compound (A1) having at least one functional group selected from an ether group, a carbonate group and an ester group and a polyol compound (A2) having no functional group, and the reactant (AB) having an isocyanate group (as described later, the isocyanate group may be unblocked or may be blocked). In the reactant (AB), when the polyol compound (A) is composed only of the polyol compound (A2), the molar ratio (B / A2) of the isocyanate group of the polyisocyanate compound (B) to the hydroxyl group of the polyol compound (A2) is 2.1 or more, the water-repellent compound (C) does not have a perfluoroalkyl group having 7 or more carbon atoms, and the mass ratio (AB / C) of the reactant (AB) to the water-repellent compound (C) is 0.05 or more. When used, the first agent and the second agent are mixed to prepare a water-repellent composition.

[0053] The kit of the present invention can be suitably used for the preparation of the waterproofing agent composition of the present invention. In addition, as described later, the waterproofing agent composition of the present invention can be prepared as an aqueous dispersion in which each component is dispersed in water. When using these kits, the first agent and the second agent can be dispersed in water as an aqueous dispersion to prepare the waterproofing agent composition of the present invention. In addition, the first agent and the second agent constituting the kit can also be prepared as aqueous dispersions of each component.

[0054] [Reactants (AB)]

[0055] The reactant (AB) contained in the waterproofing agent composition of the present invention is a reactant of a polyol compound (A) and a polyisocyanate compound (B). The polyol compound (A) forming the reactant (AB) is at least one of a polyol compound (A1) having at least one functional group selected from an ether group, a carbonate group, and an ester group, and a polyol compound (A2) not having any of the functional groups. In addition, the reactant (AB) has an isocyanate group. That is, the reactant (AB) has a urethane bond formed by the reaction of the hydroxyl group of the polyol compound (A) and the isocyanate group of the polyisocyanate compound (B).

[0056] The lower limit of the molar ratio (B / A1) of the isocyanate group of the polyisocyanate compound (B) to the hydroxyl group of the polyol compound (A1) is preferably 1 or more, for example, more than 1, 1.005 or more, or 1.007 or more. The molar ratio (B / A1) is preferably about 1 to 25, more preferably about 1.1 to 20, still more preferably about 1.2 to 15, further preferably about 1.3 to 10, and further preferably about 1.4 to 5. In addition, the mass ratio of the polyol compound (A1) to the polyisocyanate compound (B) when forming the reactant (AB) (referred to as the mass ratio (component (B) / component (A1)) or the mass ratio (B / A1)) is preferably 0.1 to 150, more preferably 0.2 to 110, further preferably 0.4 to 80, further preferably 0.6 to 55, and further preferably 0.8 to 30.

[0057] In the reactant (AB), when the polyol compound (A) is composed only of the polyol compound (A2), the molar ratio (B / A2) of the isocyanate group of the polyisocyanate compound (B) to the hydroxyl group of the polyol compound (A2) is 2.1 or more, and the molar ratio (B / A2) is preferably 2.4 or more, more preferably 2.6 or more, further preferably 2.8 or more, and further preferably 3.0 or more. In addition, the upper limit of the molar ratio (B / A2) is not particularly limited, but is preferably 25 or less, more preferably 20 or less, further preferably 15 or less, further preferably 10 or less, and further preferably 5 or less. The mass ratio of the polyol compound (A2) to the polyisocyanate compound (B) when forming the reactant (AB) (represented as mass ratio (component (B) / component (A2)) or mass ratio (B / A2)) is preferably 0.1 to 150, more preferably 0.2 to 110, further preferably 0.4 to 80, particularly preferably 0.6 to 55, and most preferably 0.8 to 30.

[0058] In the reactant (AB), when the polyol compound (A1) and the polyol compound (A2) are used in combination, the lower limit of the ratio of the number of moles of isocyanate groups of the polyisocyanate compound (B) to the total number of moles of hydroxyl groups of the polyol compound (A1) and the polyol compound (A2) (molar ratio B / (A1+A2)) is preferably 1 or more, for example, more than 1, 1.005 or more, or 1.007 or more. The molar ratio B / (A1+A2) is preferably about 1 to 25, more preferably about 1.1 to 20, further preferably about 1.2 to 15, further preferably about 1.3 to 10, and further preferably about 1.4 to 5. In addition, when a polyol compound (A1) and a polyol compound (A2) are used together in the formation of the reactant (AB), the ratio of the mass of the polyisocyanate compound (B) to the total mass of the polyol compound (A1) and the polyol compound (A2) (represented as the mass ratio (component (B) / component (A1+A2)) or the mass ratio B / (A1+A2)) is preferably 0.1 to 150, more preferably 0.2 to 110, further preferably 0.4 to 80, further preferably 0.6 to 55, and further preferably 0.8 to 30.

[0059] As described above, the reactant (AB) may have a hydroxyl group in its structure in addition to an isocyanate group and a carbamate bond. That is, the reactant (AB) may be a compound having a hydroxyl group, an isocyanate group and a carbamate bond. In addition, when the reactant (AB) has a hydroxyl group, usually, the isocyanate group becomes a blocked isocyanate group described later. Furthermore, when a polyol compound (A1) is used in the formation of the reactant (AB), the reactant (AB) may further contain at least one functional group selected from an ether group, a carbonate group and an ester group.

[0060] From the viewpoint of product stability and processing stability, the isocyanate group in the structure of the reactant (AB) may be a blocked isocyanate group (blocked isocyanate group) in which the isocyanate group is protected by a blocking agent. That is, in the present invention, the concept of the isocyanate group of the reactant (AB) includes an unblocked isocyanate group and a blocked isocyanate group (blocked isocyanate group) in which the isocyanate group is protected by a blocking agent. The isocyanate groups in the reactant (AB) may be partially or completely blocked (protected) with a blocking agent. For example, preferably, more than 50 mol% of the isocyanate groups are blocked with a blocking agent, more preferably more than 60 mol%, further preferably more than 70 mol%, particularly preferably more than 80 mol%, and most preferably more than 90 mol% are blocked with a blocking agent.

[0061] As the blocking agent for introducing the above-mentioned isocyanate group, a known blocking agent can be used, which is a compound having one or more active hydrogen in the molecule, and one or more kinds can be used alone or in appropriate combination. Examples of blocking agents include: alcohol compounds, alkylphenol compounds, phenol compounds, active methylene compounds, thiol compounds, amide compounds, imide compounds, imidazole compounds, imidazoline compounds, pyrimidine compounds, guanidine compounds, triazole compounds, carbamic acid compounds, urea compounds, oxime compounds, amine compounds, imide compounds, imine compounds, pyrazole compounds, hydrogen sulfite, etc. Among them, amide compounds, active methylene compounds, oxime compounds, pyrazole compounds, and amine compounds are preferred, and preferably, ε-caprolactam, acetylacetone, diethyl malonate, methyl ethyl ketone oxime, cyclohexanone oxime, 3-methylpyrazole, 3,5-dimethylpyrazole, dipropylamine, dibutylamine, propylbenzylamine, butylbenzylamine, diethanolamine, etc. can be used.

[0062] As described above, in the case where the isocyanate group possessed by the above-mentioned reactant (AB) is an isocyanate group protected by a blocking agent, it can also be a compound in which the hydroxyl group derived from the polyol compound (A) remains in the structure. Such a reactant (AB) can be obtained, for example, by blocking a part of the reactive functional group (isocyanate group) of the polyisocyanate compound (B) with a blocking agent, and then reacting the polyol compound (A) in an excessive manner with respect to the residual isocyanate group. At this time, the polyol compound (A) reacts with at least a part of the polyisocyanate (B), and the molar ratio of the reactive functional group and the mass ratio of the two components are as long as they are within the above range. In addition, when the difference between the reaction rate of the blocking agent and the polyol compound (A) for the isocyanate group is sufficient, a method in which the polyol compound (A), the polyisocyanate compound (B) and the blocking agent are all mixed and reacted can also be adopted.

[0063] From the viewpoint of product stability and processing stability, the above-mentioned reactant (AB) preferably has self-emulsification (dispersibility), for example, a method of introducing a nonionic hydrophilic group, a cationic hydrophilic group, or anionic hydrophilic group into a part of the isocyanate group in the reactant (AB), and a nonionic hydrophilic group is particularly preferred. As the hydrophilic compound reacted to impart self-emulsification, known hydrophilic compounds can be used, examples of which include polyoxyalkylene monoalkyl ethers such as polyethylene glycol monomethyl ether, polyethylene glycol monoethyl ether, polyethylene glycol polypropylene glycol monomethyl ether, polypropylene glycol polyethylene glycol monobutyl ether; (poly)ethylene glycols such as ethylene glycol or diethylene glycol, triethylene glycol, polyethylene glycol; block copolymers, random copolymers, random copolymers of ethylene oxide and propylene oxide, ethylene oxide and butylene oxide of polyethylene glycol, polypropylene glycol, and polytetramethylene glycol; polyoxyalkylene monoamines, polyoxyalkylene diamines, etc., preferably polyethylene glycol monomethyl ether, polyethylene glycol monoethyl ether, etc. The above-mentioned nonionic hydrophilic compounds can be used alone or in combination of two or more. Self-emulsification (dispersibility) can be imparted by introducing a specified amount of these compounds relative to the isocyanate group in the reactant (AB). The amount of these compounds introduced is preferably about 0.5 to 50 mol %, more preferably about 0.6 to 40 mol %, further preferably about 0.7 to 30 mol %, particularly preferably 0.8 to 20 mol %, and most preferably 1 to 10 mol %, based on the isocyanate groups in the reactant (AB).

[0064] The reactant (AB) may be a compound into which a portion of urea groups are introduced (excluding compounds derived from a capping agent), and the urea groups may be introduced by partial reaction with water, aliphatic polyamines such as ethylenediamine, trimethylenediamine, hexamethylenediamine, and diethylenetriamine, or alicyclic polyamines such as isophoronediamine in the production process.

[0065] Hereinafter, the polyol compound (A) and the polyisocyanate compound (B) constituting the reactant (AB) will be described in detail.

[0066] (Polyol compound (A))

[0067] The polyol compound (A) (hereinafter, sometimes described as component (A)) is a compound having a plurality of hydroxyl groups (reactive functional groups). Among the polyol compounds (A1) and (A2), the polyol compound (A) is preferably a polyol compound (A1) (hereinafter, sometimes described as component (A1)) having at least one group selected from an ether group, a carbonate group and an ester group in its structure. The polyol compound (A) may be a monomer or a substance that reacts the monomer to form a dimer or more (e.g., a polymer polyol compound that is a polymer). When reacting the monomer to form a dimer or more, the monomers that form the polyol compound (A1) may be one or more.

[0068] When the polyol compound (A1) is a polymer polyol compound, its number average molecular weight is, for example, 80 to 5000 g / mol, preferably 120 to 4000 g / mol, more preferably 160 to 3000 g / mol, and particularly preferably 200 to 2000 g / mol. When the polyol compound (A1) is a polymer polyol compound, examples of the bonding groups of its main chain include polymer polyol compounds containing at least one of carbonate groups, ester groups and ether groups as structural units. Among them, polymer polyol compounds having carbonate groups as bonding groups of the main chain, polymer polyol compounds having carbonate groups and ester groups as bonding groups of the main chain, polymer polyol compounds having ester groups as bonding groups of the main chain, and polymer polyol compounds having ether groups as bonding groups of the main chain are preferred.

[0069] As the polyol compound (A1), known polyols for polyurethane (urea) synthesis can be used, and examples thereof include polycarbonate polyols, polyester polyols, polyether polyols, and the like.

[0070] As the polycarbonate polyol, a known polycarbonate polyol can be used, and it can be obtained, for example, by a method of reacting a polyol monomer with phosgene, a method of reacting a polyol monomer with a carbonate (for example, dimethyl carbonate, diethyl carbonate, diphenyl carbonate, etc.), or the like.

[0071] The polyol monomer is not particularly limited, and examples thereof include aliphatic polyol monomers, polyol monomers having an alicyclic structure, aromatic polyol monomers, polyester polyol monomers, polyether polyol monomers, and the like.

[0072] The aliphatic polyol monomer is not particularly limited, and examples thereof include linear aliphatic diols such as ethylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, and 1,12-dodecanediol; linear aliphatic diols such as 1,2-propylene glycol, 1,3-butanediol, 2-methylene glycol, and 1,6-heptanediol; linear aliphatic diols such as ethylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, and 1,12-dodecanediol; linear aliphatic diols such as 1,2-propylene glycol, 1,3-butanediol, and 2-methylene glycol; linear aliphatic diols such as 1,2- Branched-chain aliphatic diols such as 1,3-propanediol, 1,4-pentanediol, 2-methyl-1,4-butanediol, neopentyl glycol, 1,5-hexanediol, 2-methyl-1,5-pentanediol, 3-methyl-1,5-pentanediol, 2-methyl-1,8-octanediol, 2-methyl-1,9-nonanediol, and 2-methyl-1,3-propanediol; polyols having three or more hydroxyl groups such as trimethylolpropane and pentaerythritol; and the like.

[0073] The polyol monomer having an alicyclic structure is not particularly limited, and examples thereof include 1,3-cyclopentanediol, 1,3-cyclohexanediol, 1,4-cyclohexanediol, 1,3-cyclohexanedimethanol, 1,4-cyclohexanedimethanol, 1,4-cycloheptanediol, 2,7-norbornanediol, 1,4-bis(hydroxyethoxy)cyclohexane, isosorbide, dimer diol, and the like.

[0074] The aromatic polyol monomer is not particularly limited, and examples thereof include catechol, hydroquinone, resorcinol, 1,3-benzenedimethanol, 1,4-benzenedimethanol, bisphenol A, and the like.

