Method for producing polymer molded product

By melting the molding in the polymer using the temperature range where some sheet crystals melt flow while the other part of the sheet crystal does not melt, the problem of the reduction of molecular weight and slow crystallization speed in melt forming of crystallized polymers is solved, and the processability and productivity.

CN115698399BActive Publication Date: 2024-11-29MITSUBISHI GAS CHEM CO INC +1
View PDF 44 Cites 0 Cited by

Patent Information

Application Number
CN202180039562.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-06-02
Publication Date
2024-11-29
Estimated Expiration
2041-06-02

AI Technical Summary

Technical Problem

In the prior art, crystalline polymers such as polyhydroxybutyrate can easily lead to a decrease in molecular weight and slow crystallization speed during the melt forming process, resulting in poor processability, and the commonly used crystallization nucleating agents are insufficient in effect, making it difficult to be produced in industrial production. application.

Method used

By introducing sheet crystals with different sheet thicknesses into the polymer, melt forming is performed using the temperature range where some sheet crystals melt flow while the other part of the sheet crystals do not melt, the molecular weight decrease during complete melting and the crystallization time is improved Processability.

Benefits of technology

It effectively suppresses the reduction of molecular weight during melt forming, shortens the crystallization time, improves the processability and productivity of thermoplastic polymers, and avoids stalemate problems caused by adhesion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115698399B_ABST
    Figure CN115698399B_ABST
Patent Text Reader

Abstract

The present invention provides a method for producing a polymer molded product, by which even a polymer whose molecular weight is easily reduced in a molten state does not experience a significant reduction in molecular weight during melt molding. The present invention provides a method for producing a polymer molded product, comprising the step of melt molding a polymer comprising lamellae having different lamellae thicknesses within a temperature range in which a portion of the lamellae melt and flow and the remaining portion of the lamellae remain without melting.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for molding a crystalline thermoplastic polymer having lamellae of different thickness, length, width and crystallinity, which is a method for molding in a partially molten state where a part of the crystals are not melted, rather than molding after all the crystals are melted. That is, the present invention relates to a method for melt-molding a polymer at a temperature at which lamellae with a high melting point are not easily melted, while lamellae with a low melting point and amorphous regions can melt and flow.

[0002] In addition, when the melting point of a polymer is close to the thermal decomposition temperature that causes a decrease in molecular weight due to heating, the molecular weight of the polymer may decrease in a molten state. The present invention relates to a molding method that does not cause a significant decrease in molecular weight during molding even for such a polymer.

[0003] In addition, the present invention also relates to a spinning method for preventing the phenomenon of slow crystallization speed and adhesion of fibers in the melt spinning process. Moreover, the present invention also relates to a spinning method for preventing adhesion even for polymers that have a glass transition temperature lower than room temperature and are prone to adhesion during fiberization. The so-called "adhesion" refers to a state in which fibers are adhered to each other and it is difficult for the fibers to be released from each other due to the enhanced adhesion of the polymer. Background Art

[0004] Polyhydroxyalkanoate (hereinafter referred to as PHA) is a thermoplastic polyester accumulated by microorganisms. It has attracted much attention as a biodegradable, biocompatible, and bioabsorbable plastic, and a large number of studies have been conducted (Non-Patent Document 1). There are more than 100 known monomer units that make up PHA. A representative PHA is poly-3-hydroxybutyrate (hereinafter referred to as P(3HB)) composed of (R)-3-hydroxybutyrate (also known as (R)-3-hydroxybutyric acid. hereinafter referred to as 3HB) (Non-Patent Document 1).

[0005] The melting point of P(3HB) is about 175-180°C, which is as high as that of polypropylene (hereinafter referred to as PP). Although the breaking strength of P(3HB) is comparable to that of PP, the breaking elongation is less than 5%, and the glass transition temperature is 4°C (below room temperature).

[0006] Since P(3HB) is a highly crystalline, hard and brittle material, it cannot be used as a single film or other molded product in most cases. When PHA is used industrially, methods for improving its physical properties (crystallinity, mechanical properties, etc.) include methods of introducing a second component monomer unit to form a copolymer, methods of increasing the molecular weight, and methods of compounding with different types of polymer materials.

[0007] It is known that PHA represented by P(3HB) is prone to thermal cracking. Although there is no significant weight loss near the melting point of P(3HB), the molecular weight decreases due to the breakage of the polymer chain, and there is a major problem that the molecular weight is easily reduced in the molten state. In addition, the crystallization rate of PHA is significantly slower than that of conventional industrial polymers, and the glass transition temperature is below room temperature. When PHA is molded in a heated molten state, there are the following problems in molding: the cooling time for solidification is long and the productivity is poor; in melt spinning, entanglement occurs in the amorphous state due to slow crystallization, resulting in sticking of the filaments; in order to avoid sticking, it is necessary to wind in a non-overlapping state; after winding, it takes a long cooling time for solidification (crystallization), etc. In addition, the slower crystallization rate causes a larger growth of spherulites, which also affects the reduction of physical properties of the molded body and aging over time. Copolymerization sometimes leads to a lower nucleation density, in other words, a lower crystallization rate. Even if copolymerization is performed, the above-mentioned molding problems still exist. Moreover, when it has a high molecular weight, there are other problems such as excessively high melt viscosity.

[0008] In the melt molding of thermoplastic polymers such as polyester, various crystal nucleating agents have been studied for the purpose of improving the crystallization rate.

[0009] As well-known crystal nucleating agents, there are known methods, for example, of adding inorganic single substances such as Zn powder, Al powder, graphite, and carbon black to specific polyesters; metal oxides such as ZnO, MgO, Al2O3, TiO2, MnO2, SiO2, and Fe3O4; nitrides such as aluminum nitride, silicon nitride, titanium nitride, and boron nitride; inorganic salts such as Na2CO3, CaCO3, MgCO3, CaSO4, CaSiO3, BaSO4, and Ca3(PO4)3; clays such as talc, kaolin, clay, and kaolin; organic salts such as calcium oxalate, sodium oxalate, calcium benzoate, calcium phthalate, calcium tartrate, magnesium stearate, and polyacrylate; polymer compounds such as polyester, polyethylene, and polypropylene, etc. (Patent Document 1).

[0010] In addition, talc, micronized mica, boron nitride, calcium carbonate and other granular materials have been tried as crystal nucleating agents for PHA. As a more effective crystal nucleating agent, there is a method of densely mixing an organic phosphonic acid such as cyclohexylphosphonic acid or an organic hypophosphorous acid or an ester thereof, or a derivative of these acids or esters, and a metal compound such as an oxide, hydroxide and a saturated or unsaturated carboxylate of a metal of Groups IA to VA or IB to VB of the periodic table (Patent Document 2).

[0011] In addition, as nucleating agents for PHA, there are known: sorbitol and sodium benzoate (Patent Document 3); sugar alcohols such as erythritol, D-arabitol, ribitol, xylitol, galactitol, D-mannitol, L-mannitol, D-sorbitol, myo-inositol, scyllo-inositol (Patent Document 4); polyvinyl alcohol, chitin, chitosan (Patent Document 5); polyoxyalkylenes such as polyethylene oxide, polypropylene oxide, polybutylene oxide (Patent Document 6); polylactic acid or Aliphatic polyesters such as PHA, aliphatic carboxylic acid amides, aliphatic carboxylates, aliphatic alcohols and aliphatic carboxylic acid esters (Patent Documents 7 to 9); fatty acid esters such as dimethyl adipate, di-2-ethylhexyl adipate, diisobutyl adipate, dibutyl adipate, diisodecyl adipate, dibutyl diglycol adipate, dibutyl sebacate, and di-2-ethylhexyl sebacate (Patent Document 10); cyclic compounds having C=O and a functional group selected from NH, S and O in the molecule such as indigo, quinacridone, and quinacridone fuchsin (Patent Document 11); Ketopyrroles as cyclic compounds having C=O and NH groups in the molecule (Patent Document 12); sorbitol derivatives such as dibenzylidene sorbitol and bis(p-methylbenzylidene) sorbitol (Patent Document 13); compounds containing nitrogen-containing heteroaromatic nuclei such as pyridine, pyrimidine, pyrazine, pyridazine, triazine, and imidazole (Patent Document 14); phosphate compounds (Patent Document 15); bisamides of higher fatty acids and metal salts of higher fatty acids (Patent Document 16); fatty acids and fatty amides (Patent Document 17); branched polylactic acid (Patent Document 18) ; pentaerythritol (Patent Document 19); pentaerythritol and an inorganic filler or an organic filler (Patent Document 20); sorbitol acetal, a compound having an amide bond and pentaerythritol (Patent Document 21); amino acids or phosphatidylcholines such as tryptophan, phenylalanine, p-chlorophenylalanine, m-tyrosine, phenylglycine, p-hydroxyphenylglycine, methionine, o-tyrosine and valine (Patent Documents 22 to 24); dipeptides such as aspartame (Patent Document 25); and nucleobases such as uracil and thymine (Patent Document 26).

[0012] These nucleating agents are used to promote the slower crystallization rate of aliphatic polyesters such as PHA and polylactic acid, and to improve the processability during molding. However, there are still problems such as reduced strength, poor surface appearance of the molded body, insufficient effect, and the need to add other additives. In addition, depending on the type of nucleating agent, as the crystallization after molding proceeds, it may be squeezed out of the crystal due to differences in compatibility or molecular weight, resulting in bloom or seepage. In this case, it is necessary to add additives such as dispersants, anti-agglomerants, and compatibilizers. Although the above scheme also envisions the use in vivo, and includes nucleating agents that are easily decomposed, absorbed or metabolized in vivo, that is, non-toxic fatty acids or amino acids, the current situation is that a crystallization nucleating agent with high actual effect has not yet been found.

[0013] In addition, in order to improve the crystallization characteristics of PHA, attempts have been made to blend other PHAs or biodegradable polymers. Patent documents 27 to 29 disclose adding P(3HB) with a higher melting point as a crystal nucleating agent (nucleating agent) to a P(3HB-co-3HV) copolymer composed of 3HB and 3-hydroxyvalerate (3-hydroxyvaleric acid, hereinafter referred to as 3HV), a P(3HB-co-3HHx) copolymer composed of 3HB and 3-hydroxyhexanoate (3-hydroxyhexanoic acid, hereinafter referred to as 3HHx), or a P(3HB-co-3HO) copolymer composed of 3HB and 3-hydroxyoctanoate (3-hydroxyoctanoic acid, hereinafter referred to as 3HO).

[0014] Patent Documents 27 to 29 describe a mixing method in which dry powdered PHA after blending is mixed directly or in the presence of dry ice; a mixing method in which a part or all of the dry powdered PHA is dissolved in a solvent such as chloroform and stirred and mixed, and then the solvent is evaporated to precipitate a polymer, or a solution precipitated in a poor solvent is mixed; and a mixing method in which the added high-melting-point-side P(3HB) is stirred and mixed at a temperature that does not melt the added high-melting-point-side PHA (P(3HB-co-3HV), P(3HB-co-3HHx) or P(3HB-co-3HO) in the example is melted, so-called partial melt mixing. However, it is mentioned that a small amount of P(3HB) on the high-melting-point side to be mixed must be finely and uniformly dispersed in the low-melting-point-side PHA copolymer.

[0015] Each of the above-mentioned mixing methods has disadvantages. In dry mixing, even if polymer powders are mixed, uniform mixing below the powder particle size is still limited. In solution mixing, a large amount of good solvent such as chloroform is required, and when reprecipitating and recovering, a large amount of poor solvent 5 to 10 times the amount of the good solvent is required, and when reprecipitating, the type of polymer precipitated may be biased due to the difference in solubility. In the partially molten state of the blend, the added P(3HB) with high crystallinity and high melting point is not suitable for making tiny and uniform microcrystalline nuclei because the P(3HB) particles are mixed almost at their original size without melting. The method of raising the temperature to above the melting point of P(3HB) for uniform mixing of the blend is a common melt mixing method, and near the melting point of P(3HB), PHAs represented by P(3HB) cannot avoid degradation and molecular weight reduction due to thermal cracking or stirring.

[0016] In addition to the method of trying to promote crystallization by blending P(3HB) extracted from the bacterial cell with a PHA copolymer, there is also a method reported in which P(3HB) or 3HB-rich PHA that can form a crystal nucleus is produced as a blend with other PHA copolymers in the bacterial cell during the culture period, thereby eliminating the need to blend P(3HB) with PHA after PHA is extracted from the bacterial cell. Patent document 30 describes a method of producing P(3HB) or P(3HB-co-3HHx) with a low 3HHx ratio and P(3HB-co-3HHx) with an increased 3HHx ratio by changing the carbon source supply during the culture. Patent documents 31 and 32 disclose a method of maintaining a plurality of PHA polymerases with different substrate specificities in the same bacterial cell using genetic recombination technology, thereby producing a blend of PHAs with different melting points in the same cell. Although it is also recorded that molding can be performed at a temperature below 170°C, it is not clear within what temperature range the molding can be performed. In known molding processes, molding is usually performed after melting at a temperature above the melting point of the polymer. In addition, in this document, the purpose is to increase the solidification rate (crystallization rate) of the once melted PHA blend.

[0017] Although the purpose of non-patent documents 2 to 4 is not to enable P(3HB) to become a crystal nucleus, they also record the production of wild-type PHA strains that mix and produce P(3HB) and PHA copolymers in the same bacteria, and record the production of P(3HB) homopolymers and C4 to C12 PHA copolymers by naturally maintaining PHA polymerases with different substrate specificities in the same bacteria.

