Fibers and fiber structures containing carbon powder
By using plant-derived carbon powder and specific process treatment, the problem of deodorization and coloring uniformity of black colored spun fibers is solved, improving fiber productivity and providing an environmentally friendly solution suitable for a variety of applications .
Patent Information
- Application Number
- CN202180039381.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-09-17
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2041-09-17
AI Technical Summary
The existing black color-spun fibers lack deodorization and coloring uniformity, and the use of petroleum-derived carbon black is not friendly to the environment. The spinnability and productivity of charcoal and bamboo charcoal are reduced at fine densities, and activated carbon is easy to fly and difficult to disperse evenly.
Use carbon powder from plants, such as coconut shell carbon powder, by controlling its specific surface area in the range of 250m2/g to 500m2/g, and the content between 0.2% and 7%, combined with synthetic or semi-synthetic fibers, using polyethylene For ester or polyamide fibers, the particle size distribution and specific surface area are adjusted through specific firing and crushing processes to ensure the deodorization and coloring uniformity of the fiber.
It achieves excellent deodorization and coloring uniformity, while improving fiber productivity, providing environmentally friendly black color-spun fiber suitable for a variety of clothing and material products.
Smart Images

Figure BDA0003971678200000151
Abstract
Description
Technical Field
[0001] The present invention relates to fibers and fiber structures containing carbon powder. Background Art
[0002] Black colored spun fibers have been used for clothing purposes such as black formal clothes and work clothes, as well as materials for gloves, brushes, etc. As a material constituting the fibers, carbon black is often used. Carbon black is generally produced by spraying / burning oil from petroleum as a raw material in a mist form. In order to facilitate the control of particle size, such a production method is often used.
[0003] For example, Patent Documents 1 and 2 disclose a black polyester spun fiber containing carbon black having a particle size, specific surface area, etc. within a given range. Patent Document 3 discloses a fiber containing carbon powder such as charcoal and / or bamboo charcoal in addition to carbon black, or containing carbon powder such as charcoal and / or bamboo charcoal instead of carbon black. In addition, Patent Document 4 discloses a fiber containing activated carbon.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Publication No. 2006-241640
[0007] Patent Document 2: Japanese Patent Application Laid-Open No. 9-250026
[0008] Patent Document 3: Japanese Patent Application Publication No. 2002-249922
[0009] Patent Document 4: Japanese Patent Application Publication No. 2003-38626 Summary of the invention
[0010] Problems to be solved by the invention
[0011] The black colored spun fibers described in Patent Documents 1 and 2 are fibers containing carbon black and do not have deodorizing properties. In addition, carbon black is a raw material derived from petroleum, and from the perspective of environmental protection, there is a demand for black colored spun fibers using raw materials that are not derived from petroleum. The fibers described in Patent Document 3 may contain charcoal and / or bamboo charcoal in the form of carbon powder, but in order to use charcoal and bamboo charcoal to fully exert deodorizing properties, a large amount of carbon powder needs to be used. However, in the case of containing a large amount of charcoal and bamboo charcoal, especially in the range of fine fiber, the spinning property in the fiberization process is sometimes reduced, and the productivity is reduced. In addition, sometimes the reduction in processability caused by the shedding of carbon powder becomes a problem. The fibers containing activated carbon described in Patent Document 4 may have deodorizing properties, but during the manufacture of the fibers, the activated carbon is easily scattered, so from the perspective of having to be manufactured in a specific environment, the productivity is sometimes not good. In addition, it is difficult to evenly disperse the activated carbon in the fibers, so sometimes the coloring uniformity of the black colored spun fibers is insufficient.
[0012] Therefore, an object of the present invention is to provide a black colored spun fiber which has excellent deodorizing properties and coloring uniformity and good fiber productivity.
[0013] Solutions to the problem
[0014] The present inventors have conducted intensive studies to solve the above problems and have completed the present invention. That is, the present invention includes the following preferred embodiments.
[0015] [1] A fiber containing carbon powder, wherein the fiber contains carbon powder derived from plants, wherein:
[0016] The specific surface area of the above carbon powder is 250m 2 / g or more and less than 500m 2 / g, and the content of the carbon powder is 0.2 to 7 mass % based on the mass of the fiber containing the carbon powder.
[0017] [2] The carbon powder-containing fiber according to [1], wherein the carbon powder is carbon powder derived from coconut shells.
[0018] [3] The carbon powder-containing fiber according to [1] or [2], wherein the fiber is a synthetic fiber or a semi-synthetic fiber.
[0019] [4] The carbon powder-containing fiber according to [3], wherein the fiber is a polyester fiber or a polyamide fiber.
[0020] [5] The fiber containing carbon powder according to any one of [1] to [4], wherein the average particle size D of the carbon powder is 50 It is less than 1.5μm.
[0021] [6] The fiber containing carbon powder according to any one of [1] to [5], wherein the particle size distribution of the carbon powder is D 90 The value is 4.0μm or less.
[0022] [7] The carbon powder-containing fiber according to any one of [1] to [6], wherein the single fiber fineness is 0.01 to 10 dtex.
[0023] [8] A fiber structure comprising the carbon powder-containing fiber according to any one of [1] to [7].
