A manufacturing method for reducing the magnetic substance content of natural graphite negative electrode material

By using nitrogen protection and multiple magnetic separations during the processing of natural graphite, the problem of removing elemental Fe and ferric oxide from natural graphite has been solved, thereby reducing the content of magnetic materials and improving the safety of lithium-ion batteries.

CN115739394BActive Publication Date: 2024-11-15QINGDAO TEDA CHINA RESOURCES NEW ENERGY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211475920.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-23
Publication Date
2024-11-15
Estimated Expiration
2042-11-23

AI Technical Summary

Technical Problem

Existing technologies cannot effectively remove elemental Fe and ferric oxide produced by the presence of oxygen in natural graphite, making it difficult to reduce the content of magnetic materials and affecting the safety performance of lithium-ion batteries.

Method used

By employing nitrogen-protected conveying and high-temperature treatment, combined with multiple magnetic separation steps, and through a nitrogen circulation protection mechanism and a spiral conveying mechanism, the natural graphite is ensured not to be oxidized during processing, thereby improving the efficiency of electromagnetic iron removal.

Benefits of technology

It effectively reduces the magnetic content of natural graphite anode materials, improves the safety performance of lithium-ion batteries, prevents elemental iron from oxidizing to ferric oxide, and enhances the effect of electromagnetic iron removal.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115739394B_ABST
    Figure CN115739394B_ABST
Patent Text Reader

Abstract

The present invention provides a manufacturing method for reducing the content of magnetic substances in natural graphite negative electrode materials, and relates to the technical field of natural graphite. The method comprises the following steps: S1, after inspecting the natural graphite, putting it into an impurity removal device for air separation and impurity removal; S2, coarsely crushing, finely crushing, spheroidizing and purifying the natural graphite, and then performing the first magnetic separation; S3, coating and carbonizing operations after the first magnetic separation; S4, high-temperature treatment of the treated natural graphite under nitrogen protection, and then performing the second magnetic separation; S5, packaging and storing the obtained natural graphite. The present invention transports the natural graphite in a conveying device under nitrogen protection and performs high-temperature treatment, so as to avoid the presence of FeS in the natural graphite. The Fe element decomposed during the heating process and the iron element generated by equipment wear will not be oxidized to ferric oxide under nitrogen protection. During the second magnetic separation, it will be easily adsorbed and removed by the electromagnetic iron removal equipment, thereby achieving the effect of reducing the content of magnetic substances in the natural graphite negative electrode materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of natural graphite, and in particular to a manufacturing method for reducing the content of magnetic substances in natural graphite negative electrode materials. Background Art

[0002] The commercialization of negative electrode carbon materials for lithium-ion batteries has been widely used in 3C electronic portable products, new energy vehicles and other social fields because of its high energy density, long cycle, no memory effect and green environmental protection. The content of magnetic substances in negative electrode materials is one of the important factors affecting the safety of lithium-ion batteries. The content of magnetic foreign matter has become an important criterion for measuring the quality of negative electrode materials for lithium-ion batteries. When there are trace amounts of metal impurities in the negative electrode materials, especially magnetic substances, they will pierce the diaphragm inside the battery to form a micro short circuit, seriously affecting the safety performance of the battery.

[0003] For example, Chinese patent CN111446421A discloses a graphite negative electrode for a low-magnetic impurity lithium battery and a preparation method, comprising the following steps: step one, preparing powder; step two, adding a binder; step three, granulation treatment; step four, graphitization treatment; step five, demagnetization screening; step six, installing a collector; step seven, detection and recording, wherein in the above step one, the carbon material is placed in a crusher for crushing and filtering to obtain fine powder with an average particle size of 8-15um, the filtered particles are crushed and screened again, and then the treated fine powder is oxidized, and finally the powder is collected. This preparation method uses a magnetic material metal particle collector to adsorb magnetic impurities at the graphite negative electrode, so that the magnetic impurity content at the graphite negative electrode is controlled below 0.1PPM, and the morphology of metal foreign matter can be controlled by three-dimensional screen screening, so that the metal impurities in the finished product are close to zero, which increases the safety of battery application.

