A method for producing low-cost, large-size high-alloy steel continuous casting round billets

By using the waste heat of small-sized high-temperature steel billets for heating and wrapping insulation, combined with the ultra-weak secondary cooling process, the problem of center cracks in large-sized continuous casting billets of high-alloy steel has been solved, improving material performance and production efficiency, and reducing costs and environmental impact.

CN115707537BActive Publication Date: 2024-10-18JIANGSU SHAGANG GROUP HUAIGANG SPECIAL STEEL CO LTD +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202211307962.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-25
Publication Date
2024-10-18
Estimated Expiration
2042-10-25

AI Technical Summary

Technical Problem

In steel smelting, severe central cracks often occur in large-size continuous casting billets of high-alloy steel, leading to an increase in yield and production costs. The existing annealing treatment cannot completely solve the problem.

Method used

The waste heat of small-sized high-temperature steel billets is used to heat the slow cooling pit, and the high-alloy steel large-sized round billets are fully wrapped and insulated. The annealing process is eliminated. The ultra-weak secondary cooling process and aerosol spray cooling are used to control the internal and external temperatures of the round billets. Uniformity, reducing thermal internal stress and phase change stress.

Benefits of technology

It significantly reduces the incidence of center cracks in large-size high-alloy steel continuous-cast round billets, improves the material's sawing and turning performance, increases production efficiency, avoids gas consumption and carbon dioxide emissions, and shortens the production cycle.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention discloses a method for producing a low-cost, large-size high-alloy steel continuous casting round billet, comprising the following steps: 1) a small-size round billet continuous casting machine produces a small-size low-carbon low-alloy steel continuous casting round billet, transports it into a slow cooling pit, and preheats the slow cooling pit; 2) after the small-size continuous casting round billet is put into the pit, the large-size high-alloy steel continuous casting round billet produced by the large-size continuous casting round billet casting machine immediately continues to be stacked upward layer by layer; 3) after the production of the large-size continuous casting round billet is completed, the small-size low-carbon low-alloy steel continuous casting round billet produced by another small-size round billet continuous casting machine continues to be stacked upward layer by layer, and covered with a heat preservation cover for heat preservation and slow cooling. The present invention cancels the annealing process, uses the residual heat of the small-size high-temperature steel billet to heat the slow cooling pit, and wraps the high-alloy steel large-size round billet in all directions for heat preservation, evens the internal and external temperatures of the high-alloy steel continuous casting round billet, reduces the temperature difference, reduces the thermal internal stress and phase change stress, and stably controls the large-size high-alloy steel continuous casting round billet center crack ≤1.0 level.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of steel smelting, relates to the production of large-size continuous casting round billets with large diameter round pipes, and particularly relates to a low-cost production method of large-size high-alloy steel continuous casting round billets. Background Art

[0002] With the continuous advancement of steel industry technology and the continuous casting technology, the inefficient and low yield rate die casting production method has been gradually replaced by the continuous casting production method, especially the low alloy steel billet is almost 100% produced by the continuous casting process. However, there is still a wide market demand for high alloy steel materials with large size, good hardenability, high strength and toughness and plasticity, good high and low temperature wear resistance, high temperature fatigue resistance and heat resistance, excellent cold and hot processing properties on many special equipment in special industries. However, due to the high alloy content, low thermal conductivity, large internal and external temperature difference, large structural stress, and strong crack sensitivity of high alloy steel billets, especially large size billets, the use of continuous casting process to produce large size high alloy steel continuous casting billets often results in serious center cracks leading to scrapping. The subsequent use of gas combustion heating for annealing cannot be completely avoided, which seriously affects the yield rate and production cost. Summary of the invention

[0003] In view of the deficiencies in the prior art, the purpose of the present invention is to provide a low-cost, large-size high-alloy steel continuous casting round billet production method, which eliminates the annealing process, uses the waste heat of small-size high-temperature steel billets to heat the slow cooling pit, and wraps the large-size high-alloy steel round billets for insulation in all directions, so as to even out the internal and external temperatures of the high-alloy steel continuous casting round billets, reduce the temperature difference, reduce the thermal internal stress and phase change stress, and stably control the center crack of the large-size high-alloy steel continuous casting round billets to ≤1.0 level.

