A polyamide composite membrane containing anthracene-based monomer
By using anthracene-containing monomer and ultraviolet light irradiation technology in the polyamide composite film, the problem of insufficient boron removal performance in the prior art is solved, and polyamide composite with high throughput, high salt cutoff and high retention ability is achieved membrane.
Patent Information
- Application Number
- CN202211322626.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-27
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2042-10-27
AI Technical Summary
The existing polyamide composite films lack sufficient performance in removing trace boron from seawater, especially with high throughput and high salt cutoff, and the existing methods fail to achieve the expected removal performance. .
Polyamide composite films are prepared by interfacial polymerization using anthracene-containing monomers and processed under specific wavelengths of ultraviolet light to improve the crosslinking degree and retention ability of the film. The specific steps include applying a mixed solution of acid halide reactive monomer and polyfunctional amine monomer on the surface of the porous carrier, and then adding a polyfunctional acid halide monomer for interfacial polymerization to form a polyamide composite film, and irradiating under an ultraviolet light source. to promote the [4+4] photopolymerization reaction.
It has achieved a significant improvement in the desalination capacity and the interception performance of boron in neutral regions under the premise of slightly reducing flux, significantly improving the boron removal rate, while maintaining high throughput and high salinity cutoff.
Smart Images

Figure CN115738765B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of membrane technology and relates to a preparation method and application of a polyamide composite membrane which can achieve high flux and high salt rejection rate and has good interception ability for non-dissociated boron in neutral regions. Background Art
[0002] There are a variety of techniques for removing substances (e.g., salts) dissolved in solvents (e.g., water). Composite membranes with porous carriers coated with a "thin film" polyamide layer are currently the most common type of separation membrane, wherein the polyamide film is mainly obtained by interfacial polymerization of a polar solution containing a multifunctional amine (generally containing m-phenylenediamine, isophthaloyl triamine, piperazine, aliphatic amine, polyetheramine, etc.) and a non-polar solution containing a multifunctional acyl halide (generally containing trimesoyl chloride, isophthaloyl chloride, terephthaloyl chloride, etc.). Immiscible solutions containing the corresponding monomers are sequentially coated on the surface of a carrier (polyester + polysulfone) to obtain a reverse osmosis membrane (specifically refer to the method for preparing a reverse osmosis membrane disclosed in US Pat. No. 4,277,344 of Cadotte et al.). These membranes are widely used, for example, in the case of obtaining drinking water from seawater, alkaline water, water containing harmful substances, or in the manufacture of industrial ultrapure water, wastewater treatment, and the recovery of valuable substances.
[0003] Boron is toxic to humans, animals and plants, and can cause neurological damage and growth inhibition, etc. Therefore, the World Health Organization has increasingly stringent requirements for boron content in water. However, seawater contains a large amount of boron, so boron removal is important in seawater desalination, and the requirements for the performance of removing trace boron contained in seawater are becoming increasingly stringent. Therefore, various methods for improving the boron removal performance of composite semipermeable membranes have been proposed:
[0004] For example, Patent Document 1 (CN 102781560) reports a method for improving performance by increasing the temperature of interfacial polymerization reaction and heat treating the obtained polyamide composite membrane. Document 2 (ZHAI X, MENG J, LI R, et al.Hypochlorite treatment on thin film composite RO membrane to improve boron removal performance [J]. Desalination, 2011, 274 (1-3): 136-143.) also discloses a method for contacting a composite semipermeable membrane obtained by interfacial polymerization with an aqueous solution containing free chlorine. Document 3 (CHONG CY, LAU WJ, YUSOF N, et al. Studies on the properties of RO membranes for salt and boron removal: Influence of thermal treatment methods and rinsing treatmengs [J]. Desalination, 2018, 428: 218-226) reports a method for changing the type of organic solvent to improve the deboronization of polyamide composite membranes after interfacial polymerization;
[0005] When the membrane described in Patent Document 1 or Patent Document 2 is used to pass seawater at 25°C, pH 8, boron concentration 5 ppm, and TDS concentration 3.5 wt% under an operating pressure of 5.5 MPa, the membrane permeation flux is less than 36 LMH, and the boron removal rate is no more than about 95%. It is expected to develop a composite semipermeable membrane with higher boron rejection performance and higher flux. Although the composite semipermeable membrane prepared according to Document 3 can maintain the flux while improving the boron removal performance, it is far from reaching the expected goal. Summary of the invention
[0006] The purpose of the present invention is to provide a polyamide composite membrane and a preparation method thereof in view of the deficiencies in the prior art. The polyamide composite membrane of the present invention can achieve high flux and high salt rejection rate, and also has good interception ability for boron that does not dissociate in the neutral region.