[0004] In the prior art, FeS exists in natural graphite. During the heating process, due to the presence of oxygen, it is first decomposed into Fe element. Carbon steel equipment is used in the processing of natural graphite. Due to the wear of the carbon steel equipment, when the spherical graphite is processed, the iron filings caused by the wear of the equipment exist in the form of iron element. During the carbonization and coating process, since the natural graphite is exposed to the air and the crucible is filled, there is a large amount of air. Due to the presence of oxygen, iron will be oxidized to ferric oxide during the carbonization process. Ferric oxide is weakly magnetic and is difficult to remove using electromagnetic iron removal equipment. Therefore, avoiding the reaction of the existing iron element in the early stage can effectively improve the efficiency of subsequent electromagnetic iron removal. Summary of the invention

[0005] The purpose of the present invention is to solve the problem of FeS existing in natural graphite. During the heating process, due to the presence of oxygen, it is first decomposed into Fe elemental substance. Carbon steel equipment is used in the processing of natural graphite. Due to the wear of the carbon steel equipment, when the spherical graphite stage is processed, the iron filings caused by the wear of the equipment exist in the form of iron elemental substance. During the carbonization coating process, since the natural graphite is exposed to the air and a filling crucible is filled, there is a large amount of air. Due to the presence of oxygen, iron will be oxidized into ferric oxide during the carbonization process. Ferric oxide is weakly magnetic and is difficult to remove using electromagnetic iron removal equipment. Therefore, avoiding the reaction of the existing iron elemental substance in the early stage can effectively improve the efficiency of subsequent electromagnetic iron removal.

[0006] In order to achieve the above object, the present invention adopts the following technical solution: a manufacturing method for reducing the magnetic substance content of natural graphite negative electrode material, the method comprising the following steps:

[0007] S1. After inspecting the natural graphite, put it into the impurity removal equipment for air separation and impurity removal;

[0008] S2, coarsely crushing, finely crushing, spheroidizing and purifying natural graphite and then subjecting it to first magnetic separation;

[0009] S3. After the first magnetic separation, coating and carbonization operations are performed; nitrogen atmosphere is used for pneumatic conveying before and after the coating and carbonization processes, and nitrogen atmosphere is used for protection during the coating and carbonization processes;

[0010] S4, subjecting the treated natural graphite to a second magnetic separation under nitrogen protection;

[0011] S5. Packing the obtained natural graphite and storing it in storage.

[0012] In step S4, the treated natural graphite is subjected to high temperature treatment under nitrogen protection, and then subjected to a second magnetic separation, which specifically includes the following steps:

[0013] S41, the carbonized natural graphite is transported in a conveying device under the protection of nitrogen and subjected to high temperature treatment;

[0014] S42, breaking up and mixing natural graphite;

[0015] S43, screening;

[0016] S44, performing a second magnetic separation.

[0017] Preferably, in step S2, the natural graphite is subjected to coarse crushing, fine crushing, spheroidization and purification, followed by the first magnetic separation, which specifically includes the following steps:

[0018] S21, coarsely crushing, finely crushing, spheroidizing and purifying natural graphite;

[0019] S22, classifying and purifying the crushed natural graphite;

[0020] S23, and then perform a drying process and then conduct a first magnetic separation.

[0021] Preferably, the conveying device in step S41 comprises a base plate and a storage bin, a spiral conveying mechanism is fixedly connected to the upper side of the base plate, a nitrogen circulation protection mechanism is fixedly installed on the upper side of the spiral conveying mechanism, the upper end of the nitrogen circulation protection mechanism is fixedly connected to the interior of the storage bin, a sealing mechanism is fixedly installed on one end of the spiral conveying mechanism, the nitrogen circulation protection mechanism comprises an air pressure pump, a first branch pipe is fixedly connected to the upper side of the air pressure pump, a first filter port is fixedly connected to the other end of the first branch pipe, a nitrogen pipe is fixedly connected to the outer surface of the first branch pipe, a second branch pipe is fixedly connected to the outer surface of the first branch pipe and located above the nitrogen pipe, a second filter port is fixedly connected to the other end of the second branch pipe, a conveying pipe is fixedly connected to the lower side of the air pressure pump, an inner groove is provided on the inner wall of the conveying pipe, a two-way pipe is fixedly connected to the inner wall of the inner groove, an output pipe is fixedly connected to the middle of the two-way pipe, and the other end of the output pipe is fixedly connected to the output end of the air pressure pump.