[0004] The present invention is achieved through the following technical solutions:

[0005] A method for producing a low-cost, large-size high-alloy steel continuous casting round billet comprises the following steps:

[0006] 1) The adjacent small-size round billet continuous casting machine produces small-size low-carbon low-alloy steel continuous casting round billets at a high speed, and transports them into the slow cooling pit through hot delivery rollers + crane hoisting to preheat the slow cooling pit;

[0007] 2) After the small-sized continuous casting round billets are put into the pit, the large-sized high-alloy steel continuous casting round billets produced by the large-sized continuous casting round billet casting machine will immediately continue to be placed upward layer by layer;

[0008] 3) After the production of large-sized high-alloy steel continuous casting round billets is completed, the small-sized low-carbon low-alloy steel continuous casting round billets produced at a high casting speed by another adjacent small-sized round billet continuous casting machine continue to be stacked up layer by layer, and after entering the pit, they are covered with an insulation cover for insulation and slow cooling.

[0009] A further improvement of the present invention is:

[0010] The ultra-weak cooling secondary cooling process is adopted in the production of large-size high-alloy steel continuous casting round billets, and the specific water volume is controlled at 0.02~0.05l / kg.

[0011] Furthermore, only the foot roll section is retained in the second cooling section, and the foot roll section uses an aerosol nozzle to atomize water and then spray it onto the surface of the round billet for cooling.

[0012] Furthermore, in the step 1), the specification of the continuous casting round billet is Φ350-450 mm, the carbon content of the continuous casting round billet steel is ≤0.25 wt%, and the total alloy content does not exceed 1.50 wt%.

[0013] Furthermore, in the step 1), the pulling speed of the continuous casting round billet is 0.50-1.00 m / min, and the surface temperature of the round billet after entering the pit is ≥750°C.

[0014] Furthermore, in the step 1), the number of layers of the continuously cast round billets stacked is 4 to 5.

[0015] Furthermore, the time interval between the entry of medium and high alloy steel continuous casting round billets into the pit in step 2) and the completion of the entry of small and medium-sized continuous casting round billets into the pit in step 1) is controlled within 20 minutes, and the number of layers of medium and large-sized high alloy steel continuous casting round billets in step 2) is 3 to 8 layers.

[0016] Furthermore, in the step 2), the specification of the continuous casting round billet is Φ600-800 mm, and the steel type is a steel type with a total alloy content greater than 5wt%.

[0017] Furthermore, in the step 3), the pulling speed of the low-carbon low-alloy steel continuous casting round billet is 0.50-1.00 m / min, the surface temperature of the round billet after entering the pit is ≥750°C, and the number of layers sequentially stacked upward in a tight manner is 2-3 layers.

[0018] Furthermore, in the step 3), the insulation cover is opened after the slow cooling time is ≥ 200 hours after the insulation cover is put on, and the round billet is taken out of the pit after the surface temperature drops to 100°C.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] The present invention uses the waste heat of small-sized high-temperature steel billets to heat the slow cooling pit, and comprehensively wraps and insulates large-sized round billets of high-alloy steel, thereby evenly adjusting the internal and external temperatures of the high-alloy steel continuous casting round billets, reducing the temperature difference, lowering the thermal internal stress and phase change stress, and stably controlling the center crack of the large-sized high-alloy steel continuous casting round billets to ≤ level 1.0.

[0021] The present invention uses the waste heat of small-sized high-temperature steel billets to heat the slow cooling pit, so that the ambient temperature of the slow cooling pit is increased to 500-650°C, while the surface temperature of the small-sized high-temperature steel billets is maintained at 700-800°C. After the large-sized round billets of high-alloy steel are put into the pit, they are fully covered by the high-temperature small-sized steel billets for heat preservation. The surface temperature of the round billets gradually rises to 700-800°C, the surface temperature and the center temperature gradually tend to be consistent, and the temperature difference between the inside and outside is reduced from 150-250°C to below 20°C, and then they are kept warm in the slow cooling pit for more than 200 hours. In this process, the pearlite structure formed is uniform, the grains are fine, the interlamellar spacing is large, the surface and internal hardness of the large-sized high-alloy steel continuous casting round billet are reduced, the plasticity and toughness are improved, and the sawing and turning performance of the high-alloy steel round billet is significantly improved, so that the high-alloy round billet or steel can only be sawed and turned after annealing. The processing performance; because the temperature difference between the surface and the inside of the high-alloy high round billet is reduced, the cooling rate tends to be the same, so the thermal stress formed during the slow cooling process is significantly reduced, and at the same time, the cracking caused by the martensite generated by the high-alloy steel round billet when the cooling rate is fast is avoided; the solid-state diffusion of alloy elements is accelerated, the dendrite segregation is improved, the stability of the quenching hardness is improved, and the tendency of quenching cracking is reduced. Therefore, the present invention can make the large-sized high-alloy steel continuous casting round billet reach the performance and requirements after annealing.