[0007] In order to achieve the above-mentioned object of the invention, the present invention provides a method for preparing a polyamide composite film containing anthracene monomers, comprising the following steps:
[0008] (1) applying a mixed solution of an acyl halide reactive monomer and a multifunctional amine monomer to the surface of a porous support, and then applying a multifunctional acyl halide monomer to form a polyamide composite membrane through interfacial polymerization;
[0009] (2) Irradiating the prepared polyamide composite film under a purple light source with a specific wavelength.
[0010] In step (1) of the present invention, the acyl halide reactive monomer is as shown in formula (1):
[0011]
[0012] Wherein, R1 and R2 are independently selected from the group consisting of hydrogen, amino, hydroxyl, methoxy, carboxyl, ether, sulfate and sulfonic acid, and at least one of R1 and R2 is an amino group;
[0013] R3 and R4 are independently selected from the group consisting of hydrogen, hydroxyl, methoxy, carboxyl, ether, sulfonic acid, and sulfate. Preferably, at least one of R3 and R4 is hydrogen, and more preferably, R3 is hydrogen.
[0014] R5, R6, R7, and R8 are independently selected from the group consisting of hydrogen, hydroxyl, amino, methoxy, carboxyl, sulfonic acid, sulfate, and ether, and at least one of R5, R6, R7, and R8 is an amino group, preferably R5, R6, or R8 is an amino group;
[0015] More preferably, the acyl halide reactive monomer is 2,6-diaminoanthracene, 1,8-diaminoanthracene or 1,5-diaminoanthracene.
[0016] In step (1) of the present invention, the polyfunctional amine monomer is preferably m-phenylenediamine and / or p-phenylenediamine, more preferably m-phenylenediamine;
[0017] The molar ratio of the acyl halide reactive monomer to the multifunctional amine monomer is 1:100-2:1, more preferably 1:20-1:5;
[0018] In a specific embodiment, the mixed solution containing the acyl halide reactive monomer and the multifunctional amine monomer is prepared as follows: the multifunctional amine monomer is preferably dissolved in a polar solvent A, the polar solvent A is preferably methanol, water, etc., and water is more preferred in terms of cost and safety; the acyl halide reactive monomer is preferably dissolved in a solvent B, and the solvent B is N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMA) or N-methylpyrrolidone (NMP), wherein N-methylpyrrolidone (NMP) is more preferred; and then the two solutions are mixed. The mass ratio of solvent B to polar solvent A is preferably 1:4-1:200, and more preferably 1:20-1:100.
[0019] The porous carrier can be a polysulfone-based membrane formed on a non-woven fabric, polyethersulfone, polyphenylsulfone, polyphenylene sulfide, polyphenylene ether, polyphenylene sulfide sulfone, polyamide, polyimide, polyester, vinyl polymer, cellulose polymer, etc., wherein the vinyl polymer is selected from polyethylene, polypropylene, polyvinyl chloride, polyacrylonitrile, etc., and the cellulose polymer is selected from cellulose acetate, cellulose nitrate, etc., and can be a blend of one or more thereof. The application method on the surface of the porous carrier can be coating, soaking, spraying, etc.
[0020] The multifunctional acyl halide monomer is not particularly limited, and aromatic or alicyclic multifunctional acyl halide monomers and combinations thereof can be used. Non-limiting examples of aromatic multifunctional acyl halides include: trimesoyl chloride, terephthaloyl chloride, isophthaloyl chloride, biphenyl dicarboxylic acid chloride and phthaloyl dicarboxylic acid chloride. Non-limiting examples of alicyclic multifunctional acyl halides include: cyclopropane tricarboxylic acid chloride, cyclobutane tetracarboxylic acid chloride, cyclopentane tricarboxylic acid chloride, cyclopentane tetracarboxylic acid chloride, cyclohexane tricarboxylic acid chloride, cyclopentane dicarboxylic acid chloride, cyclobutane dicarboxylic acid chloride, cyclohexane dicarboxylic acid chloride and tetrahydrofuran dicarboxylic acid chloride. A preferred multifunctional acyl halide monomer is trimesoyl chloride (TMC);
[0021] The multifunctional acyl halide monomer is dissolved in a non-polar solvent, and the non-polar solvent (oil phase) is preferably a hydrocarbon solvent. Non-limiting examples of suitable hydrocarbon solvents include: paraffins (any one or a combination of at least two of n-hexane, octane, nonane, decane, etc.), isoparaffins (any one or a combination of at least two of Isopar E, Isopar G, Isopar L, etc.) and aromatics (any one or a combination of at least two of mesitylene, m-xylene, toluene, etc.), more preferably n-decane and Isopar G;
[0022] The concentration of the multifunctional acyl halide monomer in the hydrocarbon solvent is about 0.01 to 5% by weight, preferably 0.05 to 0.5% by weight.