[0022] Preferably, a fixing clamp is fixedly connected to the outer side of the outlet of the delivery pipe, a side plate is fixedly connected to the upper side of the fixing clamp, and an upper cover is fixedly connected to the upper side of the side plate.

[0023] Preferably, a hydraulic cylinder is fixedly mounted on the lower side of the upper cover, a baffle is rotatably connected to the lower end of the movable rod of the hydraulic cylinder, and one side of the baffle is rotatably connected to one side of the fixing clamp.

[0024] Preferably, a base is fixedly connected to the lower outer portion of the conveying pipe, a feed bin is fixedly connected to the upper side of the conveying pipe, and a threaded push rod is rotatably connected to the inner wall of the conveying pipe.

[0025] Preferably, a connecting shaft is rotatably connected to the interior of the feeding bin, and a stirring fan is fixedly installed in the middle of the outer surface of the connecting shaft and in the inner cavity of the feeding bin.

[0026] Preferably, a second driven gear is fixedly installed in the middle of the outer surface of the stirring fan, a connecting block is rotatably connected to the outer surface of the stirring fan, a sleeve shaft is rotatably connected to the inside of the connecting block, a first driven gear is fixedly installed on the outer surface of the sleeve shaft, and the outer side of the first driven gear is meshingly connected to the outer side of the second driven gear.

[0027] Preferably, one end of the sleeve shaft is fixedly mounted to one end of the threaded push rod, and a driven pulley is fixedly mounted on the outer side of the other end of the sleeve shaft.

[0028] Preferably, a belt is movably connected to the outer side of the driven pulley, and a driving pulley is movably connected to the inner side of the other end of the belt. A servo motor is fixedly installed in the middle of the driving pulley, and the lower side of the servo motor is fixedly connected to the upper side of the base plate.

[0029] Compared with the prior art, the advantages and positive effects of the present invention are:

[0030] 1. In the present invention, natural graphite is transported in a conveying device under the protection of nitrogen and subjected to high-temperature treatment, so as to avoid the presence of FeS in natural graphite. The Fe element decomposed during the heating process and the iron element produced by equipment wear will not be oxidized to ferric oxide under the protection of nitrogen. During the second magnetic separation, it will be easily adsorbed and removed by the electromagnetic iron removal equipment, thereby achieving the effect of reducing the content of magnetic substances in the natural graphite negative electrode material.

[0031] 2. In the present invention, by setting a nitrogen circulation protection mechanism, natural graphite is protected by nitrogen, iron element is prevented from being reacted, and the efficiency of subsequent electromagnetic iron removal is improved. The carbonized natural graphite is placed in a storage bin, and the air pressure pump is started at this time. The air pressure pump generates suction to extract gas in the first branch pipe and the second branch pipe, and the first filter port and the second filter port connected to the first branch pipe and the second branch pipe ports respectively extract air from the upper and lower parts of the storage bin and merge into the first branch pipe. At the same time, the nitrogen pipe is connected to the nitrogen source, and the nitrogen is gathered in the first branch pipe. After being pressurized by the air pressure pump, the nitrogen enters the output pipe, and after being distributed to both sides through the two-way pipe, a part of the nitrogen flows to the left in the delivery pipe and a part flows to the right. The nitrogen to the left is returned to the lower part of the storage bin from the left end of the delivery pipe, so as to achieve a circulation flow of a part of the nitrogen to protect the natural graphite in delivery, and the nitrogen to the right prevents the air at the outlet end of the delivery pipe from entering and affecting the high-temperature treatment of the natural graphite.