[0024] Effects of the Invention
[0025] According to the present invention, a black colored spun fiber having excellent deodorizing properties and coloring uniformity and good fiber productivity can be provided. In addition, the fiber containing carbon powder of the present invention is carbon neutral, and an environmentally friendly black colored spun fiber can also be provided. DETAILED DESCRIPTION
[0026] Hereinafter, the embodiments of the present invention will be described in detail. It should be noted that the scope of the present invention is not limited to the embodiments described here, and various modifications can be made within the scope of the present invention.
[0027] The fiber containing carbon powder of the present invention contains carbon powder from plants in the fiber, wherein the specific surface area of the carbon powder is 250 m 2 / g or more and less than 500m 2 / g, and the content of the carbon powder is 0.2 to 7 mass % based on the mass of the fiber containing the carbon powder.
[0028] 〔Carbon powder〕
[0029] The carbon powder contained in the carbon powder-containing fiber of the present invention is a carbon powder derived from plants. The carbon powder derived from plants can be obtained using plants as the main raw material. It can be considered that the carbon powder derived from plants is a carbon powder having a very complex structure such as a plant-specific tissue structure, compared to carbon powders derived from non-plant raw materials, such as carbon black, and carbon powders derived from petroleum. In the present invention, by making the carbon powder a plant-derived powder having a given specific surface area, a high deodorizing property can be achieved by adding a relatively small amount of carbon powder. In addition, compared to carbon powders derived from minerals, petroleum, synthetic raw materials, etc., carbon powders derived from plants are carbon neutral, and therefore, are also advantageous from the perspective of environmental protection and commercial considerations.
[0030] In the present invention, the plant used as the raw material of the plant-derived carbon powder is not particularly limited as long as it can obtain the carbon powder having the above-given specific surface area, and examples thereof include: coconut shell, coffee beans, tea leaves, sugar cane, fruit (orange or banana), straw, or rice husk. These plants can be used alone or in combination of two or more. From the viewpoint of more easily improving the deodorizing property and productivity of the black colored spun fiber, the carbon powder from the plant is preferably a carbon powder from at least one plant selected from coconut shell, coffee beans, tea leaves, sugar cane, fruit, straw and rice husk, and more preferably a carbon powder from coconut shell. Since it can be obtained in large quantities, it is commercially advantageous to use coconut shell as the raw material plant.
[0031] As mentioned above, it is difficult to fully increase the specific surface area of carbon powders such as charcoal and bamboo charcoal, and usually the specific surface area is less than 250m 2 / g or more, it is difficult to achieve sufficient deodorization with a small amount of addition in many cases. In addition, the specific gravity of the carbon powder of the activated carbon is too low, so it is easy to scatter when manufacturing the fiber containing the carbon powder, and the manufacturing conditions are limited. In addition, due to its high specific surface area, productivity is sometimes reduced due to agglomeration and coloring uniformity cannot be obtained. In addition, carbon black is not a raw material from plants, and has a shape with cavities inside the particles but few cavities on the surface, so its deodorization property cannot be considered sufficient. Therefore, the carbon powder in the fiber containing carbon powder of the present invention is preferably a carbon powder other than bamboo charcoal, charcoal, activated carbon and carbon black. It should be noted that in this mode, as long as the fiber containing carbon powder of the present invention contains carbon powder other than bamboo charcoal, charcoal, activated carbon and carbon black, it can also contain a carbon powder selected from bamboo charcoal, charcoal, activated carbon and carbon black in addition to the carbon powder, within the range that does not damage the effect of the present invention.
[0032] The coconut used as the raw material of the coconut shell is not particularly limited, and examples thereof include oil palm, coconut tree, snake fruit, and hyacinth fruit. The coconut shell obtained from these coconuts can be used alone or in combination of two or more. Among them, coconut shells from coconut trees or oil palms, which are used as food, detergent raw materials, biodiesel raw materials, etc. and are produced in large quantities as biomass waste, are particularly preferred because they are easy to obtain and inexpensive.
[0033] The specific surface area of the carbon powder contained in the carbon powder-containing fiber of the present invention is 250 m 2 / g or more and less than 500m 2 / g. The specific surface area of carbon powder is less than 250m 2 / g, the amount of pores formed on the surface of the carbon powder is too small, so the deodorizing property of the obtained fiber is insufficient. In addition, in order to improve the deodorizing property, a large amount of carbon powder needs to be mixed in the fiber, so the productivity when manufacturing the fiber is reduced, or the carbon powder is easily lost during the manufacturing and use of the fiber. From the viewpoint of easily improving the deodorizing property and productivity of the fiber containing carbon powder, the specific surface area of the carbon powder is preferably 300m 2 / g or more, more preferably 330m 2 / g or more, more preferably 360m 2 / g or more, more preferably 380m 2 / g or more, particularly preferably 400m 2 / g or above.