[0018] On the other hand, there are also reports on the use of ultra-high molecular weight P(3HB) and the control of crystal formation without relying on molecular weight to achieve high strength. For example, ultra-high molecular weight P(3HB) with a number average molecular weight of 1.5 million (weight average molecular weight of 3 million) or more was synthesized using genetically recombinant Escherichia coli, and the ultra-high molecular weight P(3HB) was used to obtain a P(3HB) film with improved physical properties (Patent Document 33 and Non-Patent Document 5).

[0019] In addition, as a fiberization method of P(3HB) that is independent of molecular weight, a method is disclosed in which P(3HB) is melt-extruded, rapidly cooled to a temperature below the glass transition temperature + 15°C, and solidified to produce amorphous fibers, the amorphous fibers are cold-stretched to orient the molecular chains of the amorphous fibers, and heat-treated to obtain P(3HB) fibers (hereinafter also referred to as "cold stretching method") (Patent Documents 34 and 35). A method for manufacturing fibers is also disclosed, characterized in that the melt-extruded fibers are rapidly cooled to a temperature below the glass transition temperature of PHA + 15°C, and solidified to produce amorphous fibers, the amorphous fibers are placed below the glass transition temperature + 15°C, and crystalline fibers having formed microcrystalline nuclei (isothermal crystallization) are produced, the crystalline fibers are stretched, and then tension heat treatment is performed (hereinafter also referred to as "microcrystalline nucleus stretching method") (Patent Document 36).

[0020] However, the manufacturing efficiency of ultra-high molecular weight P(3HB) is poor and the cost is high; in order to obtain amorphous fibers in the cold stretching method, it is necessary to rapidly cool to a low temperature near the glass transition temperature; in the microcrystal core stretching method, since molten P(3HB) microcrystals are first generated, it is necessary to rapidly cool to a low temperature near the glass transition temperature and maintain it at low temperature for a long time. Therefore, the above method is not conducive to industrial production.

[0021] An ultrahigh molecular weight P(3HB) with a weight average molecular weight of 2.7 million produced by genetically recombinant Escherichia coli was added to a P(3HB) with a weight average molecular weight of 520,000 derived from a common microorganism, dissolved in chloroform and formed into a cast film. The film was hot pressed at 200°C, then quenched with ice water and then cold stretched to obtain a P(3HB) film with a trace amount of ultrahigh molecular weight added. When the film was heated to 200°C and the crystal growth was observed, the ultrahigh molecular weight P(3HB) played a role similar to that of a nucleating agent, suggesting that it could promote nucleation (Non-Patent Document 6). There is also a report that a small amount of ultra-high molecular weight P(3HB) with a weight average molecular weight of 3.47 million is added to P(3HB) with a weight average molecular weight of 520,000, and melt spinning is performed at 180°C, 190°C, and 200°C (Non-Patent Document 7). Although the molecular weight is reduced by heating and melting above the melting point, the addition of ultra-high molecular weight P(3HB) suppresses the thermal cracking of P(3HB) at the initial stage of cracking, and the processability of melt spinning is improved. There is also a report that by cooling to 4°C after melt spinning and adopting two-step cold stretching, the blended P(3HB) fiber added with 5% by weight of ultra-high molecular weight P(3HB) shows a strength of 740 MPa. The amount of ultra-high molecular weight P(3HB) can be used in a small amount, but since it is necessary to perform two-step cold stretching at a cooling state of 4°C, the operation is cumbersome and cannot be said to be suitable for industrialization.

[0022] In addition, there are reports that when a molten molded product is produced by melt-molding a molding material mainly composed of a biodegradable polyester having a melting point in a specific range at a heating temperature in a specific range, the cold crystallization heat and the sum of the melting heat and the cold crystallization heat are used as indicators of the crystallization ability and crystallinity of the respective molten molded products, and the molten molded product is produced by setting a specific range (Patent Document 37). There are also reports that a copolymer of 3HB and 3-hydroxyhexanoate is processed at a temperature (about 160°C) at which the crystal is not completely melted (Non-Patent Document 8). In addition, there are reports that a pipe is made of a poly (3-hydroxybutyrate) resin, wherein the difference between the melting point peak temperature and the end temperature of the melting point peak in the differential scanning calorimetry analysis of the poly (3-hydroxybutyrate) resin is 10°C or more (Patent Document 38). There is also a report describing a method for producing a biodegradable resin molded body, characterized in that when a biodegradable resin composition containing poly(3-hydroxyalkanoate) is heated and melt-kneaded to form a molded body, the residual crystal amount at the outlet of the molding machine after the heating and melt-kneading is confirmed by a spectrum of near infrared spectroscopy, and the residual crystal amount at the outlet of the molding machine is adjusted in such a way that the crystal peak obtained by near infrared spectroscopy of the above-mentioned molded body can be observed within 200 seconds just after molding (Patent Document 39). However, there is no record that the temperature of melt molding is set to a temperature higher than the outflow starting temperature obtained by the flow tester temperature rise method and indicating that the crystal melting is completely completed (especially a temperature lower than the extrapolated melting end temperature) measured by a differential scanning calorimeter.

[0023] Prior art literature

[0024] Patent Literature

[0025] Patent Document 1: Japanese Patent Application Laid-Open No. 07-126496

[0026] Patent Document 2: Japanese Patent Application Laid-Open No. 03-024151

[0027] Patent Document 3: WO2006 / 012917

[0028] Patent Document 4: WO2008 / 099586

[0029] Patent Document 5: Japanese Patent Application Publication No. 2007-077232

[0030] Patent Document 6: Japanese Patent Application Publication No. 2010-229407

[0031] Patent Document 7: Japanese Patent Application Laid-Open No. 09-278991

[0032] Patent Document 8: Japanese Patent Application Laid-Open No. 11-005849

[0033] Patent Document 9: Japanese Patent Application Laid-Open No. 07-188537

[0034] Patent Document 10: Japanese Patent Application Laid-Open No. 11-116783

[0035] Patent Document 11: Japanese Patent Application Publication No. 2003-238779

[0036] Patent Document 12: Japanese Patent Application Publication No. 2003-327803

[0037] Patent Document 13: Japanese Patent Application Laid-Open No. 10-158369

[0038] Patent Document 14: Japanese Patent Application No. 2007-517126

[0039] Patent Document 15: Japanese Patent Application Publication No. 2003-192884

[0040] Patent Document 16: Japanese Patent Application Laid-Open No. 6-299054

[0041] Patent Document 17: Japanese Patent Application Laid-Open No. 8-27363

[0042] Patent Document 18: Japanese Patent Application Publication No. 2009-024058

[0043] Patent Document 19: Japanese Patent Application Publication No. 2017-101256

[0044] Patent Document 20: WO2015 / 052876

[0045] Patent Document 21: WO2014 / 068943

[0046] Patent Document 22: Japanese Patent Application Publication No. 2006-282940

[0047] Patent Document 23: Japanese Patent Application Laid-Open No. 06-345950

[0048] Patent Document 24: Japanese Patent Publication No. 10-504583

[0049] Patent Document 25: Japanese Patent Application Publication No. 2019-119839

[0050] Patent Document 26: Japanese Patent Application Publication No. 2019-119840

[0051] Patent Document 27: Japanese Patent Publication No. 08-510498

[0052] Patent Document 28: WO2002 / 055581

[0053] Patent Document 29: WO2002 / 050461

[0054] Patent Document 30: Japanese Patent Application Publication No. 2004-250629

[0055] Patent Document 31: WO2015 / 146195

[0056] Patent Document 32: WO2017 / 056442

[0057] Patent Document 33: Japanese Patent Application Laid-Open No. 10-176070

[0058] Patent Document 34: Japanese Patent Application Publication No. 2003-328230

[0059] Patent Document 35: Japanese Patent Application Publication No. 2003-328231

[0060] Patent Document 36: WO2006 / 038373

[0061] Patent Document 37: Japanese Patent No. 4245306

[0062] Patent Document 38: WO2020 / 040093

[0063] Patent Document 39: Japanese Patent Application Publication No. 2010-241075

[0064] Non-patent literature

[0065] Non-patent literature 1: Alistair J. Anderson et al., Microbiological Reviews, Vol. 54, No. 4, 450-472, 1990

[0066] Non-patent document 2: H. Abe, et al., International Journal of Biological Macromolecules, 1994, vol. 16, 115-119.

[0067] Non-patent document 3: M. Kato et Aal., Bull. Chem. Soc. Jpn, 1996, vol. 69, 515-520.

[0068] Non-patent document 4: H. Matsusaki et al., Journal of bacteriorogy, 1998, vol. 180, 6459-6467.

[0069] Non-patent document 5: Kusaka et al., Appl. Microbiol. Biotechnol., 47 140-143 (1997). Molecular mass of poly[(R)-3-hydroxybutyric acid] produced in arecombinant Escherichia coli.

[0070] Non-patent document 6: T. Kabe et al., Macromolecules, 2012, 45, 1858-1865.

[0071] Non-patent literature 7: T. Kabe en al., ACS synposium series on Biobased Monomers, Polymers, and Materials, Chaper 5, 63-75.

[0072] Non-patent document 8: Journal of the Japan Society of Packaging Vol. 28, No. 2 (2019) 109-115. Summary of the invention

[0073] Technical problem to be solved by the invention

[0074] As mentioned above, in the existing method, a crystalline polymer (polyester) with a slow crystallization is melted and then rapidly nucleated, so that large defective spherulites are not formed, the polymer is crystallized in a manner to improve strength, and the polymer is solidified / crystallized in a manner to facilitate processing, and development is carried out from such a viewpoint. Although various attempts to promote crystallization have been made in melt molding of biodegradable crystalline polymers in order to improve the poor processability caused by the slow crystallization rate or to improve the strength, there is still room for improvement.

[0075] The object of the present invention is to provide a method for producing a polymer molded product, by which even a polymer whose molecular weight is easily reduced in a molten state will not cause a significant reduction in molecular weight during melt molding. In addition, the object of the present invention is to provide a method for producing a polymer molded product, which can shorten the crystallization time of a polymer that crystallizes slowly (such as biodegradable polyesters, etc.), improve the melt processability of the polymer in processes such as injection molding, blow molding, film molding, fiber spinning, extrusion foaming, and bead foaming, thereby improving productivity.

[0076] Technical solutions for solving technical problems

[0077] The inventors of the present invention have conducted in-depth research to solve the above-mentioned problems, and as a result, they have noticed that the semi-crystalline PHA copolymer with an appropriate composition does not have a single melting point itself, but has crystals represented by lamellae (aggregates of crystalline segments) of various thicknesses inside, and is therefore an aggregate of fine lamellae and amorphous with various melting points. In addition, the inventors have found that by melting the copolymer (in other words, partially melting) at a temperature lower than the temperature at which the copolymer as a whole can melt and at a temperature at which relatively thin fine lamellae or amorphous regions with a lower melting point can flow, it is possible to perform melt processing in a state where fine but thick lamellae are not melted. Because the thick fine lamellae that are not melted are uniformly dispersed inside or between the molecular chains, there is no need to wait for crystallization to nucleate once after melting as in the case of complete melting, but molding can be performed from a partially melted state. In addition, it has been found that the poor processing characteristics caused by the adhesion caused by the amorphous state after the polyester (PHA) is melt-processed can be significantly improved, and the significant reduction in molecular weight caused by molding at a temperature lower than the thermal cracking temperature of PHA can be prevented. The present invention was accomplished based on the above-mentioned knowledge.

[0078] According to the present invention, the following inventions are provided.

[0079] <1> The method for producing a polymer molded product comprises the steps of melt-molding a polymer containing lamellae with different lamellae thicknesses within a temperature range in which a part of the lamellae melts and flows while the other remaining lamellae do not melt but remain.

[0080] <2> like <1> The method described above, wherein the temperature range is a range higher than the outflow starting temperature obtained by a flow tester temperature increase method and lower than the temperature indicating that the crystal melting is completely completed measured by a differential scanning calorimeter.

[0081] <3> like <1> or <2> The method, wherein the temperature range is a range higher than the outflow start temperature obtained by the flow tester temperature increase method and lower than the extrapolated melting end temperature.

[0082] <4> like <1> ~ <3> The method described in any one of the above comprises the step of cooling the melted polymer in air within a temperature range in which a portion of the lamellae melt and flow, and the remaining portion of the lamellae do not melt but remain.

[0083] <5> like <1> ~ <4> The method according to any one of the preceding claims, wherein the melt molding is molding by melt extrusion.

[0084] <6> like <1> ~ <5> The method according to any one of the preceding claims, wherein the melt molding is molding by melt extrusion spinning.

[0085] <7> like <1> ~ <6> The method described in any one of the above aspects, wherein melt molding is performed once.

[0086] <8> like <1> ~ <7> The method according to any one of the preceding claims, wherein the polymer comprises a thermoplastic resin.

[0087] <9> like <1> ~ <8> The method according to any one of the preceding claims, wherein the polymer comprises polyester.

[0088] <10> like <1> ~ <9> The method according to any one of the preceding claims, wherein the polymer comprises an aliphatic polyester.

[0089] <11> <1> ~ <10> The method according to any one of the preceding claims, wherein the polymer comprises a biodegradable polymer.

[0090] <12> like <1> ~ <11> The method according to any one of the preceding claims, wherein the polymer is a copolymer containing 3-hydroxybutyric acid as a monomer unit.

[0091] <13> like <1> ~ <12> The method described in any one of the above, wherein the polymer comprises poly-L-lactic acid, poly-p-dioxanone, polybutylene succinate, polybutylene succinate adipate, or a copolymer of glycolic acid and lactic acid.