[0032] 3. In the present invention, by setting a spiral conveying mechanism, the natural graphite can be transported in small quantities, the contact surface with nitrogen can be increased, more air can be excluded, and the subsequent iron removal is convenient. After the nitrogen circulates for a period of time, the servo motor is started, and the servo motor drives the driving pulley to rotate. When the driving pulley drives the belt to rotate, the driven pulley obtains power to drive the sleeve shaft to rotate, and the sleeve shaft simultaneously drives the first driven gear and the threaded push rod to rotate, the first driven gear meshes with the second driven gear to rotate, and the second driven gear drives the connecting shaft to rotate inside the connecting block and the feeding bin, and the stirring fan is driven by the connecting shaft to break up the natural graphite in the storage bin, so that the nitrogen can fully contact the natural graphite, so that the natural graphite is effectively protected by nitrogen, and the threaded push rod rotates in the conveying pipe, and the natural graphite protected by nitrogen is moved and transported in the conveying pipe, the hydraulic cylinder works, the movable rod part is extended, and the baffle is pushed to rotate around the connection point with the fixed clamp, thereby the port of the conveying pipe is opened, and the natural graphite after high temperature treatment is transferred out. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 A schematic flow chart of a manufacturing method for reducing the magnetic substance content of natural graphite negative electrode materials proposed by the present invention;

[0034] Figure 2 A schematic diagram of the first perspective structure of a conveying device in a manufacturing method for reducing the magnetic substance content of a natural graphite negative electrode material proposed by the present invention;

[0035] Figure 3 A schematic structural diagram from a second perspective of a conveying device in a manufacturing method for reducing the magnetic substance content of a natural graphite negative electrode material proposed by the present invention;

[0036] Figure 4 A schematic diagram of the structure inside the spiral conveying mechanism of a conveying device in a manufacturing method for reducing the magnetic substance content of natural graphite negative electrode materials proposed by the present invention;

[0037] Figure 5 The present invention provides a structural schematic diagram of the power part of the spiral conveying mechanism of the conveying device in a manufacturing method for reducing the magnetic substance content of natural graphite negative electrode materials;

[0038] Figure 6 A structural schematic diagram of a sealing mechanism of a conveying device in a manufacturing method for reducing the magnetic substance content of a natural graphite negative electrode material proposed by the present invention;

[0039] Figure 7 A schematic diagram of the structure inside the nitrogen circulation protection mechanism of the conveying device in the manufacturing method for reducing the magnetic substance content of the natural graphite negative electrode material proposed by the present invention;

[0040] Figure 8 for Figure 7 Schematic diagram of the structure enlarged at point A in the middle.

[0041] Legend: 1. Bottom plate; 2. Screw conveying mechanism; 21. Base; 22. Threaded push rod; 23. Conveying pipe; 24. Coupling; 25. Stirring fan; 26. Feeding bin; 27. Second driven gear; 28. Connecting block; 29. ​​First driven gear; 210. Belt; 211. Driven pulley; 212. Sleeve shaft; 213. Driving pulley; 214. Servo motor; 3. Storage bin; 4. Nitrogen circulation protection mechanism; 41. First filter port; 42. First branch pipe; 43. Nitrogen connecting pipe; 44. Second branch pipe; 45. Second filter port; 46. Air pressure pump; 47. Output pipe; 48. Two-way pipe; 49. Inner tank; 5. Sealing mechanism; 51. Upper cover; 52. Hydraulic cylinder; 53. Side plate; 54. Baffle; 55. Fixing clamp. DETAILED DESCRIPTION

[0042] In order to more clearly understand the above-mentioned purpose, features and advantages of the present invention, the present invention is further described below in conjunction with the accompanying drawings and embodiments. It should be noted that the embodiments of the present application and the features in the embodiments can be combined with each other without conflict.

[0043] In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention may also be implemented in other ways than those described herein. Therefore, the present invention is not limited to the specific embodiments of the following disclosure.