[0034] In addition, the specific surface area of the carbon powder is 500m 2 / g or more, the specific gravity of the carbon powder is too low, so it is easy to scatter when manufacturing fibers containing carbon powder, and the manufacturing conditions are limited. In addition, its specific surface area is too high, so sometimes the productivity is reduced due to agglomeration and the coloring uniformity cannot be obtained. As the cause of agglomeration, it can be inferred that as the specific surface area increases, the surface energy increases, the primary particles become easily unstable, and the functional groups exposed on the surface of the particles increase, the electrostatic attraction increases, and therefore, it becomes easy to agglomerate. In addition, similarly, when mixed with the components constituting the fiber, the carbon powder is easy to exist in a coagulated state. As a result, when the carbon powder is mixed with the components such as the resin constituting the fiber, it is difficult to evenly disperse the carbon powder, and the black color in the black color spun fiber is prone to unevenness, and the coloring uniformity of the obtained fiber containing carbon powder is reduced. In addition, in order to obtain uniformly colored black color spun fibers, it is necessary to extend the mixing time of the carbon powder and the components constituting the fiber before spinning, and for fibers with a small single fiber fineness, the broken fibers when the fibers are spun become more due to the agglomerates, so the productivity is reduced. From the viewpoint of improving the coloring uniformity and productivity of the fiber containing the carbon powder, the specific surface area of the carbon powder is preferably 480 m 2 / g or less, more preferably 470m 2 / g or less, more preferably 460m 2 / g or less, more preferably 450m 2 / g or less. The specific surface area of the carbon powder is a BET specific surface area that can be calculated by a nitrogen adsorption method, and can be calculated, for example, by the method described in the Examples. The specific surface area of the carbon powder can be measured by using a carbon powder used as a raw material when manufacturing fibers containing carbon powder as a measurement sample, and dissolving and removing the resin constituting the fibers from the fibers containing carbon powder, and using the carbon powder obtained as a measurement sample.
[0035] As a method for producing carbon powder having a specific surface area within the above-mentioned range, the method of burning plants exemplified above can be cited. The method of burning plants to produce carbon powder is not particularly limited, and can be produced by methods known in the art. For example, it can be produced by heating the plant as a raw material for about 1 to 20 hours (carbonization treatment) in an inert gas atmosphere at a temperature of, for example, above 300°C and below 900°C. In order to adjust the specific surface area to the desired range, the carbon powder obtained by the above-mentioned burning process can be crushed and / or classified. In particular, when using plants with relatively high hardness such as coconut shells as plants, there is a tendency for coarse powder to remain easily during crushing. Therefore, from the viewpoint of easily improving the productivity of fibers containing carbon powder, it is preferred to remove the coarse powder by a crushing and / or classification process.
[0036] The inert gas is not particularly limited as long as it is a gas that does not react with the carbon powder at the above-mentioned calcination temperature. Examples thereof include nitrogen, helium, argon, krypton, or a mixed gas thereof, preferably nitrogen. In addition, the lower the concentration of impurity gases, especially oxygen, contained in the inert gas, the better. The generally permissible oxygen concentration is preferably 0 to 2000 ppm, more preferably 0 to 1000 ppm.
[0037] The pulverizer used for pulverization is not particularly limited, and for example, a bead mill, a jet mill, a ball mill, a hammer mill, or a rod mill can be used alone or in combination. From the perspective of easily obtaining a powder having a desired specific surface area, a jet mill having a classification function is preferred. On the other hand, when a ball mill, a hammer mill, or a rod mill is used, the desired specific surface area can be adjusted by performing classification after pulverization.
[0038] By performing classification after the pulverization treatment, the specific surface area and the like can be adjusted more accurately. As the classification, classification using a sieve, wet classification, or dry classification can be cited. As the wet classifier, for example, a classifier using the principles of gravity classification, inertial classification, hydraulic classification, or centrifugal classification can be cited. In addition, as the dry classifier, a classifier using the principles of sedimentation classification, mechanical classification, or centrifugal classification can be cited.
[0039] When the pulverizing step is performed, the pulverizing and classification can be performed using one device. For example, a jet mill with a dry classification function can be used for pulverizing and classification. In addition, a device in which the pulverizer and the classifier are independent can be used. In this case, the pulverizing and classification can be performed continuously or discontinuously.
[0040] The carbon powder obtained by burning plants under the temperature conditions as described above is, for example, an intermediate product in the manufacturing process of activated carbon. In the manufacture of activated carbon, a process of further activating the carbon powder obtained as described above is carried out. The activation treatment is a process in which pores are formed on the surface of the carbon powder to make it a porous carbonaceous material, thereby producing activated carbon having a large specific surface area and pore volume. As an activation treatment, for example, a gas activation treatment, a chemical activation treatment, etc. are carried out. The carbon powder contained in the fiber containing carbon powder of the present invention has a specific surface area within the above-mentioned range. The carbon powder having such a specific surface area is an unactivated carbon powder and is not activated carbon as an activated substance. Activated carbon has a specific surface area greater than 500 m 2 / g specific surface area, from this point of view, it is not the carbon powder contained in the fiber containing carbon powder of the present invention. In addition, in the manufacturing process of activated carbon, for the purpose of improving the performance of battery materials and purification materials manufactured using activated carbon, a process of removing fine powder of carbon powder as an intermediate product is sometimes performed before the activation treatment as described above. The removed fine powder is usually discarded or used as fuel. According to the present invention, the fine powder as waste can be upgraded (upcycling) as a functional raw material.
