Near infrared absorbing glass and near infrared cut-off filter
By using near-infrared absorption glass and multi-layer film structure composed of phosphate iron in the imaging element filter, the problems of insufficient visible light transmittance at night shooting and infrared interference of biometric elements are solved, and low-thickness and high-visible light transmission are achieved and high near-infrared cutoff, ensuring night shooting quality and imaging stability.
Patent Information
- Application Number
- CN202211017502.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2022-07-29
- Filing Date
- 2022-08-23
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2042-08-23
AI Technical Summary
The visible light transmittance of the existing imaging element filters is insufficient during night shooting, and the 940nm infrared ray of the biometric element interferes with the imaging quality, and it needs to be improved to improve the visible light transmittance and near-infrared cutoff capability.
A near-infrared absorbing glass consisting of 10 to 40% by weight of phosphorus and 5 to 35% by weight of iron, with a phosphorus-iron molar ratio between 1.75 to 5, combining a multi-layer film structure, including an absorbing dye layer and an anti-reflective film, Low-thickness near-infrared cutoff filters were designed to ensure that the 940nm light transmittance is less than 10%, and to maintain high visible light transmittance in the wavelength range of 420nm to 650nm.
Low thickness, high visible light transmission and high near-infrared cutoff are achieved, avoiding interference from biometric components on the camera elements, reducing the generation of glare and ghosting, and the spectral characteristics are stable at different light incident angles.
Smart Images

Figure CN115716706B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a near-infrared absorbing glass and a near-infrared cut-off filter comprising the same, and in particular to a near-infrared cut-off filter with low thickness, high visible light transmittance and high near-infrared cut-off. Background Art
[0002] As technology evolves, the market's image standards are gradually improving, and the optical characteristics of camera components are becoming more stringent. In addition to the previous miniaturization of light, thin, short, and small, the function of night shooting is also valued. Shooting in places with insufficient light naturally requires higher sensitivity to visible light. In order to meet the needs, the filter needs to be improved, especially the transmittance of visible light near the infrared region must be improved.
[0003] On the other hand, with the development of biometric technology, various products on the market, such as mobile phones, have begun to install biometric elements around the camera element. However, since the biometric element uses 940nm wavelength light as an infrared light source and due to the miniaturization of the device, the biometric element is often very close to the camera element. Therefore, the 940nm wavelength infrared light will seriously affect the imaging quality of the camera element, and it is necessary to improve the filter. Summary of the invention
[0004] To achieve the above-mentioned object, the first aspect of the present invention provides a near-infrared absorbing glass, which comprises 10 to 40 weight % of phosphorus and 5 to 35 weight % of iron, wherein the phosphorus to iron molar ratio (P / Fe) of the near-infrared absorbing glass is between 1.75 and 5, and the average transmittance of the near-infrared absorbing glass to light with a wavelength between 930 nm and 950 nm is less than 10%.
[0005] In at least one embodiment, the thickness of the near infrared absorbing glass is 0.3 mm or less. In another embodiment, the thickness of the near infrared absorbing glass is 0.2 mm or less.
[0006] In at least one embodiment, the near infrared absorbing glass has an average transmittance greater than 80% for light with a wavelength between 420 nm and 650 nm. In another embodiment, the near infrared absorbing glass has an average transmittance greater than 85% for light with a wavelength between 420 nm and 650 nm, for example when the thickness of the near infrared absorbing glass is less than 0.2 mm.
[0007] In at least one embodiment, the phosphorus to iron molar ratio is between 2 and 4, or between 2.5 and 3.5.
[0008] In at least one embodiment, the near infrared absorbing glass includes 10 wt % to 25 wt % iron.
[0009] In at least one embodiment, the near infrared absorbing glass further comprises 0.1 to 10 wt % silicon, 1 to 20 wt % aluminum, 0 to 10 wt % alkali metals, and a total of 0.1 to 20 wt % alkaline earth metals and other divalent elements.
[0010] In at least one embodiment, the alkaline earth metal and other divalent element are selected from at least one of the group consisting of magnesium, calcium, strontium, barium, and zinc. In another embodiment, the alkaline earth metal is magnesium and calcium, and the other divalent element is zinc.
[0011] In at least one embodiment, the semi-transmittance wavelength (T50%) of the near-infrared absorbing glass is greater than 700 nm, 730 nm, between 730 nm and 800 nm, or between 750 nm and 800 nm. Incidentally, in the present invention, the semi-transmittance wavelength (T50%) refers to the wavelength value (in nm) when the transmittance of light in the near-infrared region to the glass or filter is 50%.
