A polyurethane-polyurea dispersion and its preparation method and use
By introducing the reaction of 2-hydrazinoethanol and specific components in the prepolymerization stage, a polyurethane-polyurea aqueous dispersion is prepared, which solves the problem of insufficient performance of water-based synthetic leather and achieves the synthesis of soft feel, smooth touch and high performance. The leather surface layer reduces costs and promotes large-scale promotion.
Patent Information
- Application Number
- CN202211442884.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-18
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-11-18
AI Technical Summary
It is difficult for existing water-based synthetic leather to achieve a soft, elastic, plump feel and smooth touch at the same time. At the same time, due to the limitations of high-cost raw materials and preparation methods, its performance is not as good as solvent-based polyurethane, which affects large-scale promotion.
2-Hydrazinoethanol is introduced in the prepolymerization stage to avoid side reactions and residual monomer residues. Semi-crystalline polyester polyol, isocyanate, hydrophilic compounds and polyamines are used to prepare polyurethane through specific reaction and dispersion steps. -Polyurea aqueous dispersion for synthetic leather topcoats.
It has a softer feel, smooth touch, higher alcohol rubbing resistance, wet friction resistance, higher tensile strength and elongation, which reduces the cost of synthetic leather and improves its performance.
Smart Images

Figure BDA0003948836680000111 
Figure BDA0003948836680000121
Abstract
Description
Technical Field
[0001] The invention relates to the field of polyurethane, specifically to the field of synthetic leather, and more specifically to a polyurethane-polyurea aqueous dispersion and a preparation method and application thereof. Background Art
[0002] At present, most of the synthetic leathers on the market are solvent-based. A large amount of organic solvents such as dimethylformamide are used in the production process, which will cause great harm to the environment and personnel. Waterborne polyurethane uses water as a dispersion medium, which can effectively avoid environmental pollution and damage to personnel health, so it is widely used in the field of synthetic leather manufacturing. However, due to the limitations of preparation technology, waterborne synthetic leather cannot have both a soft and elastic feel and a smooth touch. Therefore, developing a soft and non-sticky polyurethane-polyurea aqueous dispersion has become an urgent problem to be solved in this industry.
[0003] CN105968309B discloses a waterborne polyurethane resin for synthetic leather fabrics, which uses polycarbonate polyol and polysiloxane polyol as raw materials, and the prepared synthetic leather fabric has soft performance and smooth feel. However, due to the high prices of polycarbonate polyol and polysiloxane polyol, the cost of the prepared synthetic leather is extremely high, which affects the large-scale promotion and use of the industry.
[0004] Because of the differences in preparation method and structure between polyurethane-polyurea aqueous dispersion and solvent-based polyurethane, the molecular weight of the obtained resin varies greatly, resulting in its various properties (strength, elongation, chemical resistance) being inferior to those of solvent-based polyurethane. How to improve the performance of the synthetic leather surface layer prepared by polyurethane-polyurea aqueous dispersion is the focus and hot spot of research in this technical field.
[0005] At present, water-based polyurethane resins prepared by adding raw materials such as polycarbonate polyols and polysiloxane polyols can balance and improve the solvent resistance, feel, strength and other properties of the synthetic leather surface layer to a certain extent. However, the amount of addition needs to be increased to achieve the above properties, resulting in a high cost for the final synthetic leather product, which is not conducive to large-scale promotion. Summary of the invention
[0006] The invention provides a polyurethane-polyurea dispersion and a preparation method and use thereof. Introducing 2-hydrazine ethanol in the prepolymerization stage without solvent can make it react completely while avoiding side reactions with carbonyl groups in the solvent and residual monomers. The dispersion is used for the surface layer of synthetic leather and has a softer feel, a smoother touch, higher alcohol resistance, wet friction resistance, higher tensile strength and elongation.