[0041] Whether the carbon powder has been activated can be confirmed by confirming the structure of the carbon powder using a transmission electron microscope (TEM) or a scanning electron microscope (SEM), for example. Therefore, the carbon powder contained in the carbon powder-containing fiber of the present invention is preferably a carbon powder having a specific surface area within the above range and having a structure that is usually formed by activation treatment and cannot be observed in a TEM or SEM image.
[0042] From the viewpoint of easily improving the spinnability and easily adjusting the specific surface area to the above range, the average particle size D of the particle size distribution of the carbon powder contained in the carbon powder-containing fiber of the present invention is 50 The average particle size D is preferably 1.5 μm or less, more preferably 1.3 μm or less, further preferably 1.2 μm or less, further more preferably 1.0 μm or less, particularly preferably 0.8 μm or less, and particularly preferably 0.7 μm or less. In addition, from the viewpoint that secondary aggregation is likely to occur when the particle size is too small, the average particle size D 50 It is preferably 0.03 μm or more, more preferably 0.05 μm or more, and even more preferably 0.1 μm or more.
[0043] From the viewpoint of improving the spinnability by easily removing the coarse particles, the particle size distribution of the carbon powder contained in the carbon powder-containing fiber of the present invention is D 90It is preferably 4.0 μm or less, more preferably 3.5 μm or less, further preferably 3.0 μm or less, and further more preferably 2.5 μm or less. In addition, from the viewpoint that secondary aggregation is easily caused when the particle size is too small, D 90 The particle size distribution of the carbon powder is preferably 0.1 μm or more, more preferably 0.2 μm or more, and even more preferably 0.5 μm or more. 50 and D 90 For example, the measurement can be performed using a centrifugal automatic particle size distribution measuring device.
[0044] 〔fiber〕
[0045] The fiber containing carbon powder of the present invention is a fiber containing the carbon powder as described above. Here, containing carbon powder in the fiber means containing carbon powder inside the fiber. It should be noted that a part of the carbon powder may be present on the surface of the fiber. The fiber may contain carbon powder inside, and there is no particular limitation as long as it is a component that can be processed into a fibrous state, for example, synthetic fibers, semi-synthetic fibers, etc. From the viewpoint of making it easy to contain carbon powder inside the fiber and easy to spin, the fiber is preferably a synthetic fiber or a semi-synthetic fiber.
[0046] Examples of synthetic fibers include polyester fibers, polyamide fibers, polyurethane fibers, polyolefin fibers, acrylic fibers, vinyl fibers, polyarylate fibers, polystyrene fibers, etc. Examples of semisynthetic fibers include regenerated cellulose fibers, cellulose derivative fibers, and regenerated protein fibers.
[0047] Polyester fibers are fibers containing polyester resins as the main component. Polyester resins are resins with the ability to form fibers that use aromatic dicarboxylic acids as the main acid components, and examples thereof include polyethylene terephthalate, polybutylene terephthalate, polytrimethylene terephthalate, polytetramethylene terephthalate, polycyclohexane dimethylene terephthalate, polyethylene 2,6-naphthalate, etc. In addition, these polyesters may be copolymers formed by copolymerizing an alcohol component such as butanediol or a dicarboxylic acid such as isophthalic acid as the third component, or may be a mixture of the above-mentioned various polyesters. Among them, polyethylene terephthalate polymers are preferred from the viewpoints of handling and cost.
[0048] Polyamide fibers are fibers containing polyamide resin as the main component. Polyamide resin is a polymer having repeating structural units linked by amide bonds, and polyamide fibers are also called nylon. In addition, aramid fibers containing aromatic polyamide polymers are also included in polyamide fibers. Examples of polyamide resins include aliphatic polyamides such as polyamide 6, polyamide 66, polyamide 610, polyamide 10, polyamide 12, and polyamide 6-12, and copolymers thereof, and semi-aromatic polyamides synthesized from aromatic dicarboxylic acids and aliphatic diamines.
[0049] Polyurethane fibers are fibers containing polyurethane resin as a main component, such as spandex fibers. Polyolefin fibers are fibers containing polyolefin resin as a main component, such as polyethylene fibers, polypropylene fibers, polymethylpentene fibers, etc. Acrylic fibers are fibers containing acrylic resin as a main component, such as acrylic fibers, modified polyacrylonitrile fibers, etc. Vinyl fibers are fibers containing vinyl resin as a main component, such as polyvinyl alcohol fibers, ethylene-vinyl alcohol copolymer fibers, vinyl chloride fibers, etc.
[0050] Regenerated cellulose fibers and cellulose derivative fibers are fibers composed of cellulose and / or its derivatives as the main component, and examples thereof include rayon, cuprammonium fibers, lyocell fibers, etc. Regenerated protein fibers are fibers composed of proteins extracted from protein-containing materials, and examples thereof include soy protein fibers, milk casein fibers, etc.
[0051] In a preferred embodiment of the carbon powder-containing fiber of the present invention, the fiber is preferably a polyester fiber or a polyamide fiber from the viewpoint of ease of mixing the powder and versatility of the fiber.