[0075] The polyester polyol monomer is not particularly limited, and examples thereof include polyester polyols of hydroxycarboxylic acid and diol such as polyester polyol of 6-hydroxycaproic acid and hexanediol, and polyester polyols of dicarboxylic acid and diol such as polyester polyol of adipic acid and hexanediol.

[0076] The polyether polyol monomer is not particularly limited, and examples thereof include polyalkylene glycols such as polyethylene glycol, polypropylene glycol, and polytetramethylene glycol.

[0077] The polycarbonate polyol may be obtained from these polyol monomers alone or in combination of two or more. Such a polycarbonate polyol is available as a commercial product.

[0078] As the polyester polyol, known polyester polyols can be used, which can be obtained, for example, by reacting a polyol monomer with a polybasic acid. The polybasic acid may be a carboxylic anhydride, a carboxylic acid halide, or a carboxylic acid ester (eg, methyl carboxylate, ethyl carboxylate, etc.) derived from a carboxylic acid.

[0079] The polyester polyol is not particularly limited, and examples thereof include polyethylene adipate diol, polybutylene adipate diol, polyethylene adipate diol, polyhexamethylene adipate diol, polyethylene succinate diol, polybutylene succinate diol, polyethylene sebacate diol, polybutylene sebacate diol, poly-ε-caprolactone diol, poly(3-methyl-1,5-pentanediol adipate) diol, poly(3-methyl-1,5-pentanediol adipate isophthalate) diol, and a polycondensate of 1,6-hexanediol and a dimer acid. Such polyester polyols can be obtained as commercial products.

[0080] As the polyether polyol, known polyether polyols can be used, for example, polytrimethylene glycol, polytetramethylene glycol, etc. In addition, compounds containing 2 to 8 active hydrogen atoms in one molecule described in

[0010] to

[0013] of JP-A-2020-2197 can be used.

[0081] As the alkylene oxide, ethylene oxide (EO), propylene oxide (PO), butylene oxide (BO), styrene oxide, etc. can be used, and they can be used alone or in combination of two or more. In addition, when two or more are used in combination, the addition method can be block addition or random addition.

[0082] As the compound containing active hydrogen atoms, water, alcohol, and amino group-containing compounds can be preferably used. As compounds obtained from water and divalent alcohols (e.g., ethylene glycol, propylene glycol, 1,3-butanediol, 1,4-butanediol, 1,6-hexanediol, 3-methylpentanediol, diethylene glycol, neopentyl glycol, 1,4-bis(hydroxymethyl)cyclohexane, 1,4-bis(hydroxyethyl)benzene, 2,2-bis(4,4'-hydroxycyclohexyl)propane), polyalkylene glycols (e.g., polyethylene glycol, polypropylene glycol, polybutylene glycol, or random copolymers or block copolymers of EO·PO, EO·BO, PO·BO, or EO·PO·BO), alkylene oxide adducts, and the like are listed.

[0083] Alkylene oxide adducts of trivalent or higher alcohols (for example, trivalent alcohols such as glycerol and trimethylolpropane; 4-8valent alcohols such as pentaerythritol, diglycerol, α-methyl glucoside, sorbitol, xylitol, mannitol, dipentaerythritol, glucose, fructose, sucrose, etc.) and alkylene oxide adducts of amino group-containing compounds (for example, ammonia; alkylamines having 1 to 20 carbon atoms; aliphatic polyamines such as ethylenediamine, trimethylenediamine, hexamethylenediamine, diethylenetriamine, etc.; alkanolamines such as monoethanolamine, diethanolamine, triethanolamine, triisopropanolamine, etc.) can also be preferably used.

[0084] In addition, the above-mentioned polyol compound (A) may be a polyol compound (A2) (hereinafter sometimes described as component (A2)) which does not have any of an ether group, a carbonate group, or an ester group in its structure. As the polyol compound (A2), for example, the above-mentioned polyol monomer, a compound containing an active hydrogen atom (a compound having two or more hydroxyl groups), etc. can be used.

[0085] The number of hydroxyl groups in one molecule of the polyol compound (A) may be 2 or more, and a polyol compound (A) having a large number of hydroxyl groups is preferred, for example, from the viewpoint of improving washing durability. However, in order to increase the possibility of gelation when reacting with the polyisocyanate compound (B), the number of hydroxyl groups in one molecule of the polyol compound (A) is preferably 2 to 5, more preferably 2 to 4, and even more preferably 2 to 3.

[0086] (Polyisocyanate compound (B))

[0087] As the polyisocyanate compound (B) (hereinafter sometimes described as component (B)), one or more known isocyanate compounds having two or more isocyanate groups (reactive functional groups) in one molecule can be used alone or in appropriate combination. In addition, in the present invention, the isocyanate group of the isocyanate compound can be a blocked isocyanate group (blocked isocyanate group) in which the isocyanate group is protected by a blocking agent. That is, in the present invention, the isocyanate group of the polyisocyanate compound (B) includes an unblocked isocyanate group and an isocyanate group protected by a blocking agent (blocked isocyanate group).

[0088] Examples of the polyisocyanate compound include aliphatic polyisocyanates, alicyclic polyisocyanates, aromatic polyisocyanates, aromatic aliphatic polyisocyanates, etc. Examples of the aliphatic polyisocyanate include 1,4-tetramethylene diisocyanate, 1,5-pentamethylene diisocyanate, 1,6-hexamethylene diisocyanate, 2,2,4-trimethylhexamethylene diisocyanate, 2,4,4-trimethylhexamethylene diisocyanate, lysine diisocyanate, dimer acid diisocyanate, etc. Examples of the alicyclic polyisocyanate include 1,3-bis(isocyanatomethyl)cyclohexane, 1,4-bis(isocyanatomethyl)cyclohexane, 3-isocyanatomethyl-3,3,5-trimethylcyclohexane (isophorone diisocyanate), bis-(4-isocyanatocyclohexyl)methane (hydrogenated MDI), norbornane Diisocyanates, etc., as aromatic polyisocyanates, examples thereof include: 2,4'-diphenylmethane diisocyanate, 4,4'-diphenylmethane diisocyanate, crude MDI, 1,4-phenylene diisocyanate, 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, 3,3'-dimethyl-4,4'-diisocyanatobiphenyl, 3,3'-dimethyl-4,4'-diisocyanatodiphenylmethane, 1,5-naphthalene diisocyanate, etc., as aromatic aliphatic polyisocyanates, examples thereof include: 1,3-phenylenedimethyl diisocyanate, 1,4-phenylenedimethyl diisocyanate, α,α,α',α'-tetramethylphenylenedimethyl diisocyanate, etc. Also preferably used are reactants of these compounds, for example, isocyanate-modified products obtained by uretdione reaction, isocyanurate reaction, carbodiimidization reaction, uretonimidization reaction, biuretization reaction, and the like with addition-type polyisocyanates, and mixtures thereof.

[0089] Here, in the case of the above-mentioned isocyanate-modified product, the reactive functional group refers to the isocyanate group remaining in the structure. For example, the number of reactive functional groups (isocyanate groups) is 3 when 1,6-hexamethylene diisocyanate is trimerized by isocyanuration reaction.

[0090] In the case of an adduct-type polyisocyanate, the reactive functional group refers to the isocyanate group remaining in the structure, as in the case of the above-mentioned modified isocyanate, but in the case of an adduct derived from the above-mentioned polyol compound (A), it is a substance separated into the polyol compound (A) as a precursor and the polyisocyanate compound (B). For example, in the case of an adduct obtained from 1 molecule of trimethylolpropane and 3 molecules of 2,4-toluene diisocyanate, the number of reactive functional groups is 3 hydroxyl groups and 6 isocyanate groups.

[0091] In the present invention, in order to obtain more excellent effects, aliphatic polyisocyanates, alicyclic polyisocyanates, aromatic polyisocyanates and aromatic aliphatic polyisocyanates can be preferably used, aliphatic polyisocyanates, alicyclic polyisocyanates and aromatic aliphatic polyisocyanates are more preferred, and aliphatic polyisocyanates and alicyclic polyisocyanates are further preferred.

[0092] (Water repellency imparting compound (C))

[0093] As the water-repellent compound (C) (hereinafter sometimes described as component (C)), various selections can be made from substances used as known water-repellents (excluding water-repellents containing perfluoroalkyl compounds having 7 or more carbon atoms) according to the target performance (e.g., water-repellency). As the water-repellent compound (C), for example, a fluorine compound having a perfluoroalkyl group having 1 to 6 carbon atoms (e.g., a fluorine-containing polymer having a structure derived from a polymerizable compound (monomer; fluorine-containing monomer) having a perfluoroalkyl group having 1 to 6 carbon atoms and a carbon-carbon double bond), a non-fluorine compound having a hydrocarbon group having 7 to 40 carbon atoms (e.g., a non-fluorine-containing polymer having a structure derived from a polymerizable compound (monomer; non-fluorine-containing monomer) having a hydrocarbon group having 7 to 40 carbon atoms and a carbon-carbon double bond). These fluorine compounds and non-fluorine compounds can be used in combination.

[0094] The fluorine compound having a perfluoroalkyl group having 1 to 6 carbon atoms is preferably a polymer containing at least a monomer represented by the following general formula (1) in a structural unit.

[0095] CH2=C(-X)-C(=O)-YZ-Rf (1)

[0096] [In the formula, X is a hydrogen atom, a monovalent organic group (such as methyl, ethyl, etc.), a halogen atom, or a group -CH2-C(=O)-YZ-Rf, Y is -O- or -NH-, Z is a direct bond or a divalent organic group, and Rf is a perfluoroalkyl group having 1 to 6 carbon atoms. In addition, when Y, Z, and Rf exist in a molecule in plurality, they may be the same or different. The above monovalent organic group does not include the group -CH2-C(=O)-YZ-Rf.]

[0097] As the polymerizable compound having a perfluoroalkyl group having 1 to 6 carbon atoms and a carbon-carbon double bond as represented by the general formula (1) above (monomer, sometimes described as C1a), any polymerizable compound having a perfluoroalkyl group having 1 to 6 carbon atoms may be used, preferably a polymerizable compound having a perfluoroalkyl group having 2 to 6 carbon atoms, more preferably a perfluoroalkyl group having 4 to 6 carbon atoms, and particularly preferably a perfluoroalkyl group having 6 carbon atoms. Specifically, a monomer having a perfluoroalkyl group having 1 to 6 carbon atoms among the fluorinated monomers described in paragraphs

[0027] to

[0037] of JP-A-2019-196463 can be used. From the viewpoint of water resistance and versatility, 3,3,4,4,5,5,6,6,6-nonafluorohexyl (meth)acrylate, 3,3,4,4,5,5,6,6,7,7,8,8,8-tridecafluorooctyl (meth)acrylate, and 3,3,4,4,5,5,6,6,7,7,8,8,8-tridecafluorooctyl α-chloroacrylate can be preferably used.

[0098] The non-fluorine compound having a hydrocarbon group having 7 to 40 carbon atoms is preferably a polymer containing at least a monomer represented by the following general formula (2) in a structural unit.

[0099] CH2=C(-X)-C(=O)-YR (2)

[0100] [In the formula, X is a hydrogen atom, a monovalent organic group (such as methyl, ethyl, etc.), a halogen atom (excluding fluorine atoms) or a group -CH2-C(=O)-YR, Y is a divalent to tetravalent linking group having at least one group selected from -O- and -NH- or -NR-, and R is a hydrocarbon group having 7 to 40 carbon atoms. In addition, when Y and R exist in a molecule in multiple numbers, each may be the same or different. The above monovalent organic group does not include the group -CH2-C(=O)-YZ-Rf.]

[0101] In the above general formula (2), Y is preferably -Y'-, -Y'-C(=O)-, -C(=O)-Y'-, -Y'-C(=O)-Y'-, -Y'-R'-, -Y'-R'-Y'-, -Y'-R'-Y'-C(=O)-, -Y'-R'-C(=O)-Y'-, -Y'-R'-Y'-C(=O)-Y'-, or -Y'-R'-Y'-R'-, Y' is a direct bond, -O- or -NH-, and R' is -(CH2) m -(m is an integer from 1 to 5) or -C6H6-(phenylene).

[0102] As the polymerizable compound (monomer, sometimes recorded as C1b) having a hydrocarbon group with 7 to 40 carbon atoms and a carbon-carbon double bond as represented by the above general formula (2), any polymerizable compound having a hydrocarbon group with 7 to 40 carbon atoms may be used, and preferably a straight-chain or branched hydrocarbon group with 7 to 40 carbon atoms, and more preferably a straight-chain hydrocarbon group. In addition, the hydrocarbon group is preferably an aliphatic hydrocarbon group, more preferably a saturated aliphatic hydrocarbon group, and particularly preferably an alkyl group. The number of carbon atoms in the hydrocarbon group is preferably 10 to 30, more preferably 12 to 26, particularly preferably 16 to 24, and most preferably 18 to 22. From the viewpoint of water resistance and versatility, lauryl (meth)acrylate, stearyl (meth)acrylate, eicosyl (meth)acrylate, behenyl (meth)acrylate, etc. can be preferably used.

[0103] In addition, non-fluorine monomers (α-substituted acrylates) as described in paragraphs

[0014] to

[0016] of JP-A-2017-66325 can be used, and for example, lauryl α-chloroacrylate, stearyl α-chloroacrylate, eicosyl α-chloroacrylate, behenyl α-chloroacrylate, etc. can be preferably used.

[0104] Furthermore, in the non-fluorine monomers (amide-containing monomers) described in paragraphs

[0015] to

[0020] of International Publication No. 2019 / 026593 and paragraphs

[0016] to

[0020] of Japanese Patent Publication No. 2019-26747, acrylic non-fluorine monomers can be used. For example, preferably, lauric acid amide ethyl (meth) acrylate, myristic acid amide ethyl (meth) acrylate, palmitic acid amide ethyl (meth) acrylate, stearic acid amide ethyl (meth) acrylate, behenic acid amide ethyl (meth) acrylate, lauryl (meth) acrylamide, cetyl (meth) acrylamide, stearyl (meth) acrylamide, behenyl (meth) acrylamide, etc. can be used.