[0007] To achieve the above object, the present invention adopts the following technical solutions:
[0008] A polyurethane-polyurea aqueous dispersion, the preparation raw materials of which include the following components:
[0009] a) a polyol having a functionality of 2 to 4, which contains not less than 80 wt% of a semi-crystalline polyester polyol;
[0010] b) isocyanates;
[0011] c) a hydrophilic compound component, wherein the hydrophilic group of the hydrophilic compound comprises one or more of an ionic group and a potential ionic group, and the hydrophilic compound contains 2 to 3 groups reactive with NCO; the ionic group is preferably a carboxylate ion, the potential ionic group is preferably a carboxyl group; the group reactive with NCO is preferably a hydroxyl group and / or an amino group;
[0012] d) an optional small molecule alcohol chain extender different from component a);
[0013] e) a compound which ionizes component c);
[0014] f) polyamines having an average molecular weight of less than 500 g / mol;
[0015] g) optionally a hydrazine compound having a molecular weight of less than 500 g / mol and containing at least one hydroxyl group.
[0016] The number average molecular weight of the component a) of the present invention is 100-15000, preferably 300-10000, more preferably 400-8000; the functionality is preferably 2-3, more preferably 2.
[0017] The semi-crystalline polyester polyol of the present invention is obtained by esterification of adipic acid, phthalic acid (including one or more of isophthalic acid, phthalic acid, and phthalic anhydride) and a small molecule diol, wherein the molar ratio of adipic acid to phthalic acid is 2.1 to 10: 1. The small molecule diol is one or more of 1,4-butanediol and 1,6-hexanediol.
[0018] The semi-crystalline polyester polyol of the present invention is preferably a polyester having a molar ratio of adipic acid to isophthalic acid of 2.1 to 10:1, esterified with 1,4-butanediol, and having a number average molecular weight of 1800 to 2200 (preferably 2000).
[0019] In the component a) of the present invention, the polyol used together with the semi-crystalline polyester polyol is preferably one or more of polyester polyol, polycaprolactone polyol, polycarbonate polyol, polyoxypropylene ether diol and polytetramethylene glycol.
[0020] Preferably, the polyester polyol is a linear polyester diol or a slightly branched polyester diol, which can be obtained, for example, by dehydration condensation of carboxylic acids and / or anhydrides such as aliphatic, alicyclic, aromatic dicarboxylic acids or polycarboxylic acids or their corresponding anhydrides and polyols by known means, and examples of the carboxylic acids and / or anhydrides include but are not limited to succinic acid, methyl succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, nonane dicarboxylic acid, decanedicarboxylic acid, terephthalic acid, isophthalic acid, phthalic acid, tetrahydrophthalic acid, hexahydrophthalic acid, cyclohexane dicarboxylic acid, Acid, maleic acid, fumaric acid, malonic acid, trimellitic acid, phthalic anhydride, trimellitic anhydride, succinic anhydride one or more; Examples of the polyols include, but are not limited to, ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,3-butanediol, 2,3-butanediol, 1,5-pentanediol, 1,6-hexanediol, 2,2-dimethyl-1,3-propanediol, 1,4-dihydroxycyclohexane, 1,4-dihydroxymethylcyclohexane, 1,8-octanediol, 1,10-decanediol, 1,12-dodecanediol one or more. Optionally, a polyol with higher functionality, such as trimethylolpropane, glycerol or pentaerythritol, may be added. Alicyclic, aromatic di- and / or polyhydroxy compounds are also suitable as polyols for preparing the polyester polyols. Also included are fatty acid-containing polyesters having an average OH functionality of about 2 and including transesterification products of castor oil with oils other than castor oil. Preferred are polyester polyols containing isophthalic acid and / or terephthalic acid and / or adipic acid, and neopentyl glycol, ethylene glycol, butanediol and / or hexanediol as structural components.
[0021] The polyester polyol can also be a homopolymer or copolymer of lactone, which can be obtained by ring-opening lactone with a suitable di- and / or higher-functional polyol with a number average molecular weight of 1000 to 4000 g / mol. Among them, lactones such as butyrolactone, ε-caprolactone, methyl-ε-caprolactone and their mixtures, polyols such as the above-mentioned polyols with a number average molecular weight of 1000 to 4000 g / mol as structural components of polyester polyols. Preferably, 1,4-butanediol, 1,6-hexanediol, 2,2-dimethyl-1,3-propanediol or their mixtures, linear polyester polyols of ring-opened ε-caprolactone are used, and polyε-caprolactone polyols are more preferably used.