[0044] Example 1

[0045] like Figure 1-8 As shown, the present invention provides a method for reducing the content of magnetic substances in natural graphite negative electrode materials, the method comprising the following steps:

[0046] Step 1: After inspecting the natural graphite, put it into the impurity removal equipment for air separation and impurity removal;

[0047] Step 2: The natural graphite is subjected to coarse crushing, fine crushing, spheroidization and purification and then subjected to the first magnetic separation, which specifically includes the following steps:

[0048] 21) Coarsely crushing, finely crushing, spheroidizing and purifying natural graphite;

[0049] 22) Classifying and purifying the crushed natural graphite;

[0050] 23) After drying, the first magnetic separation is performed;

[0051] Step 3: After the first magnetic separation, coating and carbonization operations are performed; nitrogen atmosphere is used for pneumatic conveying before and after the coating and carbonization processes, and nitrogen atmosphere is used for coating and carbonization processes;

[0052] Step 4: The treated natural graphite is subjected to high temperature treatment under nitrogen protection, and then subjected to a second magnetic separation, which specifically includes the following steps:

[0053] 41) The carbonized natural graphite is transported in a conveying device under the protection of nitrogen and subjected to high temperature treatment;

[0054] 42) Break up and mix the natural graphite;

[0055] 43) screening;

[0056] 44) performing a second magnetic separation;

[0057] Step 5: Pack the obtained natural graphite and store it in warehouse.

[0058] By transporting natural graphite in a conveying device under the protection of nitrogen and subjecting it to high-temperature treatment, it is avoided that the Fe element decomposed by FeS in the natural graphite during the heating process and the iron element produced by equipment wear will not be oxidized to ferric oxide under the protection of nitrogen. During the second magnetic separation, it will be easily adsorbed and removed by the electromagnetic iron removal equipment, thereby achieving the effect of reducing the content of magnetic substances in the natural graphite negative electrode material.

[0059] Example 2

[0060] like Figure 1-8 As shown, the conveying device in step S41 includes a base plate 1 and a storage bin 3, a screw conveying mechanism 2 is fixedly connected to the upper side of the base plate 1, a nitrogen circulation protection mechanism 4 is fixedly installed on the upper side of the screw conveying mechanism 2, the upper end of the nitrogen circulation protection mechanism 4 is fixedly connected to the interior of the storage bin 3, a sealing mechanism 5 is fixedly installed at one end of the screw conveying mechanism 2, the nitrogen circulation protection mechanism 4 includes an air pressure pump 46, a first branch pipe 42 is fixedly connected to the upper side of the air pressure pump 46, a first filter port 41 is fixedly connected to the other end of the first branch pipe 42, a nitrogen connecting pipe 43 is fixedly connected to the outer surface of the first branch pipe 42, a second branch pipe 44 is fixedly connected to the outer surface of the first branch pipe 42 and located above the nitrogen connecting pipe 43, and the first branch pipe 45 is fixedly connected to the outer surface of the first branch pipe 42. The other end of the two branch pipes 44 is fixedly connected with the second filter port 45, the lower side of the air pressure pump 46 is fixedly connected with the delivery pipe 23, the inner wall of the delivery pipe 23 is provided with an inner groove 49, the inner wall of the inner groove 49 is fixedly connected with a two-way pipe 48, the middle part of the two-way pipe 48 is fixedly connected with an output pipe 47, the other end of the output pipe 47 is fixedly connected to the output end of the air pressure pump 46, a fixing clamp 55 is fixedly connected to the outer side of the outlet of the delivery pipe 23, the upper side of the fixing clamp 55 is fixedly connected with a side plate 53, the upper side of the side plate 53 is fixedly connected with an upper cover 51, the lower side of the upper cover 51 is fixedly installed with a hydraulic cylinder 52, the lower end of the movable rod of the hydraulic cylinder 52 is rotatably connected with a baffle 54, and one side of the baffle 54 is rotatably connected to one side of the fixing clamp 55