[0023] The mass concentration ratio of the sum of the multifunctional amine monomer and the acyl halide reactive monomer in the mixed solution to the multifunctional acyl halide monomer in the hydrocarbon solvent is preferably 4:1 to 40:1.
[0024] Once the polar solution and the oil phase solution come into contact with each other, the multifunctional amine monomer and the acyl halide reactive monomer and the multifunctional acyl halide monomer undergo interfacial polymerization at the water-oil interface to form a polyamide membrane. The interfacial polymerization reaction temperature is 10-50°C, more preferably 20-30°C, and the interfacial polymerization reaction time can be less than one second, but the water-oil phase contact time is about 0.5-5 minutes, more preferably 0.5-2 minutes. Thereafter, the excess liquid can be removed by any method such as air knife, drying, hanging drop, drying, etc.
[0025] In order to promote the interfacial polymerization reaction, regulate the reaction rate and the performance of the composite membrane, the temperature of the water phase or oil phase involved in the reaction can be adjusted, and a phase transfer catalyst (such as dodecyltrimethylammonium chloride), an acid binding agent (such as sodium hydroxide, camphorsulfonic acid and triethylamine salt), a solubilizing agent (such as toluene), a complexing agent (such as phosphate compounds), a humectant (such as glycerol), etc. can be added.
[0026] In step (2) of the present invention, the polyamide composite film prepared in step (1) is irradiated by an ultraviolet light source. The wavelength of the ultraviolet light is 250-400nm, preferably 300-365nm. The irradiation time is 0.2-10 minutes, preferably 2-4 minutes.
[0027] In step (2) of the invention, when the acyl halide reactive monomers in the polymer network are exposed to ultraviolet light, the adjacent monomers can undergo a [4+4] photopolymerization reaction to form new covalent bonds, thereby increasing the crosslinking degree of the polymer. The reaction is shown in formula (2):
[0028] Formula (2):
[0029]
[0030] To further illustrate the structural changes of the polyamide composite film before and after ultraviolet irradiation in step (1), take Example 1,5-diaminoanthracene as an example, the polyamide partial structure thereof is shown in formula (3):
[0031]
[0032] After ultraviolet irradiation, the polyamide composite membrane can undergo intramolecular and intermolecular chain [4+4] cross-linking reactions or partial cross-linking, further improving the cross-linking degree of the polyamide composite membrane and enhancing the retention capacity of the composite membrane, especially the retention capacity for non-dissociated boron in the neutral region.
[0033] The polyamide composite film prepared by the present invention can optionally comprise hygroscopic polymer on at least a portion of its polyamide layer surface.Polymer comprises polymer surfactant, polyacrylic acid, polyvinyl acetate, polyalkylene oxide compound, poly-(oxazoline) compound, polyacrylamide and relevant reaction product, as those generally described in US 7815987, US7918349, US7905361 and US201 1 / 0220569.In some embodiments, these polymers can be blended and / or reacted, and can be coated from the same solution or otherwise applied to the polyamide layer surface, or apply successively.
[0034] The beneficial effects of the present invention are:
[0035] Introducing anthracene-containing acyl halide reactive monomers with large steric hindrance and capable of [4+4] photopolymerization into the aqueous phase can significantly improve the desalination capacity of the polyamide membrane while slightly reducing the flux of the membrane. It also has high rejection performance for non-dissociated boron in the neutral region. DETAILED DESCRIPTION
[0036] In order to better understand the technical solution of the present invention, the content of the present invention is further described below in conjunction with the embodiments, but the content of the present invention is not limited to the following embodiments.
[0037] 1. Sources and brands of main reagents in the embodiments and comparative examples:
[0038] Polysulfone, purchased from BASF, Germany, Ultrason S6010.
[0039] Nonwoven fabric, purchased from Zhejiang Qinglan Membrane Technology Co., Ltd., R80.
[0040] Polysulfone-based membrane, preparation method: dissolve polysulfone in N,N-dimethylformamide to prepare a solution with a solid content of 18%, use a 250-micron thick wet film preparation device to coat the polysulfone solution on the surface of the non-woven fabric, stay in the air for 4-5 seconds, soak the non-woven fabric in pure water at room temperature, and complete the phase inversion after soaking for 5 minutes. Soak the polysulfone-based membrane that has completed the phase inversion in pure water at room temperature, change the water every 2 hours, and after fully cleaning the residual solvent, cut it for use.