[0022] The polycarbonate polyol having hydroxyl groups prepared by using diols and carbonates is also suitable. The diols are preferably 1,4-butanediol and 1,6-hexanediol, and the carbonates can be diaryl carbonates and dialkyl carbonates. The diaryl carbonates include diphenyl carbonates, and the dialkyl carbonates include dimethyl carbonates.
[0023] In the component a) of the present invention, the preferred polyoxypropylene ether diol is a polyoxypropylene ether diol having a number average molecular weight of 2000 to 8000 g / mol.
[0024] The component b) of the present invention is one or more of aromatic, aliphatic and alicyclic polyisocyanates, preferably one or more of aromatic, aliphatic and alicyclic polyisocyanates having at least two isocyanate groups.
[0025] Preferably, the component b) is a diisocyanate Y(NCO)2, wherein Y represents a divalent aliphatic hydrocarbon group containing 4 to 12 carbon atoms, a divalent alicyclic hydrocarbon group containing 6 to 15 carbon atoms, a divalent aromatic hydrocarbon group containing 6 to 15 carbon atoms or a divalent aromatic aliphatic hydrocarbon group containing 7 to 15 carbon atoms. Suitable diisocyanates may be tetramethylene diisocyanate, pentamethylene diisocyanate, hexamethylene diisocyanate, dodecamethylene diisocyanate, 1,4-cyclohexane diisocyanate, isophorone diisocyanate, 4,4′-dicyclohexylmethane diisocyanate, 4,4′-dicyclohexylpropane diisocyanate, 1,4-phenylene diisocyanate, 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, 4,4′-diphenylmethane diisocyanate, 2,2′- and 2,4′-diphenylmethane diisocyanate, tetramethylxylyl diisocyanate, p-xylylene diisocyanate, p-isopropylidene diisocyanate and mixtures of these compounds.
[0026] Component b) according to the invention may also comprise small amounts of higher-functionality polyisocyanates known per se from polyurethane chemistry or modified polyisocyanates containing, for example, carbodiimide groups, allophanate groups, isocyanurate groups, urethane groups and / or biuret groups.
[0027] As a preferred solution, the component b) of the present invention is selected from one or more of hexamethylene diisocyanate, isophorone diisocyanate, dicyclohexylmethane diisocyanate, diphenylmethane diisocyanate and toluene diisocyanate.
[0028] Component c) of the present invention includes one or more of dimethylolpropionic acid, dimethylolbutanoic acid, dimethylolacetic acid, dihydroxysuccinic acid, N-(2-aminoethyl)-2-aminoethanesulfonic acid, N-(3-aminopropyl)-2-aminoethanesulfonic acid and alkali metal salts, alkaline earth metal salts and / or ammonium salts thereof, preferably dimethylolpropionic acid.
[0029] The component d) of the present invention is selected from one or more of ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,4-butylene glycol, 1,3-butylene glycol, 2,3-butylene glycol, 1,5-pentanediol, 1,6-hexanediol, neopentyl glycol, 1,4-dihydroxycyclohexane, 1,4-dimethylolcyclohexane, 1,8-octanediol, 1,10-decanediol, 1,12-dodecanediol, neopentyl glycol, 1,4-cyclohexanediol, 1,4-cyclohexanedimethanol and 2-ethyl-1,3-hexanediol; preferably neopentyl glycol and / or diethylene glycol.
[0030] The component e) of the present invention is a volatile tertiary amine that can ionize component c), preferably triethylamine.
[0031] The component f) of the present invention is preferably a polyamine having a number average molecular weight of 60 to 500 g / mol, more preferably one or more of ethylenediamine, 1,2-diaminopropane, 1,4-diaminobutane, 1,6-hexanediamine, 2-methylpentane-1,5-diamine, isophoronediamine, 4,4-diaminodicyclohexylmethane, piperazine and diethylenetriamine; further preferably ethylenediamine and / or isophoronediamine.