[0052] 〔Fiber containing carbon powder〕
[0053] The fiber containing carbon powder of the present invention contains carbon powder from plants in the fiber. The content of carbon powder in the fiber containing carbon powder is 0.2 to 7% by mass relative to the mass of the fiber containing carbon powder. When the content of carbon powder is less than 0.2% by mass, the content of carbon powder is insufficient, and therefore, sufficient deodorization cannot be obtained. From the viewpoint of easily improving deodorization, the content of carbon powder relative to the mass of the fiber containing carbon powder is preferably 0.25% by mass or more, more preferably 0.3% by mass or more, further preferably 0.4% by mass or more, and further more preferably 0.5% by mass or more. In applications requiring higher deodorization, the content of carbon powder relative to the mass of the fiber containing carbon powder can be preferably 1% by mass or more, and more preferably 3% by mass or more. In addition, when the content of carbon powder in the fiber containing carbon powder exceeds 7% by mass, it is not possible to fully suppress the breakage of the fiber when spinning, and therefore, the productivity of the fiber containing carbon powder is reduced. From the viewpoint of easily improving the productivity of the fiber containing carbon powder, the content of carbon powder is preferably 6.5 mass % or less, more preferably 6 mass % or less, further preferably 5.5 mass % or less, and further more preferably 5 mass % or less.
[0054] From the viewpoint of spinnability and hand feel, the single-filament fineness of the fiber containing carbon powder is preferably 0.01 to 10 dtex. When the single-filament fineness is above the above lower limit, it is easy to fully suppress the occurrence of broken fibers when the fibers are spun. From the viewpoint of improving spinnability, the single-filament fineness is more preferably 0.05 dtex or more, and further preferably 0.1 dtex or more. In addition, when the single-filament fineness is below the above upper limit, when the fiber is used to manufacture a braided fabric or a woven fabric, it is easy to make the finished product soft and easy to obtain a good hand feel. From the viewpoint of making a product with a good hand feel, the single-filament fineness is more preferably 7 dtex or less, and further preferably 4 dtex or less.
[0055] The total fineness of the fiber containing carbon powder is not particularly limited and can be appropriately set according to the purpose of using the fiber containing carbon powder. From the viewpoint of spinnability and versatility, the fineness is preferably 15 to 300 dtex, more preferably 20 to 200 dtex. In addition, the number of filaments is preferably 2 to 200 filaments, more preferably 3 to 100 filaments.
[0056] The strength of the fiber containing carbon powder is not particularly limited and can be appropriately set according to the purpose of using the fiber containing carbon powder. From the perspective of easily preventing broken wires and fuzzing due to guide wear when manufacturing woven fabrics, it is preferably 1 cN / dtex or more, more preferably 1.5 cN / dtex or more, and further preferably 2 cN / dtex or more. The upper limit of the strength is not particularly limited, and the strength obtained by a conventional melt spinning method is about 5.0 cN / dtex or less.
[0057] The elongation of the fiber containing carbon powder is not particularly limited, and can be appropriately set according to the purpose of using the fiber containing carbon powder. From the viewpoint of tow processability, it is preferably 10% or more, more preferably 20% or more, and further preferably 30% or more. The upper limit of the elongation is not particularly limited, but from the viewpoint of handling based on the product form, it is preferably 150% or less, and more preferably 100% or less.
[0058] The cross-sectional shape of the fiber containing carbon powder may be a fiber having a circular cross-sectional shape, a flat cross-sectional shape, a multi-lobed cross-sectional shape, a hollow cross-sectional shape, etc. The fiber containing carbon powder may be a fiber having a core-sheath structure.
[0059] As long as the effect of the present invention is not impaired, any additive may be contained in the fiber containing carbon powder of the present invention as required. Examples of such additives include antioxidants, plasticizers, heat stabilizers, ultraviolet absorbers, antistatic agents, lubricants, fillers, other polymer compounds, etc. One of these may be used, or two or more may be used in combination.
[0060] [Method for producing fiber containing carbon powder]
[0061] The fiber containing carbon powder of the present invention can be produced by using the components constituting the above-mentioned fiber, carbon powder, and other components and additives used as needed, and using a conventionally known spinning apparatus. For example, spinning can be performed by melt spinning, specifically, it can be produced by any production method such as a method of stretching after melt spinning at a low speed or a medium speed, a high-speed direct spinning stretching method, and a method of stretching and false twisting simultaneously or continuously after spinning.
[0062] As an example of a specific manufacturing method, a composition containing the components constituting the fiber, carbon powder, and any other components added can be melted using a melt extruder, the molten polymer stream is introduced into a spinning head, metered with a gear pump, ejected from a spinning nozzle of a desired shape, stretched as needed, and then wound up, thereby manufacturing the fiber of the present invention. The mixing of the components constituting the fiber and the carbon powder can be carried out by directly mixing them, or by mixing a part of the components with the carbon powder in advance to obtain a masterbatch, and mixing the masterbatch with the components constituting the fiber. The melting temperature during spinning can be appropriately adjusted according to the melting point of the components constituting the fiber, etc., and is generally preferably about 150 to 300°C. The filaments ejected from the spinning nozzle can be directly wound up at high speed without being stretched, or stretched as needed. The stretching operation is usually carried out at a temperature above the glass transition temperature of the components constituting the fiber at a stretching ratio of 0.55 to 0.9 times the elongation at break (HDmax). When the stretching ratio is less than 0.55 times the elongation at break, it is difficult to stably obtain fibers having sufficient strength, and when it exceeds 0.9 times the elongation at break, fiber breakage is likely to occur.