[0041] Unless otherwise specified, the other reagents were purchased from Shanghai Aladdin Biochemical Technology Co., Ltd. and were reagent-grade raw materials.
[0042] 2. Testing methods of polyamide membranes in embodiments and comparative examples:
[0043] Regarding the various properties of the polyamide composite membranes in the comparative examples and embodiments, the polyamide composite membranes were supplied with seawater (salt concentration of about 3.5%) at a temperature of 25°C and a pH adjusted to 7.0 at an operating pressure of 5.5 MPa for 24 hours, and the water quality of the permeate and supply water before and after the membrane was measured to obtain the various membrane properties:
[0044] Salt rejection rate calculation method:
[0045] Desalination rate (%) = 100 × {1-(salinity of permeate water / salinity of supply water)};
[0046] The calculation method of flux is:
[0047] The amount of water permeated through the membrane of the supply water (seawater) is converted into the amount of water permeated per square meter of membrane area per hour (cubic decimeter), and the membrane permeation flux (L / m 2 / h) indicates;
[0048] Calculation method of deboronization rate:
[0049] The boron concentration in the supply water and the permeate water was analyzed using an ICP emission analyzer (P-4010 manufactured by Hitachi, Ltd.), and the boron removal rate was calculated using the following formula:
[0050] Boron removal rate (%) = 100 × {1-(boron concentration in permeate water / boron concentration in feed water)}.
[0051] UV spectrum characterization method of polyamide film material: UV spectrum was tested by UV-3600 instrument made by Shimadzu to test the UV absorption spectrum of polyamide film at different irradiation times, and the absorption intensity was measured in the range of 350±5nm;
[0052] X = Abs(end) / Abs(initial)
[0053] Abs(end) is the ultraviolet absorption intensity measured at 350±5nm after the ultraviolet light source irradiation is completed, and Abs(initial) is the ultraviolet absorption intensity measured at 350±5nm when the ultraviolet light source is not irradiated.
[0054] Embodiment 1:
[0055] At 25°C, the cut polysulfone base membrane is attached to a frame, the frame size is a rectangle with a side length of 16*12cm;
[0056] First, 1,5-diaminoanthracene is dissolved in N-methylpyrrolidone, and then mixed with an aqueous solution containing m-phenylenediamine, camphorsulfonic acid, and triethylamine to obtain an aqueous phase solution, wherein the aqueous phase solution contains 0.5 wt% 1,5-diaminoanthracene, 5 wt% N-methylpyrrolidone, 4 wt% m-phenylenediamine, 6 wt% camphorsulfonic acid, and 3 wt% triethylamine;
[0057] The plate frame is immersed in the above-mentioned aqueous phase solution for 1 minute, and the excess aqueous phase is squeezed out with a rubber stick, and then the organic phase of n-decane containing 0.165wt% of trimesoyl chloride is poured onto the surface of the polysulfone-based membrane and reacted for 1 minute. At this time, the membrane surface temperature is controlled to 25°C, and then the excess solution on the membrane surface is removed with an air knife, followed by spraying with 1wt% sodium carbonate solution and pure water to remove the residual organic phase, and then washed in 90°C hot water for 2 minutes to obtain the target polyamide composite membrane, and the above-mentioned polyamide composite membrane is placed under an ultraviolet external light source (wavelength 365±10nm) for 25 seconds to obtain a polyamide composite membrane immersed in pure water for use. Subsequently, the prepared polyamide composite membrane was treated with a 0.3 wt% sodium nitrite aqueous solution with a pH of 2.2 adjusted with sulfuric acid at room temperature (25°C) for 1 minute. After the polyamide composite membrane was taken out from the sodium nitrite aqueous solution, the solution was drained and immersed in a 1 wt% sodium sulfite aqueous solution for 0.5 minutes. After the polyamide composite membrane was taken out from the sodium sulfite, it was placed in 90°C water for 2 minutes. The obtained polyamide composite membrane was tested, and the membrane flux, desalination rate and deboronization performance were the values shown in Table 2.
[0058] Embodiment 2-6:
[0059] The polyamide composite membrane used for treatment, the interface polymerization temperature, the monomer concentration and the ultraviolet light source irradiation time were changed as shown in Table 1, and the other operations were consistent with Example 1. The X value of the polyamide composite membrane of each example is shown in Table 2. After preparation, the membrane was immersed in pure water for standby use. The flux, salt rejection rate and boron removal performance of the prepared polyamide composite membrane are recorded in Table 2.