[0012] In at least one embodiment, the near infrared absorbing glass has a transmittance of less than 10% for light having a wavelength of 940 nm.
[0013] In at least one embodiment, the near infrared absorbing glass has an average transmittance greater than 80% or greater than 85% for light with a wavelength of 420 nm to 650 nm.
[0014] The second aspect of the present invention also provides a near-infrared cutoff filter, which includes the near-infrared absorbing glass of the first aspect and a multilayer film structure, wherein the multilayer film structure is selected from at least one of the group consisting of a near-infrared absorbing film, an absorbing dye layer, an anti-reflection film and an infrared reflecting film, and the thickness of the near-infrared cutoff filter is less than 0.3 mm.
[0015] In at least one embodiment, the near infrared cutoff filter has a thickness of 0.2 mm or less.
[0016] In at least one embodiment, the near infrared cutoff filter has a half transmittance wavelength (T50%) of 630 nm or more, or between 640 nm and 660 nm.
[0017] In at least one embodiment, the near infrared cutoff filter has an optical density (OD) greater than 5 for light with a wavelength of 940 nm.
[0018] In at least one embodiment, the transmittance of the near infrared cutoff filter to light with a wavelength of 700 nm is less than 5%.
[0019] In at least one embodiment, the near infrared cutoff filter has an average transmittance greater than 85% for light with a wavelength of 420 nm to 650 nm.
[0020] In at least one embodiment, the near infrared absorbing film comprises a resin substrate, an organic metal complex and a dispersant, wherein the resin substrate is selected from at least one of the group consisting of silicone resin, epoxy resin, polyurethane, polyacrylate, polyolefin, polycarbonate, polycycloolefin and polyvinyl butyral.
[0021] In at least one embodiment, the absorbing dye layer is a near infrared absorbing dye layer, an ultraviolet absorbing dye layer, or a near infrared / ultraviolet composite absorbing dye layer.
[0022] In at least one embodiment, the absorbing dye layer includes an organic dye that absorbs near infrared rays, which is selected from at least one of the group consisting of azo compounds, diimmonium compounds, dithiol metal complexes, phthalocyanine compounds, squaraine compounds and cyanine compounds.
[0023] In at least one embodiment, the dye absorbing layer includes an organic dye that absorbs ultraviolet light, which is selected from at least one of the group consisting of ketone ultraviolet absorbers, benzimidazole ultraviolet absorbers, and triazine ultraviolet absorbers.
[0024] In at least one embodiment, the anti-reflection film and the infrared reflective film are made of a material selected from TiO 2 、SiO 2 , Y 2 O 3 MgF 2 、A1 2 O 3 , Nb 2 O 5 , AlF 3 、Bi 2 O 3 , Gd 2 O 3 、LaF 3 、PbTe、Sb 2 O 3 、SiO、SiN、Ta 2 Os, ZnS, ZnSe, ZrO 2 And Na 3 AlF 6 At least one of the groups.
[0025] The near-infrared absorbing glass of the present invention has excellent visible light transmittance and a wider near-infrared transmission band at a low thickness, and the semi-transmittance wavelength can be increased to within the range of 730 to 800 nm. Therefore, the near-infrared cut-off filter made of the near-infrared absorbing glass is particularly suitable for use in situations where light is insufficient (such as dim places, at night). The semi-transmittance wavelength of the commonly used blue glass (a type of near-infrared absorbing glass) on the market is usually between 620 and 635 nm, resulting in only a lower transmittance of visible light near the infrared region; and although the semi-transmittance wavelength of common heat-absorbing glass can be increased to 750 nm, the thickness of the heat-absorbing glass must be 0.5 to 3 mm to achieve the spectral characteristics of the present invention, and cannot be achieved with a low thickness as in the present invention.
[0026] On the other hand, although the semi-transmittance wavelength of the near-infrared absorbing glass of the present invention is increased, it can still effectively block near-infrared rays, for example, making the transmittance of 940nm light less than 10%. Subsequently, a multi-layer film structure is added to the near-infrared absorbing glass to enhance the near-infrared cutoff, so that the near-infrared cutoff filter of the final product has low thickness, high visible light transmittance, and high near-infrared cutoff. The optical density value of the final 940nm light can be greater than 5, greater than 6, or even greater than 7, which can avoid interference from the biometric recognition components near the camera element. Moreover, according to tests, the wavelength and transmittance offset at different light incident angles are small, which effectively reduces the generation of flare and ghost images.
