A method for activating the electrochromic properties of NiO thin films
By performing electrochemical reaction and heat treatment in alkaline aqueous electrolyte, the problem of NiO electrochromic film performance activation is solved, and multiple stable electrochromic cycles are realized, which improves the number of cycles and reduces costs, and promotes its engineering .
Patent Information
- Application Number
- CN202211231579.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-09
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2042-10-09
AI Technical Summary
The electrochromic properties of NiO electrochromic films are difficult to activate to the initial state in aqueous alkaline electrolytes, resulting in insufficient cycle stability and hindering its engineering application.
The electrochemical reaction is carried out in the alkaline aqueous electrolyte, the voltage is adjusted and heat treatment is performed, and Ni(OH)2 is generated and redecomposed to restore the NiO film to its initial state, achieving multiple stable electrochromic cycles.
It significantly increases the number of recycled NiO electrochromic films, reduces the cost of use, and promotes its popularity in engineering applications.
Smart Images

Figure CN115710494B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of electrochromic technology, and in particular to a method for activating the electrochromic performance of a NiO thin film. Background Art
[0002] Electrochromic materials can undergo stable and reversible color changes under the action of external DC voltage, and can maintain their color state when the external voltage is disconnected. This low-energy color controllable property makes it have very important application prospects in building energy-saving windows, smart displays, and camouflage. In the development of electrochromic technology, researchers use various means such as element doping and defect regulation to improve material properties in order to enhance the material's comprehensive electrochromic performance, such as light modulation range, color change response time, and cycle stability.
[0003] However, after thousands of cycles, the color-changing performance of the electrochromic film gradually decays and it is difficult to fade to the initial state, resulting in color-changing failure. This failure state will cause the electrochromic film to become a disposable product, which will seriously increase the cost of electrochromic products, thus seriously hindering the engineering application of electrochromic materials.
[0004] Therefore, it is urgent to develop a method to activate the performance of the failed electrochromic film, restore it to or close to the initial state, increase the number of cycles of the film, improve the cycle stability of the electrochromic film, and thus reduce the cost of using electrochromic devices. The color change mechanism of electrochromic films such as WO3 is simple and single, which is ion injection and extraction. Relevant personnel have used ion anti-capture to activate its color change performance, and restored the performance of the failed WO3 electrochromic film to the initial state, effectively increasing the number of cycles of WO3.
[0005] As a typical anode electrochromic material, NiO has an ultra-high light modulation range, fast electrochromic response time and high electrochromic efficiency in aqueous alkaline electrolytes, and has a stability of thousands of cycles. However, the electrochromic mechanism of NiO in aqueous alkaline electrolytes is relatively complex, and the simple ion anti-capture method cannot activate its electrochromic performance to the initial state, which has a serious adverse effect on the engineering application of NiO electrochromic films.
[0006] Therefore, it is necessary to develop a performance activation method for NiO electrochromic films, which is of great significance to promote the engineering application of NiO electrochromic films. Summary of the invention
[0007] The present invention proposes a method for activating the electrochromic performance of a NiO thin film, which can restore the performance of a failed NiO electrochromic thin film to an initial state so that it can perform a stable electrochromic cycle again. The overall method is simple and easy to operate.
[0008] In order to achieve the above object, the technical solution adopted by the present invention is: a method for activating the electrochromic performance of NiO thin film, comprising the following steps:
[0009] S1: placing the NiO film in an alkaline aqueous electrolyte under a three-electrode system to perform a color change cycle;
[0010] S2: Adjust the electrochemical method and voltage to continue the action for 2 hours or more;
[0011] S3: The film is taken out from the electrolyte, rinsed with deionized water to remove the residual electrolyte on the surface, dried, and then heat treated at 350° C. in an argon atmosphere for 3 hours;
[0012] S4: Cool the film to room temperature.
[0013] Preferably, in the three-electrode system, the NiO film is the working electrode, the graphite is the auxiliary electrode, the silver / silver chloride electrode is the reference electrode, and the voltage is +-1V.
[0014] Preferably, the alkaline aqueous electrolyte is 1M LiOH aqueous electrolyte, KOH aqueous electrolyte or NaOH aqueous electrolyte.
[0015] Preferably, the condition for starting step S2 is that when the transmittance of the NiO film in the faded state in step S1 decreases to any value between 50% and 35% of the initial faded state, step S2 is entered.
[0016] Preferably, the adjustment voltage in step S2 is a constant voltage of -1V.
[0017] Preferably, the condition for starting step S3 is that the step S3 is entered after the film is sufficiently faded.