[0092] <14> like <1> ~ <13> The method according to any one of the preceding claims, wherein the polymer is a copolymer comprising 3-hydroxybutyric acid and 4-hydroxybutyric acid as monomer units, and the proportion of 4-hydroxybutyric acid is 5 mol% to 40 mol%.

[0093] Effects of the Invention

[0094] The method for producing a polymer molded article of the present invention can suppress the decrease in molecular weight during melt molding, even for a polymer whose molecular weight is easily reduced in a molten state. The method for producing a polymer molded article of the present invention can shorten the crystallization time of the polymer, improve the melt processability of the polymer in processes such as injection molding, blow molding, film molding, fiber spinning, extrusion foaming, and bead foaming, thereby improving productivity. BRIEF DESCRIPTION OF THE DRAWINGS

[0095] Figure 1 The flow curve (solid line) and the DSC curve (dashed line) of the sample S1 (P(3HB) homopolymer) of Comparative Example 1 obtained by the flow tester temperature rising method are shown.

[0096] Figure 2The flow curve (solid line) and DSC curve (dashed line) obtained by the flow tester temperature rise method of sample S2 (P(3HB-co-11.8 mol% 4HB)) of Example 1 are shown. The extrapolated melting end temperature (158.7°C) of Example 1 and the temperature (167.0°C) at which the DSC curve returns to the baseline are shown.

[0097] Figure 3 The flow curve (solid line) and DSC curve (dashed line) obtained by the flow tester temperature rise method of sample S3 (P (3HB-co-13.1 mol % 4HB)) of Example 2 are shown. The extrapolated melting end temperature (135.1°C) of Example 2 and the temperature (155.0°C) when the DSC curve returns to the baseline are shown.

[0098] Figure 4 The flow curve (solid line) and DSC curve (dashed line) of sample S34 (P(3HB-co-14.7 mol % 4HB)) of Example 3 obtained by the flow tester temperature increase method are shown.

[0099] Figure 5 The flow curve (solid line) and DSC curve (dashed line) of sample S5 (P(3HB-co-15.3 mol % 4HB)) of Example 4 obtained by the flow tester temperature rising method are shown.

[0100] Figure 6 The flow curve (solid line) and DSC curve (dashed line) of sample S6 (P(3HB-co-15.3 mol % 4HB)) of Example 5 obtained by the flow tester temperature increase method are shown.

[0101] Figure 7 The flow curve (solid line) and DSC curve (dashed line) of sample S7 (P(3HB-co-16.0 mol % 4HB)) of Example 6 obtained by the flow tester temperature increase method are shown.

[0102] Figure 8 The flow curve (solid line) and DSC curve (dashed line) of sample S8 (P(3HB-co-17.8 mol % 4HB)) of Example 7 obtained by the flow tester temperature increase method are shown.

[0103] Fig. 9 The flow curve (solid line) and DSC curve (dashed line) of sample S9 (P(3HB-co-17.9 mol % 4HB)) of Example 8 obtained by the flow tester temperature increase method are shown.

[0104] Fig.10The flow curve (solid line) and DSC curve (dashed line) of sample S10 (P(3HB-co-28.7 mol % 4HB)) of Example 9 obtained by the flow tester temperature increase method are shown.

[0105] Fig.11 The flow curve (solid line) and DSC curve (dashed line) of sample S11 (P(3HB-co-32.9 mol % 4HB)) of Example 10 obtained by the flow tester temperature rising method are shown.

[0106] Fig.12 The flow curve (solid line) and DSC curve (dashed line) of sample S12 (P(3HB-co-74.6 mol % 4HB)) of Comparative Example 2 obtained by the flow tester temperature increase method are shown.

[0107] Fig.13 The flow curve (solid line) and DSC curve (dashed line) of sample S13 (P(3HB-co-8.0 mol % 3HV)) of Example 24 obtained by the flow tester temperature increase method are shown.

[0108] Fig.14 The flow curve (solid line) and DSC curve (dashed line) of sample S14 (P(3HB-co-12.0 mol % 3HV)) of Example 25 obtained by the flow tester temperature increase method are shown.

[0109] Fig.15 The flow curve (solid line) and DSC curve (dashed line) of sample S15 (P(3HB-co-35.5 mol % 3HV)) of Example 26 obtained by the flow tester temperature increase method are shown.

[0110] Fig.16 The flow curve (solid line) and DSC curve (dashed line) of sample S16 (P(3HB-co-48.2 mol % 3HV)) of Example 27 obtained by the flow tester temperature increase method are shown.

[0111] Fig.17 The flow curve (solid line) and DSC curve (dashed line) of sample S17 (P(3HB-co-61.5 mol % 3HV)) of Example 28 obtained by the flow tester temperature increase method are shown.

[0112] Fig.18 The flow curve (solid line) and DSC curve (dashed line) of sample S18 ((P(3HB-co-73.2 mol % 3HV)) of Example 29 obtained by the flow tester temperature rising method are shown.

[0113] Fig.19The DSC measurement results and wide-angle X-ray diffraction patterns of Sample S7 (P(3HB-co-16 mol % 4HB)) of Reference Example 1 and Examples 6, 22, and 23 are shown.

[0114] Fig. 20 The DSC measurement results and wide-angle X-ray diffraction diagram of Sample S14 (P(3HB-co-12 mol % 3HV)) of Reference Example 2, Examples 25, 31, 32, 33, and Comparative Example 13 are shown.

[0115] Fig.21 The flow curve (solid line) and DSC curve (dashed line) of sample S19 (PGA) of Comparative Example 14 obtained by the flow tester temperature increase method are shown.

[0116] Fig. 22 The flow curve (solid line) and DSC curve (dashed line) of sample S20 (PLLA) of Example 34 obtained by the flow tester temperature increase method are shown.

[0117] Fig.23 The flow curve (solid line) and DSC curve (dashed line) of sample S21 (PGLA) of Example 35 obtained by the flow tester temperature increase method are shown.

[0118] Fig.24 The flow curve (solid line) and DSC curve (dashed line) of sample S22 (PPDO) of Example 36 obtained by the flow tester temperature increase method are shown.

[0119] Fig.25 The flow curve (solid line) and DSC curve (dashed line) of sample S23 (PBS) of Example 37 obtained by the flow tester temperature increase method are shown.

[0120] Fig.26 The flow curve (solid line) and DSC curve (dashed line) of sample S24 (PBSA) of Example 38 obtained by the flow tester temperature rising method are shown.

[0121] Fig. 27 The flow curve (solid line) and DSC curve (dashed line) of sample S25 (PCL) of Comparative Example 15 obtained by the flow tester temperature rising method are shown. DETAILED DESCRIPTION

[0122] The present invention is described in detail below.

[0123] The method for producing a polymer molded product of the present invention comprises the step of melt-molding a polymer including lamellae with different lamellae thicknesses within a temperature range in which a part of the lamellae melt and flow and the remaining part of the lamellae remain without melting.

[0124] In the present invention, the processability of a thermoplastic resin that crystallizes slowly and has poor processing characteristics can be improved by melting the resin in a temperature range that is above the outflow start temperature measured when the fluidity of the crystalline thermoplastic resin is evaluated using a flow tester and below the temperature indicating that the crystalline melting is completely completed measured by a differential scanning calorimeter (DSC), and then molding the resin.

[0125] "The temperature indicating that the crystal melting is completely finished as measured by a differential scanning calorimeter (DSC)" is preferably the extrapolated melting end temperature of the melting peak. The extrapolated melting end temperature of the melting peak can be obtained according to the records of the embodiments described later. That is, when the melting peak is a sharp peak, according to JIS-K7121, the extrapolated melting end temperature of the melting peak is the temperature at the intersection of the tangent drawn from the maximum slope point before the end of the peak and the baseline after the peak (identified by Rigaku, Thermo plus EVO software). When the melting peak shape is multi-peak superposition, the tangent is manually re-drawn for the peak on the higher temperature side, and its intersection with the baseline is used as the extrapolated melting end temperature.

[0126] Moreover, in the past, melt molding is usually melted at a temperature above the melting point such as melting point + 20 ° C, melting point + 10 ° C, melting point + 5 ° C, and then molded. In contrast, in the case of molding in a partially molten state as in the present invention, partial melting is performed at a temperature below the melting point. Therefore, in the case of a polymer having a melting point close to the thermal cracking temperature, the decomposition caused by heat can be suppressed, that is, the molecular weight can be suppressed. In addition, since the molecular weight of the polymer after molding can be maintained at a high state, it is also beneficial in terms of physical properties. Furthermore, compared with complete melting, the melting in a partially molten state is carried out at a lower temperature, so it can be inferred that not only the thermal cracking of the polymer can be reduced, but also the hydrolysis of the polymer molecular chain intervened by a trace amount of water mixed in the heated state can be reduced. Therefore, although it is generally desired that the moisture content of the raw material is low, the need for reduction or maintenance in order to make the concentration particularly low can be reduced. Thus, the following advantages can also be expected, that is, in a spinning or molding device, there is no need to set a special device for strictly maintaining the dry state of the dry raw material polymer in order to prevent the transfer of moisture in the atmosphere to the raw material polymer.

[0127] In addition, the present invention can improve the molding processability of polyester with slow melt crystallization and improve productivity without adding a crystal nucleating agent, but it does not exclude the use of a crystal nucleating agent.

[0128] As an example of the present invention, P(3HB-co-4HB) can be used as a polymer. In this case, the method of the present invention is characterized in that it includes: when P(3HB-co-4HB) is melted, a melt extrusion step is performed between a temperature at which the crystalline and amorphous regions represented by relatively thin lamellae composed of 3HB segments inside the polymer begin to melt and flow, and a temperature at which relatively thick lamellae composed of 3HB segments begin to melt.

[0129] The present invention relates to a method for producing a biodegradable polyester molded body, characterized in that melt molding is carried out in a state where a part of crystals represented by lamellae contained in a polyester copolymer (especially a PHA copolymer) remains, so that the unmelted and remaining crystals become crystal nuclei, thereby allowing molding to be carried out without waiting for primary nucleation in conventional melt molding.

[0130] Therefore, the poor molding processability of crystalline thermoplastic polymers that crystallize slowly can be improved. Unlike when completely melted, there is no need to wait for the primary nucleation of crystals, and molding can be performed immediately after partial melting, thereby improving productivity.

[0131] Part of the crystals represented by the lamellae dispersed in the bulk of the crystalline thermoplastic polymer remain unmelted and act as crystal nuclei. Therefore, there is no need for a waiting time for primary nucleation, and the adhesion caused by the low crystallinity just after melt extrusion can be reduced, making it difficult for molded bodies such as fibers or films to stick together. In addition, after melt spinning and film formation, they can be immediately wound and stretched, thereby improving productivity.

[0132] Melt spinning is performed in a state where some crystals remain unmelted and then stretched immediately, whereby the remaining unmelted crystals are oriented, the polymer chains in the amorphous state are highly oriented, and the continuous segments of the monomer units that are easy to form crystals are aggregated, thereby promoting crystallization. Since melting at a high temperature that causes thermal cracking is not performed, the molecular weight reduction caused by thermal cracking can be suppressed, so that the molecular weight of the molded body is maintained. In other words, deterioration caused by heat can be prevented. Moreover, even if there is residual moisture in the polymer, or even if it is a polymer that easily absorbs moisture in the air, since partial melt molding can reduce the melting temperature, the degree of hydrolysis affected by heat and moisture can be reduced compared to complete melt molding, and the molecular weight reduction of the polymer can be suppressed, so that the molecular weight of the molded product is maintained.

[0133] [About polymers]

[0134] The polymer is not particularly limited, and for example, the following can be used. In addition, one polymer may be used alone, or two or more polymers may be used in combination.

[0135] Polyester;

[0136] Polyamide;

[0137] Polyolefins;

[0138] Acid-modified polyolefins (maleic anhydride grafted polyethylene, maleic anhydride grafted polypropylene, etc.);

[0139] Ethylene-vinyl compound copolymers (ethylene-vinyl acetate copolymers, ethylene-vinyl alcohol copolymers, ethylene-vinyl chloride copolymers, ethylene-(meth)acrylic acid copolymers or ionomers thereof, ethylene-methyl methacrylate copolymers, etc.);

[0140] Styrene resins (polystyrene, acrylonitrile-styrene copolymer, α-methylstyrene-styrene copolymer, etc.);

[0141] Polyvinyl compounds (polymethyl acrylate, polymethyl methacrylate, etc.);

[0142] Polycarbonate;

[0143] Polyether (polyethylene oxide, etc.).

[0144] Among the above-mentioned materials, polyester, polyolefin or polyamide is preferred. Polyester, polyolefin and polyamide are described below.

[0145] <Polyester>

[0146] Examples of the polyester include polyesters formed from hydroxycarboxylic acids and ester-forming derivatives thereof; compounds formed from one or more polycarboxylic acids including dicarboxylic acids and ester-forming derivatives thereof, and one or more polyols including diols; or polyesters formed from cyclic esters.

[0147] As the polyester formed from hydroxycarboxylic acid and its ester-forming derivative, aliphatic polyester is preferred.