[0027] In addition, since the near-infrared absorbing glass of the present invention itself has excellent optical properties, the complexity of the process can be improved in the subsequent process of adding a multi-layer film structure, such as relaxing the requirements for coating, thereby reducing the difficulty of the process. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 These are the transmittance spectra of Examples 1 to 5 and Comparative Example 1 of the near infrared absorbing glass of the present invention for light with a wavelength of 350 nm to 1100 nm.
[0029] Figure 2 These are the transmittance spectra of Example 6 and Comparative Example 2 of the near infrared cut filter of the present invention for light with a wavelength of 350 nm to 1100 nm.
[0030] Figure 3 These are the transmittance spectra of Example 7 and Comparative Example 3 of the near infrared cut filter of the present invention for light with a wavelength of 350 nm to 1100 nm.
[0031] Figure 4 The transmittance spectra of Example 8 and Comparative Example 4 of the near infrared cut filter of the present invention for light with a wavelength of 350nm to 1100nm.
[0032] Figure 5 The transmittance spectra of Example 9 and Comparative Example 5 of the near infrared cut filter of the present invention for light with a wavelength of 350nm to 1100nm. DETAILED DESCRIPTION
[0033] The specific implementation of the present invention is described below by specific implementation schemes, and those skilled in the art can easily understand the spirit, advantages and effects of the present invention based on the contents contained herein. However, the implementation scheme contained herein is not intended to limit the present invention, and the present invention can also be implemented or applied through other different implementation schemes, and the details contained herein can also be given different changes or modifications according to different viewpoints and applications without departing from the spirit of the present invention.
[0034] When it is stated in this document that “includes,” “comprising,” or “has” specific elements, unless otherwise stated, other elements, components, structures, regions, parts, devices, systems, steps, or connections may also be included, rather than excluding such other elements.
[0035] The terms "upper" and "lower" described herein are only used to facilitate the explanation of the specific embodiments of the present invention, and are not used to limit the scope of the present invention. The adjustment, interchange and change of their relative positions and relationships, without substantially changing the technical content of the present invention, should be regarded as the scope of the present invention.
[0036] Unless otherwise clearly stated herein, the singular forms "a", "an" and "the" described herein also include plural forms, and "or" and "and / or" described herein can be used interchangeably.
[0037] The numerical ranges described herein are inclusive and combinable, and any numerical value falling within the numerical ranges described herein can be used as the maximum value or the minimum value to derive a sub-range; for example, the numerical range of "phosphorus-iron molar ratio (P / Fe) is between 1.75 and 5" should be understood to include any sub-range between the minimum value 1.75 and the maximum value 5, such as: 1.75 to 4, 2 to 5, and 2.5 to 3.5, etc.; and, if a numerical value falls within the various ranges described herein (such as between the maximum and minimum values), it should be deemed to be included in the present invention.
[0038] The "phosphorus to iron molar ratio" described herein refers to the molar ratio of phosphorus obtained from phosphorus oxide in the raw material and iron obtained from iron oxide in the raw material when making glass. Taking Example 3 described below as an example, assuming that all oxides in the glass total 100 mol%, of which phosphorus pentoxide accounts for 58.90 mol and ferric oxide accounts for 14.32 mol, so the phosphorus element in phosphorus pentoxide accounts for 117.80 mol and the iron element in ferric oxide accounts for 28.64 mol. After calculation, it can be known that the phosphorus to iron molar ratio of Example 3 is 4.11.
[0039] The first aspect of the present invention is a near-infrared absorbing glass comprising 10 to 75 wt% of phosphorus and 5 to 35 wt% of iron, and in one embodiment, 10 to 40 wt% of phosphorus and 5 to 35 wt% of iron. More specifically, the near-infrared absorbing glass comprises 10 to 40 wt% of phosphorus, 0.1 to 10 wt% of silicon, 1 to 20 wt% of aluminum, 5 to 35 wt% of iron, 0 to 10 wt% of alkali metals, and 0.1 to 20 wt% of alkaline earth metals and other divalent elements in total. In practice, the phosphorus content can be, for example, 10, 15, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70 or 75% by weight; the silicon content can be, for example, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5, 6, 7, 8, 9 or 10% by weight; the aluminum content can be, for example, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19 or 20% by weight; the iron content can be 5 to 35%, 10 to 35% or 10 to 30% by weight, for example, 5, 6, 7, 8, 9 , 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, 31, 32, 33, 34 or 35 weight %; the content of alkali metals can be, for example, 0, 1, 2, 3, 4, 5, 6, 7, 8, 9 or 10 weight %; the total content of alkaline earth metals and other divalent elements can be, for example, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19 or 20 weight %.