[0032] The component g) of the present invention is a hydrazine compound containing at least one hydroxyl group, preferably a hydrazine derivative containing 1 to 2 hydroxyl groups, and particularly preferably 2-hydrazinoethanol.
[0033] The aqueous dispersion of polyurethane-polyurea according to the present invention has a solid content of 35 to 40 wt %, a pH value of preferably 6 to 10, and an average particle size of generally 80 to 300 nm.
[0034] The solvent used to prepare the polyurethane-polyurea dispersion was acetone.
[0035] The present invention also provides a method for preparing the above-mentioned polyurethane-polyurea aqueous dispersion, comprising the following steps: component a), component b), component c), and component d) are mixed and reacted at 60-90° C. for 1-3 hours, preferably 2 hours, cooled to 35-45° C., preferably 40° C., then component g) is added for reaction to obtain a prepolymer of terminal isocyanate, acetone is added, and then component e) is added for neutralization, component f) is added with water under high-speed stirring for dispersion to obtain a dispersion containing acetone, and the dispersion is decompressed to remove acetone to obtain a polyurethane-polyurea aqueous dispersion without solvent.
[0036] The invention provides a polyurethane-polyurea aqueous dispersion which has a softer hand feel, a smoother touch, higher alcohol rubbing resistance, higher wet friction resistance, higher tensile strength and elongation and can be used for the surface layer of synthetic leather by introducing semi-crystalline polyester polyol and 2-hydrazinoethanol and changing the reaction mode of 2-hydrazinoethanol.
[0037] The beneficial effects of the present invention are as follows: by using a semi-crystalline polyester polyol containing a certain amount of phthalic acid structure and 2-hydrazinoethanol, a polyurethane-polyurea aqueous dispersion for a polyurethane surface layer having excellent strength, elongation, hand feel and water resistance can be obtained. DETAILED DESCRIPTION
[0038] The following examples are further descriptions of the present invention. These examples merely list limited variations to more clearly explain the present invention and do not constitute limitations on the essential contents of the present invention.
[0039] Materials used:
[0040] Polyester polyol I: poly(1,4-butylene adipate-isophthalate), poly(adipate):isophthalic acid (mol) = 2.5:1, Mn = 2000, Wanhua Chemical;
[0041] Polyester polyol II: poly(1,4-butylene adipate-isophthalate), poly(adipate:isophthalic acid) (mol) = 9.5:1, Mn = 2000, Wanhua Chemical;
[0042] Polyester polyol III: poly(1,4-butylene adipate-isophthalate), poly(adipate):isophthalic acid (mol) = 5:1, Mn = 2000, Wanhua Chemical;
[0043] Polyester polyol IV: poly(1,4-butylene isophthalate), Mn=2000, Wanhua Chemical;
[0044] Polyester polyol V: poly(1,4-butylene adipate), Mn=2000, WHP-204, Wanhua Chemical;
[0045] Polyether polyol Ⅰ: Polyoxypropylene ether diol Mn=2000, C2020D, Wanhua Chemical,
[0046] Polyether polyol II: polyoxypropylene ether diol Mn=8000, C2080, Wanhua Chemical;
[0047] Hexamethylene diisocyanate HDI Wanhua Chemical;
[0048] Isophorone diisocyanate IPDI Wanhua Chemical;
[0049] Dimethylolpropionic acid DMPA Perstorp;
[0050] Neopentyl glycol NPG BASF;
[0051] Ethylenediamine EDA BASF;
[0052] Isophorone diamine IPDA Wanhua Chemical;
[0053] 2-Hydrazinoethanol Aladdin.
[0054] The determination methods of the parameters in the following examples are as follows:
[0055] (1) Average particle size: The polyurethane aqueous dispersion was diluted with water to a concentration of 0.5 wt % and measured using a Malvern Nano-ZS90;
[0056] (2) -NCO determination: The -NCO content in the polyurethane synthesis process was determined in accordance with the Chemical Industry Standard of the People's Republic of China "HG / T2409-92 Determination of Isocyanate Content in Polyurethane Prepolymers".