[0105] In addition, non-fluorine monomers (containing carbamate or urea monomers) as described in paragraphs

[0016] to

[0023] of Japanese Patent Gazette No. 2019-26746 can be used. For example, it is preferred to use a compound obtained by reacting hydroxyalkyl (meth) acrylate or hydroxyalkyl (meth) acrylamide with a long-chain alkyl isocyanate (for example, lauryl isocyanate, myristyl isocyanate, cetyl isocyanate, stearyl isocyanate, behenyl isocyanate, etc.), or a compound obtained by reacting a side chain with an isocyanate group (for example, 2-methacryloyloxyethyl methacrylate, etc.) with a long-chain alkylamine (for example, laurylamine, myristylamine, cetylamine, stearylamine, behenylamine, etc.) or a long-chain alkyl alcohol (for example, lauryl alcohol, myristyl alcohol, cetyl alcohol, stearyl alcohol, behenyl alcohol, etc.).

[0106] As polymerizable compounds (monomers) having a hydrocarbon group having 7 to 40 carbon atoms and a carbon-carbon double bond other than the general formula (2), non-fluorinated monomers described in paragraphs

[0016] to

[0034] of JP-A-2017-538793 can be used, for example, sorbitan tristearate methacrylate (described in paragraph

[0077] ), sorbitan tristearate carbamate methacrylate (described in paragraph

[0078] ), sorbitan tristearate carbamate styrene monomer (described in paragraph

[0079] ), sorbitan trioleate methacrylate (described in paragraph

[0080] ), etc. can be preferably used.

[0107] In addition, the monomers represented by the general formula (1) and (2) can use monomers having a perfluoroalkyl group having 1 to 6 carbon atoms among the fluorine-containing monomers described in paragraphs

[0023] and paragraphs

[0026] to

[0029] of International Publication No. 2016 / 178429, for example, itaconate diesters having a perfluoroalkyl group having 1 to 6 carbon atoms (particularly the monomers described in paragraph

[0103] ) can be preferably used. In addition, among the non-fluorine-containing monomers described in paragraphs

[0025] and paragraphs

[0034] to

[0036] , monomers having a hydrocarbon group having 6 to 40 carbon atoms can be used, for example, itaconate distearyl ester can be preferably used.

[0108] As the components constituting the above-mentioned fluorine-containing polymer or the above-mentioned fluorine-free polymer, one of the above-mentioned monomers can be used alone or two or more of the above-mentioned monomers can be used in combination. In addition, as for the content, as long as it is within the range that can achieve the target performance (especially water resistance), there is no particular limitation. As the content of the above-mentioned monomer in the case of requiring high water resistance, 20 mass % or more is sufficient, preferably 30 mass % or more, more preferably 40 mass % or more, further preferably 50 mass % or more, especially preferably 60 mass % or more, and particularly preferably 70 mass % or more.

[0109] In addition, according to other required properties (for example, water repellency and washing durability), other polymerizable compounds (monomers) having carbon-carbon double bonds may be copolymerized, and the methods include known random copolymerization, alternating copolymerization, block copolymerization, graft copolymerization, etc.

[0110] As other monomers, known monomers such as those described later may be used alone or in a copolymer of two or more thereof, and their content is not particularly limited, and may be, for example, 80% by mass or less, preferably 70% by mass or less, more preferably 60% by mass or less, further preferably 50% by mass or less, particularly preferably 40% by mass or less, and particularly preferably 30% by mass or less.

[0111] The other monomers are not particularly limited, and for example, (meth)acrylic acid alkyl esters having 1 to 6 carbon atoms can be used, and examples thereof include methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, hexyl (meth)acrylate, and the like.

[0112] In addition, (meth)acrylates having a cyclic hydrocarbon group described in paragraphs

[0027] to

[0030] of JP-A-2019-26746 may be used, examples of which include cyclohexyl (meth)acrylate, tert-butylcyclohexylcyclohexyl (meth)acrylate, benzyl (meth)acrylate, isobornyl (meth)acrylate, and the like.

[0113] In addition, halogenated olefins described in paragraph

[0035] of JP-A-2019-26746 may be used, and examples thereof include vinyl chloride and vinylidene chloride.

[0114] In addition, an organosilicon compound having a polymerizable group (sometimes described as C1c) can be used. The polymerizable group can be a group introduced into the side chain and / or the end of the organosilicon. Preferably, the polymerizable group is introduced into one end or both ends, and particularly preferably one end. For example, without particular limitation, an organosilicon compound having a carbon-carbon double bond or an organosilicon compound having a mercapto group can be used, specifically, for example, an organosilicon macromolecular monomer having a polymerizable group described in paragraphs

[0036] to

[0045] of Japanese Patent Gazette No. 2019-26746. It is available as a commercial product, and examples thereof include: (meth) acrylic acid-modified silicone; X-22-174ASX, X-22-174BX, KF-2012, X-22-2404, X-22-2426, X-22-2445, X-22-164, X-22-164AS, X-22-164A, X-22-164B, X-22-164C, X-22-164E manufactured by Shin-Etsu Chemical Co., Ltd., Silaplane FM-0711, FM-0721, FM-0725, FM-7711, FM-7721, FM-7725, etc.; mercapto-modified silicone; KF-2001, KF-2004, X-22-167B, X-22-167C, etc. manufactured by Shin-Etsu Chemical Co., Ltd.

[0115] In addition, general-purpose ethylene, vinyl acetate, acrylonitrile, styrene, etc. can be used.

[0116] In addition, crosslinking monomers as described in paragraph

[0031] of Japanese Patent Application Laid-Open No. 2019-26746 can be used, without particular limitation, and monomers having, for example, hydroxyl, epoxy, chloromethyl, bromomethyl, blocked isocyanate, amino, carboxyl groups, monomers having two or more polymerizable functional groups in one molecule, etc. Examples thereof include: (meth) hydroxyalkyl acrylates such as 2-hydroxyethyl (meth) acrylate, 2,3-dihydroxypropyl (meth) acrylate, 3-chloro-2-hydroxypropyl (meth) acrylate, glycidyl (meth) acrylate, vinyl monochloroacetate, 2-[(3,5-dimethylpyrazolyl)carbonylamino]ethyl (meth) acrylate, (meth) N,N-dialkylaminoalkyl acrylates such as N,N-dimethylaminoethyl (meth) acrylate, N-hydroxymethyl (meth) acrylamide, (meth) acrylic acid, itaconic acid, 1,4-butanediol di(meth) acrylate, etc.

[0117] In addition, a reactive emulsifier as described in paragraphs

[0074] to

[0094] of JP-A-2017-155095 can also be copolymerized.

[0118] In addition, as the water repellency imparting compound (C), an isocyanate-reactive compound having at least one hydrocarbon group having 7 to 40 carbon atoms and at least one functional group capable of reacting with an isocyanate group in one molecule can be used. Examples of the isocyanate-reactive compound include compounds represented by the following general formula (3).

[0119] W[-AR]a[-B]b (3)

[0120] In the general formula (3), W is an organic group with a valence of (a+b). A is bonded to W and is -XY- or -Y-. B is bonded to W and is -XZ or -Z. a is an integer greater than 1. b is an integer greater than 1. (a+b) is 3 to 42. X is a divalent polyalkylene ether group. Y is a divalent group, which is an ether group, an ester group, an amide group, a carbamate group, a urea group or a thiol carbamate group. R is a monovalent hydrocarbon group having 7 to 40 carbon atoms. Z is a hydroxyl group, an amino group, a carboxyl group or a thiol group. In the case where B is -XZ, Z is a hydroxyl group.

[0121] In the isocyanate-reactive compound represented by the general formula (3), the hydroxyl group, amino group, carboxyl group or thiol group of the group Z is a functional group that can react with an isocyanate group. The isocyanate-reactive compound is a compound having a monovalent hydrocarbon group having 7 to 40 carbon atoms derived from the group R.

[0122] In the isocyanate-reactive compound of the general formula (3), the group W is an organic group with a valence of (a+b), preferably a residue of a polyfunctional compound. The group W is bonded with a group A and a group B. a is an integer greater than 1, b is an integer greater than 1, and (a+b) is 3 to 42. That is, the valence of the group W is 3 to 42. Preferred polyfunctional compounds include polyol compounds, polyamine compounds, polycarboxylic acid compounds, and polythiol compounds.

[0123] The polyol compound is not particularly limited, and examples thereof include trimethylolethane, trimethylolpropane, ditrimethylolpropane, 1,2,4-butanetriol, dipentaerythritol, sugars, sugar alcohols, sugar acids, amino sugars, and the like.

[0124] Examples of the sugar include glucose, erythrose, arabinose, ribose, allose, altrose, mannose, xylose, lyxose, gulose, galactose, talose, threose, glucopyranose, mannopyranose, talopyranose, allopyranose, altrose, idopyranose, gulopyranose, fructose, ribulose, mannoheptulose, sedoheptulose and the like.

[0125] Sugar alcohol is a compound generated by reducing the carbonyl group of the above-mentioned sugar (aldose or ketose). Examples of sugar alcohol include glycerol, erythritol, threitol, mannitol, sorbitol, arabitol, xylitol, ribitol, galactitol, fucitol, iditol, inositol, pentaerythritol, and heptyl alcohol.

[0126] Sugar acid is a compound in which a monosaccharide is oxidized and a carboxyl group is introduced. Examples of sugar acid include gluconic acid, glyceric acid, xylonic acid, galactaric acid, ascorbic acid, gluconolactone, and xylonolactone.

[0127] Amino sugars are compounds in which a portion of the hydroxyl groups of monosaccharides are replaced by amino groups. Examples of amino sugars include glucosamine, galactosamine, and the like.

[0128] In addition, it may be a compound derived from these compounds by a dehydration reaction, etc. Examples thereof include sorbitan (derived from sorbitol), polyglycerol (derived from glycerol), and the like.

[0129] The polyamine compound is not limited, and examples thereof include diethylenetriamine, triethylenetetramine, aminoethylethanolamine, diethanolamine, triethanolamine, and the like.

[0130] The polycarboxylic acid compound is not limited, and examples thereof include malic acid, citric acid, and the like.

[0131] The polythiol compound is not limited, and examples thereof include trimethylolpropane tris(3-mercaptopropionate), tris-[(3-mercaptopropionyloxy)-ethyl]-isocyanate, pentaerythritol tetrakis(3-mercaptopropionate), dipentaerythritol hexa(3-mercaptopropionate), and the like.

[0132] In A and B of the general formula (3), the group X is a divalent polyalkylene ether group (ie, polyoxyalkylene). Specific examples of the group X include single polymers of ethylene oxide, propylene oxide, butylene oxide, etc., and block copolymers and random copolymers obtained by combining two or more of them.

[0133] As described above, the group Y is a divalent group, and is an ether group, an ester group, an amide group, a carbamate group, a urea group, or a thiourethane group.

[0134] The group R is bonded to the group Y and is a monovalent hydrocarbon group having 7 to 40 carbon atoms, preferably a straight-chain or branched hydrocarbon group having 7 to 40 carbon atoms, and more preferably a straight-chain hydrocarbon group. In addition, the hydrocarbon group is preferably an aliphatic hydrocarbon group, more preferably a saturated or unsaturated aliphatic hydrocarbon group, and particularly preferably an alkyl group. The number of carbon atoms of the hydrocarbon group is preferably 10 to 30, more preferably 12 to 26, particularly preferably 16 to 24, and most preferably 18 to 22. Specific examples of the hydrocarbon group include: decyl, undecyl, dodecyl (lauryl), myristyl, pentadecyl, cetyl, heptadecyl, stearyl, nonadecyl, eicosyl, heneicosyl, behenyl, oleyl, etc.

[0135] As a method for introducing the group R into the general formula (3), a method of reacting a fatty acid (it should be noted that the above carbon number also includes the carbon of the carbonyl group), an aliphatic alcohol, an aliphatic monoisocyanate, an aliphatic amine, an alkyl halide, an aliphatic acid chloride, etc. with a hydroxyl group, a carboxyl group, a thiol group, an amino group, etc. of the above multifunctional compound can be adopted. Thus, the group R can be introduced into the general formula (3) by forming a bond between the group Y and the group R.

[0136] Examples of fatty acids include caprylic acid, capric acid, lauric acid, myristic acid, palmitic acid, stearic acid, arachidonic acid, behenic acid, lignoceric acid, palmitoleic acid, linoleic acid, arachidonic acid, oleic acid, erucic acid and the like.

[0137] Examples of the aliphatic alcohol include lauryl alcohol, tridecanol, myristyl alcohol, pentadecyl alcohol, cetyl alcohol, stearyl alcohol, eicosanol, heneicosanol, behenyl alcohol, oleyl alcohol and the like.

[0138] Examples of the aliphatic monoisocyanate include decyl isocyanate, undecyl isocyanate, dodecyl isocyanate, myristyl isocyanate, pentadecyl isocyanate, cetyl isocyanate, stearyl isocyanate, eicosyl isocyanate, behenyl isocyanate and the like.

[0139] Examples of the aliphatic amines include decylamine, laurylamine, myristicamine, stearylamine, behenylamine, oleylamine and the like.

[0140] Examples of the alkyl halide include chlorododecane, chlorohexadecane, chlorooctadecane, bromododecane, bromohexadecane, bromooctadecane and the like.

[0141] Examples of the fatty acid chloride include octanoyl chloride, decanoyl chloride, lauroyl chloride, myristoyl chloride, palmitoyl chloride, stearoyl chloride, and oleoyl chloride.