[0040] In at least one embodiment, the present invention controls the phosphorus to iron molar ratio (P / Fe) of the near-infrared absorbing glass to be between 1.75 and 5, between 2 and 5, between 3 and 5, between 2 and 4, or between 2.5 and 3.5. For example, the phosphorus to iron molar ratio (P / Fe) can be 1.75, 1.78, 2, 2.25, 2.5, 2.51, 2.75, 2.98, 3, 3.05, 3.25, 3.5, 3.75, 4, 4.11, 4.25, 4.5, 4.75, 4.98 or 5, but is not limited thereto.
[0041] In the present invention, the alkali metal is selected from at least one of lithium, sodium and potassium. In some embodiments, the near infrared absorbing glass of the present invention does not substantially contain alkali metals. The alkaline earth metal and other divalent elements are selected from at least one of the group consisting of beryllium, magnesium, calcium, strontium, barium, zinc, cobalt, neodymium, germanium, tin and cerium, or the alkaline earth metal and other divalent elements are selected from at least one of the group consisting of magnesium, calcium, strontium, barium and zinc, or the alkaline earth metals are calcium and magnesium, and the other divalent element is zinc.
[0042] In at least one embodiment, the near infrared absorbing glass of the present invention may further include 0 to 10 wt % of boron, and the content of boron may be, for example, 0, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5, 6, 7, 8, 9 or 10 wt %. In at least one embodiment, the near infrared absorbing glass of the present invention does not substantially include boron.
[0043] In at least one embodiment, the near infrared absorbing glass of the present invention may further include other components. In at least one specific embodiment, the near infrared absorbing glass of the present invention substantially does not include fluorine. In at least one specific embodiment, the near infrared absorbing glass of the present invention substantially does not include copper.
[0044] In order to form the near infrared absorption glass with the above-mentioned specific components and specific content range, metaphosphates, carbonates, oxides, fluorides, etc. can be selected as glass raw materials. The metaphosphates include aluminum metaphosphate, lithium metaphosphate, sodium metaphosphate, potassium metaphosphate, magnesium metaphosphate, zinc metaphosphate and calcium metaphosphate; the carbonates include sodium carbonate, potassium carbonate, magnesium carbonate and calcium carbonate; the oxides include phosphorus pentoxide, ferric oxide (ferric oxide), ferrous oxide, aluminum oxide, zinc oxide, alkaline earth metal oxides such as calcium oxide and magnesium oxide, boron oxide, silicon dioxide and alkali metal oxides, etc. The process of converting the glass raw materials into glass can adopt a known method, such as mixing the glass raw materials in a certain proportion and placing them in a crucible, then placing the crucible in a reducing atmosphere furnace, and controlling the temperature of the reducing atmosphere furnace to be between 1200°C and 1500°C, then stirring the molten glass, clarifying it, flowing out of the mold and annealing it to finally obtain a homogenized phosphate glass.
[0045] The near infrared absorbing glass of the present invention has excellent visible light transmittance at a thin thickness (e.g., less than 0.3 mm), and the semi-transmittance wavelength falls between 730 nm and 800 nm. Such spectral characteristics can be achieved by controlling the phosphorus-iron molar ratio and / or the iron content in the glass. In at least one embodiment, the iron is divalent iron (blue-green), which can be provided by ferrous oxide glass raw material.
[0046] In the known technology, if the iron content in the glass is low, divalent iron can be directly formed in an isolated environment without using a reducing agent, and the glass manufacturing process can be carried out at a relatively low temperature (for example, below 1000°C). When the iron content in the glass increases, a small amount of reducing agent needs to be added to help reduce the iron ions to avoid the formation of trivalent iron. On the other hand, when the known technology increases the iron content according to demand, due to many difficulties in the process, the iron content is often limited to not more than 10 mol%. In other words, when the iron content is not more than 10 mol%, a good reduction effect can be achieved without adding a reducing agent or only adding a small amount of reducing agent, and it is easy to obtain a blue-green glass mainly containing divalent iron, rather than a brown glass containing trivalent iron. However, due to the low iron content, the glass thickness must reach a certain level (such as more than 1 mm) to have sufficient spectral characteristics.