[0057] Example 1
[0058] Under nitrogen protection, 260g of dehydrated polyester polyol I, 4.2g of DMPA (component c), 1g of NPG (component d), 9.2g of HDI, and 46g of IPDI (component b) were added to a 1L four-necked round-bottom flask equipped with a nitrogen inlet and outlet, reacted at 80°C for 2h, and then cooled to 40°C. Then, 1.1g of 2-hydrazinoethanol (component g) was added to the four-necked flask, and the mixture was stirred at 80°C until -NCO reached 1.90wt%, cooled to 50°C, and 301.5g of acetone was added for dilution. The mixture was cooled to 35°C, 3.16 g of triethylamine (component e) was added for neutralization under stirring, the mixture was reacted for 10 min under stirring, and then 782.4 g of deionized water was added for dispersion under stirring at 1200 rpm within 10 min. After the dispersion was completed, an IPDA (component f) aqueous solution (8.8 g of IPDA was dissolved in 42 g of water) was added at 30°C and stirred for 10 min. The acetone was then separated by distillation to obtain a solvent-free polyurethane polyurea aqueous dispersion having a solid content of 30.2 wt % and an average particle size of 160 nm.
[0059] Example 2
[0060] Under nitrogen protection, 343g of dehydrated polyester polyol II, 28g of polyether polyol I (component a), 7.56g of DMPA (component c), 1.4g of NPG (component d), 18.9g of HDI, and 61.6g of IPDI (component b) were added to a 1L four-necked round-bottom flask equipped with a nitrogen inlet and outlet, reacted at 80°C for 2h, and then cooled to 40°C. Then, 4.76g of 2-hydrazinoethanol (component g) was added to the four-necked flask, and the mixture was stirred at 75°C until -NCO reached 1.22wt%, and then cooled to 50°C. 533 g of acetone was added to dilute the mixture, and the temperature was lowered to 35° C. 5.7 g of triethylamine (component e) was added to neutralize the mixture under stirring, and the mixture was reacted for 10 min under stirring. Then, 368 g of deionized water was added to disperse the mixture within 10 min under stirring at 1200 rpm. After the dispersion was completed, an IPDA (component f) aqueous solution (4.5 g of IPDA was dissolved in 42 g of water) was added at 30° C. and stirred for 10 min. The acetone was then separated by distillation to obtain a solvent-free polyurethane polyurea aqueous dispersion having a solid content of 30.1 wt % and an average particle size of 136 nm.
[0061] Example 3
[0062] Under nitrogen protection, 245g of dehydrated polyester polyol III, 20g of polyether polyol I (component a), 7g of DMPA (component c), 4.8g of DEG (component d), and 72g of IPDI (component b) were added to a 1L four-necked round-bottom flask equipped with a nitrogen inlet and outlet, reacted at 80°C for 2h, and then cooled to 40°C. Then, 0.4g of 2-hydrazinoethanol (component g) was added to the four-necked flask, and the mixture was stirred at 85°C until -NCO reached 2.05wt%, cooled to 50°C, 314g of acetone was added to dilute, and cooled to At 35°C, 5.28 g of triethylamine (component e) was added for neutralization under stirring, and the mixture was reacted for 10 min under stirring. Then, 840 g of deionized water was added for dispersion within 10 min under stirring at 1200 rpm. After the dispersion was completed, a mixed aqueous solution of IPDA and EDA (component f) (7.5 g of IPDA and 0.8 g of EDA dissolved in 42 g of water) was added at 30°C and stirred for 10 min. The acetone was then separated by distillation to obtain a solvent-free polyurethane polyurea aqueous dispersion having a solid content of 30.1 wt % and an average particle size of 123 nm.
[0063] Comparative Example 1
[0064] 1.5 g of diethylene glycol (DEG) was used to replace the 2-hydrazinoethanol in Example 1, and the rest was the same as in Example 3 to prepare a solvent-free polyurethane polyurea aqueous dispersion with a solid content of 30.1 wt % and an average particle size of 115 nm.
[0065] Comparative Example 2
[0066] The polyester polyol I in the formula of Example 1 was replaced by polyester polyol V, and the rest was the same as Example 1 to prepare a solvent-free polyurethane polyurea aqueous dispersion with a solid content of 30.2 wt % and an average particle size of 145 nm.