[0142] The isocyanate-reactive compound is preferably a reaction product of the above-mentioned polyfunctional compound and at least one selected from the group consisting of the above-mentioned fatty acid, aliphatic alcohol, aliphatic monoisocyanate, aliphatic amine, alkyl halide and fatty acid chloride. The reaction product has a hydrocarbon skeleton derived from the above-mentioned polyfunctional compound and has a functional group (preferably a hydroxyl group, an amino group, a carboxyl group, a thiol group) that can react with an isocyanate group.

[0143] In the isocyanate-reactive compound, the number of functional groups reactive with an isocyanate group in one molecule is preferably 1 to 7, more preferably 1 to 5, and even more preferably 1 to 3.

[0144] There are no particular limitations, but in terms of versatility, sorbitan fatty acid esters (e.g., sorbitan monostearate, sorbitan distearate, sorbitan tristearate, sorbitan tribehenate, sorbitan trioleate, etc.), pentaerythritol fatty acid esters (e.g., pentaerythritol distearate, etc.), and citric acid esters (e.g., tristearyl citrate, etc.) can be preferably used.

[0145] The above-mentioned isocyanate-reactive compound (C2a, sometimes described as a carbamate system (before isocyanate reaction)) can impart excellent water resistance by further reacting with a polyisocyanate compound. For example, the following method can be adopted: after mixing the isocyanate-reactive compound and the polyisocyanate compound (including a blocked isocyanate compound), the mixture is treated (made to adhere) to a substrate (fiber, etc.), and the two components are reacted on the substrate by heat treatment to impart water resistance.

[0146] In addition, it is also preferred to treat the substrate after obtaining a compound (C2b, ​​sometimes described as a carbamate system (after isocyanate reaction)) in which two components are partially or completely reacted in advance. There is no particular limitation, and examples thereof include: compounds disclosed in Japanese Patent Table 2017-533976 (specifically, compounds described in Examples 1 to 143), compounds described in U.S. Publication No. 2010 / 0190397 (specifically, compounds described in Components 1 to 9; Reaction products (S)).

[0147] The water repellency-imparting compound (C) also preferably contains an organosilicon-based compound having at least an alkyl group having 3 to 50 carbon atoms (sometimes referred to as C3).

[0148] Although not particularly limited, examples thereof include organic silicon compounds such as dimethyl silicone oil introduced with a hydrocarbon group having 3 to 50 carbon atoms, silanol-terminated dimethyl silicone oil, methyl hydrogen silicone oil, and methylphenyl silicone oil.

[0149] The hydrocarbon group is preferably a linear or branched hydrocarbon group having 3 to 50 carbon atoms, and more preferably a linear hydrocarbon group. In addition, the hydrocarbon group is preferably an aliphatic hydrocarbon group, more preferably a saturated aliphatic hydrocarbon group, and particularly preferably an alkyl group. The hydrocarbon group preferably has 8 to 40 carbon atoms, more preferably 10 to 32, particularly preferably 12 to 30, and most preferably 16 to 28 carbon atoms.

[0150] As the silicone compound, commercially available alkyl-modified silicone, alkyl·aralkyl-modified silicone, alkyl·polyether-modified silicone, fatty acid amide-modified silicone, fatty acid ester-modified silicone and the like can be used.

[0151] Examples of the alkyl-modified silicone include KF-412, KF-413, KF-414, KF-415, KF-4003, KF-4701, KF-4917, KF-7235B, and X-22-7322 manufactured by Shin-Etsu Chemical Co., Ltd.; BELSIL CDM 3526VP, BELSIL CM 7026VP, and BELSIL SDM 5055VP manufactured by Asahi Kasei Wacker Silicone Co., Ltd.; Silwax E1316, Silwax H416, Silwax B116, Silwax L118, Silwax J1022, Silwax D222, Silwax D226, Silwax D1026, Silwax J226, Silax wax D026, Silwax J1032, Silwax D221M, and Silwax J219M, J221M, Silwax Di-1021M, Silwax 3H32, etc.

[0152] Examples of the alkyl-aralkyl modified silicone include X-22-1877 manufactured by Shin-Etsu Chemical Co., Ltd., WACKER TN manufactured by Asahi Kasei Wacker Silicone Co., Ltd., Silwax 3H12-MS, Silwax 3H2-MS, Silwax 3H-MS, Silwax DO-MS, etc. manufactured by SILTECH.

[0153] Examples of the alkyl polyether-modified silicone include Silube T308-16, Silube T310 to A16, and Silube J208-812 manufactured by SILTECH.

[0154] Examples of the fatty acid amide-modified silicone include KF-3935 manufactured by Shin-Etsu Chemical Co., Ltd. and the like.

[0155] Examples of the fatty acid ester-modified silicone include X-22-715 manufactured by Shin-Etsu Chemical Co., Ltd., and the like.

[0156] In addition, the organosilicon compounds (specifically, organopolysiloxanes 1 to 3) introduced with a glycidyl group or an amino group described in US Patent Application No. 2010 / 0190397 are mentioned.

[0157] (Amount of each ingredient used)

[0158] The waterproofing agent composition of the present invention may be a processing liquid at a concentration suitable for treating textile products directly, or may be a stock solution diluted with water before use in treating textile products (for example, the stock solution may be diluted 5 to 1000 times and used as a processing liquid).

[0159] In the waterproofing agent composition of the present invention, the lower limit of the ratio of the mass of the reactant (AB) to the mass of the water repellency imparting compound (C) (referred to as mass ratio (component (AB) / component (C)) or mass ratio (AB / C)) is 0.05 or more, preferably 0.07 or more, more preferably 0.1 or more, further preferably 0.2 or more, particularly preferably 0.3 or more, and most preferably 0.4 or more. The upper limit is 100 or less, preferably 30 or less, more preferably 20 or less, further preferably 15 or less, particularly preferably 10 or less, and most preferably 8 or less.

[0160] When the water repellent composition of the present invention is directly used as a processing liquid having a concentration for treating fiber products, the content of the reactant (AB) in the water repellent composition of the present invention is preferably about 0.001 to 60% by mass, more preferably about 0.01 to 50% by mass, further preferably about 0.01 to 40% by mass, and particularly preferably about 0.01 to 35% by mass. In addition, the content of the water repellency imparting compound (C) is preferably about 0.001 to 60% by mass, more preferably about 0.01 to 50% by mass, further preferably about 0.01 to 40% by mass, and particularly preferably about 0.01 to 35% by mass.

[0161] When the water repellent composition of the present invention is directly used as a processing liquid having a concentration for treating fiber products, the water content in the water repellent composition of the present invention may be appropriately selected in consideration of processability in order to obtain the target performance.

[0162] The reactant (AB) and the water-repellency-imparting compound (C) can be prepared separately as aqueous dispersions. When the water-repellent composition of the present invention is directly prepared as a processing liquid with a concentration for treating fiber products, the water-repellent composition of the present invention can be prepared as an aqueous dispersion mixed with each component by mixing the respective aqueous dispersions.

[0163] In addition to the reactant (AB), the water-repellency imparting compound (C), and water, the water-repellent composition of the present invention may contain other ingredients. Other ingredients preferably include surfactants, organic solvents, other additives, and other ingredients that are known to be used in water-repellent compositions. Other ingredients may be used alone or in combination of two or more. However, as described above, the water-repellent composition of the present invention preferably does not contain a C8 fluorine-based water-repellent (a compound having a perfluoroalkyl group with more than 7 carbon atoms).

[0164] The waterproofing agent composition of the present invention may contain any additive as the above-mentioned other components as long as it produces the effect of the present invention. Examples of the additive include: waterproofing aids, crosslinking agents (D), softeners, anti-slip agents, anti-wrinkle agents, flame retardants, antistatic agents, heat-resistant agents and other fiber agents, antioxidants, ultraviolet absorbers, pigments, metal powder pigments, rheology control agents, curing accelerators, deodorants, antibacterial agents and other well-known additives. For example, examples of waterproofing aid components include zirconium compounds, and zirconium acetate, zirconium hydrochloride, and zirconium nitrate are particularly preferred. As the anti-slip agent, a known anti-slip agent can be used, for example, colloidal silica, fumed silica can be used, and in addition, an organosilicon resin compound (described in paragraphs

[0059] to

[0063] of Japanese Patent Application Laid-Open No. 2018-104866; for example, MQ resin, MT resin, MDT resin, etc.), hydrophobic treatment, or hydrophobic treatment and hydrophilic treatment silica described in Japanese Patent Application Laid-Open No. 2017-206775 and Japanese Patent Application Laid-Open No. 2018-104866 can also be preferably used. These additives can be used alone or in combination of two or more.

[0165] As crosslinking agent (D), epoxy crosslinking agent, carbodiimide crosslinking agent, oxazoline crosslinking agent, glyoxal crosslinking agent, melamine crosslinking agent, isocyanate crosslinking agent (also including blocked isocyanate crosslinking agent in which isocyanate group is protected by blocking agent), etc. are listed. It should be noted that isocyanate crosslinking agent (D1) (sometimes described as polyisocyanate compound (D1)) is different from the above-mentioned reactant (AB). Specifically, isocyanate crosslinking agent (D1) has at least one of isocyanate group and blocked isocyanate group, but when isocyanate crosslinking agent (D1) is a reactant of polyol compound and polyisocyanate compound, polyol compound does not have any of ether group, carbonate group and ester group, and the molar ratio of isocyanate group of polyisocyanate compound to hydroxyl group of polyol compound is less than 2.1.

[0166] (Isocyanate crosslinking agent (D1))

[0167] As the isocyanate crosslinking agent (D1), one kind or two or more kinds of polyisocyanate compounds (B) may be used alone or in appropriate combination. The crosslinkable functional group of the isocyanate crosslinking agent (D1) is specifically an isocyanate group or a blocked isocyanate group.

[0168] As the polyisocyanate compound constituting the isocyanate crosslinking agent (D1), a blocked polyisocyanate compound in which 50 mol% or more, preferably 60 mol% or more, and more preferably 70 mol% or more of the isocyanate group is blocked with a blocking agent can be suitably used. As the blocked isocyanate compound, various known blocked isocyanates can be used, and the blocked isocyanate compound can be prepared by reacting various known isocyanate compounds with various known blocking agents.

[0169] The blocking agent for introducing the isocyanate compound is the same as the above-mentioned blocking agent.

[0170] The isocyanate crosslinking agent (D1) may be self-emulsifiable. As the polyisocyanate compound having self-emulsifiable properties, for example, an isocyanate compound in which a nonionic hydrophilic group, a cationic hydrophilic group or anionic hydrophilic group is introduced into a part of the isocyanate compound can be used. Preferably, a polyisocyanate compound in which a nonionic hydrophilic group having an oxyethylene group is introduced can be used. As a hydrophilic compound that reacts with an isocyanate compound in order to impart self-emulsification, examples thereof include: polyoxyalkylene monoalkyl ethers such as polyethylene glycol monomethyl ether, polyethylene glycol monoethyl ether, polyethylene glycol polypropylene glycol monomethyl ether, polypropylene glycol polyethylene glycol monobutyl ether, etc.; (poly)ethylene glycols such as ethylene glycol, or diethylene glycol, triethylene glycol, polyethylene glycol, etc.; block copolymers, random copolymers, random copolymers of ethylene oxide and propylene oxide, ethylene oxide and butylene oxide, block copolymers of polyethylene glycol, polypropylene glycol, polytetramethylene glycol; polyoxyalkylene monoamines, polyoxyalkylene diamines, etc., preferably polyethylene glycol monomethyl ether, polyethylene glycol monoethyl ether, etc. The above-mentioned nonionic hydrophilic compounds can be used alone or in combination of two or more. By introducing a specified amount of these compounds relative to the isocyanate group, self-emulsification can be imparted to the polyisocyanate compound. Regarding the amount of these compounds introduced, relative to the isocyanate group, the lower limit is preferably 1 mol% or more, the upper limit is preferably 50 mol% or less, more preferably 40 mol% or less, further preferably 30 mol% or less, and the range is preferably about 1 to 50 mol%, more preferably about 1 to 40 mol%, further preferably about 1 to 30 mol%.

[0171] As described above, the water repellent composition of the present invention can be prepared as an aqueous dispersion in which at least the reaction product (AB) of the polyol compound (A) and the isocyanate compound (B) and the water repellency imparting compound (C) are dispersed in water. These aqueous dispersions can be prepared by mixing aqueous dispersions of the respective components.

[0172] In the present invention, the aqueous dispersion of each component can be manufactured by known methods, and its example includes: each component is mixed with a surfactant and then water is added to disperse the method, and a known dispersion machine is used to disperse the method mechanically. As a dispersion machine, a homomixer, a homogenizer, a colloid mill, a pipeline mixer, a bead mill, etc. can be used. In addition, when carrying out aqueous dispersion, a known organic solvent can be added. When using an organic solvent, the removal process of the solvent can be set as required (for example, vacuum distillation is removed, etc.).

[0173] As the surfactant, one or more of nonionic surfactants, anionic surfactants, cationic surfactants, and amphoteric surfactants can be used.

[0174] Examples of the nonionic surfactant include polyoxyethylene alkyl ethers, polyoxyethylene alkylphenyl ethers, polyoxyethylene fatty acid esters, sorbitan fatty acid esters, polyoxyethylene sorbitan fatty acid esters, polyoxyethylene sorbitol fatty acid esters, glycerol fatty acid esters, polyoxyethylene glycerol fatty acid esters, polyglycerol fatty acid esters, sucrose fatty acid esters, polyoxyethylene alkylamines, polyoxyethylene fatty acid amides, fatty acid alkanolamides, alkyl alkanolamides, acetylenic glycols, oxyethylene adducts of acetylenic glycols, polyethylene glycol polypropylene glycol block polymers, and the like.