[0047] With the demand for thinner glass, the iron content in the glass must be increased (such as an iron content higher than 10 mol%). However, in this case, the glass is not reducible enough, and the amount of reducing agent (such as charcoal, glucose, etc.) used is also increased. At this time, the ratio of glass raw materials must be adjusted with the reducing agent, and the amount of reducing agent used is also limited. Adding too much reducing agent will cause the glass to crystallize. In order to achieve a sufficient reduction effect, the process may be further adjusted, such as additionally giving a reducing gas (such as a nitrogen-hydrogen mixed gas) as a reducing agent to ensure that divalent iron is obtained. Moreover, the high iron content also requires the glass manufacturing process to be carried out at a higher temperature (such as above 1300°C), and the process requirements become higher. In addition, when the iron content in the glass is too high (for example, higher than 30 mol%), the glass is easy to crystallize and difficult to form, and even if a reducing agent is used, it cannot provide sufficient reducing power, so that a large amount of undesirable trivalent iron is obtained.
[0048] After many experiments, the present invention can finally stably obtain divalent iron under suitable glass raw material ratio and reducing conditions, so that the phosphorus iron molar ratio and / or iron content in the glass are within a specific range. In at least one embodiment, the iron content in the glass can be controlled to be above 10 mol%, above 12 mol%, or above 15 mol%, and below 30 mol%, below 26 mol%, or below 24 mol%, for example, 10, 11, 11.12, 12, 13, 14, 14.32, 15, 16, 17, 18, 19, 19.32, 20, 20.18, 21, 22, 23, 23.48, 24, 25, 26, 27, 28, 29, 29.98, 30 mol%.
[0049] In at least one embodiment, the near-infrared absorbing glass is thin, with a thickness of 0.3 mm or less, 0.2 mm or less, or 0.1 mm to 0.3 mm, such as 0.3, 0.25, 0.2, 0.15 or 0.1 mm, but not limited thereto. Generally speaking, the thinner the thickness of the near-infrared absorbing glass, the worse its near-infrared absorption effect, so the thickness of the near-infrared cut-off filter on the market is usually limited by the thickness of the near-infrared absorbing glass, and is between 0.3 and 0.5 mm. In contrast, the near-infrared absorbing glass of the present invention still has excellent optical properties at a low thickness.
[0050] The near infrared absorbing glass of the first aspect of the present invention has excellent optical properties, and its semi-transmittance wavelength (T50%) is closer to the near infrared region than the known blue glass. The semi-transmittance wavelength (T50%) of the near infrared absorbing glass of the present invention is at least 700nm, and can be between 730nm and 800nm, or between 750nm and 800nm, such as 730, 735, 740, 745, 750, 755, 760, 765, 770, 775, 780, 785, 790, 795 or 800nm, but not limited thereto. Therefore, the light in the entire visible light region is maintained at a high transmittance, and the high transmittance can be represented by an average transmittance of more than 80% or more than 85% for light with a wavelength of 420nm to 650nm, such as 81%, 82%, 83%, 84%, 85%, 86%, 87%, 88%, 89% or 90%, but not limited thereto.
[0051] Although the semi-transmittance wavelength (T50%) of the near-infrared absorbing glass of the present invention is high, it still has a good near-infrared absorbing ability. Specifically, the transmittance of the near-infrared absorbing glass of the present invention to the light with a wavelength of 940nm is less than 10%, and the average transmittance to the light with a wavelength of 930nm to 950nm is less than 10%, for example, 9.5%, 9%, 8.5%, 8%, 7.5%, 7%, 6.5%, 6%, 5.5%, 5%, 4.5%, 4%, 3.5%, 3%, 2.5%, 2%, 1.5% or 1%, but not limited thereto.
[0052] A second aspect of the present invention provides a near infrared cut filter, which is made of the near infrared absorbing glass of the first aspect.
[0053] The near infrared cutoff filter of the second aspect of the present invention comprises the near infrared absorbing glass and a multilayer film structure, wherein the multilayer film structure is at least one selected from the group consisting of a near infrared absorbing film, an absorbing dye layer, an anti-reflection film and an infrared reflecting film.
[0054] The multilayer film structure is formed on the surface of the near-infrared absorbing glass, for example, on one surface of the near-infrared absorbing glass, or on both surfaces of the near-infrared absorbing glass. Moreover, the multilayer film structure can be formed by known methods such as dip coating, spray coating, spin coating, blade coating, roller coating, evaporation or sputtering.
[0055] In at least one embodiment, the thickness of the near-infrared cutoff filter is less than 0.3 mm, less than 0.2 mm, or 0.1 mm to 0.3 mm, such as 0.3, 0.25, 0.2, 0.15 or 0.1 mm, but not limited thereto. Since the near-infrared absorbing glass has excellent optical properties, the multilayer film structure can be thinned or part of the multilayer film structure can be omitted, so that the near-infrared cutoff filter still has excellent optical properties at a low thickness.