[0067] Comparative Example 3
[0068] Under nitrogen protection, 287g of dehydrated polyester polyol II, 84g of polyether polyol I (component a), 7.56g of DMPA (component c), 1.4g of NPG (component d), 18.9g of HDI, and 61.6g of IPDI (component b) were added to a 1L four-necked round-bottom flask equipped with a nitrogen inlet and outlet, reacted at 80°C for 2h, and then cooled to 40°C. Then, 4.76g of 2-hydrazinoethanol (component g) was added to the four-necked flask, and the mixture was stirred at 75°C until -NCO reached 1.18wt%, and then cooled to 50°C. 533 g of acetone was added for dilution, and the temperature was lowered to 35° C. 5.7 g of triethylamine (component e) was added for neutralization under stirring, and the mixture was reacted for 10 min under stirring, and then 368 g of deionized water was added for dispersion within 10 min under stirring at 1200 rpm. After the dispersion was completed, an IPDA (component f) aqueous solution (4.5 g of IPDA was dissolved in 42 g of water) was added at 30° C. and stirred for 10 min. The acetone was then separated by distillation to obtain a solvent-free polyurethane polyurea aqueous dispersion having a solid content of 30.3 wt % and an average particle size of 125 nm.
[0069] Comparative Example 4
[0070] The polyester polyol III in the formula of Example 3 was replaced by polyester polyol IV, and the rest was the same as Example 3 to prepare a solvent-free polyurethane polyurea aqueous dispersion with a solid content of 30.0 t% and an average particle size of 138 nm.
[0071] Test results:
[0072] The polyurethane polyurea water dispersion resins of the above examples and comparative examples were prepared into synthetic leather surface layers according to the formulation in Table 1 and the performance tests were carried out. The results are shown in Table 2:
[0073] Smoothness: Fold the finished leather in half and rub it, the smoothness is 1 to 5 points from low to high;
[0074] Feel: Rub the finished leather with your hands and rate it on a scale of 1 to 5 based on the soft and elastic feel;
[0075] Hot bonding: stick two finished leathers together, heat them in a 50℃ oven with a load of 3kg for 24 hours, separate the two leathers, and score the hot bonding from low to high according to the adhesion degree, from 1 to 5 points;
[0076] Wet friction: Martindale abrasion tester;
[0077] Alcohol rub resistance: color fastness tester.
[0078] Table 1 Polyurethane polyurea water dispersion resin configuration formula for preparing surface resin
[0079] Material Name Mass / g Polyurethane polyurea aqueous dispersion 100 Black paste, S19-LR20, Shiming 8 3248, Hangzhou Chongyao 2 CX-100, DSM 0.8 5289w, Slok 1
[0080] Table 2 Evaluation results of synthetic leather surface performance
[0081]
[0082]
[0083] It can be seen from Table 2 that, compared with the comparative example, the synthetic leather surface layer prepared in the embodiment has excellent smoothness, feel, hot stickiness, wet friction, alcohol resistance and other properties, and the overall comprehensive performance is better than that of the synthetic leather surface layer prepared in the comparative example.
[0084] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.
Claims
1. A polyurethane-polyurea aqueous dispersion, the raw materials for its preparation comprising the following components: a) a polyol with a functionality of 2 to 4, comprising not less than 80 wt% of a semi-crystalline polyester polyol, wherein the semi-crystalline polyester polyol is obtained by esterification of adipic acid, phthalic acid and a small molecule diol, wherein the molar ratio of adipic acid to phthalic acid is 2.1 to 10:1; and the small molecule diol is one or more of 1,4-butanediol and 1,6-hexanediol; b) isocyanates; c) a hydrophilic compound component, wherein the hydrophilic group of the hydrophilic compound comprises one or more of an ionic group and a potential ionic group, and the hydrophilic compound contains 2 to 3 groups reactive with NCO; d) a small molecule alcohol chain extender different from component a); e) a compound which ionizes component c); f) polyamines having an average molecular weight of less than 500 g / mol; g) 2-Hydrazinoethanol.