[0060] Comparative Example 1
[0061] At 25°C, the cut polysulfone-based membrane is attached to a plate frame, the size of the plate frame is a rectangle with a side length of 16*12cm, and the plate frame is immersed in an aqueous solution containing 4.5wt% m-phenylenediamine, 6wt% camphorsulfonic acid, and 3wt% triethylamine for 1 minute, and the excess aqueous solution on the surface is removed with a rubber stick, and then the organic phase of n-decane containing 0.165wt% trimesoyl chloride is poured onto the surface of the polysulfone-based membrane and reacted for 1 minute. At this time, the membrane surface temperature is controlled to 25°C, and then the excess solution on the membrane surface is removed with an air knife, followed by spraying with 1wt% sodium carbonate solution and pure water to remove the residual organic phase on the membrane surface, and then washing in 90°C hot water for 2 minutes to obtain a polyamide composite membrane immersed in pure water for standby use, and the subsequent treatment method is consistent with Example 1.
[0062] Comparative Example 2
[0063] The polyamide composite membrane used for treatment was changed as shown in Table 1. Other operations were the same as in Example 1. After preparation, the membrane was immersed in pure water for standby use. The flux, salt rejection rate and boron removal performance of the prepared polyamide composite membrane are recorded in Table 2.
[0064] Table 1
[0065]
[0066] Table 2
[0067] X Value Desalination rate / % Flux / LMH Boron removal rate / % Comparative Example 1 0 99.71 40.2 88.6 Comparative Example 2 0 99.72 38 89.5 Example 1 0.55 99.76 37 92 Example 2 0.7 99.72 38.2 90.8 Example 3 0.22 99.85 36 96.8 Example 4 0.55 99.8 37.4 93.2 Example 5 0.45 99.75 39.5 91.5 Example 6 0.38 99.8 38 94
Claims
1. A polyamide composite membrane, characterized in that: The monomers prepared contain a compound represented by formula (1): Wherein, the compound represented by formula (1) is selected from 2,6-diaminoanthracene, 1,8-diaminoanthracene or 1,5-diaminoanthracene; The preparation method of the polyamide composite film comprises the following steps: (1) applying a solution containing an acyl halide reactive monomer, a multifunctional amine monomer and a solution containing a multifunctional acyl halide monomer to the surface of a porous support, and forming a polyamide composite membrane by interfacial polymerization; (2) irradiating the prepared polyamide composite film under an ultraviolet light source with a specific wavelength; Wherein, the acyl halide reactive monomer is selected from 2,6-diaminoanthracene, 1,8-diaminoanthracene or 1,5-diaminoanthracene.
2. A method for preparing a polyamide composite film, comprising the following steps: (1) applying a solution containing an acyl halide reactive monomer, a multifunctional amine monomer and a solution containing a multifunctional acyl halide monomer to the surface of a porous support, and forming a polyamide composite membrane by interfacial polymerization; (2) irradiating the prepared polyamide composite film under an ultraviolet light source with a specific wavelength; Wherein, the acyl halide reactive monomer is 2,6-diaminoanthracene, 1,8-diaminoanthracene or 1,5-diaminoanthracene.
3. The preparation method according to claim 2, wherein The multifunctional amine monomer is selected from m-phenylenediamine and p-phenylenediamine.
4. The method according to claim 2 or 3, wherein: The molar ratio of the acyl halide reactive monomer to the multifunctional amine monomer is 1:100-2:
1.
5. The method according to claim 4, wherein: The molar ratio of the acyl halide reactive monomer to the multifunctional amine monomer is 1:20-1:
5.
6. The preparation method according to claim 2, wherein: The multifunctional acyl halide monomer is an aromatic or alicyclic multifunctional acyl halide monomer.
7. The preparation method according to claim 6, wherein: The multifunctional acyl halide monomer is trimesoyl chloride.
8. The preparation method according to claim 2, wherein: The interfacial polymerization reaction temperature is 10-50° C., and the interfacial polymerization reaction time is 0.5-5 minutes.
9. The preparation method according to claim 2, wherein: The interfacial polymerization reaction temperature is 20-30° C., and the interfacial polymerization reaction time is 0.5-2 minutes.
10. The preparation method according to claim 2, wherein: The wavelength of ultraviolet light is 250-400nm.
11. The preparation method according to claim 2, wherein: The wavelength of ultraviolet light is 300-365nm.
12. The preparation method according to any one of claims 2, 10-11, wherein: The irradiation time in step (2) is 0.2-10 minutes.