[0056] In at least one embodiment, the semi-transmittance wavelength (T50%) of the near-infrared cutoff filter is between 640nm and 660nm, such as 640, 641, 642, 643, 644, 645, 646, 647, 648, 649, 650, 651, 652, 653, 654, 655, 656, 657, 658, 659 or 660nm, but not limited thereto. Because the semi-transmittance wavelength of the near-infrared absorbing glass is high, when the spectrum is improved by a multilayer film structure, the semi-transmittance wavelength of the near-infrared cutoff filter is also high, so that the transmittance in the visible light region is significantly improved. Specifically, the average transmittance of the near-infrared cutoff filter for light with a wavelength of 420nm to 650nm is greater than 85%, such as 86%, 87%, 88%, 89% or 90%, but not limited thereto.
[0057] In at least one embodiment, the optical density value (OD) of the near-infrared cutoff filter for light with a wavelength of 940 nm is greater than 5, greater than 6, or greater than 7, such as 5.1, 5.2, 5.3, 5.4, 5.5, 5.6, 5.7, 5.8, 5.9, 6, 6.5, 7, 7.5 or 8, but not limited thereto. In at least one embodiment, the transmittance of the near-infrared cutoff filter for light with a wavelength of 700 nm is less than 5%, such as 4.5%, 4%, 3.5%, 3%, 2.5%, 2%, 1.5% or 1%, but not limited thereto. The above shows that the near-infrared cutoff filter of the present invention has excellent infrared cutoff capability.
[0058] In at least one embodiment, the near-infrared absorbing film comprises a resin substrate, an organic metal complex and a dispersant, wherein the resin substrate is selected from at least one of the group consisting of silicone resin, epoxy resin, polyurethane, polyacrylate, polyolefin, polycarbonate, polycycloolefin and polyvinyl butyral. The near-infrared absorbing film can absorb near-infrared rays to further reduce the transmittance of near-infrared rays.
[0059] In at least one embodiment, the absorbing dye layer is a near-infrared absorbing dye layer, an ultraviolet absorbing dye layer or a near-infrared / ultraviolet composite absorbing dye layer. The absorbing dye layer includes an organic dye that absorbs near-infrared light, which is selected from at least one of the group consisting of azo compounds, diimmonium compounds, dithiol metal complexes, phthalocyanine compounds, squaraine compounds, and cyanine compounds, which can further reduce the transmittance of near-infrared light. The absorbing dye layer includes an organic dye that absorbs ultraviolet light, which is selected from at least one of the group consisting of ketone ultraviolet absorbers, benzimidazole ultraviolet absorbers, and triazine ultraviolet absorbers, which can reduce the transmittance of near-ultraviolet light.
[0060] In at least one embodiment, the anti-reflection film and the infrared reflective film are made of a material selected from TiO 2 、SiO 2 , Y 2 O 3 MgF 2 、A1 2 O 3 , Nb 2 O 5 , AlF 3 、Bi 2 O 3 , Gd 2 O 3 、LaF 3 、PbTe、Sb 2 O 3 、SiO、SiN、Ta 2 Os, ZnS, ZnSe, ZrO 2 And Na 3 AlF 6 In another embodiment, TiO 2 and SiO 2 It is obtained by alternately evaporating with a thickness of 10nm to 200nm.
[0061] The following describes embodiments of the present invention. Those skilled in the art can easily understand other advantages and effects of the present invention from the contents described in this specification.