[0148] Aliphatic polyesters include homopolymers of aliphatic hydroxycarboxylic acids (e.g., poly 3-hydroxypropionic acid, poly 3-hydroxybutyric acid, poly 3-hydroxyvaleric acid, poly 4-hydroxybutyric acid, poly 3-hydroxyhexanoic acid, poly 3-hydroxyoctanoic acid, poly 4-hydroxyvaleric acid, poly 4-hydroxyhexanoic acid, poly 5-hydroxyvaleric acid, poly 2-hydroxybutyric acid, poly 2-hydroxyvaleric acid, poly 2-hydroxyhexanoic acid, polylactic acid, polyglycolic acid, polycaprolactone, etc.), copolymers (e.g., copolymers of 3-hydroxypropionic acid and 3-hydroxybutyric acid, copolymers of 3-hydroxypropionic acid and 3-hydroxyvaleric acid, copolymers of 3-hydroxypropionic acid and 4-hydroxybutyric acid, copolymers of 3-hydroxypropionic acid and 3-hydroxyoctanoic acid, copolymers of 3-hydroxypropionic acid and 3-hydroxyoctanoic acid, copolymers of 3-hydroxybutyric acid and 3-hydroxyvaleric acid, copolymers of 3-hydroxybutyric acid and 4-hydroxybutyric acid, copolymers of 3-hydroxybutyric acid and 3-hydroxyhexanoic acid, copolymers of 3-hydroxybutyric acid and 3-hydroxyoctanoic acid, copolymers of 3-hydroxyvaleric acid and 4-hydroxybutyric acid, copolymers of 3-hydroxyvaleric acid and 3-hydroxyhexanoic acid, copolymers of 3-hydroxyvaleric acid and 3-hydroxyoctanoic acid, copolymers of lactic acid and glycolic acid, copolymers of lactic acid and ε-caprolactone, copolymers of lactic acid and 3-hydroxypropionic acid, copolymers of lactic acid and 3-hydroxybutyric acid, lactic acid copolymers of glycolic acid and 3-hydroxypropionic acid, copolymers of glycolic acid and 3-hydroxybutyric acid, copolymers of glycolic acid and 3-hydroxyvaleric acid, copolymers of glycolic acid and 4-hydroxybutyric acid, copolymers of glycolic acid and 3-hydroxyhexanoic acid, copolymers of glycolic acid and 3-hydroxyoctanoic acid, copolymers of glycolic acid and ε-caprolactone, copolymers of glycolic acid and 3-hydroxypropionic acid, copolymers of glycolic acid and 3-hydroxybutyric acid, copolymers of glycolic acid and 3-hydroxyvaleric acid, copolymers of glycolic acid and 4-hydroxybutyric acid, copolymers of glycolic acid and 3-hydroxyhexanoic acid, copolymers of glycolic acid and 3-hydroxyoctanoic acid, copolymers of ε-caprolactone and 3-hydroxypropionic acid, copolymers of ε-caprolactone and 3-hydroxybutyric acid, copolymers of ε-caprolactone and 3-hydroxyvaleric acid The present invention also includes copolymers composed of three or more monomers such as copolymers of ε-caprolactone and 4-hydroxybutyric acid, copolymers of ε-caprolactone and 3-hydroxyhexanoic acid, and copolymers of ε-caprolactone and 3-hydroxyoctanoic acid) and terpolymers, homopolymers (e.g., polybutylene succinate, etc.) and copolymers (e.g., copolymers of butanediol, succinic acid and adipic acid, etc.) of aliphatic polyol carboxylic acids, copolymers composed of aliphatic hydroxycarboxylic acids, aliphatic polyols and aliphatic polycarboxylic acids (e.g., block copolymers of polylactic acid and polybutylene succinate), polydioxanone and dioxanone-containing copolymers, and mixtures of the above compounds.

[0149] In the polymer used in the present invention, in order to form a polymer structure of crystalline segments such as lamellar or fringed micelle structures, spherulites, dendrites, shish-kebab structures, and extended chain crystals, it is preferred that a chain structure sufficient to realize a crystalline microstructure is repeatedly present in the polymer chain, such as a lactic acid chain, a glycolic acid chain, an ε-caprolactone chain, a 3-hydroxypropionic acid chain, a 3-hydroxybutyric acid chain, a 3-hydroxyvaleric acid chain, a 4-hydroxybutyric acid chain, a 3-hydroxyhexanoic acid chain, a 3-hydroxyhexanoic acid chain, a 3-hydroxyoctanoic acid chain, a 4-hydroxyvaleric acid chain, a 4-hydroxyhexanoic acid chain, a 5-hydroxyvaleric acid chain, a 2-hydroxybutyric acid chain, a 2-hydroxyvaleric acid chain, a 2-hydroxyhexanoic acid chain, a butylene succinate chain, a butylene succinate adipate chain, and the like. When stereoisomers or optical isomers exist as monomer units, a crystalline segment composed of a chain formed by the same stereoisomer is required, for example, an L-lactic acid chain, a D-lactic acid chain, an R-3-hydroxybutyric acid chain, an S-3-hydroxybutyric acid chain, an R-3-hydroxyvaleric acid chain, an S-3-hydroxyvaleric acid chain, an R-3-hydroxycaproic acid chain, an S-3-hydroxycaproic acid chain, etc. The chain structure of the same stereoisomer is an important factor for forming a crystal structure. In the case of a polyester containing a monomer unit having stereoisomers or optical isomers, the crystallinity is reduced and it is difficult to obtain a crystalline segment. In particular, in the case of synthesizing a polymer composed of these monomer units using a biological method, a binary copolymer or a ternary or higher copolymer having an R-3-hydroxybutyric acid chain and other monomer units introduced as a second component is more preferred.

[0150] The aliphatic polyester can be produced by any method of chemical synthesis or biosynthesis. In order to ensure a crystalline segment obtained from the chain structure, when containing a monomer unit having a stereoisomer, for example, a copolymer of L-lactic acid and glycolic acid, a copolymer of D-lactic acid and glycolic acid, a copolymer of R-3-hydroxybutyric acid and 4-hydroxybutyric acid, a copolymer of S-3-hydroxybutyric acid and 4-hydroxybutyric acid, a copolymer of R-3-hydroxybutyric acid and ε-caprolactone, a copolymer of S-3-hydroxybutyric acid and ε-caprolactone, and the like are preferably a copolymer formed of any stereoisomer.

[0151] When the polyester contains 3-hydroxybutyric acid units and 4-hydroxybutyric acid units, the ratio of 4-hydroxybutyric acid units relative to all monomer units is preferably 5 mol% or more and 40 mol% or less. The ratio of 4-hydroxybutyric acid relative to all monomer units may be 5 mol% or more, 6 mol% or more, 7 mol% or more, 8 mol% or more, 9 mol% or more, 10 mol% or more, 11 mol% or more, 12 mol% or more, 13 mol% or more, 14 mol% or more, 15 mol% or more, or 16 mol% or more, and may be 17 mol% or more, 18 mol% or more, 19 mol% or more, or 20 mol% or more. The proportion of 4-hydroxybutyric acid units relative to all monomer units can be 35 mol% or less, 34 mol% or less, 33 mol% or less, 32 mol% or less, 31 mol% or less, 30 mol% or less, 29 mol% or less, 28 mol% or less, 27 mol% or less, 26 mol% or less, 25 mol% or less, 24 mol% or less, 23 mol% or less, 22 mol% or less, or 21 mol% or less.

[0152] When the polyester contains 3-hydroxybutyric acid units and 3-hydroxyvaleric acid units, the ratio of 3-hydroxyvaleric acid units relative to all monomer units is preferably 5 mol% or more and 90 mol% or less. Relative to all monomer units, the ratio of 3-hydroxyvaleric acid units may be 5 mol% or more, 6 mol% or more, 7 mol% or more, 8 mol% or more, 9 mol% or more, 10 mol% or more, 15 mol% or more, 20 mol% or more, 25 mol% or more, 30 mol% or more, 35 mol% or more, or 40 mol% or more, or 45 mol% or more, 50 mol% or more, 55 mol% or more, or 60 mol% or more. Relative to all monomer units, the ratio of 3-hydroxyvaleric acid units may be 90 mol% or less, 85 mol% or less, 80 mol% or less, 75 mol% or less, 70 mol% or less, or 65 mol% or less.

[0153] The polyester may be a polyester formed from one or more selected from polycarboxylic acids including dicarboxylic acids and ester-forming derivatives thereof, and one or more selected from polyols including diols.

[0154] Specific examples of dicarboxylic acids include oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, dodecanedioic acid, tetradecanedioic acid, hexadecanedioic acid, octadecanedioic acid, 3-cyclobutanedicarboxylic acid, 1,3-cyclopentanedicarboxylic acid, 1,2-cyclohexanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, 1,4-cyclohexanedicarboxylic acid, 2,5-norbornanedicarboxylic acid, dimer acid, and the like; saturated aliphatic dicarboxylic acids or ester-forming derivatives thereof such as fumaric acid, maleic acid, and itaconic acid; and unsaturated aliphatic dicarboxylic acids or ester-forming derivatives thereof such as phthalic acid, isophthalic acid, terephthalic acid, 1,3-naphthalene dicarboxylic acid, 1,2-cyclohexanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, 1,4-cyclohexanedicarboxylic acid, 2,5-norbornanedicarboxylic acid, and dimer acid. , 4-naphthalenedicarboxylic acid, 1,5-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, 2,7-naphthalenedicarboxylic acid and other naphthalenedicarboxylic acids, aromatic dicarboxylic acids or their ester-forming derivatives such as 4,4'-biphenyldicarboxylic acid, 4,4'-diphenylsulfonedicarboxylic acid, 4,4'-diphenyletherdicarboxylic acid, 1,2-di(phenoxy)ethane-p,p'-dicarboxylic acid, anthracenedicarboxylic acid, etc., aromatic dicarboxylic acids containing metal sulfonate groups or their lower alkyl ester derivatives such as 5-sodium sulfoisophthalate, 2-sodium sulfoterephthalate, 5-lithium sulfoterephthalate, 2-lithium sulfoterephthalate, 5-potassium sulfophthalate, 2-potassium sulfoterephthalate, etc.

[0155] Among the above dicarboxylic acids, terephthalic acid, isophthalic acid, and naphthalene dicarboxylic acids are particularly preferably used from the viewpoint of physical properties of the obtained polyester. In addition, other dicarboxylic acids may be copolymerized as required.

[0156] Specific examples of diols include ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, diethylene glycol, triethylene glycol, 1,2-butylene glycol, 1,3-butylene glycol, 2,3-butylene glycol, 1,4-butylene glycol, 1,5-pentanediol, neopentyl glycol, 1,6-hexanediol, 1,2-cyclohexanediol, 1,3-cyclohexanediol, 1,4-cyclohexanediol, 1,2-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, 1,4-cyclohexanedimethanol, 1,4-cyclohexanedimethanol, 1,10-decamethylene glycol, Aliphatic diols such as 1,12-dodecanediol, polyethylene glycol, polytrimethylene glycol, and polytetramethylene glycol; aromatic diols such as hydroquinone, 4,4'-dihydroxybisphenol, 1,4-bis(β-hydroxyethoxy)benzene, 1,4-bis(β-hydroxyethoxyphenyl)sulfone, bis(p-hydroxyphenyl)ether, bis(p-hydroxyphenyl)sulfone, bis(p-hydroxyphenyl)methane, 1,2-bis(p-hydroxyphenyl)ethane, bisphenol A, bisphenol C, 2,5-naphthalene diol, and diols to which ethylene oxide is added.

[0157] Specific examples of the polyol other than these diols include trimethylolmethane, trimethylolethane, trimethylolpropane, pentaerythritol, glycerin, hexanetriol, and the like.

[0158] Specific examples of the cyclic ester include ε-caprolactone, β-propiolactone, β-methyl-β-propiolactone, δ-valerolactone, glycolide, and lactide.

[0159] Specific examples of the ester-forming derivatives of polycarboxylic acids and hydroxycarboxylic acids include their alkyl esters, acid chlorides, acid anhydrides, and the like.

[0160] <Polyolefin>

[0161] Examples of the polyolefin used in the oxygen absorbing composition include polyethylene such as low-density polyethylene, medium-density polyethylene, high-density polyethylene, linear low-density polyethylene, linear ultra-low-density polyethylene, and other polyethylenes; olefin homopolymers such as polypropylene, polybutene-1, and poly-4-methylpentene-1; copolymers of ethylene and α-olefin such as ethylene-propylene random copolymers, ethylene-propylene block copolymers, ethylene-propylene-polybutene-1 copolymers, and ethylene-cyclic olefin copolymers; ethylene-α,β-unsaturated carboxylic acid copolymers such as ethylene-(meth)acrylic acid copolymers, ethylene-α,β-unsaturated carboxylic acid ester copolymers such as ethylene-ethyl (meth)acrylate copolymers, ion crosslinked products of ethylene-α,β-unsaturated carboxylic acid copolymers, and other ethylene copolymers such as ethylene-vinyl acetate copolymers; cyclic olefin ring-opening polymers and hydrogenated products thereof; cyclic olefin-ethylene copolymers; and graft-modified polyolefins obtained by graft-modifying these polyolefins with acid anhydrides such as maleic anhydride.

[0162] <Polyamide>

[0163] Examples of the polyamide include polyamides having as main structural units units derived from lactam or aminocarboxylic acid, aliphatic polyamides having as main structural units units derived from aliphatic diamines and aliphatic dicarboxylic acids, partially aromatic polyamides having as main structural units units derived from aliphatic diamines and aromatic dicarboxylic acids, partially aromatic polyamides having as main structural units units derived from aromatic diamines and aliphatic dicarboxylic acids, etc. In addition, the polyamide referred to here may be a compound copolymerized with monomer units other than the main structural units as required.

[0164] Specific examples of the lactam or aminocarboxylic acid include lactams such as ε-caprolactam and laurolactam, aminocarboxylic acids such as aminocaproic acid and aminoundecanoic acid, and aromatic aminocarboxylic acids such as p-aminomethylbenzoic acid.