[0018] Preferably, in step 3, Ni(OH)2 is thermally decomposed into NiO.
[0019] Preferably, the color change cycle in step S1 is performed more than 2000 times.
[0020] Preferably, the NiO thin film is prepared by the following steps:
[0021] S11: Using FTO conductive glass as the substrate, immerse the FTO film in a mixed solution of 5% NaOH: hydrogen peroxide = 30:1 for 5 hours;
[0022] S12: The FTO glass obtained in S11 was ultrasonically cleaned in acetone and alcohol solution for 30 minutes respectively, and dried with nitrogen gas;
[0023] S13: Place the above FTO glass in a polytetrafluoroethylene liner at an angle with the conductive surface facing downward, and then add the precursor solution;
[0024] S14: Place the polytetrafluoroethylene liner into a high-temperature reactor, seal it, and place it in an oil bath at 120°C for 4 hours;
[0025] S15: After the reaction is completed, the FTO glass is taken out after being cooled naturally to room temperature, and the surface of the film is rinsed with deionized water;
[0026] S16: After drying, heat treatment is performed at 350° C. for 3 h in an argon atmosphere to obtain a nano-sheet NiO electrochromic film.
[0027] Preferably, the precursor solution is formed by dissolving 0.125M nickel nitrate hexahydrate and 0.125M hexamethylenetetramine in deionized water and stirring the mixture thoroughly.
[0028] The present invention provides a method for activating the electrochromic performance of a NiO film, which restores the performance of the failed NiO electrochromic film to its initial state through an electrochemical reaction between an alkaline solution and the NiO film, followed by a heat treatment in an inert atmosphere, so that the film can be subjected to a stable electrochromic cycle again. This method can activate the film multiple times, greatly improving the recyclability of the NiO electrochromic film. This method fills the gap in the technology for activating the electrochromic performance of NiO films in alkaline electrolytes, and is of great significance for increasing the number of cycles of NiO electrochromic films, reducing the cost of engineering applications, and promoting the engineering application of electrochromic materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] The above and other objects, features and advantages of the exemplary embodiments of the present invention will become readily understood by reading the detailed description below with reference to the accompanying drawings. In the accompanying drawings, several embodiments of the present invention are shown in an exemplary and non-limiting manner, in which:
[0030] Figure 1 The schematic diagram of the curve of the transmittance during the activation process of the NiO electrochromic film performance in one embodiment is schematically shown. DETAILED DESCRIPTION
[0031] The principle and spirit of the present invention will be described below with reference to several exemplary embodiments. It should be understood that these embodiments are provided only to enable those skilled in the art to better understand and implement the present invention, and are not intended to limit the scope of the present invention in any way.
[0032] The method for activating the electrochromic performance of a NiO film provided by the present invention generates Ni(OH)2 and NiOOH through an electrochemical reaction between an alkaline solution and the NiO film, and then applies a reverse constant voltage for a certain period of time and performs a heat treatment to decompose the Ni(OH)2 into NiO by heat, thereby restoring the performance of the failed NiO electrochromic film to its initial state, so that the film can once again undergo a stable electrochromic cycle.
[0033] In one embodiment, a method for activating the electrochromic properties of a NiO thin film comprises the following steps:
[0034] S1: placing the NiO film in an alkaline aqueous electrolyte under a three-electrode system to perform a color change cycle; during the color change cycle of this step, as the electrochromic cycle proceeds, the NiO film undergoes a chemical reaction to gradually generate more NiOOH, so that the transmittance of the NiO film in the faded state gradually decreases;
[0035] S2: Adjust the electrochemical method, adopt the constant voltage method, adjust the voltage, and continue to act for 2 hours or more;
[0036] S3: The film is taken out from the electrolyte, rinsed with deionized water to remove the residual electrolyte on the surface, dried, and then heat treated at 350° C. in an argon atmosphere for 3 hours;
[0037] S4: Cool the film to room temperature.
[0038] Among them, in the three-electrode system, NiO film is the working electrode, graphite is the auxiliary electrode, silver / silver chloride electrode is the reference electrode, and the voltage is +-1v.
[0039] Wherein, the alkaline aqueous electrolyte is 1M LiOH aqueous electrolyte, KOH aqueous electrolyte or NaOH aqueous electrolyte. 1M represents 1 mol / L molar concentration, which refers to the amount of solute contained in a unit volume of solution. Preferably, the alkaline aqueous electrolyte is 1M LiOH aqueous electrolyte.