[0063] For stretching, there are cases where the fiber is temporarily wound up after being ejected from the spinning nozzle and then stretched, and cases where it is implemented after stretching, and any of these cases can be used in the present invention. The stretching operation is usually performed by hot stretching, and any method such as hot air, hot plate, hot roller, water bath, etc. can be used. In addition, the extraction speed is different in the case of temporarily winding up and then stretching, the case of spinning stretching and winding up through a process of direct spinning and stretching, and the case of winding up directly at high speed without stretching. The extraction is performed in the range of about 500 to 6000 m / min. When it is lower than 500 m / min, the productivity is poor, and at an ultra-high speed exceeding 6000 m / min, fiber breakage is likely to occur. In addition, the cross-sectional shape of the fiber of the present invention is not particularly limited, and a conventional melt spinning method can be used to form a perfect circular, hollow, or irregular cross-section according to the shape of the nozzle. In addition, it can have a core-sheath structure, which is composed of a core part or a sheath part formed based on a composition containing a component constituting the fiber and carbon powder, and a sheath part or a core part containing a component constituting the fiber. From the viewpoint of the process passability in fiberization and weaving, a perfect circle is preferred.
[0064] 〔Fiber structure〕
[0065] The fiber containing carbon powder of the present invention can be used as various fiber structures (fiber aggregates), and the present invention also provides a fiber structure containing the fiber containing carbon powder of the present invention. Here, the "fiber structure" may be a multifilament, spun yarn, knitted fabric, nonwoven fabric, paper, artificial leather, and filler formed only from the fiber containing carbon powder of the present invention, a knitted fabric, nonwoven fabric formed by partially using the fiber containing carbon powder of the present invention, a knitted fabric with other fibers such as natural fibers, chemical fibers, synthetic fibers, and semi-synthetic fibers, a knitted fabric used as a processed yarn such as a blended yarn, a mixed yarn, a twisted yarn, a mixed yarn, a crimped yarn, a cotton-blended nonwoven fabric, a fiber laminate, and the like.
[0066] The carbon powder-containing fiber of the present invention and the fiber structure containing the carbon powder-containing fiber of the present invention have excellent deodorizing properties and black coloring uniformity. Therefore, the carbon powder-containing fiber and the fiber structure of the present invention can be used as clothing products such as shirts, pants, coats, uniforms, work clothes, underwear, leggings, socks, sportswear, black formal clothes, interior fabrics such as curtains and carpets, gloves, brushes, filters, sheets, and other material products.
[0067] Example
[0068] The present invention will be described below by way of examples, but the present invention is not limited to these examples. It should be noted that, unless otherwise specified, % in the examples is relative to mass. First, the measurement method of each physical property value is described.
[0069] <Particle size distribution measurement method>
[0070] The particle size distribution of the carbon powder was measured using a centrifugal automatic particle size distribution measuring apparatus CAPA-500 manufactured by Horiba, Ltd. 50 and D 90 .
[0071] <Specific surface area>
[0072] The specific surface area of the carbon powder was measured using a high-precision surface area / pore distribution measuring device (Microtrac BEL "BELSORP28SA"). After the sample was vacuum degassed at 300°C for 5 hours, the nitrogen adsorption isotherm at 77K was measured. The obtained adsorption isotherm was used for multi-point analysis by the BET method, and the specific surface area was calculated from the straight line in the relative pressure region of P / P0 = 0.01 to 0.1 of the obtained curve.
[0073] <Production Example 1: Production of Coconut Shell Carbon Powder 1>
[0074] The coconut shell flakes were calcined (carbonized) at 500°C in a nitrogen atmosphere, washed and dried, dry-ground, and classified to recover the fine powder. The particle size at this time was: D 50 =1.5μm, D 90 =3.8μm. Then, dry pulverization was performed again to obtain coconut shell carbon powder 1. The particle size of coconut shell carbon powder 1 is: D 50 =0.7μm, D 90 =2.2μm, specific surface area is 440m 2 / g.
[0075] <Production Example 2: Production of Coconut Shell Carbon Powder 2>
[0076] The coconut shell flakes were calcined (carbonized) at 500°C in a nitrogen atmosphere, washed and dried, dry-pulverized, and classified to recover the fine powder to obtain coconut shell carbon powder 2. The particle size of coconut shell carbon powder 2 is: 50 =1.3μm, D 90 =3.8μm, specific surface area is 420m 2 / g.
[0077] <Production Example 3: Production of Coconut Shell Carbon Powder 3>
[0078] The coconut shell flakes were calcined (carbonized) at 450°C in a nitrogen atmosphere, washed and dried, dry-ground, and classified to recover the fine powder. The particle size at this time was: D 50 =1.5μm, D 90 =3.8μm. Then, dry pulverization was performed again to obtain coconut shell carbon powder 3. The particle size of coconut shell carbon powder 3 is: D 50 =0.8μm, D 90 =2.2μm, specific surface area is 270m 2 / g.
[0079] <Production Example 4: Production of Coconut Shell Carbon Powder 4>
[0080] The coconut shell flakes were calcined (carbonized) at 400°C in a nitrogen atmosphere, washed and dried, dry-ground, and classified to recover the fine powder. The particle size at this time was: D 50 =1.5μm, D 90 =3.8μm. Then, dry pulverization was performed again to obtain coconut shell carbon powder 4. The particle size of coconut shell carbon powder 4 is: D 50 =0.8μm, D 90 =2.4μm, specific surface area is 190m 2 / g.