[0165] Specific examples of aliphatic diamines include aliphatic diamines having 2 to 12 carbon atoms or functional derivatives thereof, alicyclic diamines, and the like. In addition, the aliphatic diamine may be a linear aliphatic diamine or a branched chain aliphatic diamine. Specific examples of such linear aliphatic diamines include aliphatic diamines such as ethylenediamine, 1-methylethylenediamine, 1,3-propylenediamine, tetramethylenediamine, pentamethylenediamine, hexamethylenediamine, heptamethylenediamine, octamethylenediamine, nonamethylenediamine, decamethylenediamine, undecamethylenediamine, and dodecamethylenediamine. Specific examples of alicyclic diamines include cyclohexanediamine, 1,3-bis(aminomethyl)cyclohexane, and 1,4-bis(aminomethyl)cyclohexane.

[0166] Specific examples of aliphatic dicarboxylic acids include linear aliphatic dicarboxylic acids and alicyclic dicarboxylic acids. In particular, linear aliphatic dicarboxylic acids having an alkylene group having 4 to 12 carbon atoms are preferred. As linear aliphatic dicarboxylic acids, adipic acid, sebacic acid, malonic acid, succinic acid, glutaric acid, pimelic acid, suberic acid, azelaic acid, undecanoic acid, undecanedioic acid, dodecanedioic acid, dimer acid and functional derivatives thereof are mentioned. As alicyclic dicarboxylic acids, 1,4-cyclohexane dicarboxylic acid, hexahydroterephthalic acid, hexahydroisophthalic acid, etc. are mentioned.

[0167] Specific examples of the aromatic diamine include m-xylylenediamine, p-xylylenediamine, and p-bis(2-aminoethyl)benzene.

[0168] Specific examples of the aromatic dicarboxylic acid include terephthalic acid, isophthalic acid, phthalic acid, 2,6-naphthalene dicarboxylic acid, diphenyl-4,4′-dicarboxylic acid, diphenoxyethane dicarboxylic acid, and functional derivatives thereof.

[0169] Specific polyamides include polyamide 4, polyamide 6, polyamide 10, polyamide 11, polyamide 12, polyamide 4,6, polyamide 6,6, polyamide 6,10, polyamide 6T, polyamide 9T, polyamide 6IT, polym-phenylenediamine adipamide (polyamide MXD6), isophthalic acid copolymerized polym-phenylenediamine adipamide (polyamide MXD6I), polym-phenylenediamine sebacate (polyamide MXD10), polym-phenylenediamine lauroyl (polyamide MXD12), poly-1,3-diaminocyclohexane adipamide (polyamide BAC6), polym-phenylenediamine sebacate (polyamide PXD10), etc. More preferred polyamides include polyamide 6, polyamide MXD6, and polyamide MXD6I.

[0170] <Molecular weight of polymer>

[0171] Regarding aliphatic hydroxycarboxylic acid polymers such as polyhydroxyalkanoates, the weight average molecular weight measured by gel permeation chromatography converted by polystyrene is preferably 100,000 or more, more preferably 200,000 or more, and further can be 300,000 or more, 400,000 or more, or 500,000 or more. The weight average molecular weight measured by gel permeation chromatography converted by polystyrene can be 600,000 or more, 700,000 or more, 800,000 or more, 900,000 or more, 1,000,000 or more, 1,100,000 or more, 1,200,000 or more, 1,300,000 or more, 1,400,000 or more, 1,500,000 or more, 2,000,000 or more, 3,000,000 or more, or 4,000,000 or more. The upper limit of the weight average molecular weight measured by gel permeation chromatography converted by polystyrene is not particularly limited, and is usually 20 million or less, and can be 10 million or less, 8 million or less, 7 million or less, 6 million or less, 5 million or less, 4 million or less, or 3 million or less. However, in the case of melt molding, taking into account the decrease in molecular weight due to thermal cracking and the viscosity during melting not becoming too high, the weight average molecular weight measured by gel permeation chromatography converted to polystyrene is preferably 400,000 to 2.5 million, more preferably 500,000 to 2.2 million, and further preferably 600,000 to 2,000,000.

[0172] Regarding the molecular weight of the polymer other than the aliphatic hydroxycarboxylic acid polymer, an appropriate molecular weight can be used as appropriate depending on the type of the polymer.

[0173] <Preferred Embodiment of Polymer>

[0174] The polymer of the present invention may be any of a random polymer, a block polymer, an alternating polymer or a graft polymer, and is preferably a random polymer.

[0175] The polymer preferably includes a thermoplastic resin.

[0176] The polymer is more preferably a biodegradable polymer, and further preferably a bioabsorbable polymer. Biodegradability means that it can be decomposed by microorganisms or enzymes in the natural environment (such as soil, compost, lakes, seawater, etc.), or can be decomposed into non-toxic components in the body. Bioabsorbability means that it can be metabolized by organisms such as humans or animals.

[0177] The melting point of the polymer is not particularly limited, but is preferably 180°C or less, more preferably 175°C or less, and further preferably less than 175°C. The melting point of the polymer may be 170°C or less, 160°C or less, 150°C or less, 140°C or less, or 130°C or less. The lower limit of the melting point of the polymer is not particularly limited, but may generally be 40°C or more, 50°C or more, 60°C or more, 70°C or more, 80°C or more, 90°C or more, or 100°C or more. In the case where the polymer has multiple melting points, the melting point of the main component may be within the above range.

[0178] [About melt molding]

[0179] In the present invention, the polymer is melt-molded. When the polymer is melt-molded, additives may be added as long as the effects of the present invention are not impaired.

[0180] As additives, there can be mentioned one or more selected from antioxidants, heat stabilizers (such as hindered phenols, hydroquinones, phosphites and their substitutes, etc.), ultraviolet absorbers (such as resorcinol, salicylate), anti-coloring agents (phosphites, hypophosphites, etc.), lubricants, release agents (montanic acid and its metal salts, its esters, its half esters, stearyl alcohol, stearamide and polyethylene wax, etc.), colorants (dyes or pigments, etc.), carbon black as a conductive agent or colorant, plasticizers, flame retardants (bromine flame retardants, phosphorus flame retardants, red phosphorus, silicone flame retardants, etc.), flame retardant aids and antistatic agents.

[0181] The method of adding the additive to the polymer is not particularly limited, and examples thereof include dry blending, solution blending, and addition during polymer polymerization.

[0182] The polymer can be molded by a known melt molding method such as injection molding, injection compression molding, compression molding, extrusion molding (melt extrusion molding), blow molding, compression molding, spinning (melt extrusion spinning), etc.

[0183] The number of times of melt molding is not particularly limited, but it is preferably performed only once.

[0184] In the present invention, the step of curing after molding can be carried out in a molding die, in a gas (e.g., air, nitrogen, etc.) or in a liquid (e.g., water, alcohol, glycerol or a mixture thereof, etc.). That is, the polymer partially melted by the method of the present invention can be cooled in a molding die, in a gas or in a liquid, thereby curing. Preferably, the partially melted polymer can be cooled in a molding die, in air or in water. More preferably, the partially melted polymer can be cooled in a molding die or in air.

[0185] As the polymer molded article produced by the method of the present invention, there can be mentioned injection molded articles, extrusion molded articles, compression molded articles, sheets, pipes, various films such as unstretched films, uniaxially stretched films, and biaxially stretched films, various fibers such as unstretched yarns and super-stretched yarns, etc. In addition, as the polymer molded article produced by the method of the present invention, it can be tubular or in a shape other than tubular.

[0186] The present invention is described in detail below by showing examples, comparative examples, and reference examples. In addition, the descriptions of the examples, comparative examples, reference examples, and embodiments in the specification of the present invention are for the purpose of helping to understand the content of the present invention, and such descriptions cannot be used as a basis for narrowly interpreting the technical scope of the present invention. In addition, the thermoplastic polymers used in the following examples and comparative examples are as follows.

[0187] Example

[0188] <Polymer used>

[0189] As poly 3-hydroxybutyric acid (P(3HB)), “Biogreen (registered trademark)” (Mw: 940,000) manufactured by Mitsubishi Gas Chemical Co., Ltd. was used.

[0190] The P(3HB-co-4HB) copolymer was produced by the culture method according to the method described in WO2019 / 044837. By appropriately changing the type and supply ratio of the carbon source used, P(3HB-co-4HB) copolymers with various 4HB ratios were produced.

[0191] The P(3HB-co-3HV) copolymer used was Biopol (8.0 mol % 3HV product and 12.0 mol % 3HV product) produced by ICI. In addition, the 3HV-rich P(3HB-co-3HV) copolymer was produced by a culture method according to the method described in Japanese Patent Application Laid-Open No. 04-084890 and Japanese Patent Application Laid-Open No. 01-069622.

[0192] The polyglycolic acid (PGA) used was "PGA (MFR (240, 10) = 0.5 ~ 5.0 g / 10min)" produced by BMG Co., Ltd., the poly-L-lactic acid (PLLA) used was "PLLA (Mw: 470,000)" produced by BMG Co., Ltd., the polycaprolactone (PCL) used was "Capa6800 (Mw: 80,000)" produced by Ingevity, and the copolymer of glycolic acid and L-lactic acid used was "PGLA (90:10) (glycolic acid 88.5 mol%: L-lactic acid 11.5 mol%, MFR (240, 10) = 2.75)" produced by BMG Co., Ltd.

[0193] As poly(p-dioxanone) (PPDO), "PPDO" produced by BMG Corporation was used.

[0194] As polybutylene succinate (PBS), “BioPBS (registered trademark) FZ91PB (MFR 190, 10) = 5 g / 10 min)” manufactured by Mitsubishi Chemical Corporation was used, and as polybutylene succinate adipate, “BioPBS (registered trademark) FD92PB (MFR 190, 10) = 4 g / 10 min)” manufactured by Mitsubishi Chemical Corporation was used.

[0195] The method of extracting PHA from bacterial cells is well known. It can be a solvent extraction method using a halogenated hydrocarbon solvent such as chloroform for extraction and precipitation using a poor solvent such as hexane or methanol. It can also be an aqueous extraction method such as described in Japanese Patent Publication No. 04-061638, Japanese Patent Application Laid-Open No. 07-177894, and WO2004 / 029266.

[0196] Various evaluation methods and melt extrusion methods used for analysis methods of thermoplastic polymers are described.

[0197] (1) Molecular weight determination of thermoplastic polymers

[0198] [PHA molecular weight determination (gel permeation chromatography (GPC) method)]

[0199] The molecular weight of PHA was determined by gel permeation chromatography as shown below.

[0200] Chloroform was added to make PHA about 0.5 mg / ml, dissolved at 60°C for 4 hours, then returned to room temperature, and insoluble matter was removed by filtration using a PTFE filter with a pore size of 0.2 μm to prepare a measurement sample. GPC conditions are as follows.

[0201] Apparatus: HPLC Prominence system manufactured by Shimadzu Corporation;

[0202] Column: Showa Denko Shodex K-806L (2 in series);

[0203] Column temperature: 40 °C;

[0204] Mobile phase: chloroform (1 ml / min);

[0205] Detector: RI (40°C);

[0206] Standards: Shodex polystyrene molecular weight standards (6.87 million to 12.70);

[0207] Injection volume: 60 μl;

[0208] Analysis time: 30 minutes.

[0209] (2) Determination of the outflow starting temperature of thermoplastic polymers

[0210] [Measurement of the outflow starting temperature of thermoplastic polymers using a flow tester]

[0211] Thermoplastic polymers were measured using a flow tester CFT-500D (Capillary Rheometer Flowtester, manufactured by Shimadzu Corporation) or CFT-500EX (manufactured by Shimadzu Corporation). Regarding the sample amount used for the measurement, the thermoplastic polymer in the form of granules, powders, films, etc. is about 1.2 g, which is filled into a cylinder for measurement. In the case of using a powdered polymer, it can also be formed using an appropriate granulator or molding machine and then filled into a cylinder. The mold (nozzle) uses a product with a diameter of 1.0 mm and a thickness of 1.0 mm, and an extrusion load of 5 kg is applied. After a preheating time of 240 seconds at an initial setting temperature of 30°C to 140°C (appropriately selected according to the type and melting point of the polymer), the stroke length (mm) and the temperature curve when the temperature is uniformly increased to 130°C to 260°C (appropriately selected according to the type and melting point of the polymer) at a rate of 3°C / min are obtained. As the temperature rises, the thermoplastic polymer is heated and the polymer begins to flow out of the mold. The temperature at this point is referred to as the flow start temperature.

[0212] (3) Determination of melting behavior of thermoplastic polymers

[0213] [Measurement of thermal properties using differential scanning calorimeter (DSC)]

[0214] The melting behavior of thermoplastic polymers represented by polyhydroxyalkanoates was measured using a differential scanning calorimeter (Rigaku, Thermo plus EVO DSC8230). The measurement atmosphere was set to nitrogen (30 ml / min), and the temperature was raised from 30°C to 130°C to 260°C at 20°C / min (appropriately selected according to the type and melting point of the polymer). The sample was set to about 1 mg, and an aluminum sample pan was used. Indium was used for temperature correction.

[0215] When the melting peak is a sharp peak, according to JIS-K7121, the extrapolated melting end temperature of the melting peak is set to the temperature at the intersection of the tangent line drawn from the maximum slope point before the peak ends and the baseline after the peak (identified by Rigaku, Thermo plus EVO software). When the melting peak shape is multi-peak overlap, manually re-draw the tangent line for the peak on the high temperature side, and use its intersection with the baseline as the extrapolated melting end temperature.