[0022] The present invention reduces gas consumption and carbon dioxide emissions by eliminating the annealing process, while significantly improving production efficiency. The time from production to delivery of large-size high-alloy steel continuous casting round billets can be shortened by at least 10 days. DETAILED DESCRIPTION

[0023] Example 1

[0024] 1. An adjacent small-size round billet continuous casting machine produces Φ380mm 20 steel (total alloy content 0.90%) continuous casting round billets with a pulling speed of 0.58m / min. The round billets are transported into the slow cooling pit through hot roller conveyor + crane. The surface temperature of the round billets is 780℃ after entering the pit.

[0025] 2. After the number of layers of Φ380mm 20 steel in the slow cooling pit reaches 4, it will no longer be stacked in the pit. 15 minutes later, the Φ600mm high-alloy steel 12Cr5Mo (total alloy content is 6.30%) continuous casting round billets produced by the large-size continuous casting round billet casting machine will continue to be stacked layer by layer;

[0026] 3. The mold protection slag of peritectic steel is used in the production of Φ600mm 12Cr5Mo; the superheat is 20-28℃, the pulling speed is 0.25m / min, and the temperature of the straightening machine is 900℃; the ultra-weak cooling secondary cooling process is adopted, and the specific water volume is controlled to be 0.04l / kg; the crystallizer electromagnetic stirring current is 400A, the frequency is 1Hz; the end electromagnetic stirring current is 500A, the frequency is 3Hz;

[0027] 4. After the Φ600mm 12Cr5Mo production furnace 8 is finished, the Φ380mm 20 steel continuous casting round billets produced by another adjacent small-size round billet continuous casting machine continue to be placed upward layer by layer in a tight code;

[0028] 5. The surface temperature of the Φ380mm 20 steel continuous casting round billet is 775℃ after entering the pit. After the number of layers of tightening codes reaches 3, it will not continue to enter the pit. It will be covered with an insulation cover immediately. After the slow cooling time reaches 200 hours, the insulation cover will be opened. After the surface temperature of the round billet drops to 100℃, it will be taken out of the pit for inspection and grinding.

[0029] The Φ600mm 12Cr5Mo produced in this example has a central crack of level 0.5 and a central porosity of level 1.0. The low-magnification quality is good and meets the technical requirements of downstream users.

[0030] The Φ380mm 20 steel continuous casting round billet produced has good macrostructure and performance without any adverse effects.

[0031] Example 2

[0032] 1. An adjacent small-size round billet continuous casting machine produces Φ380mm 45 steel (total alloy content is 1.25%) continuous casting round billets with a pulling speed of 0.56m / min. The round billets are transported into the slow cooling pit through hot roller conveyor + crane. The surface temperature of the round billets after entering the pit is 770℃.

[0033] 2. After the number of layers of Φ380mm 45 steel in the slow cooling pit reaches 5, it will no longer be stacked in the pit. 14 minutes later, the Φ700mm high-alloy steel 30Cr2Ni4MoV (total alloy content is 6.10%) continuous casting round billets produced by the large-size continuous casting round billet casting machine will continue to be stacked layer by layer;

[0034] 3. Special high-nickel steel mold protection slag is used in the production of Φ700mm 30Cr2Ni4MoV; the superheat is 15-25℃, the pulling speed is 0.22m / min, and the temperature of the straightening machine is 895℃; the ultra-weak cooling secondary cooling process is adopted, and the specific water volume is controlled at 0.05l / kg; the crystallizer electromagnetic stirring current is 420A, the frequency is 1Hz; the terminal electromagnetic stirring current is 550A, the frequency is 3Hz;

[0035] 4. After the Φ700mm 30Cr2Ni4MoV production furnace 7 is put into the pit, the Φ380mm 45 steel continuous casting round billets produced by another adjacent small-size round billet continuous casting machine continue to be placed upward layer by layer in a tight code;

[0036] 5. The surface temperature of the Φ380mm 45 steel continuous casting round billet is 770℃ after entering the pit. After the number of layers of tightening codes reaches 3, it will not continue to enter the pit. It will be covered with an insulation cover immediately. After the slow cooling time reaches 200 hours, the insulation cover will be opened. After the surface temperature of the round billet drops to 100℃, it will be taken out of the pit for inspection and grinding.