[0040] In one embodiment, if Figure 1 As shown, the condition for starting step S2 is that when the faded transmittance of the NiO film in step S1 decreases to any value between 50% and 35% of the initial faded transmittance, step S2 is entered. Optionally, when the faded transmittance decreases to 50%, 45%, 40%, 35% or other values, step S2 is entered. Preferably, when the faded transmittance decreases to 50%, step S2 is entered.
[0041] In one embodiment, the adjustment voltage in step S2 is a constant voltage of -1 V. In this step, the NiO film will continue to undergo chemical reactions to generate more Ni(OH)2, thereby continuing to fade.
[0042] In one embodiment, the condition for starting step S3 is that the film is sufficiently faded before entering step S3. When the film is sufficiently faded, the faded transmittance of the NiO film is restored to more than 80% of the initial faded transmittance, preferably more than 85%.
[0043] Among them, in step S3, Ni(OH)2 is thermally decomposed into NiO. In step S3, the film sample is taken out from the electrolyte, rinsed with deionized water to remove the residual electrolyte on the surface, and then dried and heat-treated at 350°C in an argon atmosphere for 3 hours, so that the Ni(OH)2 on the film sample is thermally decomposed into NiO and a new NiO film is regenerated.
[0044] Among them, in step S4, after the NiO film sample is cooled to room temperature, the NiO electrochromic film is again placed in the same electrochemical reaction system as step S1, that is, 1M LiOH aqueous solution is used as electrolyte, NiO film is used as working electrode, graphite electrode is used as auxiliary electrode, silver / silver chloride electrode is used as reference electrode, and the cycle voltage is +-1v. Electrochromic cycle is performed, and the results show that its electrochromic performance is restored to the initial state.
[0045] Preferably, the color change cycle in step S1 is repeated for more than 2000 times. Generally, the electrochromic performance of the NiO film restored to the initial state can withstand 2000 color change cycles in step S1. After that, the faded transmittance of the film will be greatly reduced, for example, it will drop rapidly from 70% of the faded transmittance to below 50%, or even to below 40%. At this time, the performance can be reactivated and reactivated by step S2 of the present invention.
[0046] According to subsequent practical application requirements, steps S1 to S4 may be repeated twice or more for the NiO film.
[0047] The NiO thin film electrochromic performance activation method of the present invention can be repeated for many times, which greatly increases the use frequency and life of the thin film, prolongs the product life cycle, reduces production costs, and is conducive to the widespread application of electrochromic products.
[0048] In one embodiment, the NiO electrochromic film is prepared by a constant temperature hydrothermal method, and the NiO film is prepared by the following steps:
[0049] S11: Using FTO conductive glass as a substrate, immersing the FTO film in a mixed solution of 5% NaOH: hydrogen peroxide = 30:1 for 5 hours to increase the bonding force between the film and the substrate; wherein, a 2cm*5cm FTO conductive glass can be used as the substrate;
[0050] S12: The FTO glass obtained in S11 was ultrasonically cleaned in acetone and alcohol solution for 30 minutes respectively, and dried with nitrogen gas;
[0051] S13: Place the above FTO glass in a polytetrafluoroethylene liner at an angle with the conductive surface facing downward, and then add the precursor solution;
[0052] S14: Place the polytetrafluoroethylene liner into a high-temperature reactor, seal it, and place it in an oil bath at 120°C for 4 hours;
[0053] S15: After the reaction is completed, the FTO glass is taken out after being cooled naturally to room temperature, and the surface of the film is rinsed with deionized water to remove residual impurities;
[0054] S16: After drying, heat treatment is performed at 350° C. for 3 h in an argon atmosphere to obtain a nano-sheet NiO electrochromic film.
[0055] Preferably, the precursor solution is formed by dissolving 0.125M nickel nitrate hexahydrate and 0.125M hexamethylenetetramine in deionized water and stirring the mixture thoroughly.
[0056] In a specific implementation process of the present invention, the activation of the NiO electrochromic film performance is achieved by the following steps, specifically:
[0057] The NiO electrochromic film prepared by the above constant temperature hydrothermal method was used as a sample, and a color change cycle was carried out in a three-electrode system in a 1M LiOH aqueous electrolyte, wherein the NiO film was the working electrode, graphite was the auxiliary electrode, and the silver / silver chloride electrode was the reference electrode. The voltage was +-1v. As the electrochromic cycle proceeded, the transmittance in the faded state gradually decreased until the transmittance in the faded state was only 50% or 35% of the initial faded state.