[0081] <Production Example 5: Production of charcoal powder>
[0082] The wood of Quercus occidentalis was burned at 1200°C and then rapidly cooled to 350°C. The white charcoal (binchotan) produced by this was dry-pulverized to obtain charcoal powder. The particle size of the obtained charcoal powder is: 50 =0.5μm, D 90 =1.9μm, specific surface area is 240m 2 / g.
[0083] <Example 1>
[0084] The coconut shell carbon powder 1 obtained in Manufacturing Example 1 was added to polyamide 6 (nylon 61011FK manufactured by Ube Industries, Ltd.) in a ratio such that the content of carbon powder 1 relative to the mass of the finally obtained fiber containing carbon powder was as shown in Table 1, and kneaded using a twin-screw extruder at a temperature of 280 to 300° C. to obtain a resin composition. A spinneret having 24 holes and a circular cross-sectional shape was used to spin the obtained resin composition at a spinning temperature of 250°C and a discharge amount of 29.4 g / min. After cooling air at a temperature of 25°C and a humidity of 60% was blown to the spun yarn at a speed of 1.0 m / sec, the yarn was introduced into a tubular heater (internal temperature 160°C) with a length of 1.0 m, an inlet diameter of 8 mm, an outlet diameter of 10 mm, and an inner diameter of 30 mmφ and a position 1.2 m below the spinning spinneret. After being stretched in the tubular heater, oil was supplied to the yarn fed from the tubular heater through an oiling nozzle, and the yarn was wound up at a speed of 3500 m / min via two extraction rollers to obtain a fiber 1 containing carbon powder of 84 dtex / 24 filaments.
[0085] <Examples 2 and 3>
[0086] Carbon powder-containing fibers 2 and 3 were obtained in the same manner as in Example 1 except that the content of the coconut shell carbon powder 1 was changed to the amount shown in Table 1.
[0087] <Example 4>
[0088] Fibers 4 containing carbon powder were obtained in the same manner as in Example 2 except that a spinneret having a cross-shaped cross section was used.
[0089] <Example 5>
[0090] The coconut shell carbon powder 1 was mixed with polyamide 6 (nylon 6 1011FK manufactured by Ube Industries, Ltd.) so that the content of the carbon powder 1 relative to the mass of the finally obtained carbon powder-containing fiber became the content shown in Table 1, the obtained resin composition was used as the sheath component, the polyamide 6 (nylon 6 1015B manufactured by Ube Industries, Ltd.) was used as the core component, and a spinneret having a core-sheath cross-sectional shape was used. Fiber 5 containing carbon powder was obtained in the same manner as in Example 1, except that the spinneret had a core-sheath cross-sectional shape.
[0091] <Example 6>
[0092] Carbon powder-containing fibers 6 were obtained in the same manner as in Example 2 except that the coconut shell carbon powder 2 obtained in Production Example 2 was used instead of the coconut shell carbon powder 1.
[0093] <Example 7>
[0094] Carbon powder-containing fibers 7 were obtained in the same manner as in Example 2 except that the coconut shell carbon powder 3 obtained in Production Example 3 was used instead of the coconut shell carbon powder 1 .
[0095] <Example 8>
[0096] Fiber 8 containing carbon powder was obtained in the same manner as in Example 1 except that a spinneret having 96 holes and a circular cross-sectional shape was used and spinning was carried out at a spinning temperature of 250°C and a discharge amount of 29.4 g / min and the fineness was changed to 84 dtex / 96 filaments.
[0097] <Comparative Examples 1 and 2>
[0098] Carbon powder-containing fibers 9 and 10 were obtained in the same manner as in Example 1 except that the content of the coconut shell carbon powder 1 was changed to the amount shown in Table 1.
[0099] <Comparative Example 3>
[0100] Carbon powder-containing fibers 11 were obtained in the same manner as in Example 2 except that the coconut shell carbon powder 4 obtained in Production Example 4 was used instead of the coconut shell carbon powder 1.
[0101] <Comparative Example 4>
[0102] Fibers 1 containing charcoal fine powder were obtained in the same manner as in Example 2 except that the charcoal fine powder obtained in Production Example 5 was used instead of the coconut shell carbon powder 1.
[0103] <Comparative Example 5>
[0104] Carbon black (Vulcan XC-72 manufactured by CABOT, with a specific surface area of 214 m 2Fibers containing carbon black were obtained in the same manner as in Example 1 except that the coconut shell carbon powder 1 was replaced with 0.1% / g.
[0105] <Comparative Example 6>
[0106] Activated carbon (Kuraray Coal PW-D, surface area: 1500 m 2 Fibers containing activated carbon were obtained in the same manner as in Example 1 except that the coconut shell carbon powder 1 was replaced with 0.1% Coconut shell carbon powder 1.
[0107] <Comparative Example 7>
[0108] Except having changed the content of charcoal fine powder into the amount shown in Table 1, it carried out similarly to the comparative example 4, and obtained the fiber 2 containing charcoal fine powder.