[0175] Examples of the anionic surfactant include sulfuric acid ester salts of higher alcohols, higher alkyl sulfonates, higher carboxylates, alkylbenzene sulfonates, polyoxyethylene alkyl sulfates, polyoxyethylene alkylphenyl ether sulfates, vinyl sulfosuccinate, and the like.

[0176] Examples of the cationic surfactant include amine salts, amide amine salts, quaternary ammonium salts, and imidazolium salts. Specific examples include, but are not limited to, amine salt-type surfactants such as alkylamine salts, polyoxyethylene alkylamine salts, alkylamide amine salts, amino alcohol fatty acid derivatives, polyamine fatty acid derivatives, and imidazolines; and quaternary ammonium salt-type surfactants such as alkyltrimethylammonium salts, dialkyldimethylammonium salts, alkyldimethylbenzylammonium salts, alkylpyridinium salts, alkylisoquinolinium salts, and benzethonium chloride.

[0177] Examples of the amphoteric surfactant include alkylamine oxides, alanines, imidazoline betaines, amide betaines, betaine acetate, and the like. Specifically, examples include long-chain amine oxides, lauryl betaine, stearyl betaine, lauryl carboxymethyl hydroxyethyl imidazoline betaine, lauryl dimethylaminoacetic acid betaine, and fatty acid amide propyl dimethylaminoacetic acid betaine.

[0178] When the waterproofing agent composition of the present invention contains a surfactant, the content can be appropriately selected according to the purpose. It is not particularly limited, for example, as the content for water-based, it is preferably about 0.1 to 30 parts by mass, more preferably about 0.2 to 25 parts by mass, further preferably about 0.3 to 20 parts by mass, particularly preferably about 0.4 to 15 parts by mass, and most preferably about 0.5 to 10 parts by mass, relative to 100 parts by mass of the solid content of the waterproofing agent composition.

[0179] When the surfactant is a compound described in the water repellency imparting compound (C), the surfactant is included in the concept of the water repellency imparting compound (C). Examples of such surfactants include sorbitan fatty acid esters and polyoxyethylene sorbitan fatty acid esters.

[0180] As described above, the present invention may be in the form of the above-mentioned kit.

[0181] The two-component kit of the present invention is used to prepare the water repellent composition of the present invention. Therefore, the types and contents of the reactants (AB), water repellency imparting compound (C), and other components are the same as those of the water repellent of the present invention.

[0182] 2. Waterproof fiber products

[0183] The water-repellent fiber product of the present invention is a product treated with the water-repellent composition of the present invention. That is, the water-repellent fiber product of the present invention is produced by bringing the water-repellent composition of the present invention into contact with a fiber product. The details of the water-repellent composition of the present invention are as described above.

[0184] The fiber products treated with the water repellent composition of the present invention are not particularly limited as long as they are made of fibers, and examples thereof include natural fibers such as cotton, silk, linen, and wool, synthetic fibers such as polyester, nylon, acrylic fiber, and spandex, and fiber products using these. In addition, the form and shape of the fiber products are also not limited to raw material forms such as staple fibers, filaments, tows, and silk, and may be various processed forms such as fabrics, knitted fabrics, cotton wool, nonwoven fabrics, paper, sheets, and films.

[0185] The waterproofing composition of the present invention can be used to waterproof fiber products (cloth, etc.) by a known method. Examples of the method for treating fiber products using the waterproofing composition of the present invention include a continuous method or an intermittent method. In addition, when the waterproofing composition of the present invention is a stock solution, the waterproofing composition is diluted with water to prepare a processing solution in order to achieve a concentration suitable for treatment (for example, a solid content concentration of about 0.01 to 6% by mass).

[0186] As a continuous method, when preparing the processing liquid, in addition to water, it is also preferred to arbitrarily add various agents, such as cross-linking agents. Then, the object to be processed (i.e., fiber products) is continuously fed into an impregnation device filled with the processing liquid, and after the processing liquid is impregnated into the object to be processed, the unnecessary processing liquid is removed. As an impregnation device, there is no particular limitation, and it is preferred to use a padding machine, a roller licking imparting device, a gravure coating imparting device, a spray imparting device, a foam imparting device, a coating imparting device, etc., and a padding machine type is particularly preferred. Then, a dryer is used to remove the residual water in the object to be processed. As a dryer, there is no particular limitation, and a flat-width dryer such as a hot air blower and a tenter is preferred. This continuous method is preferably used when the object to be processed is a cloth such as a fabric.

[0187] In addition, the intermittent method includes a process of immersing the treated object in a processing liquid and a process of removing the residual water in the treated object. It is preferred that the intermittent method be adopted when the treated object is not in the form of cloth, such as in the case of single strands, wool tops, yarn strips, bundles, tows, silk, etc., or when woven fabrics, etc. are not suitable for the continuous method. In the immersion process, for example, a staple dyeing machine, a bobbin dyeing machine, a liquid flow dyeing machine, an industrial washing machine, a warp beam dyeing machine, etc. can be used. In the operation of removing water, hot air dryers such as bobbin dryers, warp beam dryers, and drum dryers, high-frequency dryers, etc. can be used. It is preferred that the treated object to which the waterproofing agent composition of the present invention is attached is subjected to dry heat treatment.

[0188] The temperature of the dry heat treatment is preferably 120 to 180°C, particularly preferably 160 to 180°C. The time of the dry heat treatment is about 10 seconds to 10 minutes, preferably 30 seconds to 3 minutes, particularly preferably 1 to 2 minutes. In addition, before the dry heat treatment under the above conditions, a pre-drying step at about 80 to 120°C may be provided. There is no particular limitation on the method of dry heat treatment, but a tenter is preferably used when the object to be treated is in the form of cloth.

[0189] In addition, the waterproof fiber product may be subjected to coating treatment. As described above, as coating agents applied to the waterproof fiber product, for example, acrylic resins and polyurethane resins are listed. The waterproof fiber product is coated in order to improve the waterproofness (water resistance), adjust the air permeability, feel, and moisture permeability, and various selections can be made to obtain the target performance.

[0190] Example

[0191] The present invention will be described in detail below by showing examples and comparative examples. However, the present invention is not limited to the examples. It should be noted that in the following examples, "%" means "mass %" unless otherwise specified.

[0192] Preparation of aqueous dispersion of reactant (AB)

[0193] <Production Example AB-1>

[0194] Duranate 24A-100 (biuret form of hexamethylene diisocyanate, manufactured by Asahi Kasei Chemicals Co., Ltd., NCO% = 23.5) 100g (NCO group 0.560mol), dipropylene glycol 12.5g (OH group 0.186mol), polyoxyethylene monomethyl ether (average molecular weight 2000g / mol) 14.9g (OH group 0.007mol) and acetone 100g were added to a flask, and stirred and mixed at room temperature. The internal temperature was raised to 60°C, 0.05g of Neostann U-600 (manufactured by Nitto Kasei Co., Ltd.) was added as a catalyst, and the reaction was carried out until the isocyanate content reached 6.8%. After cooling to 40°C, 35.2g of 3,5-dimethylpyrazole (NH group 0.366mol) was added, and the reaction was carried out until the isocyanate content reached 0%. The internal temperature was cooled to 30°C, and 480g of ion exchange water was added dropwise to make it dispersed in water. Acetone was distilled off under reduced pressure, and ion-exchanged water was added to obtain an aqueous dispersion having a solid content concentration of 20%.

[0195] <Production Example AB-2>

[0196] Duranate 24A-100 (biuret form of hexamethylene diisocyanate, manufactured by Asahi Kasei Chemicals, NCO% = 23.5) 100g (NCO group 0.560mol), PTMG-650 (polytetramethylene ether glycol, manufactured by Mitsubishi Chemical Corporation, average molecular weight 650g / mol) 60.6g (OH group 0.187mol), polyoxyethylene monomethyl ether (average molecular weight 2000g / mol) 14.9g (OH group 0.007mol) and acetone 150g were added to a flask and stirred and mixed at room temperature. The internal temperature was raised to 60°C, 0.18g of Neostann U-600 (manufactured by Nitto Kasei Co., Ltd.) was added as a catalyst, and the reaction was carried out until the isocyanate content reached 4.7%. After cooling to 40°C, 35.1g of 3,5-dimethylpyrazole (NH group 0.365mol) was added, and the reaction was carried out until the isocyanate content reached 0%. The mixture was cooled to an internal temperature of 30°C, and 650 g of ion-exchanged water was added dropwise to obtain an aqueous dispersion. Acetone was distilled off under reduced pressure, and ion-exchanged water was added to obtain an aqueous dispersion having a solid content concentration of 20%.

[0197] <Production Example AB-3>

[0198] Duranate 24A-100 (biuret form of hexamethylene diisocyanate, manufactured by Asahi Kasei Chemicals Co., Ltd., NCO% = 23.5) 100g (NCO group 0.560mol), 1,4-butanediol 8.4g (OH group 0.187mol), polyoxyethylene monomethyl ether (average molecular weight 2000g / mol) 14.9g (OH group 0.007mol) and acetone 100g were added to a flask, and stirred and mixed at room temperature. The internal temperature was raised to 60°C, 0.09g of Neostann U-600 (manufactured by Nitto Kasei Co., Ltd.) was added as a catalyst, and the reaction was carried out until the isocyanate content reached 6.9%. After cooling to 40°C, 35.1g of 3,5-dimethylpyrazole (NH group 0.365mol) was added, and the reaction was carried out until the isocyanate content reached 0%. The internal temperature was cooled to 30°C, and 480g of ion exchange water was added dropwise to make it dispersed in water. Acetone was distilled off under reduced pressure, and ion-exchanged water was added to obtain an aqueous dispersion having a solid content concentration of 20%.

[0199] <Production Example AB-4>

[0200] Duranate 24A-100 (biuret form of hexamethylene diisocyanate, manufactured by Asahi Kasei Chemicals Co., Ltd., NCO% = 23.5) 100 g (NCO group 0.560 mol), 1,4-butanediol 8.4 g (OH group 0.187 mol), polyoxyethylene monomethyl ether (average molecular weight 2000 g / mol) 14.9 g (OH group 0.007 mol), polyoxypropylene trimethylolpropane ether (hydroxyl value 398 mg KOH / g) 3.7 g (OH group 0.026 mol) and acetone 100 g were added to a flask and stirred and mixed at room temperature. The internal temperature was raised to 60°C, 0.09 g of Neostann U-600 (manufactured by Nitto Kasei Co., Ltd.) was added as a catalyst, and the reaction was carried out until the isocyanate content reached 6.3%. After cooling to 40°C, 32.6 g of 3,5-dimethylpyrazole (0.339 mol of NH group) was added and reacted until the isocyanate content reached 0%. The mixture was cooled to an internal temperature of 30°C and 480 g of ion exchange water was added dropwise to make an aqueous dispersion. Acetone was distilled off under reduced pressure and ion exchange water was added to obtain an aqueous dispersion with a solid content concentration of 20%.

[0201] <Production Example AB-5>

[0202] In a flask, 100 g of Duranate 24A-100 (biuret form of hexamethylene diisocyanate, manufactured by Asahi Kasei Chemicals, NCO% = 23.5) (NCO group 0.560 mol), 60.6 g of PTMG-650 (polytetramethylene ether glycol, manufactured by Mitsubishi Chemical Corporation, average molecular weight 650 g / mol) (OH group 0.187 mol), 14.9 g of polyoxyethylene monomethyl ether (average molecular weight 2000 g / mol) (OH group 0.007 mol), 3.7 g of polyoxypropylene trimethylolpropane ether (hydroxyl value 398 mg KOH / g) (OH group 0.026 mol) and 135 g of acetone were added and stirred and mixed at room temperature. The internal temperature was raised to 60°C, 0.09 g of Neostann U-600 (manufactured by Nitto Kasei Co., Ltd.) was added as a catalyst, and the mixture was reacted until the isocyanate content reached 4.5%. After cooling to 40°C, 32.6 g of 3,5-dimethylpyrazole (0.339 mol of NH group) was added and reacted until the isocyanate content reached 0%. The mixture was cooled to an internal temperature of 30°C and 650 g of ion exchange water was added dropwise to make an aqueous dispersion. Acetone was distilled off under reduced pressure and ion exchange water was added to obtain an aqueous dispersion with a solid content concentration of 20%.

[0203] <Production Example AB-6>

[0204] In a flask, 100 g of Duranate 24A-100 (biuret form of hexamethylene diisocyanate, manufactured by Asahi Kasei Chemicals, NCO% = 23.5) (NCO group 0.560 mol), 23.3 g of PTMG-250 (polytetramethylene ether glycol, manufactured by Mitsubishi Chemical Corporation, average molecular weight 210 g / mol) (OH group 0.222 mol), 14.9 g of polyoxyethylene monomethyl ether (average molecular weight 2000 g / mol) (OH group 0.007 mol), 3.7 g of polyoxypropylene trimethylolpropane ether (hydroxyl value 398 mg KOH / g) (OH group 0.026 mol) and 90 g of acetone were added and stirred and mixed at room temperature. The internal temperature was raised to 60°C, 0.09 g of Neostann U-600 (manufactured by Nitto Kasei Co., Ltd.) was added as a catalyst, and the mixture was reacted until the isocyanate content reached 5.5%. After cooling to 40°C, 29.2 g of 3,5-dimethylpyrazole (0.304 mol of NH group) was added and reacted until the isocyanate content reached 0%. The mixture was cooled to an internal temperature of 30°C and 550 g of ion exchange water was added dropwise to make an aqueous dispersion. Acetone was distilled off under reduced pressure and ion exchange water was added to obtain an aqueous dispersion with a solid content concentration of 20%.