[0216] (4) Partial melt extrusion and melt extrusion of thermoplastic polymers

[0217] [Melt spinning at a constant temperature using a flow tester]

[0218] Melt extrusion spinning was performed using a flow tester CFT-500D (manufactured by Shimadzu Corporation) or CFT-500EX (manufactured by Shimadzu Corporation).

[0219] <Various Analysis Results>

[0220] The measurement results of DSC and CFT (capillary flow tester) of the PHA copolymer containing 4HB are shown in Table 1 below.

[0221] [Table 1]

[0222] Table 1 Partial melt spinning conditions and heating state change behavior of PHA copolymers containing 4HB

[0223]

[0224] <Comparative Example 1> Sample S1

[0225] P(3HB) (as sample S1) with a Mw of 940,000 was analyzed using a flow tester (CFT) and DSC. The CFT outflow start temperature was 181.0°C, and the peak width of the crystalline melting peak measured by DSC was approximately 140-189°C. The apex of the crystalline melting peak was 175.0°C, the DSC extrapolated melting end temperature was 179.7°C, and the temperature at which the melting point peak reached the baseline was 188.7°C. It was confirmed that the DSC extrapolated melting end temperature was lower than the CFT outflow start temperature, and if it was not in a completely molten state, it would not flow out. That is, at a temperature below the DSC extrapolated melting end temperature, it would not flow out, and partial melt extrusion could not be achieved. Figure 1 The measurement results of CFT and DSC are shown.

[0226] <Example 1> Sample S2

[0227] CFT and DSC were used to analyze P (3HB-co-11.8 mol% 4HB) with a Mw of 1.16 million (as sample S2). The CFT outflow start temperature was 131.3°C, and the peak width of the crystalline melting peak measured by DSC was about 80-167°C. The apex of the crystalline melting peak was 95.2°C and 141.8°C, the DSC extrapolated melting end temperature was 158.7°C, and the temperature at which the melting point peak reached the baseline was 167.0°C. As a result, the DSC extrapolated melting end temperature was higher than the CFT outflow start temperature, and partial melt extrusion could be achieved in the range of 131.3°C or more and less than 158.7°C. Figure 2 The measurement results of CFT and DSC are shown.

[0228] Melt spinning was performed at 135°C (Example 11) and 150°C (Example 12) as the temperature at which partial melting could be achieved, and at 170°C (Comparative Example 3) and 180°C (Comparative Example 4) as the temperature at which almost all melting could be achieved.

[0229] Compared with the Mw before melt spinning of 1.16 million, the Mw after partial melt spinning at 135°C is 1.1 million, the Mw after partial melt spinning at 150°C is 1.08 million, the Mw after melt spinning at 170°C is 720,000, and the Mw after melt spinning at 180°C is 460,000. Regarding the residual rate of molecular weight Mw after melt spinning at each temperature, when the molecular weight Mw before melt spinning is 1.16 million is 100%, relative to 95% at 135°C, 93% at 150°C, 62% at 170°C, and 39% at 180°C, it is clear that being able to spin at a lower temperature is effective in suppressing the decrease in molecular weight. In particular, when partial melt spinning is performed at 135°C and 150°C, which is not a completely molten state, the suppression of molecular weight reduction is significant. The results are shown in Table 2.

[0230] In addition, in the partial melt extrusion spinning performed at 135°C and 150°C, the adhesion of the polymer immediately after spinning, which was observed in the melt extrusion spinning at 170°C and 180°C, was suppressed, no agglutination occurred, and the crystallization time of about 30 minutes to 1 hour at room temperature was not required, and the process of winding or stretching could be transferred. That is, it is shown that the partial melt extrusion spinning can shorten the crystallization time, improve the melt processability of the polymer, and improve the productivity.

[0231] [Table 2]

[0232] Table 2 Changes in the melting state before and after melt extrusion and the molecular weight Mw after melt extrusion of sample S2 (P(3HB-co-11.8 mol % 4HB)) at various temperatures

[0233]

[0234] *1: Mw before melt extrusion;

[0235] *2: Mw after melt extrusion;

[0236] *3: Mw residual ratio: [weight average molecular weight after melt extrusion (Mw) ÷ weight average molecular weight before melt extrusion (Mw)] × 100.

[0237] <Example 2> Sample S3

[0238] P (3HB-co-13.1 mol% 4HB) with a Mw of 1 million was analyzed using CFT and DSC (as sample S3). The CFT outflow start temperature was 125.1°C, and the peak width of the crystalline melting peak obtained by DSC was about 49 to 144°C. The crystalline melting peak apex was 63.7°C and 114.8°C, the DSC extrapolated melting end temperature was 135.1°C, and the temperature at which the melting point peak reached the baseline was 155.0°C. It was confirmed that the DSC extrapolated melting end temperature was higher than the CFT outflow start temperature, and partial melt extrusion could be achieved in the range of 125.1 to 135.1°C. Figure 3 The measurement results of CFT and DSC are shown.

[0239] Melt spinning was carried out at 126°C (Example 13), 130°C (Example 14), and 135°C (Example 15) as temperatures capable of achieving partial melting, and at 150°C (Comparative Example 5), 160°C (Comparative Example 6), and 170°C (Comparative Example 7) as temperatures capable of achieving almost complete melting.

[0240] Relative to the Mw of 1 million before melt spinning, the Mw after partial melt spinning at 126°C was 950,000, the Mw after partial melt spinning at 130°C was 970,000, the Mw after partial melt spinning at 135°C was 970,000, the Mw after partial melt spinning at 140°C was 920,000, the Mw after melt spinning at 150°C was 820,000, the Mw after melt spinning at 160°C was 650,000, and the Mw after melt spinning at 170°C was 540,000. The residual rate of molecular weight Mw after melt spinning at each temperature was 95% at 126°C, 97% at 130°C, 97% at 135°C, 82% at 150°C, 65% at 160°C, and 53% at 170°C, with the molecular weight Mw before melt spinning being 1,000,000 as 100%. It was found that being able to spin at a lower temperature, especially being able to spin at a low temperature to achieve a partially molten state, is effective in suppressing the decrease in molecular weight. In particular, in partial melt spinning performed at 135°C or below, which is obviously not a completely molten state, the decrease in molecular weight is significantly suppressed.

[0241] The results are shown in Table 3.

[0242] In melt spinning at 170°C, the extruded polymer had strong adhesion, and agglutination was observed, and the solidified polymer could not be unwound after winding. On the other hand, the yarns subjected to partial melt extrusion spinning at 135°C or below showed almost no adhesion, and could be wound and stretched without agglutination immediately after spinning. That is, it was shown that partial melt extrusion spinning can shorten the crystallization time, improve the melt processability of the polymer, and increase productivity.

[0243] [Table 3]

[0244] Table 3 Changes in the melting state before and after melt extrusion and the molecular weight Mw after melt extrusion of sample S3 (P(3HB-co-13.1 mol % 4HB)) at various temperatures

[0245]

[0246] *1: Mw before melt extrusion;

[0247] *2: Mw after melt extrusion;

[0248] *3: Mw residual ratio: [weight average molecular weight after melt extrusion (Mw) ÷ weight average molecular weight before melt extrusion (Mw)] × 100.

[0249] <Example 3> Sample S4

[0250] P (3HB-co-14.7 mol% 4HB) with a Mw of 900,000 (as sample S4) was analyzed using CFT and DSC. The CFT outflow start temperature was 113.9°C, and the peak width of the crystalline melting peak obtained by DSC was about 88-145°C. The crystalline melting peak apex was 93.6°C, the DSC extrapolated melting end temperature was 140.9°C, and the temperature at which the melting point peak reached the baseline was 144.7°C. It was confirmed that the DSC extrapolated melting end temperature was higher than the CFT outflow start temperature, and partial melt extrusion could be achieved in the range of 113.9°C or more and less than 140.9°C. Figure 4 The measurement results of CFT and DSC are shown.

[0251] Melt spinning was performed at 115°C (Example 16), 130°C (Example 17), and 140°C (Example 18) as the temperature at which partial melting could be achieved, and at 170°C (Comparative Example 8) as the temperature at which almost all melting could be achieved.

[0252] Compared with the Mw before melt spinning of 900,000, the Mw after partial melt spinning at 115°C is 890,000, the Mw after partial melt spinning at 130°C is 840,000, the Mw after melt spinning at 140°C is 870,000, the Mw after melt spinning at 150°C is 870,000, and the Mw after melt spinning at 170°C is 550,000. Regarding the residual rate of molecular weight Mw after melt spinning at each temperature, when the molecular weight Mw before melt spinning is 900,000 as 100%, it is 99% at 115°C, 94% at 130°C, 97% at 140°C, and 61% at 170°C, which clearly shows that being able to spin at a lower temperature is effective in suppressing the decrease in molecular weight. In particular, in low-temperature partial melt spinning in a partially molten state below 140°C, the suppression of molecular weight decrease is significant. The results are shown in Table 4.

[0253] In melt spinning at 170°C, the extruded polymer had strong adhesion, and agglutination was observed, and the solidified polymer could not be unwound after winding. On the other hand, the yarns subjected to partial melt extrusion spinning at 140°C or below showed almost no adhesion, and could be wound and stretched without agglutination immediately after spinning. That is, it was shown that partial melt extrusion spinning can shorten the crystallization time, improve the melt processability of the polymer, and increase productivity.

[0254] [Table 4]

[0255] Table 4 shows the melting state of sample S4 (P(3HB-co-14.7 mol % 4HB)) before and after melt extrusion at various temperatures and the change in molecular weight Mw after melt extrusion.

[0256]

[0257] *1: Mw before melt extrusion;

[0258] *2: Mw after melt extrusion;

[0259] *3: Mw residual ratio: [weight average molecular weight after melt extrusion (Mw) ÷ weight average molecular weight before melt extrusion (Mw)] × 100.

[0260] <Example 4> Sample S5

[0261] P (3HB-co-15.3 mol% 4HB) with a Mw of 750,000 (as sample S5) was analyzed using CFT and DSC. The CFT outflow start temperature was 109.4°C, and the peak width of the crystalline melting peak obtained by DSC was about 58-170°C. The crystalline melting peak apexes were 65.5°C, 92.7°C, 110.0°C, and 164.3°C, and the DSC extrapolated melting end temperatures were 80.0°C, 109.0°C, 130.2°C, and 168.9°C, and the temperature at which the melting point peak reached the baseline was 172.6°C. It was confirmed that the DSC extrapolated melting end temperature was higher than the CFT outflow start temperature, and partial melt extrusion could be achieved in the range of 109.4°C or more and less than 168.9°C. Figure 5 The measurement results of CFT and DSC are shown.

[0262] Melt spinning was performed at 115°C (Example 19), 120°C (Example 20), and 125°C (Example 21) as the temperature at which partial melting can be achieved.

[0263] The Mw before melt spinning was 750,000, and the Mw after partial melt spinning at 115°C, 120°C, and 125°C was 750,000. It was found that spinning in a partially melted state at a temperature significantly lower than 150°C was effective in suppressing the decrease in molecular weight. The results are shown in Table 5.

[0264] The yarns partially melt-spun at 125°C or below showed little stickiness and could be wound and stretched without sticking immediately after spinning. That is, partial melt-spinning can shorten the crystallization time, improve the melt processability of the polymer, and increase productivity.

[0265] [Table 5]

[0266] Table 5 Changes in the melting state before and after melt extrusion and the molecular weight Mw after melt extrusion of sample S5 (P(3HB-co-15.3 mol % 4HB)) at various temperatures

[0267]

[0268] *1: Mw before melt extrusion;

[0269] *2: Mw after melt extrusion;

[0270] *3: Mw residual ratio: [weight average molecular weight after melt extrusion (Mw) ÷ weight average molecular weight before melt extrusion (Mw)] × 100.

[0271] <Example 5> Sample S6

[0272] P (3HB-co-15.3 mol% 4HB) with a Mw of 710,000 (as sample S6) was analyzed using CFT and DSC. The CFT outflow start temperature was 113.8°C, and the peak width of the crystalline melting peak obtained by DSC was about 81-155°C. The apex of the crystalline melting peak was 91.2°C, the DSC extrapolated melting end temperature was 145.6°C, and the temperature at which the melting point peak reached the baseline was 161.1°C. It was confirmed that the DSC extrapolated melting end temperature was higher than the CFT outflow start temperature, and partial melt extrusion could be achieved in the range of 113.8°C or more and less than 145.6°C. Figure 6 The measurement results of CFT and DSC are shown.

[0273] Melt spinning was carried out at a temperature of 160°C (Comparative Example 9) or 170°C (Comparative Example 10) at which almost all the fibers were melted.

[0274] The Mw before melt spinning was 710,000, the Mw after melt spinning at 160°C was 480,000, and the Mw after melt spinning at 170°C was 310,000, which clearly shows that it is difficult to avoid a decrease in molecular weight when melt spinning is performed at a high temperature of 160°C or 170°C, which is not a partially molten state. The results are shown in Table 6.

[0275] The polymer extruded by melt spinning at 160° C. or 170° C. exhibits strong adhesion, and requires a crystallization solidification time of about 30 minutes to 1 hour at room temperature for stretching.

[0276] [Table 6]

[0277] Table 6 Changes in the melting state before and after melt extrusion and the molecular weight Mw after melt extrusion of sample S6 (P(3HB-co-15.3 mol % 4HB)) at various temperatures

[0278]

[0279] *1: Mw before melt extrusion;

[0280] *2: Mw after melt extrusion;

[0281] *3: Mw residual ratio: [weight average molecular weight after melt extrusion (Mw) ÷ weight average molecular weight before melt extrusion (Mw)] × 100.