[0058] Then the electrochemical method was adjusted to continue the action at a constant voltage of -1v for 2 hours;
[0059] After the film is fully faded, the film sample is taken out from the electrolyte, rinsed with deionized water to remove the residual electrolyte on the surface, dried and heat treated at 350 °C for 3 hours in an argon atmosphere to decompose Ni(OH)2 into NiO.
[0060] After the sample was cooled to room temperature, the NiO electrochromic film was again placed in the same electrochemical reaction system as in step S1 above, i.e., 1M LiOH aqueous solution was used as electrolyte, NiO film was used as working electrode, graphite electrode was used as auxiliary electrode, silver / silver chloride electrode was used as reference electrode, and the cycle voltage was +-1V. The electrochromic cycle was performed, and the results showed that the electrochromic performance was restored to the initial state.
[0061] After 2000 cycles, the electrochromic performance of the film decayed again, also manifested as a decrease in the transmittance in the faded state;
[0062] Activate again using the same activation method as above, i.e. enter steps S2 to S4;
[0063] Afterwards, the electrochromic cycle is performed for the third time, and step S1 is repeated, and the electrochromic performance of the film shows the same electrochromic performance as the initial state.
[0064] This shows that this method can activate the film multiple times, greatly improving the recyclability of the NiO electrochromic film.
[0065] Although the above specific embodiments describe the spirit and principle of the present invention, it should be understood that the present invention is not limited to the disclosed specific embodiments, and the division of various aspects does not mean that the features in these aspects cannot be combined to benefit, and this division is only for the convenience of expression. The present invention is intended to cover various modifications and equivalent arrangements included in the spirit and scope of the attached claims.
Claims
1. A method for activating the electrochromic properties of NiO thin films, It is characterized in that The following steps are involved: S1: placing the NiO film in an alkaline aqueous electrolyte under a three-electrode system for color change cycle; in the three-electrode system, the NiO film is the working electrode, graphite is the auxiliary electrode, the silver / silver chloride electrode is the reference electrode, and the voltage is +-1v; when the faded transmittance of the NiO film in step S1 decreases to any value between 50% and 35% of the initial faded state, proceed to step S2; S2: Adjust the electrochemical method, adjust the voltage, and continue the action for 2 hours or more; wherein the adjusted voltage is a constant voltage of -1V; S3: The film is taken out from the electrolyte, rinsed with deionized water to remove the residual electrolyte on the surface, dried, and then heat treated at 350° C. in an argon atmosphere for 3 hours; S4: Cool the film to room temperature.
2. A method for activating the electrochromic properties of a NiO thin film according to claim 1, It is characterized in that The alkaline aqueous electrolyte is 1M LiOH aqueous electrolyte, KOH aqueous electrolyte or NaOH aqueous electrolyte.
3. The method for activating the electrochromic properties of a NiO thin film according to claim 1, It is characterized in that The condition for starting step S3 is that the film is sufficiently faded before entering step S3.
4. The method for activating the electrochromic properties of a NiO thin film according to claim 1, It is characterized in that In step S3, Ni(OH)2 is thermally decomposed into NiO.
5. The method for activating the electrochromic properties of a NiO thin film according to claim 1, It is characterized in that The color change cycle in step S1 is repeated more than 2000 times.
6. A method for activating the electrochromic properties of a NiO thin film according to claim 1, It is characterized in that The NiO film is prepared by the following steps: S11: Using FTO conductive glass as the substrate, immerse the FTO film in a mixed solution of 5% NaOH: hydrogen peroxide = 30:1 for 5 hours; S12: The FTO glass obtained in S11 was ultrasonically cleaned in acetone and alcohol solution for 30 minutes respectively, and dried with nitrogen gas; S13: Place the above FTO glass in a polytetrafluoroethylene liner at an angle with the conductive surface facing downward, and then add the precursor solution; S14: Place the polytetrafluoroethylene liner into a high-temperature reactor, seal it, and place it in an oil bath at 120°C for 4 hours; S15: After the reaction is completed, the FTO glass is taken out after being cooled naturally to room temperature, and the surface of the film is rinsed with deionized water; S16: After drying, heat treatment is performed at 350° C. for 3 h in an argon atmosphere to obtain a nano-sheet NiO electrochromic film.
7. A method for activating the electrochromic properties of a NiO thin film according to claim 6, It is characterized in that The precursor solution is formed by dissolving 0.125M nickel nitrate hexahydrate and 0.125M hexamethylenetetramine in deionized water and stirring the mixture thoroughly.
Citation Information
Patent Citations
Hydrothermal preparation method of multilayer nanosheet NiO electrochromic film based on gradient temperature
CN114933420A
High-performance and reliable electrochromic device and method for preparing the same
KR1020220048833A