[0062] Example
[0063] Please refer to Table 1 and Table 2. Table 1 shows the proportion of the main element oxides in the glass (expressed in weight % and mole %), and Table 2 shows the proportion of the main elements in the glass (expressed in weight %). Weigh 100 to 300 g of the raw materials such as phosphates, metaphosphates, oxides, etc. corresponding to the glass components in the table in proportion, and mix them thoroughly to obtain a glass raw material composition. The glass raw material composition is placed in a crucible, and then the crucible is placed in a reducing atmosphere furnace, and the temperature of the reducing atmosphere furnace is controlled to be between 1200°C and 1500°C. Thereafter, the molten glass is stirred, clarified, flowed out of the mold and annealed to obtain the near-infrared absorbing glass of the embodiment and the comparative example. Taking Example 3 as an example, the thickness of the prepared near-infrared absorbing glass is 0.2 mm. According to Table 1, the main element oxides of the glass in Example 3 include 65.33% by weight of phosphorus pentoxide P 2 O 5 , 0.94 wt% silicon dioxide SiO 2 , 11.15 wt% aluminum oxide Al 2 O 3 , 17.87 wt% of ferric oxide Fe 2 O 3 , 1.21 wt% calcium oxide CaO, 1.57 wt% magnesium oxide MgO, 1.93 wt% zinc oxide ZnO (alkaline earth metal oxides and other divalent element oxides total 4.71 wt%). In addition, in Example 3, phosphorus pentoxide accounts for 58.9 mol%, so the phosphorus element is 117.80 mol, and ferric oxide accounts for 14.32 mol%, so the iron element is 28.64 mol, and the phosphorus-iron molar ratio can be calculated to be 4.11. On the other hand, according to Table 2, the main elements of the glass of Example 3 include 28.51 wt% phosphorus, 0.5 wt% silicon, 6.05 wt% aluminum, 12.78 wt% iron, 0.89 wt% calcium, 0.97 wt% magnesium, and 1.57 wt% zinc (alkaline earth metals and other divalent elements total 3.43 wt%). The glass components of other embodiments 1, 2, 4, 5 and comparative example 1 are also as shown in Table 1 and Table 2, and the content ratio of phosphorus and iron is specially adjusted, wherein the definition and calculation method of phosphorus-iron molar ratio are the same as those of the above-mentioned embodiment 3, and will not be repeated here. The thickness and phosphorus-iron molar ratio of each embodiment and comparative example are shown in Table 3, wherein the phosphorus-iron molar ratio of embodiment 1 is about 1.78 and the thickness is 0.1 mm; the phosphorus-iron molar ratio of embodiment 2 is about 2.98 and the thickness is 0.15 mm; the phosphorus-iron molar ratio of embodiment 4 is about 4.98 and the thickness is 0.3 mm; the phosphorus-iron molar ratio of embodiment 5 is about 2.51 and the thickness is 0.2 mm; comparative example 1 does not add iron and the thickness is 0.2 mm. Figure 1The transmittance spectrum of the near infrared absorbing glass embodiment of the present invention is shown, and the glass thickness and spectrum data are shown in Table 4.
[0064] Table 1
[0065]
[0066] Table 2
[0067]
[0068] Table 3
[0069] Example 1 Example 2 Example 3 Example 4 Example 5 Comparative Example 1 thickness 0.1mm 0.15mm 0.2mm 0.3mm 0.2mm 0.2mm Phosphorus to Iron Molar Ratio 1.78 2.98 4.11 4.98 2.51 N / A
[0070] Table 4
[0071] Example 1 Example 2 Example 3 Example 4 Example 5 Comparative Example 1 Glass thickness(mm) 0.1 0.15 0.2 0.3 0.2 0.2 420-650nm Tavg% 86.91 87.29 86.91 89.01 83.30 79.57 650nm T% 83.66 84.56 83.52 82.54 77.48 39.05 T50% 779.91 784.91 784.19 799.41 731.21 632.00 930-950nm Tavg% 8.22 8.16 8.53 6.84 0.95 5.62 940nm T% 8.29 8.22 8.60 6.90 0.96 5.58
[0072] Depend on Figure 1 As shown in Table 4, the average transmittance values of Examples 1 to 5 in the visible light region are greater than those of Comparative Example 1. The reason is that the semi-transmittance wavelength of Comparative Example 1 is only as low as 632.00nm, and its transmittance is greatly attenuated after 550nm, that is, the visible light transmittance of 550nm to 760nm is poor; while the semi-transmittance wavelength of Examples 1 to 5 is as high as above 730nm, and the spectrum shows that the transmittance in the visible light region is almost maintained at a plateau shape of more than 80%, and only slowly decreases after 650nm.
[0073] On the other hand, although the semi-transmittance wavelength of the near-infrared absorbing glass of the present invention is as high as 730nm or more, the transmittance of light with a wavelength of 940nm can still be reduced to less than 10%, which is equivalent to Comparative Example 1 and will not increase the burden of the subsequent multilayer film structure.
[0074] Figures 2 to 5 It is the transmittance spectrum of the embodiment of the near infrared cut-off filter of the present invention, which is obtained by adding a near infrared absorbing film, an absorbing dye layer, an anti-reflection film and an infrared reflecting film on the surface of the near infrared absorbing glass.
[0075] Table 5
[0076]
[0077] Depend on Figures 2 to 5 As shown in Table 5, the near infrared cut-off filters of Examples 6 to 9 have better transmittance in the visible light region, because the semi-transmittance wavelengths of Examples 6 to 9 are between 648 and 650 nm, and their visible light transmittances between 550 nm and 700 nm are better than those of Comparative Examples 2 to 5. The near infrared cut-off properties of Examples 6 to 9 are equivalent to those of Comparative Examples 2 to 5, and are not deteriorated by increasing the semi-transmittance wavelength.