[0109] The fibers of Examples and Comparative Examples obtained as described above were tested for color unevenness of yarn bundles, spinnability, and deodorizing properties as follows.
[0110] <Evaluation of uneven color of yarn bundle>
[0111] After a cylindrical braided fabric was made by a cylindrical braiding machine using the fibers of the examples and comparative examples, the L of the cylindrical web was measured using a spectrophotometer "CM-3700A" manufactured by Konica Minolta Co., Ltd. under the conditions of mirror reflection treatment: SCE, measurement diameter: LAV (25.4 mm), UV condition: 100% Full, field of view: 2°, and main light source: C light source. * The values were measured. The measurement was performed 5 times, and the difference between the maximum and minimum values of the obtained measurement results was calculated, and the color unevenness of the tow was evaluated according to the following criteria. The smaller the difference between the maximum and minimum values, the smaller the color deviation.
[0112] ○:L * The difference between the maximum and minimum values is less than 2
[0113] ×:L * The difference between the maximum and minimum values is 2 or more
[0114] It should be noted that, in the case of the fiber obtained in Example 1, L * The minimum value of L is 19.2, the maximum value is 19.8, and the difference is 0.6. In the case of the fiber obtained in Example 6, L * The minimum value of L is 17.8, the maximum value is 18.3, and the difference is 0.5. In contrast, in the case of the fiber obtained in Comparative Example 6, L * The minimum value is 17.0, the maximum value is 19.2, and the difference is 2.2.
[0115] <Evaluation of spinnability>
[0116] When fibers were produced continuously for 12 hours under the conditions of the above-described Examples and Comparative Examples, the number of times fiber breakage occurred was measured and evaluated based on the following criteria.
[0117] ◎: The number of broken threads in 12 hours is less than 1 time
[0118] ○: The number of wire breakages in 12 hours is 2 or more and 10 or less
[0119] ×: The number of wire breakages in 12 hours is 11 or more
[0120] <Evaluation of deodorizing properties>
[0121] Based on the deodorizing test method according to the SEK mark fiber product certification standard of KAKEN TEST CENTER, the test was conducted using the ammonia detector tube method, and the residual ammonia concentration after 2 hours was measured. In addition, the deodorizing performance was evaluated according to the following criteria.
[0122] ◎: The residual concentration of ammonia after 2 hours is less than 20%
[0123] ○: The residual concentration of ammonia after 2 hours is more than 20% and less than 50%
[0124] ×: The residual concentration of ammonia after 2 hours exceeds 50%
[0125]
[0126] In the carbon powder-containing fibers of Examples 1 to 8, the content of carbon powder relative to the mass of the carbon powder-containing fibers was 0.2 to 7% by mass, and the specific surface area of the carbon powder was 250 m 2 / g or more and less than 500m 2 / g, it was confirmed that the fiber had spinnability and deodorizing properties, and the color unevenness of the fiber bundle was small. In contrast, in the case of Comparative Example 1, in which the content of carbon powder was as low as 0.1 mass%, sufficient deodorizing properties were not obtained. In addition, in the case of Comparative Example 2, in which the content of carbon powder was higher than 7 mass%, fiber breakage occurred during fiber production, and it was considered that the spinnability was not sufficient. In addition, in the case of the fiber containing a specific surface area of 190m 2 In the case of Comparative Example 3 using carbon powder of 100 g / g, Comparative Example 4 using charcoal powder, and Comparative Example 5 using carbon black, sufficient deodorizing properties were not obtained. In addition, in the case of Comparative Example 6 using activated carbon, uniform coloring properties were not obtained. It should be noted that, in Comparative Example 7 using a large amount of charcoal powder, deodorizing properties were obtained, but the spinnability was poor.
Claims
1. A fiber containing carbon powder, wherein the fiber contains carbon powder from coconut shell, wherein: The specific surface area of the carbon powder is 330 m 2 / g and above 480m 2 / g or less, and the content of the carbon powder is 0.2 to 7 mass % based on the mass of the fiber containing the carbon powder.
2. The carbon powder-containing fiber according to claim 1, wherein The fibers are synthetic fibers or semi-synthetic fibers.
3. The carbon powder-containing fiber according to claim 2, wherein: The fiber is polyester fiber or polyamide fiber.
4. The carbon powder-containing fiber according to claim 1 or 2, wherein: Average particle size of carbon powder D 50 It is less than 1.5μm.
5. The carbon powder-containing fiber according to claim 1 or 2, wherein: Particle size distribution of carbon powder 90 The value is 4.0μm or less.
6. The carbon powder-containing fiber according to claim 1 or 2, wherein the single fiber fineness is 0.01 to 10 dtex. 7 . A fiber structure comprising the carbon powder-containing fiber according to claim 1 .
Citation Information
Patent Citations
Master batch type black-colored polyester fiber
JP1997250026A
Single fiber containing carbon powder in interior of fiber, processed material and loose fiber mass composed of the same single fiber, processed material and loose fiber mass comprising carbon powder on fiber surface or among fibers and method producing the same
JP2002249922A
Stretched molding of active carbon-containing polyolefin resin
JP2003038626A
Black spun-dyed polyester fiber
JP2006241640A
Negative ion-generating acrylic fiber having changed ion balance and method for producing the same