[0282] <Example 6> Sample S7

[0283] P (3HB-co-16.0 mol% 4HB) with a Mw of 620,000 (as sample S7) was analyzed using CFT and DSC. The CFT outflow start temperature was 94.0°C, and the peak width of the crystalline melting peak obtained by DSC was about 57-178°C. The apex of the crystalline melting peak was 99.4°C, the DSC extrapolated melting end temperature of the main melting peak was 105.8°C, the DSC extrapolated melting end temperature of the gentle melting peak following the main melting peak was 139.7°C, the DSC extrapolated melting end temperature of the high temperature side melting peak was 175.9°C, and the temperature at which the melting point peak reached the baseline was 178.2°C. It was confirmed that the DSC extrapolated melting end temperature was higher than the CFT outflow start temperature, and partial melt extrusion could be achieved within the range of above 94.0°C and below 175.9°C. Figure 7 The measurement results of CFT and DSC are shown.

[0284] Melt spinning was performed at 130°C (Example 22) and 160°C (Example 23) as the temperature at which partial melting can be achieved.

[0285] The Mw before melt spinning was 620,000, the Mw after partial melt spinning at 130°C was 610,000, the Mw after partial melt spinning at 160°C was 500,000, and the Mw after melt spinning at 170°C was 440,000. Regarding the residual rate of molecular weight Mw after melt spinning at each temperature, when the molecular weight Mw before melt spinning was 620,000 as 100%, it was 98% at 130°C, 81% at 160°C, and 71% at 170°C. In the case of sample S7 where a part of the crystals melted at the high temperature part (near 172°C) in DSC were mixed, it can be considered that at the temperature of 160 and 170°C, a part of the crystals remained without melting, but since it is a relatively high temperature for the melting temperature of PHA, a decrease in molecular weight was observed. When melt spinning was performed at a low temperature such as 130°C, the decrease in molecular weight was significantly suppressed, and it was confirmed that the ability to perform spinning at a lower temperature is effective in suppressing the decrease in molecular weight.

[0286] [Table 7]

[0287] Table 7 Changes in the melting state before and after melt extrusion and the molecular weight Mw after melt extrusion of sample S7 (P(3HB-co-16.0 mol% 4HB)) at various temperatures

[0288]

[0289] *1: Mw before melt extrusion;

[0290] *2: Mw after melt extrusion;

[0291] *3: Mw residual ratio: [weight average molecular weight after melt extrusion (Mw) ÷ weight average molecular weight before melt extrusion (Mw)] × 100.

[0292] <Example 7> Sample S8

[0293] P (3HB-co-17.8 mol% 4HB) with a Mw of 580,000 (as sample S8) was analyzed using CFT and DSC. The CFT outflow start temperature was 96.2°C, and the peak width of the crystalline melting peak obtained by DSC was about 43-177°C. The apexes of the crystalline melting peaks were 47.5°C and 100.6°C, and at 166.6°C there was also an apex of a small melting peak believed to be derived from 3HB-rich crystals. The DSC extrapolated melting end temperature of the main melting peak was 107.3°C, the DSC extrapolated melting end temperature of the gentle melting peak following the main melting peak was 142.1°C, the DSC extrapolated melting end temperature of the high temperature side melting peak was 175.6°C, and the temperature at which the melting point peak reached the baseline was 177.6°C. It was confirmed that the DSC extrapolated melting end temperature was higher than the CFT outflow start temperature, and partial melt extrusion could be achieved within the range of above 96.2°C and below 175.6°C. Figure 8 The measurement results of CFT and DSC are shown.

[0294] <Example 8> Sample S9

[0295] P (3HB-co-17.9 mol% 4HB) with a Mw of 630,000 (as sample S9) was analyzed using CFT and DSC. The CFT outflow start temperature was 131.3°C, and the peak width of the crystalline melting peak obtained by DSC was about 90-149°C. The apex of the crystalline melting peak was 116.9°C and 131.7°C, the DSC extrapolated melting end temperature was 146.0°C, and the temperature at which the melting point peak reached the baseline was 151.7°C. It was confirmed that the DSC extrapolated melting end temperature was higher than the CFT outflow start temperature, and partial melt extrusion could be achieved in the range of 131.3°C or more and less than 146.0°C. Fig. 9 The measurement results of CFT and DSC are shown.

[0296] <Example 9> Sample S10

[0297] P (3HB-co-28.7 mol% 4HB) with a Mw of 1.05 million (as sample S10) was analyzed using CFT and DSC. The CFT outflow start temperature was 109.5°C, and the peak width of the crystalline melting peak obtained by DSC was about 39-167°C. The apex of the crystalline melting peak was 47.0°C and 164.0°C, the DSC extrapolated melting end temperature was 55.9°C and 166.7°C, and the temperature at which the melting point peak reached the baseline was 170.3°C. Although the melting peak on the high temperature side may also be a peak resulting from the admixture of a small amount of 3HB-rich PHA and biosynthesis, the DSC extrapolated melting end temperature is higher than the CFT outflow start temperature, and it is believed that there are residual crystalline components in the range above 109.5°C and below 166.7°C, confirming that partial melt extrusion can be achieved within this range. Fig.10 The measurement results of CFT and DSC are shown.

[0298] <Example 10> Sample S11

[0299] P (3HB-co-32.9 mol% 4HB) with a Mw of 1.04 million (as sample S11) was analyzed using CFT and DSC. The CFT outflow start temperature was 123.1°C, and the peak width of the crystalline melting peak obtained by DSC was about 40-148°C. The apex of the crystalline melting peak was 44.8°C, 79.1°C, and 123.8°C, the DSC extrapolated melting end temperature was 55.9°C, 88.1°C, and 144.7°C, and the temperature at which the melting point peak reached the baseline was 151.4°C. It was confirmed that the DSC extrapolated melting end temperature was higher than the CFT outflow start temperature, and partial melt extrusion could be achieved within the range of 123.1°C to 144.7°C. Fig.11The measurement results of CFT and DSC are shown.

[0300] <Comparative Example 2> Sample S12

[0301] P (3HB-co-74.6 mol% 4HB) with a Mw of 1.11 million was analyzed using CFT and DSC (as sample S12). The CFT outflow start temperature was 94.6°C, and the peak width of the crystalline melting peak obtained by DSC was about 39 to 72°C. The apex of the crystalline melting peak was 58.7°C, the DSC extrapolated melting end temperature was 64.1°C, and the temperature at which the melting point peak reached the baseline was 72.1°C. It was confirmed that the DSC extrapolated melting end temperature was lower than the CFT outflow start temperature, and if it was not in a completely molten state above 94.6°C, it would not flow out. Fig.12 The measurement results of CFT and DSC are shown.

[0302] The measurement results of DSC and CFT of the PHA copolymer containing 3HV are shown in Table 8 below.

[0303] [Table 8]

[0304] Table 8 Partial melt spinning conditions and heating state change behavior of PHA copolymers containing 3HV

[0305]

[0306] <Example 24> Sample S13

[0307] P (3HB-co-8.0 mol% 3HV) with a Mw of 460,000 (as sample S13) was analyzed using CFT and DSC. The CFT outflow start temperature was 151.6°C, and the peak width of the crystalline melting peak obtained by DSC was about 125-174°C. The apex of the crystalline melting peak was 152.1°C, the DSC extrapolated melting end temperature was 164.9°C, and the temperature at which the melting point peak reached the baseline was 173.9°C. It was confirmed that the DSC extrapolated melting end temperature was higher than the CFT outflow start temperature, and partial melt extrusion could be achieved in the range of 151.6°C or more and less than 164.9°C. Fig.13 The measurement results of CFT and DSC are shown.

[0308] Melt spinning was performed at 160°C (Example 30) as a temperature at which partial melting could be achieved, and at 175°C (Comparative Example 11) and 185°C (Comparative Example 12) as a temperature at which almost all melting could be achieved.

[0309] The Mw before melt spinning was 460,000, the Mw after melt spinning at 160°C was 450,000, the Mw after melt spinning at 175°C was 390,000, and the Mw after melt spinning at 185°C was 360,000. Regarding the residual rate of the molecular weight Mw after melt spinning at each temperature, when the molecular weight Mw before melt spinning was 460,000 as 100%, it was 97% at 160°C, 86% at 175°C, and 79% at 185°C.

[0310] Not only the P(3HB-co-4HB) copolymer but also the P(3HB-co-3HV) copolymer including other monomer units showed a remarkable effect of suppressing the decrease in molecular weight when melt-spinning was performed at a lower temperature.

[0311] In melt spinning at 185°C, the extruded polymer had strong adhesion, and agglutination was observed, and the solidified polymer could not be unwound after winding. On the other hand, the yarns subjected to partial melt extrusion spinning at 160°C showed almost no adhesion, and could be wound and stretched without agglutination immediately after spinning. That is, it was shown that partial melt extrusion spinning can shorten the crystallization time, improve the melt processability of the polymer, and increase productivity.

[0312] [Table 9]

[0313] Table 9 Changes in the melting state before and after melt extrusion and the molecular weight Mw after melt extrusion of sample S13 (P(3HB-co-8.0 mol% 3HV)) at various temperatures

[0314]

[0315] *1: Mw before melt extrusion;

[0316] *2: Mw after melt extrusion;

[0317] *3: Mw residual ratio: [weight average molecular weight after melt extrusion (Mw) ÷ weight average molecular weight before melt extrusion (Mw)] × 100.

[0318] <Example 25> Sample S14

[0319] P (3HB-co-12.0 mol% 3HV) with a Mw of 190,000 (as sample S14) was analyzed using CFT and DSC. The CFT outflow start temperature was 140.4°C, and the peak width of the crystalline melting peak obtained by DSC was about 124-166°C. The apex of the crystalline melting peak was 144.9°C, the DSC extrapolated melting end temperature was 156.7°C, and the temperature at which the melting point peak reached the baseline was 165.7°C. It was confirmed that the DSC extrapolated melting end temperature was higher than the CFT outflow start temperature, and partial melt extrusion could be achieved in the range of 140.4°C or more and less than 156.7°C. Fig.14 The measurement results of CFT and DSC are shown.

[0320] Melt spinning was performed at 145°C (Example 31), 150°C (Example 32), and 155°C (Example 33) as temperatures capable of partial melting, and at 170°C (Comparative Example 13) as a temperature capable of almost complete melting.

[0321] Relative to the Mw of 190,000 before melt spinning, the Mw after melt spinning at 145°C, 150°C, and 155°C was 190,000, and the Mw after melt spinning at 170°C was 160,000. Regarding the residual rate of the molecular weight Mw after melt spinning at each temperature, when the molecular weight Mw of 190,000 before melt spinning was 100%, relative to 98% at 145°C, 98% at 150°C, 98% at 155°C, and 83% at 170°C.

[0322] Not only the P(3HB-co-4HB) copolymer but also the P(3HB-co-3HV) copolymer showed a remarkable effect of suppressing the decrease in molecular weight when melt-spinning was performed at a lower temperature.

[0323] In melt spinning at 170°C, the extruded polymer had strong adhesion, and agglutination was observed, and the solidified polymer could not be unwound after winding. On the other hand, the yarns subjected to partial melt extrusion spinning at 150°C or below showed almost no adhesion, and could be wound and stretched without agglutination immediately after spinning. That is, it was shown that partial melt extrusion spinning can shorten the crystallization time, improve the melt processability of the polymer, and increase productivity.

[0324] [Table 10]

[0325] Table 10 Changes in the melting state before and after melt extrusion and the molecular weight Mw after melt extrusion of sample S14 (P(3HB-co-12.0 mol% 3HV)) at various temperatures

[0326]

[0327] *1: Mw before melt extrusion;

[0328] *2: Mw after melt extrusion;

[0329] *3: Mw residual ratio: [weight average molecular weight after melt extrusion (Mw) ÷ weight average molecular weight before melt extrusion (Mw)] × 100.

[0330] <Example 26> Sample S15

[0331] P (3HB-co-35.5 mol% 3HV) with a Mw of 330,000 (as sample S15) was analyzed using CFT and DSC. The CFT outflow start temperature was 85.1°C, and the peak width of the crystalline melting peak obtained by DSC was about 45-173°C. The apex of the crystalline melting peak was 89.0°C, and at 165.4°C there was also a apex of a small melting peak believed to be derived from 3HB-rich crystals. The DSC extrapolated melting end temperature of the main melting peak was 106.0°C, the DSC extrapolated melting end temperature of the high-temperature side melting peak was 173.0°C, and the temperature at which the melting point peak reached the baseline was 174.6°C. It was confirmed that the DSC extrapolated melting end temperature was higher than the CFT outflow start temperature, and partial melt extrusion could be achieved in the range of above 85.1°C and below 173.0°C. Even if it is assumed that there is no component mixed in that shows a small melting peak on the high temperature side that is believed to originate from 3HB-rich crystals, the extrapolated melting end temperature of the low temperature side melting peak reaches 106.0°C, which shows that in this case partial melt extrusion can be achieved in the range above 85.1°C and below 106.0°C. Fig.15 The measurement results of CFT and DSC are shown.