[0205] <Production Example AB-7>

[0206] In a flask, 100 g of Duranate 24A-100 (biuret form of hexamethylene diisocyanate, manufactured by Asahi Kasei Chemicals, NCO% = 23.5) (NCO group 0.560 mol), 37.3 g of Sannix PP-400 (polyoxypropylene glycol, manufactured by Sanyo Chemical Industries, Ltd., average molecular weight 400 g / mol) (OH group 0.187 mol), 14.9 g of polyoxyethylene monomethyl ether (average molecular weight 2000 g / mol) (OH group 0.007 mol), 3.7 g of polyoxypropylene trimethylolpropane ether (hydroxyl value 398 mg KOH / g) (OH group 0.026 mol) and 110 g of acetone were added and stirred and mixed at room temperature. The internal temperature was raised to 60°C, 0.09 g of Neostann U-600 (manufactured by Nitto Kasei Co., Ltd.) was added as a catalyst, and the mixture was reacted until the isocyanate content reached 5.4%. After cooling to 40°C, 32.6 g of 3,5-dimethylpyrazole (0.339 mol of NH group) was added and reacted until the isocyanate content reached 0%. After cooling to an internal temperature of 30°C, 600 g of ion exchange water was added dropwise to make an aqueous dispersion. Acetone was distilled off under reduced pressure, and ion exchange water was added to obtain an aqueous dispersion with a solid content concentration of 20%.

[0207] <Production Example AB-8>

[0208] In a flask, 93.3 g (0.187 mol of OH group) of Eternacoll UC-100 (polycarbonate diol; main skeleton cyclohexanedimethanol, manufactured by Ube Industries, Ltd., average molecular weight 1000 g / mol), 14.9 g (0.007 mol of OH group) of polyoxyethylene monomethyl ether (average molecular weight 2000 g / mol), 3.7 g (0.026 mol of OH group) of polyoxypropylene trimethylolpropane ether (hydroxyl value 398 mgKOH / g) and 140 g of acetone were added, and the temperature was raised to 60°C, and the mixture was stirred and mixed. Then, 100 g (0.560 mol of NCO group) of Duranate 24A-100 (biuret form of hexamethylene diisocyanate, manufactured by Asahi Kasei Chemicals Co., Ltd.) was added and mixed, and 0.14 g of Neostann U-600 (manufactured by Nitto Kasei Co., Ltd.) was further added as a catalyst to react until the isocyanate content reached 4.0%. After cooling to 40°C, 32.6 g (0.339 mol of NH group) of 3,5-dimethylpyrazole was added and reacted until the isocyanate content reached 0%. The mixture was cooled to an internal temperature of 30°C, and 800 g of ion exchange water was added dropwise to make it aqueous. Acetone was distilled off under reduced pressure, and ion exchange water was added to obtain an aqueous dispersion having a solid content concentration of 20%.

[0209] <Production Example AB-9>

[0210] 93.3 g (0.187 mol of OH group) of BENEBiOL NL1010DB (polycarbonate diol; main skeleton 1,4-butanediol 1,10-decanediol, manufactured by Mitsubishi Chemical Corporation, average molecular weight 1000 g / mol), 29.8 g (0.015 mol of OH group) of polyoxyethylene monomethyl ether (average molecular weight 2000 g / mol) and 170 g of acetone were added to a flask, and the mixture was heated to an internal temperature of 60°C and stirred and mixed. Then, 100 g (0.560 mol of NCO group) of Duranate 24A-100 (biuret form of hexamethylene diisocyanate, manufactured by Asahi Kasei Chemicals, NCO% = 23.5) was added and mixed, and 0.09 g of Neostann U-600 (manufactured by Nitto Kasei Co., Ltd.) was further added as a catalyst, and the mixture was reacted until the isocyanate content reached 3.8%. After cooling to 40°C, 34.4 g of 3,5-dimethylpyrazole (0.358 mol of NH group) was added and reacted until the isocyanate content reached 0%. The mixture was cooled to an internal temperature of 30°C and 760 g of ion exchange water was added dropwise to make an aqueous dispersion. Acetone was distilled off under reduced pressure and ion exchange water was added to obtain an aqueous dispersion with a solid content concentration of 20%.

[0211] <Production Example AB-10>

[0212] In a flask, 100 g of Duranate 24A-100 (biuret form of hexamethylene diisocyanate, manufactured by Asahi Kasei Chemicals Co., Ltd., NCO% = 23.5) (NCO group 0.560 mol), 93.3 g of Kuraray Polyol P-1012 (polyester diol; polycondensate of 3-methyl-1,5-pentanediol, adipic acid, and isophthalic acid, manufactured by Kuraray Co., Ltd., average molecular weight 1000 g / mol) (OH group 0.187 mol), 29.8 g of polyoxyethylene monomethyl ether (average molecular weight 2000 g / mol) (OH group 0.015 mol) and 170 g of acetone were added and stirred and mixed at room temperature. The internal temperature was raised to 60°C, 0.09 g of Neostann U-600 (manufactured by Nitto Kasei Co., Ltd.) was added as a catalyst, and the mixture was reacted until the isocyanate content reached 3.8%. After cooling to 40°C, 34.4 g of 3,5-dimethylpyrazole (0.358 mol of NH group) was added and reacted until the isocyanate content reached 0%. The mixture was cooled to an internal temperature of 30°C and 620 g of ion exchange water was added dropwise to make an aqueous dispersion. Acetone was distilled off under reduced pressure and ion exchange water was added to obtain an aqueous dispersion with a solid content concentration of 20%.

[0213] <Production Example AB-11>

[0214] In a flask, 100 g (NCO group 0.314 mol) of Coronate L (trimethylolpropane adduct of toluene diisocyanate (molar ratio 3:1), manufactured by Tosoh Corporation, NCO%=13.4, ethyl acetate solution with a solid content concentration of 75%), 34 g (OH group 0.105 mol) of PTMG-650 (polytetramethylene ether glycol, manufactured by Mitsubishi Chemical Corporation, average molecular weight 650 g / mol), 8.4 g (OH group 0.004 mol) of polyoxyethylene monomethyl ether (average molecular weight 2000 g / mol), and 130 g of acetone were added and stirred and mixed at room temperature. The internal temperature was raised to 60°C, 0.002 g of Neostann U-600 (manufactured by Nitto Kasei Co., Ltd.) was added as a catalyst, and the mixture was reacted until the isocyanate content reached 3.2%. After cooling to 40°C, 17.9 g (0.205 mol) of methyl ethyl ketoxime was slowly added using a dropping funnel and reacted until the isocyanate content reached 0%. After cooling to an internal temperature of 30°C, 740 g of ion exchange water was added dropwise to make an aqueous dispersion. Acetone was distilled off under reduced pressure, and ion exchange water was added to obtain an aqueous dispersion with a solid content concentration of 20%.

[0215] <Production Example AB-12>

[0216] 100 g of VESTANAT T1890 / 100 (isocyanurate of isophorone diisocyanate, manufactured by Evonik, NCO% = 17.3) (NCO group 0.412 mol) and 140 g of acetone were added to a flask, and the mixture was heated to an internal temperature of 45°C and stirred and mixed. Then, 44.6 g of PTMG-650 (polytetramethylene ether glycol, manufactured by Mitsubishi Chemical Corporation, average molecular weight 650 g / mol) (OH group 0.137 mol) and 22 g of polyoxyethylene monomethyl ether (average molecular weight 2000 g / mol) (OH group 0.011 mol) were added, the internal temperature was raised to 60°C, and 0.09 g of Neostann U-600 (manufactured by Nitto Chemical Industry Co., Ltd.) was added as a catalyst, and the mixture was reacted until the isocyanate content reached 3.6%. After cooling to 40°C, 23 g (0.264 mol) of methyl ethyl ketone oxime was slowly added using a dropping funnel and reacted until the isocyanate content reached 0%. After cooling to an internal temperature of 30°C, 560 g of ion exchange water was added dropwise to make it an aqueous dispersion. Acetone was distilled off under reduced pressure, and ion exchange water was added to obtain an aqueous dispersion with a solid content concentration of 20%.

[0217] <Production Example AB-13>

[0218] In a flask, 100 g of Duranate 24A-100 (biuret form of hexamethylene diisocyanate, manufactured by Asahi Kasei Chemicals, NCO% = 23.5) (NCO group 0.560 mol), 60.6 g of PTMG-650 (polytetramethylene ether glycol, manufactured by Mitsubishi Chemical Corporation, average molecular weight 650 g / mol) (OH group 0.187 mol), 14.9 g of polyoxyethylene monomethyl ether (average molecular weight 2000 g / mol) (OH group 0.007 mol), 3.7 g of polyoxypropylene trimethylolpropane ether (hydroxyl value 398 mg KOH / g) (OH group 0.026 mol) and 130 g of acetone were added and stirred and mixed at room temperature. The internal temperature was raised to 60°C, 0.09 g of Neostann U-600 (manufactured by Nitto Kasei Co., Ltd.) was added as a catalyst, and the mixture was reacted until the isocyanate content reached 4.6%. After cooling to 40°C, 29.6 g (0.339 mol) of methyl ethyl ketoxime was slowly added using a dropping funnel and reacted until the isocyanate content reached 0%. After cooling to an internal temperature of 30°C, 640 g of ion exchange water was added dropwise to make it an aqueous dispersion. Acetone was distilled off under reduced pressure, and ion exchange water was added to obtain an aqueous dispersion with a solid content concentration of 20%.

[0219] <Production Example AB-14>

[0220] In a flask, 100 g of Duranate 24A-100 (biuret form of hexamethylene diisocyanate, manufactured by Asahi Kasei Chemicals, NCO% = 23.5) (NCO group 0.560 mol), 60.6 g of PTMG-650 (polytetramethylene ether glycol, manufactured by Mitsubishi Chemical Corporation, average molecular weight 650 g / mol) (OH group 0.187 mol), 14.9 g of polyoxyethylene monomethyl ether (average molecular weight 2000 g / mol) (OH group 0.007 mol), 3.7 g of polyoxypropylene trimethylolpropane ether (hydroxyl value 398 mg KOH / g) (OH group 0.026 mol) and 140 g of acetone were added and stirred and mixed at room temperature. The internal temperature was raised to 60°C, 0.09 g of Neostann U-600 (manufactured by Nitto Kasei Co., Ltd.) was added as a catalyst, and the mixture was reacted until the isocyanate content reached 4.5%. After cooling to 40°C, 35.6 g of diethanolamine (hereinafter referred to as DEA) (0.339 mol of NH groups) was slowly added using a dropping funnel, and the reaction was performed until the isocyanate content reached 0%. The mixture was cooled to an internal temperature of 30°C, and 640 g of ion exchange water was added dropwise to make an aqueous dispersion. Acetone was distilled off under reduced pressure, and ion exchange water was added to obtain an aqueous dispersion having a solid content concentration of 20%.

[0221] <Production Example AB-15>

[0222] In a flask, 100 g of Duranate 24A-100 (biuret form of hexamethylene diisocyanate, manufactured by Asahi Kasei Chemicals, NCO% = 23.5) (NCO group 0.560 mol), 60.6 g of PTMG-650 (polytetramethylene ether glycol, manufactured by Mitsubishi Chemical Corporation, average molecular weight 650 g / mol) (OH group 0.187 mol) and 130 g of methyl isobutyl ketone were added and stirred and mixed at room temperature. The internal temperature was raised to 60°C, 0.09 g of Neostann U-600 (manufactured by Nitto Kasei Co., Ltd.) was added as a catalyst, and the reaction was carried out until the isocyanate content reached 5.4%. After cooling to 40°C, 35.9 g of 3,5-dimethylpyrazole (NH group 0.373 mol) was added, and the reaction was carried out until the isocyanate content reached 0%. The mixture was cooled to an internal temperature of 30°C, and 88 g of propylene glycol monomethyl ether and 15.2 g of a 40 mol ethylene oxide adduct of tristyrenated phenol were added and mixed. Then, 500 g of ion exchange water was added and the mixture was dispersed in water using a high pressure homogenizer (400 bar). Then, ion exchange water was added to obtain an aqueous dispersion having a solid content concentration of 21.5%.

[0223] <Production Example AB-16>

[0224] Duranate 24A-100 (biuret form of hexamethylene diisocyanate, manufactured by Asahi Kasei Chemicals Co., Ltd., NCO% = 23.5) 100g (NCO group 0.560mol), polyoxyethylene monomethyl ether (average molecular weight 2000g / mol) 14.9g (OH group 0.007mol) and acetone 200g were added to a flask, and stirred and mixed at room temperature. The internal temperature was raised to 40°C, and 31.4g (NH group 0.327mol) of 3,5-dimethylpyrazole was added. The internal temperature was raised to 60°C, and 0.09g of Neostann U-600 (manufactured by Nitto Kasei Co., Ltd.) was added as a catalyst, and the reaction was carried out until the isocyanate content reached 2.7%. Polyoxypropylene trimethylolpropane ether (hydroxyl value 398mg KOH / g) 42.8g (OH group 0.304mol) was added, and the reaction was carried out until the isocyanate content reached 0%. The mixture was cooled to an internal temperature of 30°C, and 580 g of ion-exchanged water was added dropwise to obtain an aqueous dispersion. Acetone was distilled off under reduced pressure, and ion-exchanged water was added to obtain an aqueous dispersion having a solid content concentration of 20%.

[0225] <Production Example AB-17>

[0226] In a flask, 100 g (0.560 mol of NCO group) of Duranate 24A-100 (biuret form of hexamethylene diisocyanate, manufactured by Asahi Kasei Chemicals Co., Ltd., NCO% = 23.5), 14.9 g (0.007 mol of OH group) of polyoxyethylene monomethyl ether (average molecular weight 2000 g / mol) and 200 g of acetone were added, and stirred and mixed at room temperature. The internal temperature was raised to 40°C, and 29.8 g (0.310 mol of NH group) of 3,5-dimethylpyrazole was added. The internal temperature was raised to 60°C, and 0.09 g of Neostann U-600 (manufactured by Nitto Kasei Co., Ltd.) was added as a catalyst, and the mixture was reacted until the isocyanate content reached 2.9%. 60.3 g (0.429 mol of OH group) of polyoxypropylene trimethylolpropane ether (hydroxyl value 398 mg KOH / g) was added, and the mixture was reacted until the isocyanate content reached 0%. The mixture was cooled to an internal temperature of 30°C, and 580 g of ion-exchanged water was added dropwise to obtain an aqueous dispersion. Acetone was distilled off under reduced pressure, and ion-exchanged water was added to obtain an aqueous dispersion having a solid content concentration of 20%.