[0061] By setting the nitrogen circulation protection mechanism 4, the natural graphite is protected by nitrogen to avoid the reaction of the iron element, and the efficiency of subsequent electromagnetic iron removal is improved. The carbonized natural graphite is placed in the storage bin 3, and the air pressure pump 46 is started at this time. The air pressure pump 46 generates suction to extract the gas in the first branch pipe 42 and the second branch pipe 44. The first filter port 41 and the second filter port 45 connected to the ports of the first branch pipe 42 and the second branch pipe 44 respectively extract the air in the upper and lower parts of the storage bin 3 and merge them into the first branch pipe 42. At the same time, the nitrogen pipe 43 is connected to the nitrogen source, and the nitrogen is gathered in the first branch pipe 42. After being pressurized by the air pressure pump 46, the nitrogen enters the output pipe 47. After being distributed to both sides through the two-way pipe 48, part of the nitrogen goes to the left in the delivery pipe 23, and part goes to the right. The nitrogen going to the left returns from the left end of the delivery pipe 23 to the lower part of the storage bin 3, thereby achieving a circulation flow of part of the nitrogen to protect the natural graphite being transported, and the nitrogen going to the right prevents the air from entering the outlet end of the delivery pipe 23 to affect the high-temperature treatment of the natural graphite.

[0062] Example 3

[0063] like Figure 1-8 As shown, the lower outer portion of the conveying pipe 23 is fixedly connected to the base 21, the upper side of the conveying pipe 23 is fixedly connected to the feeding bin 26, the inner wall of the conveying pipe 23 is rotatably connected to the threaded push rod 22, the inside of the feeding bin 26 is rotatably connected to the connecting shaft 24, the middle of the outer surface of the connecting shaft 24 and the inner cavity of the feeding bin 26 are fixedly installed with a stirring fan 25, the middle of the outer surface of the stirring fan 25 is fixedly installed with a second driven gear 27, the outer surface of the stirring fan 25 is rotatably connected to a connecting block 28, the inside of the connecting block 28 is rotatably connected to a sleeve shaft 212, and the sleeve shaft 212 is fixedly installed with a second driven gear 27. A first driven gear 29 is fixedly mounted on the outer surface of the first driven gear 29, the outer side of the first driven gear 29 is meshedly connected with the outer side of the second driven gear 27, one end of the sleeve shaft 212 is fixedly mounted on one end of the threaded push rod 22, a driven pulley 211 is fixedly mounted on the outer side of the other end of the sleeve shaft 212, a belt 210 is movably connected to the outer side of the driven pulley 211, a driving pulley 213 is movably connected to the inner side of the other end of the belt 210, a servo motor 214 is fixedly mounted on the middle part of the driving pulley 213, and the lower side of the servo motor 214 is fixedly connected to the upper side of the base plate 1.

[0064] By setting up the spiral conveying mechanism 2, it is possible to transport the natural graphite in small quantities, increase the contact surface with the nitrogen, and remove more air, which is convenient for subsequent iron removal. After the nitrogen circulates for a period of time, the servo motor 214 is started, and the servo motor 214 drives the driving pulley 213 to rotate. When the driving pulley 213 drives the belt 210 to rotate, the driven pulley 211 obtains power to drive the sleeve shaft 212 to rotate. The sleeve shaft 212 simultaneously drives the first driven gear 29 and the threaded push rod 22 to rotate. The first driven gear 29 meshes with the second driven gear 27 to rotate, and the second driven gear 27 is driven to rotate. 27 drives the connecting shaft 24 to rotate inside the connecting block 28 and the feeding bin 26, and the stirring fan 25 is driven by the connecting shaft 24 to break up the natural graphite in the storage bin 3, so that the nitrogen can fully contact the natural graphite, so that the natural graphite is effectively protected by the nitrogen. The threaded push rod 22 rotates in the conveying pipe 23, and the natural graphite protected by nitrogen is moved and conveyed in the conveying pipe 23. The hydraulic cylinder 52 works, and the movable rod part is extended to push the baffle 54 to rotate around the connection point with the fixed clamp 55, so that the port of the conveying pipe 23 is opened, and the natural graphite after high-temperature treatment is transferred out.