[0037] The Φ700mm 30Cr2Ni4MoV produced in this example has a center crack of level 0 and a center porosity of level 1.0. The low-magnification quality is good and meets the technical requirements of downstream users.

[0038] The Φ380mm 45 steel continuous casting round billet produced has good macrostructure and performance without any adverse effects.

Claims

1. A method for producing large-scale high-alloy steel continuous casting round billets at low cost, characterized in that: The following steps are involved: 1) Adjacent small-size round billet continuous casting machines produce small-size low-carbon low-alloy steel continuous casting round billets at high casting speeds, transport them to a slow cooling pit via a hot roller conveyor and a crane, and preheat the slow cooling pit; wherein the low-carbon low-alloy steel continuous casting round billets have a specification of Φ350-450mm, a carbon content of ≤0.25 wt%, and a total alloy content of no more than 1.50 wt%; the casting speed of the low-carbon low-alloy steel continuous casting round billets is 0.50-1.00 m / min, and the surface temperature of the low-carbon low-alloy steel continuous casting round billets after entering the pit is ≥750°C; 2) After the small-sized continuous casting round billets are put into the pit, the large-sized high-alloy steel continuous casting round billets produced by the large-sized continuous casting round billet casting machine are immediately placed upward in layers; the high-alloy steel continuous casting round billets have a size of 600-800mm and a steel grade with a total alloy content greater than 5wt%; 3) After the production of large-sized high-alloy steel continuous casting round billets is completed, the small-sized low-carbon low-alloy steel continuous casting round billets produced at a high drawing speed by another adjacent small-sized round billet continuous casting machine continue to be stacked upward layer by layer, and are covered with insulation covers for insulation and slow cooling after entering the pit; wherein, the drawing speed of the low-carbon low-alloy steel continuous casting round billets is 0.50-1.00 m / min, the surface temperature of the low-carbon low-alloy steel continuous casting round billets after entering the pit is ≥750°C, and the number of layers stacked upward in sequence is 2-3 layers; after the insulation cover is covered and the slow cooling time is ≥200 hours, the insulation cover is removed, and the low-carbon low-alloy steel continuous casting round billets are removed from the pit after the surface temperature drops to 100°C.

2. The method for producing large-scale high-alloy steel continuous casting round billets at low cost according to claim 1, characterized in that: The ultra-weak secondary cooling process is used in the production of large-size high-alloy steel continuous casting round billets, and the water content is controlled at 0.02~0.05l / kg.

3. The method for producing large-scale high-alloy steel continuous casting round billets at low cost according to claim 1, characterized in that: In the step 1), the low-carbon low-alloy steel continuous casting round billets are stacked in 4 to 5 layers.

4. The method for producing large-scale high-alloy steel continuous casting round billets at low cost according to claim 1, characterized in that: The time interval between the time of putting the medium and high alloy steel continuous casting round billets into the pit and the time of finishing putting the medium and small size low carbon low alloy steel continuous casting round billets into the pit in step 1) is controlled within 20 minutes. The number of layers of the medium and large size high alloy steel continuous casting round billets in step 2) is 3 to 8.

5. The method for producing large-scale high-alloy steel continuous casting round billets at low cost according to claim 2, characterized in that: Only the foot roll section is retained in the secondary cooling section, which uses an aerosol nozzle to atomize water and spray it onto the surface of large-size high-alloy steel continuous casting round billets for cooling.

Citation Information

Patent Citations

  • Method for annealing medium-high carbon steel continuous steel blanks

    CN107447079A

  • Method of arc-shaped continuous casting production of high-carbon high-alloy ledeburite steel

    CN110616296A

  • Method for continuous casting of nickel-base alloy with large-specification round billet

    CN110951940A

  • Temperature control type energy-saving burial pit for annealing treatment by utilizing waste heat of continuous casting billet

    CN215879786U

  • Spring steel waste heat destressing softening annealing system

    CN216274293U