[0078] Observe again Figure 5 Example 9 and Comparative Example 5 show that visible light illuminates the near-infrared cutoff filter at an angle of 0 and 30 degrees, respectively. Regardless of Example 9 or Comparative Example 5, the similarity of the two angle spectra is extremely high, that is, the wavelength shift and transmittance shift are low, which can reduce the possibility of glare and ghosting during imaging. It can be seen that the near-infrared cutoff filter of the present invention is not degraded by increasing the semi-transmittance wavelength of the near-infrared absorbing glass.
Claims
1. A near infrared absorbing glass, characterized in that: include: 10 to 40% by weight phosphorus; 5 to 35% by weight iron; 3 to 20 wt. % aluminum; 0.1 to 10 wt. % silicon; 0 to 10% by weight of alkali metal; as well as 0.1 to 20% by weight of alkaline earth metals and other divalent elements, The molar ratio of phosphorus to iron in the near-infrared absorbing glass is between 1.75 and 5, and the average transmittance of the near-infrared absorbing glass to light with a wavelength between 930 nm and 950 nm is less than 10%.
2. The near infrared absorbing glass according to claim 1, wherein The near infrared absorbing glass has a thickness of 0.3 mm or less.
3. The near infrared absorbing glass according to claim 2, characterized in that: The near infrared absorbing glass has a thickness of 0.2 mm or less.
4. The near infrared absorbing glass according to claim 1, wherein The near-infrared absorption glass has an average transmittance greater than 80% for light with a wavelength between 420nm and 650nm.
5. The near infrared absorbing glass according to claim 3, wherein: The near-infrared absorption glass has an average transmittance greater than 85% for light with a wavelength between 420nm and 650nm.
6. The near infrared absorbing glass according to claim 1, wherein: The phosphorus-iron molar ratio is between 2 and 4.
7. The near infrared absorbing glass according to claim 6, wherein: The phosphorus-iron molar ratio is between 2.5 and 3.
5.
8. The near infrared absorbing glass according to claim 1, wherein The near infrared absorbing glass includes 10 to 25 wt % of iron.
9. The near infrared absorbing glass according to claim 1, wherein The near infrared absorbing glass has a semi-transmittance wavelength of 700 nm or more.
10. The near infrared absorbing glass according to claim 9, wherein The semi-transmittance wavelength of the near-infrared absorption glass is between 730nm and 800nm.
11. The near infrared absorbing glass according to claim 1, wherein The alkaline earth metal and other divalent elements are at least one selected from the group consisting of magnesium, calcium, strontium, barium and zinc.
12. The near infrared absorbing glass according to claim 1, wherein The alkaline earth metals are magnesium and calcium, and the other divalent element is zinc.
13. A near infrared cut-off filter, characterized in that: It comprises the near-infrared absorbing glass according to claim 1 and a multilayer film structure, wherein the multilayer film structure is selected from at least one of the group consisting of a near-infrared absorbing film, an absorbing dye layer, an anti-reflection film and an infrared reflecting film, and the thickness of the near-infrared cutoff filter is less than 0.3 mm. 14 . The near infrared cut filter according to claim 13 , wherein the thickness of the near infrared cut filter is 0.2 mm or less. 15 . The near infrared cut filter according to claim 13 , wherein a half-transmittance wavelength of the near infrared cut filter is 630 nm or longer.
16. The near infrared cut filter according to claim 15, characterized in that: The semi-transmittance wavelength of the near infrared cut-off filter is between 640nm and 660nm.
17. The near infrared cut filter according to claim 13, characterized in that: The optical density value of the near-infrared cutoff filter for light with a wavelength of 940 nm is greater than 5.
18. The near infrared cut filter according to claim 13, characterized in that: The transmittance of the near infrared cut-off filter to light with a wavelength of 700 nm is less than 5%.
19. The near infrared cut filter according to claim 13, characterized in that: The average transmittance of the near infrared cut-off filter to light with a wavelength of 420nm to 650nm is greater than 85%.
Citation Information
Patent Citations
Lead-free low-melting-point glass with excellent comprehensive performance and application method thereof
CN104445920A
Optical product for near infrared cut-off filter included in camera module, and near infrared cut-off filter for camera module, comprising same
CN110114704A
Ultraviolet, visible and near-infrared light absorbing glass as well as preparation method and application thereof
CN110156317A
Far infrared light absorbing material
JP1994346044A
Infrared absorption glass
JP2009263190A