[0065] The method of use and working principle of the device are as follows: natural graphite is placed in the storage bin 3, and the air pressure pump 46 is started at this time. The air pressure pump 46 generates suction to extract the gas in the first branch pipe 42 and the second branch pipe 44, and the first filter port 41 and the second filter port 45 connected to the ports of the first branch pipe 42 and the second branch pipe 44 respectively extract the air in the upper and lower parts of the storage bin 3 and merge into the first branch pipe 42. At the same time, the nitrogen pipe 43 is connected to the nitrogen source, and the nitrogen is gathered in the first branch pipe 42. After being pressurized by the air pressure pump 46, the nitrogen enters the output pipe 47, and after being distributed to both sides through the two-way pipe 48, part of the nitrogen flows to the left in the conveying pipe 23, and part flows to the right. The nitrogen to the left is returned from the left end of the conveying pipe 23 to the lower part of the storage bin 3, so as to achieve a circulation flow of part of the nitrogen to protect the natural graphite in conveying, and the nitrogen to the right prevents the air at the outlet end of the conveying pipe 23 from entering and affecting the high-temperature treatment of the natural graphite. After the nitrogen circulates for a period of time, the servo is started. The motor 214 and the servo motor 214 drive the driving pulley 213 to rotate. When the driving pulley 213 drives the belt 210 to rotate, the driven pulley 211 obtains power to drive the sleeve shaft 212 to rotate. The sleeve shaft 212 simultaneously drives the first driven gear 29 and the threaded push rod 22 to rotate. The first driven gear 29 engages with the second driven gear 27 to rotate. The second driven gear 27 drives the connecting shaft 24 to rotate inside the connecting block 28 and the feeding bin 26. The stirring fan 25 is driven by the connecting shaft 24 to break up the natural graphite in the storage bin 3, so that the nitrogen can fully contact the natural graphite, so that the natural graphite is effectively protected by the nitrogen. The threaded push rod 22 rotates in the conveying pipe 23, and the natural graphite protected by the nitrogen is moved and conveyed in the conveying pipe 23. The hydraulic cylinder 52 works, and the movable rod part is extended to push the baffle 54 to rotate around the connection point with the fixing clamp 55, so that the port of the conveying pipe 23 is opened, and the natural graphite after high temperature treatment is transferred out.

[0066] The above description is only a preferred embodiment of the present invention and does not limit the present invention in other forms. Any technician familiar with the profession may use the technical content disclosed above to change or modify it into an equivalent embodiment with equivalent changes and apply it to other fields. However, any simple modification, equivalent change and modification made to the above embodiment based on the technical essence of the present invention without departing from the content of the technical solution of the present invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. A method for reducing the content of magnetic substances in natural graphite negative electrode materials, characterized in that: The method comprises the following steps: S1. After inspecting the natural graphite, put it into the impurity removal equipment for air separation and impurity removal; S2, coarsely crushing, finely crushing, spheroidizing and purifying natural graphite and then subjecting it to first magnetic separation; S3. The natural graphite after the first magnetic separation is coated and carbonized; the pneumatic conveying before and after the coating and carbonization process is protected by nitrogen atmosphere, and the coating and carbonization process is protected by nitrogen atmosphere; S4, subjecting the treated natural graphite to a second magnetic separation under nitrogen protection; S5, packaging the obtained natural graphite and storing it in warehouse; In step S4, the treated natural graphite is subjected to high temperature treatment under nitrogen protection, and then subjected to a second magnetic separation, which specifically includes the following steps: S41, the carbonized natural graphite is transported in a conveying device under the protection of nitrogen and subjected to high temperature treatment; S42, breaking up and mixing natural graphite; S43, screening; S44, performing a second magnetic separation; The conveying device in step S41 comprises a bottom plate (1) and a storage bin (3), wherein a screw conveying mechanism (2) is fixedly connected to the upper side of the bottom plate (1), a nitrogen circulation protection mechanism (4) is fixedly installed on the upper side of the screw conveying mechanism (2), the upper end of the nitrogen circulation protection mechanism (4) is fixedly connected to the interior of the storage bin (3), a sealing mechanism (5) is fixedly installed on one end of the screw conveying mechanism (2), the nitrogen circulation protection mechanism (4) comprises an air pressure pump (46), a first branch pipe (42) is fixedly connected to the upper side of the air pressure pump (46), the other end of the first branch pipe (42) is fixedly connected to a first filter port (41), and the first branch pipe (42) is fixedly connected to the first filter port (41). A nitrogen connecting pipe (43) is fixedly connected to the outer surface of a branch pipe (42); a second branch pipe (44) is fixedly connected to the outer surface of the first branch pipe (42) and located above the nitrogen connecting pipe (43); a second filter port (45) is fixedly connected to the other end of the second branch pipe (44); a delivery pipe (23) is fixedly connected to the lower side of the air pressure pump (46); an inner groove (49) is formed on the inner wall of the delivery pipe (23); a two-way pipe (48) is fixedly connected to the inner wall of the inner groove (49); an output pipe (47) is fixedly connected to the middle of the two-way pipe (48); and the other end of the output pipe (47) is fixedly connected to the output end of the air pressure pump (46).