[0227] <Production Example AB-18>

[0228] In a flask, 100 g (0.560 mol of NCO group) of Duranate 24A-100 (biuret form of hexamethylene diisocyanate, manufactured by Asahi Kasei Chemicals Co., Ltd., NCO% = 23.5), 14.9 g (0.007 mol of OH group) of polyoxyethylene monomethyl ether (average molecular weight 2000 g / mol) and 200 g of acetone were added, and stirred and mixed at room temperature. The internal temperature was raised to 40°C, and 35.6 g (0.370 mol of NH group) of 3,5-dimethylpyrazole was added. The internal temperature was raised to 60°C, and 0.09 g of Neostann U-600 (manufactured by Nitto Kasei Co., Ltd.) was added as a catalyst, and the mixture was reacted until the isocyanate content reached 2.2%. 78.3 g (0.556 mol of OH group) of polyoxypropylene trimethylolpropane ether (hydroxyl value 398 mg KOH / g) was added, and the mixture was reacted until the isocyanate content reached 0%. The mixture was cooled to an internal temperature of 30°C, and 580 g of ion-exchanged water was added dropwise to obtain an aqueous dispersion. Acetone was distilled off under reduced pressure, and ion-exchanged water was added to obtain an aqueous dispersion having a solid content concentration of 20%.

[0229] [Table 1]

[0230]

[0231] In Table 1, "HDI" represents hexamethylene diisocyanate, "TDI" represents toluene diisocyanate, "IPDI" represents isophorone diisocyanate, "DMP" represents dimethylpyrazole, "MEK" represents methyl ethyl ketone, "DEA" represents diethanolamine, "MPEG" represents polyoxyethylene monomethyl ether, and "BI" represents a blocked isocyanate group. In addition, in Table 1, in the expression "NCO of component (B)", NCO is a blocked isocyanate group (BI).

[0232] Preparation of aqueous dispersion of water-repellent compound (C)

[0233] <Production Example C-1>

[0234] 83 g of stearyl acrylate, 2 g of 2-hydroxyethyl methacrylate, 1 g of stearyl trimethyl ammonium chloride, 6 g of polyoxyethylene (EO addition mole number: 7 moles) lauryl ether, 2 g of polyoxyethylene (EO addition mole number: 21 moles) lauryl ether, 0.1 g of dodecyl mercaptan, 30 g of dipropylene glycol and 190 g of ion exchange water were added to an autoclave and dispersed in water by high-speed stirring at 50°C. Then, the mixture was treated with a high-pressure homogenizer (400 bar) while maintaining the temperature at 40°C to obtain an aqueous dispersion. After nitrogen substitution in the autoclave, 15 g of vinyl chloride was added by pressure injection, and 0.3 g of azobis(isobutylamidine) dihydrochloride was added, and the mixture was reacted at 60°C for 10 hours under a nitrogen atmosphere. Ion exchange water was added to adjust the solid content concentration to 21.8%, and an aqueous dispersion of an acrylic polymer was obtained.

[0235] <Production Example C-2>

[0236] 98 g of stearyl acrylate, 2 g of 2-hydroxyethyl methacrylate, 1 g of stearyl trimethyl ammonium chloride, 6 g of polyoxyethylene (EO addition mole number: 7 moles) lauryl ether, 2 g of polyoxyethylene (EO addition mole number: 21 moles) lauryl ether, 0.1 g of dodecyl mercaptan, 30 g of dipropylene glycol and 190 g of ion exchange water were added to a flask and dispersed in water by high-speed stirring at 50°C. Then, the mixture was treated with a high-pressure homogenizer (400 bar) while being maintained at 40°C to obtain an aqueous dispersion. 0.3 g of azobis(isobutylamidine) dihydrochloride was added to the emulsion and reacted at 60°C for 10 hours under a nitrogen atmosphere. Ion exchange water was added to adjust the solid content concentration to 21.8%, and an aqueous dispersion of an acrylic polymer was obtained.

[0237] <Production Example C-3>

[0238] 94 g of stearyl acrylate, 4 g of KF-2012 (free radical reactive organopolysiloxane macromonomer, manufactured by Shin-Etsu Chemical Co., Ltd.), 2 g of 2-hydroxyethyl methacrylate, 1 g of stearyl trimethylammonium chloride, 6 g of polyoxyethylene (EO addition mole number: 7 moles) lauryl ether, 2 g of polyoxyethylene (EO addition mole number: 21 moles) lauryl ether, 0.1 g of dodecyl mercaptan, 30 g of dipropylene glycol and 190 g of ion exchange water were added to a flask and dispersed in water by high-speed stirring at 50°C. Then, the mixture was treated with a high-pressure homogenizer (400 bar) while being maintained at 40°C to obtain an aqueous dispersion. 0.3 g of azobis(isobutylamidine) dihydrochloride was added to the emulsion and reacted at 60°C for 10 hours under a nitrogen atmosphere. Ion exchange water was added to adjust the solid content concentration to 21.8%, and an aqueous dispersion of acrylic-organosilicone polymer was obtained.

[0239] <Production Example C-4>

[0240] 117 g of BELSIL CDM 3526VP (alkyl (C26-28) modified silicone; melting point about 35°C (paste), manufactured by Asahi Kasei Wacker Silicone Co., Ltd.) and 63 g of methyl isobutyl ketone were added to a flask and melted at 60°C. 5.7 g of ethylene oxide 30 mol adduct of stearylamine and 1.8 g of acetic acid (90% aqueous solution) were dissolved in 400 g of ion exchange water at 60°C and added dropwise. The temperature was maintained and aqueous dispersion was performed using a high-pressure homogenizer (400 bar). Then, methyl isobutyl ketone was distilled off under reduced pressure, and ion exchange water was added to obtain an aqueous dispersion having a solid content concentration of 21%.

[0241] <Production Example C-5>

[0242] 117 g of Silwax D226 (alkyl (C26-28) modified silicone; melting point about 54°C (waxy), manufactured by SILTECH) and 63 g of methyl isobutyl ketone were added to a flask and melted at 70°C. 5.7 g of 30 mol of ethylene oxide adduct of stearylamine and 1.8 g of acetic acid (90% aqueous solution) were dissolved in 400 g of ion exchange water at 60°C and added dropwise. The temperature was maintained and aqueous dispersion was performed using a high-pressure homogenizer (400 bar). Then, methyl isobutyl ketone was distilled off under reduced pressure, and ion exchange water was added to obtain an aqueous dispersion having a solid content concentration of 21%.

[0243] <Production Example C-6>

[0244] Add 117 g of Emasol S-30V (sorbitan tristearate; hydroxyl value 67.9 mgKOH / g, manufactured by Kao Corporation) and 63 g of methyl isobutyl ketone to a flask and melt them at 60°C. Dissolve 5.7 g of ethylene oxide 30 mol adduct of stearylamine and 1.8 g of acetic acid (90% aqueous solution) in 400 g of ion exchange water at 60°C and add dropwise. Maintain the temperature and perform aqueous dispersion using a high-pressure homogenizer (400 bar). Then, distill off the methyl isobutyl ketone under reduced pressure, add ion exchange water, and obtain an aqueous dispersion having a solid content concentration of 21%.

[0245] <Production Example C-7>

[0246] 47.5 g of stearyl acrylate, 2.5 g of glycidyl methacrylate, 145 g of pure water, 15 g of tripropylene glycol, 1.5 g of sorbitan monooleate, 2 g of polyoxyethylene (EO addition mole number: 18 moles) secondary alkyl (C12-14) ether, and 1.5 g of dioctadecyl dimethyl ammonium chloride were added to an autoclave, and emulsified and dispersed by ultrasonic waves at 60° C. for 15 minutes under stirring. After nitrogen substitution in the autoclave, 0.5 g of 2,2-azobis(2-amidinopropane) dihydrochloride was added, and the mixture was reacted at 60° C. for 3 hours. Ion exchange water was added to adjust the solid content concentration to 21.3%, and an aqueous dispersion of an acrylic polymer was obtained.

[0247] <Production Example C-8>

[0248] 70 g (0.09 mol of OH group) of Emazol S-30V (sorbitan tristearate; hydroxyl value 68.6 mgKOH / g, manufactured by Kao Corporation) and 80 g of methyl isobutyl ketone were added to a flask and melted at 50°C. Then, 17 g (0.09 mol of NCO group) of Duranate 24A-100 (biuret form of hexamethylene diisocyanate, manufactured by Asahi Kasei Chemicals, NCO% = 23.5) and 10 mg of diazabicycloundecene were added, and the temperature was raised to 80°C to react until the isocyanate content reached 0%. 3.1 g of dimethyl stearylamine, 2.1 g of acetic acid (90% aqueous solution) and 1.6 g of Tergitol TMN-10 (polyethylene glycol trimethyl nonyl ether, manufactured by Dow Chemical, 90% aqueous solution) were dissolved in 220 g of ion exchange water at 60°C and added dropwise. The temperature was maintained and aqueous dispersion was performed using a high-pressure homogenizer (400 bar). Then, methyl isobutyl ketone was distilled off under reduced pressure, and ion-exchanged water was added to obtain an aqueous dispersion having a solid content concentration of 21%.

[0249] Table 2 shows the water repellency-imparting compounds (C) produced in the above-mentioned production examples.

[0250] [Table 2]

[0251]

[0252] Preparation of aqueous dispersion of isocyanate crosslinking agent (D1)

[0253] <Production Example D-1>

[0254] Add 100 g (0.560 mol of NCO group) of Duranate 24A-100 (biuret form of hexamethylene diisocyanate, manufactured by Asahi Kasei Chemicals Co., Ltd., NCO% = 23.5) and 65.9 g of methyl isobutyl ketone to a flask and start stirring. Add 53.8 g (0.560 mol) of 3,5-dimethylpyrazole to it, keep it at 50°C, and react it until the isocyanate content becomes zero, thereby obtaining a blocked isocyanate compound. Mix 30.8 g of methyl isobutyl ketone, 65.9 g of propylene glycol monomethyl ether, and 0.31 g of stearyl trimethyl ammonium chloride as a cationic surfactant to prepare a uniform solution. After slowly adding 175.8 g of ion exchange water while stirring, use a high-pressure homogenizer (400 bar) to perform aqueous dispersion. Then, the organic solvent is distilled off under reduced pressure, and ion exchange water is added to obtain an aqueous dispersion of the isocyanate compound with a solid content concentration of 20% (Table 3).

[0255] (Production Example D-2)

[0256] 20.0 g (0.064 mol of NCO group) of Coronate L (trimethylolpropane adduct of toluene diisocyanate (molar ratio 3:1), manufactured by Tosoh Corporation, NCO% = 13.4, ethyl acetate solution with a solid content concentration of 75%) and 15.0 g of methyl isobutyl ketone were added to a flask and stirred. Next, 5.6 g (0.064 mol) of methyl ethyl ketone oxime was slowly added using a dropping funnel, and the mixture was reacted at 55°C until the NCO content reached 0%. After cooling, 1.4 g of 30 mol of ethylene oxide adduct of tristyrenated phenol was added to make it uniform. After adding 80 g of ion exchange water, an aqueous dispersion was performed using a high-pressure homogenizer (400 bar). Then, the organic solvent was distilled off under reduced pressure, and ion exchange water was added to obtain an aqueous dispersion of the isocyanate compound with a solid content concentration of 21.4% (Table 3).

[0257] [Table 3]

[0258]

[0259] In Table 3, "HDI" represents hexamethylene diisocyanate, "TDI" represents toluene diisocyanate, "DMP" represents dimethylpyrazole, "MEK" represents methyl ethyl ketone, "MPEG" represents polyoxyethylene monomethyl ether, and "BI" represents a blocked isocyanate group. In addition, in Table 3, in the description of "NCO of component (B)", NCO is a blocked isocyanate group (BI).

[0260] <Example 1>

[0261] 3.8 g of the aqueous dispersion of Production Example AB-1 (active ingredient concentration 20.0%) and 3.8 g of the aqueous dispersion of Production Example C-1 (active ingredient concentration 20.0%) were mixed to prepare a waterproofing agent composition (stock solution). Then, water was added to make a total of 100 g to prepare a waterproofing agent composition (processing liquid). The above-mentioned waterproofing agent composition (processing liquid) contains 0.76 mass% of component (AB) and 0.76 mass% of component (C) as shown in Table 5. Next, the test cloth was passed through the above-mentioned waterproofing agent composition (processing liquid) by a continuous method, and the unnecessary solution was squeezed out by a liquid squeezer at a certain pressure, dried at 110°C for 90 seconds, and cured at 170°C for 60 seconds. As the test cloth, polyester taffeta (weight per unit area 65 g / m 2 , PET taffeta) and nylon high-density taffeta (weight per unit area 60g / m 2 , hereinafter referred to as Ny high-density taffeta), the liquid-entrapment rate of polyester taffeta is 31%, and the liquid-entrapment rate of nylon high-density taffeta is 48%.

[0262] <Examples 2-38, 41-45 and Comparative Examples 1-9>

[0263] The same operation as in Example 1 was carried out to prepare the water repellent composition (processing fluid) so that the content of each component became the content described in the following Tables 5 to 11.

[0264] <Examples 39 and 40>

[0265] The same operation was performed except that the heat treatment conditions of Example 1 were changed to drying at 110°C for 90 seconds and curing at 170°C for 300 seconds, and the contents of the components in the water repellent composition (processing fluid) were the contents described in Table 11 below.