[0332] <Example 27> Sample S16

[0333] P (3HB-co-48.2 mol% 3HV) with a Mw of 830,000 (as sample S16) was analyzed using CFT and DSC. The CFT outflow start temperature was 83.8°C, and the peak width of the crystalline melting peak obtained by DSC was about 50-178°C. The apexes of the crystalline melting peaks were 75.0°C and 88.7°C, and at 165.7°C there was also a apex of a small melting peak believed to be derived from 3HB-rich crystals. The DSC extrapolated melting end temperature of the main melting peak was 94.8°C, the DSC extrapolated melting end temperature of the high-temperature side melting peak was 173.7°C, and the temperature at which the melting point peak reached the baseline was 177.7°C. It was confirmed that the DSC extrapolated melting end temperature was higher than the CFT outflow start temperature, and partial melt extrusion could be achieved in the range of above 83.8°C and below 173.7°C. Even if it is assumed that there is no component mixed in that shows a small melting peak on the high temperature side that is believed to originate from 3HB-rich crystals, the extrapolated melting end temperature of the low temperature side melting peak reaches 94.8°C, which shows that in this case partial melt extrusion can be achieved in the range above 83.8°C and below 94.8°C. Fig.16The measurement results of CFT and DSC are shown.

[0334] <Example 28> Sample S17

[0335] P (3HB-co-61.5 mol% 3HV) with a Mw of 730,000 (as sample S17) was analyzed using CFT and DSC. The CFT outflow start temperature was 84.5°C, and the peak width of the crystalline melting peak obtained by DSC was about 56-178°C. The apex of the crystalline melting peak was 90.5°C, and at 166.3°C there was also an apex of a small melting peak believed to originate from 3HB-rich crystals. The DSC extrapolated melting end temperature of the main melting peak was 97.5°C, the DSC extrapolated melting end temperature of the high-temperature side melting peak was 173.2°C, and the temperature at which the melting point peak reached the baseline was 178.5°C. It was confirmed that the DSC extrapolated melting end temperature was higher than the CFT outflow start temperature, and partial melt extrusion could be achieved in the range of above 84.5°C and below 173.2°C. Even if it is assumed that there is no component mixed in that shows a small melting peak on the high temperature side that is believed to originate from 3HB-rich crystals, the extrapolated melting end temperature of the low temperature side melting peak reaches 97.5°C, which shows that in this case partial melt extrusion can be achieved in the range of above 84.5°C and below 97.5°C. Fig.17 The measurement results of CFT and DSC are shown.

[0336] <Example 29> Sample S18

[0337] P (3HB-co-73.2 mol% 3HV) with a Mw of 730,000 (as sample S18) was analyzed using CFT and DSC. The CFT outflow start temperature was 91.1°C, and the peak width of the crystalline melting peak obtained by DSC was about 64-179°C. The apex of the crystalline melting peak was 95.0°C, and at 166.9°C there was also a apex of a small melting peak believed to be derived from 3HB-rich crystals. The DSC extrapolated melting end temperature of the main melting peak was 101.3°C, the DSC extrapolated melting end temperature of the high-temperature side melting peak was 174.3°C, and the temperature at which the melting point peak reached the baseline was 178.2°C. It was confirmed that the DSC extrapolated melting end temperature was higher than the CFT outflow start temperature, and partial melt extrusion could be achieved in the range of above 91.1°C and below 174.3°C. Even if it is assumed that there is no component mixed in that shows a small melting peak on the high temperature side that is believed to originate from 3HB-rich crystals, the extrapolated melting end temperature of the low temperature side melting peak reaches 101.3°C, which shows that in this case partial melt extrusion can be achieved in the range of above 91.1°C and below 101.3°C. Fig.18 The measurement results of CFT and DSC are shown.

[0338] <Analysis of Partially Melted State>

[0339] From the melting peak shape of the thermoplastic polymer observed during the DSC heating process, it can be considered that the crystal structure remains when the melt is formed in the area below the extrapolated melting end temperature. When the outflow start temperature of the flow tester heating method is lower than the extrapolated melting end temperature of DSC, it can be considered that the melt molding between the CFT outflow start temperature and the DSC extrapolated melting end temperature is molding in a partially molten state. The wide-angle X-ray diffraction method (WAXD) was used to analyze the changes in the polymer crystal structure during the DSC heating process.

[0340] <Reference Example 1>

[0341] 2 mg of the sample S7 and P (3HB-co-16.0 mol% 4HB) used in Examples 6, 22, and 23 were placed in an X-ray capillary and placed in a temperature increasing device capable of measuring DSC. The temperature was increased at a rate of 10°C / min while wide-angle X-rays were taken. The wide-angle X-rays were measured in 2°C increments and for 1 second. The DSC measurement was performed from about 50°C to 200°C. The DSC curve and the diffraction diagram of the wide-angle X-ray measurement at this time are shown in FIG. Fig.19 .

[0342] Two endothermic (melting) peaks were observed in the DSC curve. The endothermic peak on the low temperature side is considered to be the melting peak of the thinner lamellae. The endothermic peak on the high temperature side is considered to be the melting peak of the thicker lamellae. In the wide-angle X-ray diagram, two ring-shaped patterns showing the clear presence of crystals were confirmed. Even if the endothermic peak on the low temperature side is exceeded, the two peaks derived from the crystals do not disappear, so it can be seen that thicker crystals remain.

[0343] As shown in Example 6, the sample can be partially melt extruded in the range of 94.0°C or more and less than 175.9°C. In practice, melt extrusion spinning can also be achieved at 130°C within this range (Example 22). According to the wide-angle X-ray diagram, a peak (ring pattern) derived from crystallization was also confirmed at 130°C. Therefore, it was proved that when the sample was melt-spun at 130°C, it was possible to spin in a state where not all crystals were melted, that is, in a partially melted state.

[0344] <Reference Example 2>

[0345] Place 2 mg of sample S14 and P (3HB-co-12.0 mol% 3HV) used in Examples 25, 31, 32, 33, and Comparative Example 13 in an X-ray capillary and place in a temperature increasing device capable of measuring DSC. Heat at a temperature increasing rate of 10°C / min while capturing wide-angle X-rays. Wide-angle X-rays are measured in 2°C increments and with a capture time of 1 second. DSC measurements are performed from about 50°C to 200°C. The DSC curve and wide-angle X-ray measurement diffraction diagram at this time are shown in FIG. Fig. 20.

[0346] There is only one endothermic peak in their DSC curves. In the wide-angle X-ray diagram, two clear diffraction patterns originating from crystals were observed. As shown in Example 25, the sample can be partially melt-extruded in the range of 140.4°C or more and less than 156.7°C. In practice, partial melt-extrusion spinning can be achieved at 145°C, 150°C, and 155°C within this range (Examples 31, 32, and 33). Fig.21 The diffraction pattern at 150°C shown in Figure 4 of the wide-angle X-ray diagram of the invention proves that there is a pattern derived from crystallization even at a melt spinning temperature of 150°C, and spinning can be performed in a state where not all crystals are melted, that is, in a partially molten state. The wide-angle X-ray diffraction pattern at 160°C, which is located between the extrapolated melting end temperature of 156.7°C and the temperature at which the melting peak reaches the baseline of 165.7°C ( Fig. 20 In 5), a ring pattern derived from the crystals can also be vaguely confirmed, so it can be considered that at a temperature of 160°C, although almost all the crystals have melted, a very small amount of crystals remain.

[0347] The measurement results of DSC and CFT of other biodegradable polymers are shown in Table 11 below.

[0348] [Table 11]

[0349] Table 11 Partial melt spinning conditions and heating state changes of other biodegradable polymers

[0350]

[0351] <Comparative Example 14> Sample S19 (PGA)

[0352] Polyglycolic acid (PGA) (as sample S19) of BMG Co., Ltd. was analyzed using a flow tester (CFT) and DSC. The CFT outflow start temperature was 233.9°C, and the peak width of the crystal melting peak obtained by DSC was about 195-240°C. The apex of the crystal melting peak was 228.0°C, the DSC extrapolated melting end temperature was 232.7°C, and the temperature at which the melting point peak reached the baseline was 240.0°C. It was confirmed that the DSC extrapolated melting end temperature was lower than the CFT outflow start temperature, and if it was not in a completely molten state, it would not flow out. Fig.21 The measurement results of CFT and DSC are shown.

[0353] <Example 34> Sample S20 (PLLA)

[0354] CFT and DSC were used to analyze PLLA (as sample S20) with a Mw of 470,000 produced by BMG Co., Ltd. The CFT outflow start temperature was 193.6°C, and the peak width of the crystal melting peak obtained by DSC was about 155-204°C. The apex of the crystal melting peak was 193.6°C, the DSC extrapolated melting end temperature was 198.4°C, and the temperature at which the melting point peak reached the baseline was 204.4°C. It was confirmed that the DSC extrapolated melting end temperature was higher than the CFT outflow start temperature, and partial melt extrusion could be achieved within a range of 193.6°C or higher and lower than 198.4°C. Fig. 22 The measurement results of CFT and DSC are shown.

[0355] <Example 35> Sample S21 (PGLA)

[0356] PGLA (as sample S21) of BMG Co., Ltd. was analyzed using CFT and DSC. The CFT outflow start temperature was 203.5°C, and the peak width of the high-temperature side crystalline melting peak obtained by DSC was about 190-221°C. The apex of the crystalline melting peak was 207.3°C, the DSC extrapolated melting end temperature was 212.6°C, and the temperature at which the melting point peak reached the baseline was 220.8°C. It was confirmed that the DSC extrapolated melting end temperature was higher than the CFT outflow start temperature, and partial melt extrusion could be achieved within the range of 203.5°C or more and less than 212.6°C. Fig.23 The measurement results of CFT and DSC are shown. <Example 36> Sample S22 (PPDO)

[0357] PPDO (as sample S22) of BMG Co., Ltd. was analyzed using CFT and DSC. The CFT outflow start temperature was 108.4°C, and the peak width of the high-temperature side crystalline melting peak obtained by DSC was about 77-124°C. The crystalline melting peak apex was 104.2°C and 113.1°C, the DSC extrapolated melting end temperature was 117.3°C, and the temperature at which the melting point peak reached the baseline was 123.6°C. It was confirmed that the DSC extrapolated melting end temperature was higher than the CFT outflow start temperature, and partial melt extrusion could be achieved in the range of 108.4°C or more and less than 117.3°C. Fig.24 The measurement results of CFT and DSC are shown.

[0358] <Example 37> Sample S23 (PBS)

[0359] PBS of Mitsubishi Chemical Corporation (as sample S23) was analyzed using CFT and DSC. The CFT outflow start temperature was 117.7°C, and the peak width of the crystal melting peak obtained by DSC was about 80 to 124°C. The apex of the crystal melting peak was 115.0°C, the DSC extrapolated melting end temperature was 119.5°C, and the temperature at which the melting point peak reached the baseline was 124.4°C. It was confirmed that the DSC extrapolated melting end temperature was higher than the CFT outflow start temperature, and partial melt extrusion could be achieved in the range of 117.7°C or more and less than 119.5°C. Fig.25 The measurement results of CFT and DSC are shown.

[0360] <Example 38> Sample S24 (PBSA)

[0361] PBSA of Mitsubishi Chemical Corporation (as sample S24) was analyzed using CFT and DSC. The CFT outflow start temperature was 87.3°C, and the peak width of the crystal melting peak obtained by DSC was about 55 to 98°C. The apex of the crystal melting peak was 90.1°C, the DSC extrapolated melting end temperature was 94.5°C, and the temperature at which the melting point peak reached the baseline was 98.4°C. It was confirmed that the DSC extrapolated melting end temperature was higher than the CFT outflow start temperature, and partial melt extrusion could be achieved in the range of 87.3°C or more and less than 94.5°C. Fig.26 The measurement results of CFT and DSC are shown.

[0362] <Comparative Example 15> Sample S25 (PCL)

[0363] Ingevity's polycaprolactone (PCL) (as sample S25) was analyzed using a flow tester (CFT) and DSC. The CFT outflow start temperature was 69.3°C, and the peak width of the crystalline melting peak obtained by DSC was about 35 to 70°C. The crystalline melting peak apex was 59.3°C, the DSC extrapolated melting end temperature was 63.7°C, and the temperature at which the melting point peak reached the baseline was 70.4°C. It was confirmed that the DSC extrapolated melting end temperature was lower than the CFT outflow start temperature, and if it was not in a completely molten state, it would not flow out. Fig. 27 The measurement results of CFT and DSC are shown.

Claims

1. A method for producing a polymer molded product, characterized in that: include: The step of melt-molding a polymer including lamellae having different lamellae thicknesses within a temperature range where a portion of the lamellae melt and flow while the remaining portion of the lamellae remain without melting, The temperature range is a range higher than the outflow start temperature obtained by the flow tester temperature increase method and lower than the extrapolated melting end temperature. The polymer is a copolymer containing 3-hydroxybutyric acid and 4-hydroxybutyric acid as monomer units, and the proportion of 4-hydroxybutyric acid is 5 mol% or more and 40 mol% or less.

2. The method according to claim 1, characterized in that: The method comprises cooling the melted polymer in air within a temperature range in which a part of the lamellae melt and flow and the other part of the lamellae remain without melting.

3. The method according to claim 1 or 2, characterized in that: The melt molding is molding by melt extrusion.

4. The method according to claim 1 or 2, characterized in that: The melt molding is performed by melt extrusion spinning.

5. The method according to claim 1 or 2, characterized in that: Perform melt molding once.

Citation Information

Patent Citations

  • Preparation of copolymer

    JP1989069622A

  • 3-hydroxybutylate polymer compound

    JP1991024151A

  • Removal of cell substance other than 3-hydroxybutyrate polymer from microorganism containing 3-hydroxybutyrate polymer

    JP1992061638B2

  • Production of copolymer