2. A method for reducing the magnetic substance content of natural graphite negative electrode material according to claim 1, characterized in that: In the step S2, the natural graphite is subjected to coarse crushing, fine crushing, spheroidization and purification and then subjected to the first magnetic separation, which specifically includes the following steps: S21, coarsely crushing, finely crushing, spheroidizing and purifying natural graphite; S22, classifying and purifying the finely crushed and spheroidized natural graphite; S23, and then perform a drying process and then conduct a first magnetic separation.

3. A method for reducing the magnetic substance content of natural graphite negative electrode material according to claim 1, characterized in that: A fixing clamp (55) is fixedly connected to the outside of the outlet of the delivery pipe (23), a side plate (53) is fixedly connected to the upper side of the fixing clamp (55), and an upper cover (51) is fixedly connected to the upper side of the side plate (53).

4. A method for reducing the magnetic substance content of natural graphite negative electrode material according to claim 3, characterized in that: A hydraulic cylinder (52) is fixedly mounted on the lower side of the upper cover (51), a baffle (54) is rotatably connected to the lower end of a movable rod of the hydraulic cylinder (52), and one side of the baffle (54) is rotatably connected to one side of the fixing clamp (55).

5. A method for reducing the magnetic substance content of natural graphite negative electrode material according to claim 4, characterized in that: The lower outer portion of the delivery pipe (23) is fixedly connected to a base (21), the upper side of the delivery pipe (23) is fixedly connected to a material feeding bin (26), and the inner wall of the delivery pipe (23) is rotatably connected to a threaded push rod (22).

6. A method for reducing the magnetic substance content of natural graphite negative electrode material according to claim 5, characterized in that: The interior of the feeding bin (26) is rotatably connected to a connecting shaft (24), and a stirring fan (25) is fixedly mounted in the middle of the outer surface of the connecting shaft (24) and located in the inner cavity of the feeding bin (26).

7. A method for reducing the magnetic substance content of natural graphite negative electrode material according to claim 6, characterized in that: A second driven gear (27) is fixedly mounted on the middle of the outer surface of the stirring fan (25); a connecting block (28) is rotatably connected to the outer surface of the stirring fan (25); a sleeve shaft (212) is rotatably connected to the interior of the connecting block (28); a first driven gear (29) is fixedly mounted on the outer surface of the sleeve shaft (212); and the outer side of the first driven gear (29) is meshingly connected to the outer side of the second driven gear (27).

8. A method for reducing the magnetic substance content of natural graphite negative electrode material according to claim 7, characterized in that: One end of the sleeve shaft (212) is fixedly mounted to one end of the threaded push rod (22), and a driven pulley (211) is fixedly mounted on the outside of the other end of the sleeve shaft (212).

9. A method for reducing the magnetic substance content of natural graphite negative electrode material according to claim 8, characterized in that: The outer side of the driven pulley (211) is movably connected to a belt (210), the inner side of the other end of the belt (210) is movably connected to a driving pulley (213), a servo motor (214) is fixedly mounted in the middle of the driving pulley (213), and the lower side of the servo motor (214) is fixedly connected to the upper side of the bottom plate (1).