[0266] [Test evaluation method]

[0267] (Waterproofness Evaluation)

[0268] For the obtained processed fabric, evaluation is carried out according to the waterproofness test (spray test) in 7.2 of JIS L 1092:2009. The evaluation is carried out according to the following criteria. When the performance is slightly better, a "+" is added to the grade, and when the performance is slightly worse, a "-" is added to the grade.

[0269] 5: There is no attachment of moisture or water droplets on the surface.

[0270] 4: The surface is not wet, but shows the attachment of small water droplets.

[0271] 3: The surface shows small individual water droplet-like wetness.

[0272] 2: Half of the surface shows wetness, showing a state where small individual wetness penetrates the fabric.

[0273] 1: The entire surface shows wetness.

[0274] (Evaluation of washing durability of waterproofness)

[0275] For the obtained processed fabric, 10 washes (HL-10) are carried out according to Method 103 in Appendix 1 of JIS L 0217 (1995). For the obtained washed fabric, the above waterproof test is carried out. The waterproof test is carried out respectively after air drying (N) or after tumble drying (66 ± 5°C: 40 minutes, T).

[0276] (Evaluation of chalk mark resistance)

[0277] Using the processed Ny high-density taffeta, evaluation is carried out respectively by the following <Method A> and <Method B>.

[0278] <Method A>

[0279] Use a metal comb to rub the surface of the processed fabric, and visually observe whether the marks remain on the fabric. Evaluation is carried out in 5 grades as follows.

[0280] 5: There are no marks at all

[0281] 4: Almost no marks can be seen

[0282] 3: Slightly marks can be seen

[0283] 2: Marks can be seen

[0284] 1: Obvious marks can be seen

[0285] <Method B>

[0286] Refer to the steps of 9.2 Friction Tester Type II (Gakushin Type) Method (dry test) of JIS L 0849:2013, install a friction white cotton cloth on the friction piece (500g), and rub the surface of the processed cloth back and forth 50 times. Use a spectrocolorimeter (made by Nippon Denshoku Industries; SE-2000, lens: 6mm, C light source, field of view 2 degrees) to measure the color change (ΔE*) before and after friction. Measure 5 points and record the average value in each table. The smaller the value, the smaller the color change. In addition, for the records in Table 4, refer to the records in Japanese Patent Gazette No. 2009-177415.

[0287] [Table 4]

[0288] ΔE* evaluate 0.2 or less Unable to measure area 0.3 Color measurement reproduction accuracy of the same object 0.6 Practical tolerance range considering various error factors 1.2 Most people can easily see the color difference when judging side by side. 2.5 When judged separately, it can be seen that they are almost the same.

[0289] (Evaluation of stitch slippage)

[0290] Using the processed PET taffeta, a test was conducted by warp slippage under a load of 117.7 N in accordance with JIS L 1096:2010 8.23.1 stitch slippage method B, and stitch slippage (mm) was measured. The stitch slippage of the untreated fabric was 0.8 mm.

[0291] (Peel strength test)

[0292] The processed Ny high-density taffeta was calendered at 160°C and a nip pressure of 100kg / cm. For the calendered surface, a coating resin composition having the following composition was applied using a knife coater, dried at 150°C for 2 minutes, and then aged at 80°C for 10 hours. The coated surface was thermally pressed (150°C, 10 seconds, 1.0kgf / cm2) with MELCO tape BW-II (hot melt adhesive tape, San Chemicals Ltd., width 25mm, color RB) in the warp direction, and the peel strength [N / 25mm width] was measured using Autograph (manufactured by Shimadzu Corporation; AG-5kNX) in accordance with JISL 1086:2013 7.10.1. The peel strength was set as the average value of 3 test pieces.

[0293] [Coating resin composition]

[0294] PASCOL NJ-1 (aqueous dispersion of polyurethane resin, manufactured by Meisei Chemical Industry Co., Ltd.) 100 parts by mass

[0295] SU-268A (blocked isocyanate crosslinking agent, manufactured by Meisei Chemical Industry Co., Ltd.) 5 parts by mass

[0296] A suitable amount of thickener was prepared (viscosity 10000 mPa·s (B-type viscometer; rotor No. 4, 30 rpm)).

[0297] The composition, water resistance, chalk mark resistance, pin slip resistance and peel strength test results of the water repellent composition of each example and comparative example are shown in Tables 5 to 11 below. In Tables 5 to 11, the expression "%" of the reactant (AB), the isocyanate crosslinking agent (D1) and the water repellency imparting compound (C) refers to the content (mass %) of each component in the water repellent composition (processing fluid).

[0298] [Table 5]

[0299]

[0300] Compared with Comparative Examples 1 and 3, improvement in chalk mark resistance was observed in Examples 1 to 10. In addition, no adverse effects on pin slippage and peel strength were observed in Examples 5 to 8. In Comparative Example 2, the molar ratio (B / A2) of the reactive functional group (hydroxyl group and isocyanate group) was 2, and improvement in chalk mark resistance was not observed. In contrast, in Example 3, the molar ratio (B / A2) of the reactive functional group (hydroxyl group and isocyanate group) was 3, and improvement in chalk mark resistance was observed.

[0301] [Table 6]

[0302]

[0303] In Examples 11 to 16, a crosslinking agent (isocyanate crosslinking agent (D1)) was added under the conditions of Example 5, but no adverse effect on chalk mark resistance was observed.

[0304] [Table 7]

[0305]

[0306] When comparing Example 17 with Comparative Example 4, Example 18 with Comparative Example 5, Example 19 with Comparative Example 6, and Example 20 with Comparative Example 7, improvement in chalk mark resistance was observed under all conditions. In Example 20, a C6 fluorine-based water repellent (Asahi Guard E-SERIES AG-E082, solid content concentration 20%, active ingredient concentration about 20%, manufactured by AGC Corporation, hereinafter referred to as AG-E082) containing a fluorine compound having a perfluoroalkyl group with 1 to 6 carbon atoms was used for investigation.

[0307] [Table 8]

[0308]

[0309] In Examples 21 to 24, water resistance and chalk mark resistance were evaluated for the mixing ratio of Example 5. When the mass ratio of component (AB) / component (C) was 0.12 or more, improvement in chalk mark resistance was observed, and 0.43 or more was relatively excellent, and 1 or more was the most excellent result.

[0310] [Table 9]

[0311]

[0312] Compared with Comparative Example 8, improvement in chalk mark resistance was observed in Examples 25 to 30. When the mass ratio of component (AB) / component (C) was 0.13 or more, improvement in chalk mark resistance was observed, and when it was 0.41 or more, the result was the most excellent. In addition, when Comparative Example 8 was compared with Example 28, almost no adverse effect on pin slippage was observed, and improvement in peel strength was observed.

[0313] [Table 10]

[0314]

[0315] Compared with Comparative Example 9, improvement in chalk mark resistance was observed in Examples 31 to 37. When the mass ratio (component (AB) / component (C)) was 0.19 or more, improvement in chalk mark resistance was observed, and when it was 0.50 or more, the result was the most excellent. In addition, when Comparative Example 9 was compared with Examples 33 and 37, although the pin slipping property was slightly deteriorated, the peel strength was improved.

[0316] [Table 11]

[0317]

[0318] In Examples 38 to 41, the case where the types of the polyisocyanate compound and the blocking agent of the reactant (AB) were changed was studied. In Example 42, the case where the reactant (AB) did not have self-emulsification (dispersibility) was studied. In Examples 43 to 45, the case where the reactant (AB) had a hydroxyl group as a reactive functional group in addition to the blocked isocyanate group was studied. Compared with Comparative Examples 1 and 3, improvements in chalk mark resistance were observed in Examples 38 to 45.

Claims

1. A waterproofing agent composition, characterized in that: It contains at least: a reaction product (AB) of a polyol compound (A) and a polyisocyanate compound (B), and a water-repellency-imparting compound (C); The polyol compound (A) is at least one of a polyol compound (A1) and a polyol compound (A2), wherein the polyol compound (A1) has at least one functional group selected from the group consisting of an ether group, a carbonate group and an ester group, and the polyol compound (A2) does not have any of the above functional groups; The reactant (AB) has an isocyanate group, In the reactant (AB), when the polyol compound (A) is composed only of the polyol compound (A2), the molar ratio B / A2 of the isocyanate group of the polyisocyanate compound (B) to the hydroxyl group of the polyol compound (A2) is 2.1 or more, The water repellency-imparting compound (C) does not have a perfluoroalkyl group having 7 or more carbon atoms, The mass ratio AB / C of the reactant (AB) to the water repellency imparting compound (C) is 0.05 or more, The polyol compound (A1) is a polymer polyol compound having at least one group selected from the group consisting of an ether group, a carbonate group and an ester group as a bonding group forming a main chain, The water repellency imparting compound (C) comprises at least one selected from the group consisting of a fluorine compound having a perfluoroalkyl group having 1 to 6 carbon atoms, a non-fluorine compound having a hydrocarbon group having 7 to 40 carbon atoms, and an organosilicon compound having at least an alkyl group having 3 to 50 carbon atoms, The polyol compound (A) does not contain a compound represented by the following general formula (3): W[-A-R] a [-B] b (3) In the general formula (3), W is an organic group with a valence of (a+b); A is bonded to W and is -XY- or -Y-; B is bonded to W and is -XZ or -Z; a is an integer greater than 1; b is an integer greater than 1; (a+b) is 3 to 42; X is a divalent polyalkylene ether group; Y is a divalent group, which is an ether group, ester group, amide group, carbamate group, urea group or thiol carbamate group; R is a monovalent hydrocarbon group having 7 to 40 carbon atoms; Z is a hydroxyl group, an amino group, a carboxyl group or a thiol group; wherein, when B is -XZ, Z is a hydroxyl group.

2. The waterproofing agent composition according to claim 1, wherein In the reactant (AB), when the polyol compound (A) is composed only of the polyol compound (A1), the ratio of the number of moles of isocyanate groups of the polyisocyanate compound (B) to the number of moles of hydroxyl groups of the polyol compound (A1), i.e., the molar ratio B / A1, is in the range of 1 to 25.

3. The waterproofing agent composition according to claim 1 or 2, wherein: In the reactant (AB), the ratio of the number of moles of isocyanate groups of the polyisocyanate compound (B) to the total number of moles of hydroxyl groups of the polyol compound (A1) and the polyol compound (A2), i.e., the molar ratio B / (A1+A2), is in the range of 1 to 25.

4. The waterproofing agent composition according to claim 1 or 2, wherein The isocyanate group in the structure of the reactant (AB) is a blocked isocyanate group.

5. The waterproofing agent composition according to claim 4, wherein The reactant (AB) has a hydroxyl group in its structure.

6. The waterproofing agent composition according to claim 1 or 2, wherein: The reactant (AB) has at least one group selected from the group consisting of a nonionic hydrophilic group, a cationic hydrophilic group, and an anionic hydrophilic group.

7. The waterproofing agent composition according to claim 1 or 2, wherein: The water repellent composition comprises a cross-linking agent (D).

8. The waterproofing agent composition according to claim 1 or 2, wherein: The water repellent composition further comprises a surfactant.

9. A water-repellent fiber product, which is obtained by treating the fiber product with the water-repellent composition according to any one of claims 1 to 8. 10 . A method for producing a water-repellent fiber product, comprising the step of bringing the water-repellent composition according to claim 1 into contact with a fiber product.

11. A kit for preparing a waterproofing agent composition, comprising: A first agent comprising at least a reactant (AB) of a polyol compound (A) and a polyisocyanate compound (B); and a second agent comprising at least a water-repellency-imparting compound (C), The polyol compound (A) is at least one of a polyol compound (A1) having at least one functional group selected from the group consisting of an ether group, a carbonate group, and an ester group, and a polyol compound (A2) having no functional group. The reactant (AB) has an isocyanate group, In the reactant (AB), when the polyol compound (A) is composed only of the polyol compound (A2), the molar ratio B / A2 of the isocyanate group of the polyisocyanate compound (B) to the hydroxyl group of the polyol compound (A2) is 2.1 or more, The water repellency-imparting compound (C) does not have a perfluoroalkyl group having 7 or more carbon atoms, The mass ratio AB / C of the reactant (AB) to the water repellency imparting compound (C) is 0.05 or more, The polyol compound (A1) is a polymer polyol compound having at least one group selected from the group consisting of an ether group, a carbonate group and an ester group as a bonding group forming a main chain, The water repellency imparting compound (C) comprises at least one selected from the group consisting of a fluorine compound having a perfluoroalkyl group having 1 to 6 carbon atoms, a non-fluorine compound having a hydrocarbon group having 7 to 40 carbon atoms, and an organosilicon compound having at least an alkyl group having 3 to 50 carbon atoms, The first agent and the second agent are mixed when used to prepare a waterproofing agent composition. The polyol compound (A) does not contain a compound represented by the following general formula (3): W[-AR] a [-B] b (3) In the general formula (3), W is an organic group with a valence of (a+b); A is bonded to W and is -XY- or -Y-; B is bonded to W and is -XZ or -Z; a is an integer greater than 1; b is an integer greater than 1; (a+b) is 3 to 42; X is a divalent polyalkylene ether group; Y is a divalent group, which is an ether group, an ester group, an amide group, a carbamate group, a urea group or a thiol carbamate group; R is a monovalent hydrocarbon group having 7 to 40 carbon atoms; Z is a hydroxyl group, an amino group, a carboxyl group or a thiol group; wherein, When B is -XZ, Z is hydroxy.

12. The kit according to claim 11, wherein The isocyanate group in the structure of the reactant (AB) is a blocked isocyanate group.

13. The kit according to claim 12, wherein The reactant (AB) has a hydroxyl group in its structure.