2. The polyurethane-polyurea aqueous dispersion according to claim 1, characterized in that The number average molecular weight of the component a) is 100-15000 and the functionality is 2-3.
3. The polyurethane-polyurea aqueous dispersion according to claim 1, characterized in that The number average molecular weight of the component a) is 300 to 10,000, and the functionality is 2.
4. The polyurethane-polyurea aqueous dispersion according to claim 1, characterized in that The number average molecular weight of the component a) is 400-8000.
5. The polyurethane-polyurea aqueous dispersion according to claim 1, characterized in that: The ionic groups in the c) hydrophilic compound component are carboxylate ions, the potential ionic groups are carboxyl groups, and the groups reactive with NCO are hydroxyl groups and / or amino groups.
6. The polyurethane-polyurea aqueous dispersion according to claim 1, characterized in that The semi-crystalline polyester polyol is esterified with 1,4-butanediol in a molar ratio of adipic acid to isophthalic acid of 2.1 to 10:1; the number average molecular weight is 1800 to 2200.
7. The polyurethane-polyurea aqueous dispersion according to claim 6, characterized in that The number average molecular weight of the semi-crystalline polyester polyol is 2000.
8. The polyurethane-polyurea aqueous dispersion according to claim 1, characterized in that In the component a), the polyol used together with the semi-crystalline polyester polyol is selected from one or more of polyester polyol, polycaprolactone polyol, polycarbonate polyol, polyoxypropylene ether diol and polytetramethylene glycol.
9. The polyurethane-polyurea aqueous dispersion according to claim 1, characterized in that: In the component a), the polyol used together with the semi-crystalline polyester polyol is a polyoxypropylene ether diol having a number average molecular weight of 2,000 to 8,000.
10. The polyurethane-polyurea aqueous dispersion according to claim 1, characterized in that: Component c) is dimethylolpropionic acid; and / or, component d) is selected from one or more of ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,4-butylene glycol, 1,3-butylene glycol, 2,3-butylene glycol, 1,5-pentanediol, 1,6-hexanediol, neopentyl glycol, 1,4-dihydroxycyclohexane, 1,4-dimethylolcyclohexane, 1,8-octanediol, 1,10-decanediol, 1,12-dodecanediol, neopentyl glycol, 1,4-cyclohexanediol, 1,4-cyclohexanedimethanol and 2-ethyl-1,3-hexanediol.
11. The polyurethane-polyurea aqueous dispersion according to claim 1, characterized in that: The component e) is triethylamine; and / or the component f) is selected from polyamines having a number average molecular weight of 60 to 500 g / mol.
12. The polyurethane-polyurea aqueous dispersion according to claim 11, characterized in that The component f) is selected from one or more of ethylenediamine, 1,2-diaminopropane, 1,4-diaminobutane, 1,6-hexanediamine, 2-methylpentane-1,5-diamine, isophoronediamine, 4,4-diaminodicyclohexylmethane, piperazine and diethylenetriamine.
13. A method for preparing a polyurethane-polyurea aqueous dispersion according to any one of claims 1 to 12, comprising the following steps: Component a), component b), component c) and component d) are mixed and reacted at 60-90° C. for 1-3 hours, cooled to 35-45° C., and then component g) is added to react to obtain a terminal isocyanate prepolymer, acetone is added, and then component e) is added for neutralization, and component f) water is added under high-speed stirring for dispersion to obtain a dispersion containing acetone, and the acetone is removed.
14. The method according to claim 13, characterized in that The reaction time was 2 h, and the temperature was lowered to 40°C.
15. Use of the polyurethane-polyurea aqueous dispersion according to any one of claims 1 to 12 or the polyurethane-polyurea aqueous dispersion prepared by the method according to claim 13 or 14, characterized in that: Used to prepare synthetic leather surface.
Citation Information
Patent Citations
A kind of waterborne polyurethane resin for synthetic leather fabric and preparation method thereof
CN105968309B
Aqueous polyurethane-polyurea dispersions
CN102083879A
Self-crosslinking polyurethane-polyurea aqueous dispersion and preparation method and application thereof
CN110294830A